Graphitization furnace and battery production system
By adjusting the electrode distance and size in the graphitization furnace, a uniform electric field is formed, which solves the problem of uneven distribution of electric field intensity, improves the quality and consistency of graphitized products, and meets the high-performance needs of battery anode materials.
Patent Information
- Application Number
- CN202310484921.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-10-29
AI Technical Summary
In existing graphitization furnaces, the electric field intensity is unevenly distributed during the graphitization process, resulting in inconsistent quality of graphitized products and affecting the performance of battery anode materials.
Design a graphitization furnace in which a first electrode and a ring-shaped electrode part are arranged in the furnace body. By adjusting the distance and size of the first electrode and the ring-shaped electrode part, a uniform electric field intensity distribution is formed to uniformly heat the material and improve the quality of the graphitized product. quality.
Through uniform electric field heating, the consistency and quality of graphitized products are improved, meeting the high performance requirements of battery anode materials and reducing the chance of material clogging.
Smart Images

Figure CN118856871A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of industrial equipment, and in particular to a graphitization furnace and a battery production system. Background Art
[0002] With the rapid development of energy technology, batteries have become an indispensable part of human life. At present, carbon materials are widely used in the negative electrode materials of batteries. Among them, graphitized carbon materials (also known as graphite materials) have been widely used in commercial applications due to their long service life, stable structure and low cost.
[0003] The graphitization furnace is a device that can generate graphite materials. The quality of the graphitized products generated by it is extremely important for the production and manufacturing of batteries. In view of this, how to improve the quality of graphitized products is a technical problem that needs to be solved urgently. Summary of the invention
[0004] The embodiments of the present application provide a graphitization furnace and a battery production system, which can improve the quality of graphitized products.
[0005] In a first aspect, a graphitization furnace is provided, comprising: a furnace body, wherein a material channel is arranged in the furnace body; a first electrode, wherein at least a portion of the first electrode is located in the material channel; a second electrode having a polarity opposite to that of the first electrode, comprising an annular electrode portion, wherein the annular electrode portion is protruded from an inner wall of the material channel along a radial direction of the material channel and surrounds a partial channel section of the material channel; along an extension direction of the material channel, a distance between an end face of the first electrode and a first plane is H1, an inner diameter of the annular electrode portion is D1, and H1 and D1 satisfy: 0.4≤H1 / D1≤5; wherein the first plane is a plane where a surface of the annular electrode portion facing the first electrode is located.
[0006] Through the technical solution of the embodiment of the present application, the distance H1 between the end face of the first electrode 220 and the first plane and the inner diameter D1 of the annular electrode portion satisfy 0.5≤H1 / D1≤5, so that an electric field with a relatively uniform electric field strength distribution can be formed between the end face 221 of the first electrode 220 and the surface of the end face 221 of the annular electrode portion 231 facing the first electrode 220, so as to uniformly heat the material passing through the electric field, which is beneficial to improving the consistency of the graphitized product, thereby improving the quality of the graphitized product.
[0007] In some possible implementations, H1 and D1 satisfy: 0.8≤H1 / D1≤1.5.
[0008] After a large number of experimental verifications, when H1 and D1 satisfy 0.8≤H1 / D1≤1.5, the quality of graphitized products can be further improved.
[0009] In some possible implementations, the value range of H1 is 350-3000 mm.
[0010] After a large number of experimental verifications, H1 in the range of 350 to 3000 mm is conducive to forming a more concentrated electric field and is not prone to material blockage.
[0011] In some possible implementations, the value range of D1 is 430-2400 mm.
[0012] After a large number of experimental verifications, D1 in the range of 430 to 2400 mm is conducive to forming a more concentrated electric field and is not prone to material blockage.
[0013] In some possible implementations, the outer diameter of the annular electrode portion is D2, and D1 and D2 satisfy: 1.17≤D2 / D1≤3.
[0014] In the above embodiment, the outer diameter D2 and the inner diameter D1 of the annular electrode portion satisfy 1.17≤D2 / D1≤3, which can not only make the electric field reach the temperature required for the graphitization process, but also make the graphitization path length moderate. The material is heated for a sufficient time, and the pores of the graphitized product can be repaired to an acceptable level, thereby improving the quality of the graphitized product.
[0015] In some possible implementations, D1 and D2 satisfy: 1.24≤D2 / D1≤2.51.
[0016] After a large number of experimental verifications, when D1 and D2 satisfy 1.24≤D2 / D1≤2.51, the quality of graphitized products can be further improved.
[0017] In some possible implementations, the value range of D2 is 580-2750 mm.
[0018] After a large number of experimental verifications, D2 in the range of 580 ~ 2750mm is conducive to the formation of a more concentrated electric field.
[0019] In some possible implementations, along the radial direction of the material channel, the thickness dimension of the annular electrode portion is T, and H1 and T satisfy: 0.6≤H1 / T≤7.4.
[0020] In the above embodiment, the thickness dimension T of the annular electrode portion and the distance H1 between the end surface of the first electrode and the first plane satisfy 0.6≤H1 / T≤7.4, so that the electric field can reach the temperature required for the graphitization process, and the length of the graphitization path can be moderate. The material is heated for a sufficient time, and the pores of the graphitized product can be repaired to a qualified level, thereby improving the quality of the graphitized product. In addition, the probability of material blockage can be reduced.
[0021] In some possible implementations, H1 and T satisfy: 0.81≤H1 / T≤5.
[0022] After a large number of experimental verifications, when H1 and T satisfy 0.81≤H1 / T≤5, the quality of graphitized products can be further improved.
[0023] In some possible implementations, the value range of T is 130-1500 mm.
[0024] A large number of experimental verifications have shown that T in the range of 130 to 1500 mm is conducive to the formation of a more concentrated electric field.
[0025] In some possible implementations, the first electrode is a cylindrical electrode, the diameter of the first electrode is D3, and D3 and D1 satisfy: 1≤D1 / D3≤3.4.
[0026] In the above embodiment, the diameter D3 of the first electrode and the inner diameter D1 of the annular electrode portion satisfy 1≤D1 / D3≤3.4, which can not only form an electric field with a relatively uniform electric field intensity distribution, but also make the temperature of all areas in the electric field reach the temperature required for the graphitization process as much as possible, so as to uniformly and effectively heat the material, thereby improving the quality of the graphitized product, but also facilitate the uniform flow of the material in the material channel and reduce the probability of material blockage.
[0027] In some possible implementations, D1 and D3 satisfy: 1≤D1 / D3≤2.
[0028] After a large number of experimental verifications, when D1 and D3 satisfy 1≤D1 / D3≤2, the quality of graphitized products can be further improved.
[0029] In some possible implementations, the value range of D3 is 350-1200 mm.
[0030] After a large number of experimental verifications, D3 in the range of 350 to 1200 mm is conducive to the formation of a more concentrated electric field.
[0031] In some possible implementations, the first electrode is a cylindrical electrode, the diameter of the first electrode is D3, and D3 and H1 satisfy: 0.7≤H1 / D3≤4.7.
[0032] In the above embodiment, the diameter D3 of the first electrode and the distance H1 between the end face of the first electrode and the first plane satisfy 0.7≤H1 / D3≤4.7, which can not only form an electric field with a relatively uniform electric field intensity distribution, but also make the temperature required for the graphitization process reach the electric field, so as to evenly and effectively heat the material passing through the electric field, thereby improving the quality of the graphitized product.
[0033] In some possible implementations, D3 and H1 satisfy: 0.7≤H1 / D3≤2.
[0034] After a large number of experimental verifications, when D3 and H1 satisfy 0.7≤H1 / D3≤2, the quality of graphitized products can be further improved.
[0035] In some possible implementations, along the radial direction of the material channel, the cross-sectional area of the first electrode is S1, the cross-sectional area of the annular electrode portion is S2, and S1 and S2 satisfy: 0.8≤S2 / S1≤18.
[0036] In the above embodiment, the cross-sectional area S1 of the first electrode and the cross-sectional area S2 of the annular electrode portion along the radial direction of the material channel satisfy 0.8≤S2 / S1≤18, so that the temperature required for the graphitization process can be reached in the electric field, and the material can be heated for a sufficient time so that the pores of the graphitized product can be repaired to an acceptable level, thereby improving the quality of the graphitized product.
[0037] In some possible implementations, S1 and S2 satisfy: 1.2≤S2 / S1≤12.
[0038] After a large number of experimental verifications, when S1 and S2 satisfy 1.2≤S2 / S1≤12, the quality of graphitized products can be further improved.
[0039] In some possible implementations, the value range of S1 is 0.12 to 1.2 m 2 .
[0040] After a lot of experimental verification, S1 is between 0.12 and 1.2 m 2 Within the range, it is conducive to forming a more concentrated electric field.
[0041] In some possible implementations, the value range of S2 is 0.15 to 2.5 m 2 .
[0042] After a lot of experimental verification, S2 is between 0.15 and 2.5 m 2 Within the range, it is conducive to forming a more concentrated electric field.
[0043] In some possible embodiments, the second electrode further includes a current-conducting electrode portion; one end of the current-conducting electrode portion is connected to the annular electrode portion, and the other end is connected to a power supply; the contact surface area between the current-conducting electrode portion and the annular electrode portion is S3, the outer surface area of the annular electrode portion is S4, and S3 and S4 satisfy: 1.5≤S4 / S3≤8.
[0044] In the above embodiment, the outer side surface area S4 of the annular electrode portion and the contact surface area S3 between the guide electrode portion and the annular electrode portion satisfy 1.5≤S4 / S3≤8, so that the contact surface area S3 can meet the current density requirement and avoid current deviation, thereby making the temperature required for the graphitization process reach in the electric field, thereby improving the quality of the graphitized product.
[0045] In some possible implementations, S3 and S4 satisfy: 3≤S4 / S3≤5.
[0046] After a large number of experimental verifications, when S3 and S4 satisfy 3≤S4 / S3≤5, the quality of graphitized products can be further improved.
[0047] In some possible implementations, the value range of S3 is 0.15 to 1.1 m 2 .
[0048] After a lot of experimental verification, S3 is between 0.15 and 1.1 m 2 Within this range, it is beneficial for a large current to pass through the contact surface between the annular electrode portion and the guide electrode portion, so that there is sufficient current density in the electric field.
[0049] In some possible implementations, the value range of S4 is 0.5 to 7 m 2 .
[0050] After a lot of experimental verification, S3 is between 0.15 and 1.1 m 2 Within this range, the annular electrode portion is advantageously provided with a larger current density, thereby ensuring sufficient current density in the electric field.
[0051] In some possible embodiments, along the radial direction of the material channel, the bottom surface of the guide electrode portion is flush with the bottom surface of the annular electrode portion; along the extension direction of the material channel, the height dimension of the annular electrode portion is H2, and the height dimension of the guide electrode portion is H3, and H2 and H3 satisfy: 1≤H2 / H3≤4.
[0052] The above implementation makes the height dimension H2 of the annular electrode portion and the height dimension H3 of the guide electrode portion satisfy 1≤H2 / H3≤4, which not only takes into account the manufacturing cost of the annular electrode portion, but also forms a more concentrated electric field to centrally heat the material, thereby improving the quality of the graphitized product.
[0053] In some possible implementations, H2 and H3 satisfy: 1≤H2 / H3≤1.8.
[0054] After a large number of experimental verifications, S3 and S4 satisfy 1≤H2 / H3≤1.8, which can further improve the quality of graphitized products.
[0055] In some possible implementations, the value range of H2 is 400-2000 mm.
[0056] After a large number of experimental verifications, H2 in the range of 400 to 2000 mm is conducive to the formation of an umbrella-shaped electric field.
[0057] In some possible implementations, the value range of H3 is 300 to 1200 mm.
[0058] After a large number of experimental verifications, H2 in the range of 400 to 2000 mm is conducive to the formation of an umbrella-shaped electric field.
[0059] In some possible implementations, the graphitization furnace further includes a first heat-insulating layer, which is disposed at the innermost side of the furnace body and forms a partial channel section of the material channel.
[0060] In the above embodiment, by providing the first insulation layer, the temperature of the heating zone formed between the first electrode and the second electrode can be insulated, so that the heating zone is maintained in a high temperature range, the graphitization degree of the material is uniform, and the consistency of the graphitized product can be improved.
[0061] In some possible implementations, the thermal conductivity of the first thermal insulation layer is 0.05-5w / mk; or the compressive strength of the first thermal insulation layer is 0.1-40MPa; or the temperature resistance of the first thermal insulation layer is 1800-3200°C.
[0062] In the above embodiment, by setting the thermal conductivity of the first thermal insulation layer, the first thermal insulation layer can reduce the heat loss of the graphitization furnace under the thermal conductivity, thereby improving the energy utilization rate. By setting the compressive strength of the first thermal insulation layer, the first thermal insulation layer can have a high-strength heat resistance effect, and by setting the heat resistance of the first thermal insulation layer, the first thermal insulation layer can have a high-strength heat resistance effect, thereby improving the service life of the graphitization furnace.
[0063] In some possible implementations, the graphitization furnace further includes a second thermal insulation layer disposed on a side of the first thermal insulation layer facing the outside of the furnace body.
[0064] In the above embodiment, by providing a second insulation layer outside the first insulation layer, the temperature of the heating zone formed between the first electrode and the second electrode can be further insulated, so that the heating zone is maintained in a high temperature range, the degree of graphitization of the material is uniform, and the consistency of the graphitized product can be further improved.
[0065] In some possible implementations, the thermal conductivity of the second thermal insulation layer is 0.1-20w / mk; or the compressive strength of the second thermal insulation layer is 20-60MPa; or the temperature resistance of the second thermal insulation layer is 1500-3200°C; or the ash content of the second thermal insulation layer is 0.1-10%.
[0066] In the above embodiment, by setting the thermal conductivity of the second thermal insulation layer, the second thermal insulation layer can reduce the heat loss of the graphitization furnace under the thermal conductivity and improve the energy utilization rate. By setting the compressive strength of the second thermal insulation layer, the second thermal insulation layer can have a high-strength support effect; by setting the temperature resistance of the second thermal insulation layer, the second thermal insulation layer can have a high-strength temperature resistance effect; by setting the ash content of the second thermal insulation layer, the influence of excessive ash content on the quality of the second thermal insulation layer can be reduced, thereby improving the service life of the graphitization furnace.
[0067] In some possible implementations, the graphitization furnace further includes a third thermal insulation layer disposed on a side of the second thermal insulation layer facing the outside of the furnace body.
[0068] In the above embodiment, by providing the third thermal insulation layer outside the second thermal insulation layer, the energy loss of the first thermal insulation layer and the second thermal insulation layer can be reduced, and the energy utilization rate and the thermal insulation effect can be improved.
[0069] In some possible implementations, the third thermal insulation layer contains more than 30% alumina; or the compressive strength of the third thermal insulation layer is 1-60 MPa; or the temperature resistance of the third thermal insulation layer is 1000-2000°C.
[0070] In the above embodiment, by setting alumina material in the third thermal insulation layer, the third thermal insulation layer can have a certain anti-oxidation function; by setting the compressive strength of the third thermal insulation layer, the third thermal insulation layer can have a higher strength supporting effect; by setting the temperature resistance of the third thermal insulation layer, the third thermal insulation layer can have a higher strength heat resistance effect, thereby improving the service life of the graphitization furnace.
[0071] In a second aspect, a battery production system is provided, comprising: a graphitization furnace according to the first aspect or any possible embodiment of the first aspect, wherein the graphitization furnace is used to produce negative electrode graphite material for a battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0072] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments of the present application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the drawings without paying creative work.
[0073] Figure 1 It is a schematic structural diagram of a graphitization furnace;
[0074] Figure 2 is a front cross-sectional view of a graphitization furnace provided in an embodiment of the present application;
[0075] Figure 3 is a top cross-sectional view of a graphitization furnace provided in an embodiment of the present application;
[0076] Figure 4 is a front cross-sectional view of a graphitization furnace provided in an embodiment of the present application;
[0077] Figure 5 is a top cross-sectional view of a graphitization furnace provided in an embodiment of the present application;
[0078] Figure 6 is a front cross-sectional view of another graphitization furnace provided in an embodiment of the present application;
[0079] Figure 7 This is a front cross-sectional view of another graphitization furnace provided in an embodiment of the present application.
[0080] In the drawings, the drawings are not drawn to scale. DETAILED DESCRIPTION
[0081] The following detailed description and drawings of the embodiments of the present application are used to illustrate the principles of the present application, but cannot be used to limit the scope of the present application, that is, the present application is not limited to the described embodiments.
[0082] In the description of the present application, it should be noted that, unless otherwise specified, "multiple" means more than two; the terms "upper", "lower", "left", "right", "inside", "outside", etc., indicating the orientation or positional relationship, are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application. In addition, the terms "first", "second", "third", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance. "Vertical" is not strictly vertical, but is within the allowable error range. "Parallel" is not strictly parallel, but is within the allowable error range.
[0083] The directional words appearing in the following description are all directions shown in the figures, and do not limit the specific structure of this application. In the description of this application, it should also be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be directly connected or indirectly connected through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to the specific circumstances.
[0084] The present application relates to a graphitization furnace, which can transform the carbon atoms of a carbon material from an irregularly arranged structure into an ordered graphite crystal structure by heating, thereby realizing graphitization of the carbon material. The graphitization is to improve the thermal and electrical conductivity of the carbon material, improve the thermal shock resistance and chemical stability of the carbon material, make the carbon material have lubricity and wear resistance, improve the purity of the carbon material, reduce the hardness of the carbon material, make it easier to machine, etc.
[0085] At present, graphitization furnaces can be mainly used for high-temperature treatments such as sintering and graphitization of carbon materials, graphitization of polyimide (PI) films, graphitization of thermal conductive materials, sintering of carbon fiber ropes, sintering and graphitization of carbon fiber filaments, graphite purification, and other materials that can be graphitized under carbon environments. In some specific applications, graphite materials treated by graphitization furnaces can be used to form negative electrode materials for batteries. For example, graphite materials can be used as a major negative electrode material for current lithium batteries.
[0086] In this application, a battery refers to a physical module that includes one or more battery cells to provide electrical energy. A battery generally includes a casing for encapsulating one or more battery cells. Optionally, the battery cells may include lithium-ion secondary batteries, lithium-ion primary batteries, lithium-sulfur batteries, sodium-lithium-ion batteries, sodium-ion batteries, or magnesium-ion batteries, etc., which are not limited in the embodiments of the present application. Among them, graphite can be used as the negative electrode active material of the battery cell, and cooperates with the positive electrode active material of the battery cell (for example, lithium cobalt oxide, lithium iron phosphate, ternary lithium or lithium manganese oxide, etc.) to realize the movement of metal ions to form an electric current.
[0087] In some designs of graphitization furnaces, a positive electrode and a negative electrode are provided in the graphitization furnace. One end of the positive electrode and the negative electrode are connected to a DC power supply or an AC power supply, and the other ends are arranged opposite to each other, and an electric field can be formed between the two. When the carbon material entering the graphitization furnace passes through the electric field, the electric field will energize the carbon material, and the carbon material can reach the graphitization temperature through its own resistance heating, thereby realizing the graphitization conversion.
[0088] As an example, in some specific implementations, the positive electrode is a columnar electrode placed vertically in the material channel, and the negative electrode is a ring electrode located in the lower part of the furnace body and placed horizontally. An umbrella-shaped electric field is formed between the lower surface of the positive electrode and the upper surface of the negative electrode facing the positive electrode. When the material (carbon material) passes through the umbrella-shaped electric field, Joule heat will be generated based on its own resistance, thereby enabling graphitization of the material. Under this embodiment, the electric field strength distribution in the umbrella-shaped electric field is uneven, especially when the distance between the positive electrode and the negative electrode is too long, the difference in electric field strength in different areas of the electric field is more obvious. When the electric field strength distribution in different areas is uneven, the current density in different areas is not equal, which will cause the Joule heat generated by the material passing through different areas of the electric field to be unequal, thereby affecting the consistency of the graphitized product and reducing the quality of the graphitized product.
[0089] In view of this, the present application provides a graphitization furnace, which includes a furnace body, a first electrode, and a second electrode with a polarity opposite to that of the first electrode. A material channel is arranged in the furnace body, at least part of the first electrode is located in the material channel, and the second electrode includes an annular electrode portion, which is protruding from the inner wall of the material channel along the radial direction of the material channel and surrounds a part of the channel section of the material channel. Along the extension direction of the material channel, the distance H1 between the end face of the first electrode and the first plane and the inner diameter D1 of the annular electrode portion meet certain numerical conditions. The first plane is the plane where the surface of the annular electrode portion facing the first electrode is located. An electric field with a relatively uniform electric field intensity distribution can be formed between the first electrode and the second electrode to uniformly heat the material passing through the electric field, which is conducive to improving the consistency of the graphitized product, thereby improving the quality of the graphitized product.
[0090] The graphitization furnace involved in this application can be applied to any graphite production system, for example, a sintering and graphitization system of carbon materials, a PI film graphitization system, a thermal conductive material graphitization system, a carbon fiber rope / carbon fiber filament sintering graphitization system, a graphite purification system, etc. This application does not limit the specific application scenario of the graphitization furnace.
[0091] As an example, in some practical applications, the graphitized product (graphite material) generated by the graphitization furnace involved in this application can be used as the negative electrode material of the battery. That is, in this application, the graphitization furnace can be applied to the battery production system. The graphitization furnace can be used as a type of process equipment in the battery production line.
[0092] Figure 1 FIG. 1 shows a front view of a graphitization furnace 100. Figure 1 As shown, the main body of the graphitization furnace 100 is arranged vertically, and mainly includes a furnace body 1 and various functional units arranged in the furnace body 1. Specifically, Figure 1 As shown, the graphitization furnace may include a loading unit, a DC power supply unit, and a cooling and discharging unit.
[0093] The feeding unit mainly includes a silo 2 and a material pipe 3. The silo 2 is arranged above the furnace body 1, and the silo 2 is connected to the feed port on the furnace body through the material pipe 3. Optionally, a material shut-off valve 4 can also be arranged at the connection between the silo 2 and the material pipe 3 to control the flow of the material in the material channel 12.
[0094] Optionally, the material entering the graphitization furnace 100 is a graphitizable carbonaceous material, such as petroleum coke, coal coke, and asphalt. After entering the graphitization furnace, the material undergoes four stages of preheating, calcination, graphitization, and cooling to complete the graphitization process, such as obtaining a negative electrode material product, and volatile tail gas escapes during the process.
[0095] Optionally, the number of the silos 2 can be 2, 4 or more and evenly distributed above the furnace body 1.
[0096] The DC power supply unit may include a positive electrode 5, a negative electrode 6 and a DC transformer 7. Figure 1 As shown, the positive electrode 5 can extend into the furnace along the opening above the furnace body 1 and be suspended in the material channel 12, and the negative electrode 6 can be arranged in the middle and lower part of the furnace body 1. The negative electrode 6 can penetrate the furnace body 1.
[0097] The DC transformer 7 can supply power to the furnace body 1, and the power supply can be controlled at 600-1500kW. The positive electrode 5 and the negative electrode 6 can apply voltage to the material passing between the electrodes. The DC current flows through the material from the positive electrode of the DC transformer 7, and the material generates Joule heat by its own resistance, so that the furnace core temperature is about 3000°C or higher, thereby forming a stable temperature field between the positive electrode 5 and the negative electrode 6. The current passing through the material returns to the negative electrode of the DC transformer 7 from the negative electrode 6, forming a current flow loop.
[0098] Optionally, the DC power supply unit may further include a fixed brake 8, a conductive member 9, a cable 10 and a copper busbar 11. The positive electrode 5 is fixed by the fixed brake to the top of the furnace body 1. The conductive member 9 is fixed below the fixed brake 8, conducts current to the positive electrode 5, is connected to the copper busbar 11 by the cable 10, and is connected to the positive and negative ends of the DC transformer 7 by the copper busbar 11.
[0099] Alternatively, the positive electrode 5 and the negative electrode 6 may be graphite electrodes.
[0100] The cooling and discharging unit is mainly used to cool the graphitized material. Figure 1 As shown, the cooling and discharging unit may include a low-temperature cooling section 13, which may be a water cooling jacket. The low-temperature cooling section 13 may also be provided with a water inlet 14 and a water outlet 15, and the cooling medium may be circulating water.
[0101] Optionally, the graphitization furnace 100 may further include a furnace body heating unit (not shown in the figure). For example, a furnace cover and a furnace body lining. The furnace cover may be arranged on the upper part of the furnace body 1 to seal and insulate, and the furnace body lining is arranged around the inner wall of the furnace body 1 to insulate and heat the high temperature of the furnace core.
[0102] Figures 2 to 6 The structure diagrams of the graphitization furnace 200 provided in the embodiment of the present application are shown respectively, wherein Figure 2 , Figure 4 and Figure 6 The main cross-sectional view is Figure 3 and Figure 5 is a top view of the cross section. Figures 2 to 5 As shown, the graphitization furnace 200 may include a furnace body 210, a first electrode 220, and a second electrode 230 with a polarity opposite to that of the first electrode 220. The furnace body 210 is provided with a material channel 211, at least part of the first electrode 220 is located in the material channel 211, and the second electrode 230 includes an annular electrode portion 231, which is protruding from the inner wall 2111 of the material channel 211 along the radial direction of the material channel 211 and surrounds a part of the channel section of the material channel 211. Along the extension direction of the material channel 211, the distance between the end face 221 of the first electrode 220 and the first plane is H1, and the inner diameter of the annular electrode portion 231 is D1, and H1 and D1 satisfy: 0.4≤H1 / D1≤5. The first plane is the plane where the surface 2311 of the annular electrode portion 231 facing the first electrode 220 is located.
[0103] A cavity is formed inside the furnace body 210 , and a material channel 211 may be formed in the cavity. The material for generating graphite material may flow in the material channel 211 and be graphitized under the action of high temperature.
[0104] Alternatively, if Figure 2 As shown, the material channel 211 can penetrate the wall of the furnace body 210 , and after the material passing through the material channel 211 is converted into graphite material, it can be output to the outside of the furnace body 210 through the material channel 211 .
[0105] Optionally, the extension direction of the material channel 211 may be parallel to the gravity direction, and the material entering the material channel 211 may flow in the material channel 211 under the action of gravity. Alternatively, in other alternative embodiments, the extension direction of the material channel 211 may also be other directions. In this embodiment, other auxiliary components may be provided inside the furnace body 210 to drive the carbonaceous material to flow in the material channel 211.
[0106] The first electrode 220 and the second electrode 230 may be respectively the positive electrode and the negative electrode of the graphitization furnace 200. The first electrode 220 may be fixedly arranged at the opening of the furnace body 210 by a fixing device, at least a portion of the first electrode 220 may be located in the material channel 211, that is, located inside the furnace body 210, and another portion of the first electrode 220 may be located outside the furnace body 210. The second electrode 230 may be arranged through the wall of the furnace body 210, and at least a portion of the second electrode 230 may be located outside the furnace body 210. The portions of the first electrode 220 and the second electrode 230 located outside the furnace body 210 may be connected to a power source through an electrical connector, so that an electric field is formed between the portions of the first electrode 220 and the second electrode 230 located inside the furnace body 210, so as to heat the material passing through the material channel 211.
[0107] Optionally, the first electrode 220 and the second electrode 230 may be graphite electrodes. In some embodiments, the first electrode 220 may be a positive electrode, and its current density may be 18 to 26 A / cm 2 The current load can be 50000-75000A, and the resistivity can be less than 6 micro-ohms. The second electrode 230 can be a negative electrode, and its current density can be 10-20A / cm 2 , the current load can be 20000~30000A, and the resistivity can be less than 8 microohms.
[0108] Continue to refer to Figure 2 The annular electrode portion 231 of the second electrode 230 is protruded from the inner wall 2111 of the material channel 211 along the radial direction of the material channel 211, so that an umbrella-shaped electric field can be formed between the end face 221 of the first electrode 220 and the surface 2311 of the annular electrode portion 231 facing the first electrode 220. The part of the channel section of the material channel 211 surrounded by the second electrode 230 can be understood as the electrode wall of the second electrode 230 can be used as the channel wall of the part of the channel section in the material channel 211. In this way, after the material enters the material channel 211 and is heated by the umbrella-shaped electric field, it flows out from the hollow part of the annular electrode portion 231, and then flows out of the furnace body 210, to obtain a graphitized product after graphitization.
[0109] It should be noted that, in the embodiment of the present application, the end surface 221 of the first electrode 220 refers to the surface of one end of the first electrode 220 facing the second electrode 230 along the extension direction of the material channel 211 .
[0110] In one embodiment, in order to support the annular electrode portion 231 and prevent the annular electrode portion 231 from falling, the discharge section 212 of the material channel 211 may be flush with the inner diameter of the annular electrode portion 231 along the radial direction of the material channel 211 .
[0111] Continue to refer to Figure 2, along the extension direction of the material channel 211, the distance between the end surface 221 of the first electrode 220 and the first plane is H1, and the inner diameter of the annular electrode portion is D1, wherein the first plane is the plane where the surface 2311 of the annular electrode portion 231 facing the first electrode 220 is located. In the embodiment of the present application, H1 and D1 satisfy: 0.5≤H1 / D1≤5.
[0112] Optionally, in some embodiments, the value range of H1 may be 350 to 3000 mm.
[0113] After a large number of experimental verifications, H1 in the range of 350 to 3000 mm is conducive to forming a more concentrated electric field and is not prone to material blockage.
[0114] Optionally, in some embodiments, the value range of D1 may be 430 to 2400 mm.
[0115] After a large number of experimental verifications, D1 in the range of 430 to 2400 mm is conducive to forming a more concentrated electric field and is not prone to material blockage.
[0116] Optionally, in some embodiments, the outer diameter D2 of the annular electrode portion 231 may range from 580 to 2750 mm.
[0117] After a large number of experimental verifications, D2 in the range of 580 ~ 2750mm is conducive to the formation of a more concentrated electric field.
[0118] Optionally, in some embodiments, the thickness T of the annular electrode portion 231 may be in the range of 130 to 1500 mm.
[0119] A large number of experimental verifications have shown that T in the range of 130 to 1500 mm is conducive to the formation of a more concentrated electric field.
[0120] It should be understood that the thickness T is the difference between the outer diameter D2 and the inner diameter D1, that is, T=D2-D1.
[0121] Alternatively, if Figure 6 As shown, the height H2 of the annular electrode portion 231 may range from 400 to 2000 mm.
[0122] After a large number of experimental verifications, H2 in the range of 400 to 2000 mm is conducive to the formation of an umbrella-shaped electric field.
[0123] Optional, such as Figure 5 and Figure 6As shown, the second electrode 230 includes, in addition to the annular electrode portion 231, a conducting electrode portion 232. One end of the conducting electrode portion 232 is connected to the annular electrode portion 231, and the other end is connected to the power supply. The bottom surface of the conducting electrode portion 232 can be flush with the bottom surface of the annular electrode portion 231. The height H3 of the conducting electrode portion 232 ranges from 300 to 1200 mm.
[0124] After a large number of experimental verifications, H2 in the range of 400 to 2000 mm is conducive to the formation of an umbrella-shaped electric field.
[0125] Optionally, in some embodiments, the first electrode 220 may be a cylindrical electrode.
[0126] Optionally, in some embodiments, the diameter D3 of the first electrode 220 may be in the range of 350 to 1200 mm.
[0127] After a large number of experimental verifications, D3 in the range of 350 to 1200 mm is conducive to the formation of a more concentrated electric field.
[0128] It should be understood that the umbrella-shaped electric field is formed between the end face 221 of the first electrode 220 and the surface of the annular electrode portion 231 facing the first electrode 220. Taking the first electrode 220 as a positive electrode and the second electrode 230 as a negative electrode as an example, the electric field strength near the end face 221 of the first electrode 220 is generally greater than the electric field strength in other areas of the electric field. When the ratio of H1 to D1 is too large, the higher the height of the area covered by the electric field, the greater the difference in electric field strength in various areas of the electric field. After the material enters the electric field, it passes through different electric field areas with different electric field strengths, which will cause the consistency of the graphitized product to deteriorate, thereby reducing the quality of the graphitized product.
[0129] In the embodiment of the present application, H1 and D1 satisfy 0.5≤H1 / D1≤5, so that an electric field with a relatively uniform electric field strength distribution can be formed between the end face 221 of the first electrode 220 and the surface of the end face 221 of the annular electrode portion 231 facing the first electrode 220, so as to uniformly heat the material passing through the electric field, which is beneficial to improving the consistency of the graphitized product, thereby improving the quality of the graphitized product.
[0130] In order to verify whether the above-mentioned numerical range of H1 / D1 can improve the quality of graphitized products, the relevant evaluation parameters of graphitized products corresponding to different H1 / D1 ratios are measured below.
[0131] In the embodiments of the present application, the relevant evaluation parameters of the graphitized product include the degree of graphitization. The degree of graphitization is the main indicator for evaluating graphitized products. The degree of graphitization is an indicator for measuring the degree to which carbon atoms in the graphitized product form a close-packed hexagonal graphite crystal structure. The closer the lattice size is to the lattice constant of ideal graphite, the higher the degree of graphitization. Generally, a degree of graphitization of 90% is used as the qualification standard for graphitized products. As an example and not a limitation, the degree of graphitization of the graphitized product can be measured by X-ray diffraction analysis, which is a common method used by those skilled in the art to measure the degree of graphitization and will not be repeated here.
[0132] It should be understood that the embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are specified in the embodiments, the techniques or conditions described in the literature in the art or the product specifications are used. If the materials or instruments used do not specify the manufacturer, they are all conventional products that can be obtained commercially.
[0133] Test process 1: With the first electrode 220 as the positive electrode, the second electrode 230 as the negative electrode, the power supply when controlling the closed loop is 1200KW, the outer diameter D2 of the annular electrode portion 231 of the second electrode 230 is 1350mm, the diameter D3 of the first electrode 220 is 600mm, the height H2 of the annular electrode portion 231 is 910mm, and the height H3 of the guide electrode portion 232 is 700mm, the graphitization degree of the graphitized product produced by the graphitization furnace 200 is recorded at different H1 / D1. The H1 / D1 ratio and the test results are shown in Table 1. Among them, the graphitization degree of the graphitized product can be calculated by using an X-ray diffractometer through the peak value measured.
[0134] Table 1
[0135] H1(mm) D1(mm) H1 / D1 Graphitization degree (%) 400 900 0.44 81.29 450 900 0.50 92.15 500 900 0.56 93.39 720 900 0.80 94.19 900 900 1.00 94.38 1100 900 1.22 94.76 1350 900 1.50 93.57 2500 1470 1.70 92.27 2500 906 2.76 92.18 2500 581 4.30 90.73 2500 500 5.0 90.21 2500 430 5.81 84.172
[0136] It can be seen from Table 1 that when H1 and D1 satisfy 0.5≤H1 / D1≤5, the graphitization degree of the graphitized product is above 90%, which meets the standard quality requirements of graphitized products. When H1 and D1 do not satisfy 0.5≤H1 / D1≤5, the graphitization degree of the graphitized product is less than 90%, which does not meet the standard quality requirements of graphitized products.
[0137] Therefore, as verified by the above test, the above numerical range of H1 / D1 can make the graphitized product meet the standard quality requirements, thereby reducing the probability of unqualified graphitized products and improving the quality of graphitized products.
[0138] In some possible implementations, H1 and D1 satisfy 0.8≤H1 / D1≤1.5.
[0139] It can also be seen from the experimental data in Table 1 above that when H1 and D1 satisfy 0.8≤H1 / D1≤1.5, the graphitization degree of the graphitized product can exceed 93.5%, which can further improve the quality of the graphitized product.
[0140] In some possible implementations, continue to refer to Figure 2 and Figure 3 , the inner diameter D1 and the outer diameter D2 of the annular electrode portion 231 satisfy: 1.17≤D2 / D1≤3.
[0141] It should be understood that the electric field is formed between the end face 221 of the first electrode 220 and the surface 2311 of the annular electrode portion 231 facing the first electrode 220. When the ratio of the outer diameter D2 to the inner diameter D1 of the annular electrode portion 231 is too large, that is, the wall of the annular electrode portion 231 is too thick, the surface 2311 of the annular electrode portion 231 facing the first electrode 220 is too large, the electric field covers a large area, and the electric field intensity is low, and the temperature required for the graphitization process may not be reached, resulting in a low degree of graphitization of the graphitized product. When the ratio of the D2 phase to D1 is too small, that is, the wall of the annular electrode portion 231 is too thin, and the thickness of the electric field is too thin along the radial direction of the material channel 211, the graphitization path of the material is short, the heating time is insufficient, and the graphitization process cannot be completed, resulting in the inability to repair the pores of the graphitized product to a qualified level.
[0142] It should be understood that the specific surface area is an important indicator to characterize whether the pores of the graphitized product have been repaired to a qualified level. The better the pores of the graphitized product are repaired, such as the more regular the crystal structure of the surface of the graphitized product and the fewer defects, the closer the specific surface area is to the qualified range.
[0143] Specific surface area refers to the surface area per gram of solid material. When graphite material is used as the negative electrode material of lithium-ion batteries, the specific surface area is a very important parameter of lithium-ion battery materials. If the specific surface area of the graphite material is too large, it will cause excessive initial capacity loss. The specific surface area of graphite materials is related to the shape and surface structure of graphite particles. For example, artificial graphite has a special microporous structure with a large specific surface area. It contains more active sites and a larger reaction area, which improves the utilization rate of active materials and exhibits high capacity and high rate performance. However, during the first charge and discharge process, the electrolyte consumed by the formation of the SEI film is relatively large, resulting in a large proportion of irreversible capacity. If the specific surface area of the graphite particles is too small, the kinetic performance of the battery will deteriorate. Therefore, only graphite materials need to have a suitable specific surface area. Usually, the specific surface area is set between 1.1 and 1.3 m 2 / g of graphite material is considered to be a qualified battery negative electrode material. As an example but not limitation, the specific surface area can be detected by volume adsorption method, weight adsorption method, flow adsorption method, permeability method, gas adhesion method, etc. The above methods are commonly used by those skilled in the art in measuring specific surface area and will not be repeated here.
[0144] It should be noted that the graphitization degree of the graphitized product is positively correlated with the specific surface area.
[0145] In the embodiment of the present application, the outer diameter D2 and the inner diameter D1 of the annular electrode portion 231 satisfy 1.17≤D2 / D1≤3, which can not only make the electric field reach the temperature required for the graphitization process, but also make the graphitization path length moderate. The material is heated for a sufficient time, and the channels of the graphitized product can be repaired to an acceptable level, thereby improving the quality of the graphitized product.
[0146] In some possible implementations, D1 and D2 satisfy 1.24≤D2 / D1≤2.51.
[0147] A large amount of experimental data shows that when D1 and D2 satisfy 1.24≤D2 / D1≤2.51, the pores of the graphitized product can be further repaired, thereby further improving the quality of the graphitized product.
[0148] In some possible implementations, such as Figure 4 As shown, along the radial direction of the material channel 211 , the thickness dimension of the annular electrode portion 231 is T, and T and H1 satisfy: 0.6≤H1 / T≤7.4.
[0149] When the ratio of H1 to T is too large, for example, when the distance H1 is large and T is small, the uneven distribution of the electric field strength is more obvious, which is easy to affect the consistency of the graphitized product. In addition, along the radial direction of the material channel 211, the thickness of the electric field is too thin, which will cause the graphitization path of the material to be shorter, the heating time is insufficient, and the graphitization process cannot be completed, resulting in the inability to repair the pores of the graphitized product to a qualified level. When the ratio of H1 to T is too small, for example, when H1 is small and T is large, it may cause material blockage, reduce the efficiency of graphitization, and the wall of the annular electrode part 231 is too thick, and the electric field strength in the vicinity of the annular electrode part 231 is low, which may not reach the temperature required for the graphitization process, thereby resulting in a low degree of graphitization of the graphitized product.
[0150] In the embodiment of the present application, the thickness dimension T of the annular electrode portion 231 and the distance H1 between the end surface 221 of the first electrode 220 and the first plane satisfy 0.6≤H1 / T≤7.4, so that the electric field can reach the temperature required for the graphitization process, and the graphitization path length is moderate, the material is heated for a sufficient time, and the pores of the graphitized product can be repaired to a qualified level, thereby improving the quality of the graphitized product. In addition, the probability of material blockage can also be reduced.
[0151] In some possible implementations, H1 and T satisfy 0.81≤H1 / T≤5.
[0152] A large amount of experimental data shows that when H1 and T satisfy 0.81≤H1 / T≤5, the quality of graphitized products can be further improved.
[0153] In order to verify whether the above numerical ranges of D2 / D1 and H1 / T can improve the quality of graphitized products, the specific surface areas of graphitized products corresponding to different D2 / D1 and H1 / T ratios were measured.
[0154] Test process 2: Different from test process 1, this test uses H1 as 1100mm and D3 as 600mm, and records the specific surface area of the graphitized product produced by the graphitization furnace at different D2 / D1 and H1 / T ratios. The test results of the ratios of D2 / D1 and H1 / T and the specific surface area are shown in Table 2. Among them, the specific surface area of the graphitized product can be directly measured using a specific surface area analyzer.
[0155] Table 2
[0156]
[0157] It can be seen from Table 2 above that the outer diameter D2 and the inner diameter D1 of the annular electrode portion 231 satisfy 1.17≤D2 / D1≤3, and the specific surface area of the graphitized product is 1.1-1.3m 2 / g range, which meets the requirements for battery negative electrode materials. When the outer diameter D2 and the inner diameter D1 of the annular electrode portion 231 do not satisfy 1.17≤D2 / D1≤3, such as D2 / D1=1.14, the specific surface area of the graphitized product is not within the range of 1.1 to 1.3 m 2 / g range, which does not meet the requirements for battery negative electrode materials.
[0158] In addition, it can be seen from Table 2 above that when D2 and D1 satisfy 1.24≤D2 / D1≤2.51, the specific surface area of the graphitized product is far away from the specific surface area boundary value of 1.1m 2 / g and 1.3m 2 / g, the quality of graphitized products is more stable, and the quality of graphitized products can be further improved.
[0159] It can be seen from Table 2 above that H1 and T satisfy 0.6≤H1 / T≤7.4, and the specific surface area of the graphitized product is 1.1~1.3m 2 / g range, which meets the requirements for battery negative electrode materials. When H1 and T do not satisfy 0.6≤H1 / T≤7.4, such as H1 / T=8.46, the specific surface area of the graphitized product is not within the range of 1.1~1.3m 2 / g range, which does not meet the requirements for battery negative electrode materials.
[0160] In addition, it can be seen from Table 2 above that when H1 and T satisfy 0.81≤H1 / T≤5, the specific surface area of the graphitized product is far away from the specific surface area boundary value of 1.1m 2 / g and 1.3m 2 / g, the quality of graphitized products is more stable, and the quality of graphitized products can be further improved.
[0161] In some possible embodiments, continue to refer to Figures 2 to 4 The first electrode 220 may be a cylindrical electrode, and the diameter of the first electrode 220 is D3, and D3 and the inner diameter D1 of the annular electrode portion 231 satisfy: 1≤D1 / D3≤5.
[0162] Optionally, the first electrode 220 can be coaxially arranged with the material channel 211, that is, along the radial direction of the material channel 211, the first electrode 220 can be arranged at the center of the material channel 211. Of course, the first electrode 220 may not be coaxially arranged with the material channel 211, and this application does not limit this.
[0163] It should be understood that an umbrella-shaped electric field can be formed between the end face 221 of the first electrode 220 and the surface of the annular electrode portion 231 facing the first electrode 220. When the ratio of the inner diameter D1 of the annular electrode portion 231 to the diameter D3 of the first electrode 220 is large, for example, when the inner diameter D1 is large and D3 is small, the phenomenon of uneven distribution of the electric field intensity in the electric field is more obvious, and the temperature of some areas in the electric field may not reach the temperature required for the graphitization process, thereby resulting in a low degree of graphitization of the graphitized product. When the ratio of the inner diameter D1 of the annular electrode portion 231 to the diameter D3 of the first electrode 220 is small, for example, when the inner diameter D1 is small and D3 is large, the shape of the electric field may change, that is, it is not an umbrella shape, which may easily lead to the electric field being unable to heat the material centrally and unable to reach the temperature required for the graphitization process, thereby resulting in a low degree of graphitization of the graphitized product, thereby reducing the quality of the graphitized product. In addition, the material is prone to blockage in the material channel 211, reducing the efficiency of graphitization.
[0164] In the embodiment of the present application, the diameter D3 of the first electrode 220 and the inner diameter D1 of the annular electrode portion 231 satisfy 1≤D1 / D3≤3.4, which can not only form an electric field with a relatively uniform electric field intensity distribution, but also make the temperature of all regions in the electric field reach the temperature required for the graphitization process as much as possible to heat the material uniformly and effectively, thereby improving the quality of the graphitized product, but also facilitate the uniform flow of the material in the material channel 211, reducing the probability of material blockage.
[0165] In order to verify whether the above numerical range of D1 / D3 can improve the quality of graphitized products, the graphitization degree of graphitized products corresponding to different D1 / D3 ratios was measured.
[0166] Test process 3: Different from test process 1, in this test, H1 is 1100 mm, D3 is 600 mm, and the outer diameter D2 of the annular electrode portion 231 is 1350 mm. The graphitization degree of the graphitized product produced by the graphitization furnace 200 is recorded at different D1 / D3. The D1 / D3 ratio and the test results are shown in Table 3.
[0167] Table 3
[0168] D3(mm) D1(mm) D1 / D3 Graphitization degree (%) 600 480 Less than 1 90.16 600 600 1 95.14 600 1200 2 95.25 600 2040 3.4 94.87 600 2400 Greater than 3.4 90.25
[0169] It can be seen from Table 3 above that when the diameter D3 of the first electrode 220 and the inner diameter D1 of the annular electrode portion 231 satisfy 1≤D1 / D3≤3.4, the graphitization rate of the graphitized product is above 94%, far exceeding the qualified standard (90%), which can improve the quality of the graphitized product.
[0170] In some possible implementations, D1 and D3 satisfy 1≤D1 / D3≤2.
[0171] It can also be seen from Table 3 above that the diameter D3 of the first electrode 220 and the inner diameter D1 of the annular electrode portion 231 satisfy 1≤D1 / D3≤2, and the graphitization rate exceeds 95%, which can further improve the quality of the graphitized product.
[0172] In some possible implementations, continue to refer to Figure 4 , the diameter D3 of the first electrode and the distance H1 between the end surface 221 of the first electrode 220 and the first plane may satisfy: 0.7≤H1 / D3≤4.7.
[0173] It should be understood that an umbrella-shaped electric field is formed between the end face 221 of the first electrode and the surface 2311 of the annular electrode portion 231, and the electric field strength near the end face 221 of the first electrode in the umbrella-shaped electric field is relatively large. In other words, the temperature of this area is relatively high compared to other areas. If the ratio of H1 to D3 is too large, for example, H1 is large and D3 is small, the greater the difference in electric field strength in each area of the electric field, the greater the temperature difference, and even the temperature of some areas cannot reach the temperature required for the graphitization process, resulting in the material passing through the area. The degree of graphitization does not meet the standard. If the ratio of H1 to D3 is too small, for example, H1 is small and D3 is large, the electric field strength in the electric field is low, and it may not be possible to reach the temperature required for the graphitization process, resulting in the degree of graphitization not meeting the standard.
[0174] In the embodiment of the present application, the diameter D3 of the first electrode 220 and the distance H1 between the end face 221 of the first electrode 220 and the first plane satisfy 0.7≤H1 / D3≤4.7. This not only allows an electric field with a relatively uniform electric field strength distribution to be formed between the end face 221 of the first electrode 220 and the surface of the end face 221 of the annular electrode portion 231 facing the first electrode 220, but also allows the temperature required for the graphitization process to be reached in the electric field, so as to evenly and effectively heat the material passing through the electric field, thereby improving the quality of the graphitized product.
[0175] In order to verify whether the above-mentioned numerical range of H1 / D3 can improve the quality of graphitized products, the graphitization degree of graphitized products corresponding to different H1 / D3 ratios was measured.
[0176] Test process 4: Different from test process 1, this test uses H1 as 600 mm and D1 as 900 mm, and records the graphitization degree of the graphitized product produced by the graphitization furnace 200 at different H1 / D3. The H1 / D3 ratio and the test results are shown in Table 4.
[0177] Table 4
[0178] H1(mm) D3(mm) H1 / D3 Graphitization degree (%) 600 480 Less than 0.7 90.34 600 600 0.7 95.23 600 1200 2 95.37 600 2040 4.7 94.82 600 2400 Greater than 4.7 90.45
[0179] It can be seen from Table 4 above that when H1 and D3 satisfy 0.7≤H1 / D3≤4.7, the graphitization rate of the graphitized product is above 94%, which can improve the quality of the graphitized product.
[0180] In some possible implementations, H1 and D3 satisfy 0.7≤H1 / D3≤2.
[0181] It can also be seen from Table 4 above that when H1 and D3 satisfy 0.7≤H1 / D3≤2, the degree of graphitization exceeds 95%, which can further improve the quality of the graphitized product.
[0182] like Figure 5As shown, S1 is the cross-sectional area of the first electrode 220 along the radial direction of the material channel 211. S2 is the cross-sectional area of the annular electrode portion 231 along the radial direction of the material channel 211. It should be understood that S1 can be calculated based on the diameter D3 of the first electrode 220. S2 can be calculated based on the inner diameter D1 and the outer diameter D2 of the annular electrode portion 231.
[0183] In some possible implementations, along the radial direction of the material channel 211 , the cross-sectional area S1 of the first electrode 220 and the cross-sectional area S2 of the annular electrode portion 231 satisfy: 0.8≤S2 / S1≤18.
[0184] Optionally, in some embodiments, the value range of S1 is 0.12 to 1.2 m. 2 .
[0185] After a lot of experimental verification, S1 is between 0.12 and 1.2 m 2 Within the range, it is conducive to forming a more concentrated electric field.
[0186] Optionally, in some embodiments, the value range of S2 is 0.15 to 2.5 m 2 .
[0187] After a lot of experimental verification, S2 is between 0.15 and 2.5 m 2 Within the range, it is conducive to forming a more concentrated electric field.
[0188] It should be understood that the size of the umbrella-shaped electric field region is related to the cross-sectional area S1 of the first electrode 220 along the radial direction of the material channel 211, and the cross-sectional area S2 of the annular electrode portion 231 along the radial direction of the material channel 211. When S2 / S1 is too large, for example, S2 is large and S1 is small, the electric field intensity in the vicinity of the first electrode 220 is low, and the temperature required for the graphitization process may not be reached, resulting in a low degree of graphitization of the graphitized product and the inability to repair the pores of the graphitized product to a qualified level. When S2 / S1 is too small, for example, S2 is small and S1 is large, the graphitization path of the material in the electric field is short, and the heating time is insufficient, resulting in the inability to repair the pores of the graphitized product to a qualified level.
[0189] In the embodiment of the present application, the cross-sectional area S1 of the first electrode 220 and the cross-sectional area S2 of the annular electrode portion 221 along the radial direction of the material channel 211 satisfy 0.8≤S2 / S1≤18, so that the temperature required for the graphitization process can be reached in the electric field, and the material can be heated for a sufficient time so that the pores of the graphitized product can be repaired to an acceptable level, thereby improving the quality of the graphitized product.
[0190] In order to verify whether the above S2 / S1 value range can improve the quality of graphitized products, the specific surface areas of graphitized products corresponding to different S2 / S1 ratios were measured.
[0191] Test process 5: Different from test process 1, this test uses H1 as 1100mm and D1 as 900mm to record the specific surface area of the graphitized product at different S2 / S1 ratios. The S2 / S1 ratio and test results are shown in Table 5.
[0192] Table 5
[0193]
[0194] It can be seen from Table 5 above that when S1 and S2 satisfy 0.8≤S2 / S1≤18, the specific surface area of the graphitized product is between 1.1 and 1.3 m 2 / g range, meeting the requirements for battery negative electrode materials.
[0195] In some possible implementations, S1 and S2 satisfy 1.2≤S2 / S1≤12.
[0196] It can also be seen from Table 5 above that when S1 and S2 satisfy 1.2≤S2 / S1≤12, the specific surface area of the graphitized product is far away from the specific surface area boundary value of 1.1m 2 / g and 1.3m 2 / g, that is, the quality of graphitized products is more stable and better, which can further improve the quality of graphitized products.
[0197] In some possible implementations, continue to refer to Figure 5 The contact surface area between the guide electrode portion 232 and the annular electrode portion 231 is S3, the outer surface area of the annular electrode portion 231 is S4, and S3 and S4 satisfy: 1.5≤S4 / S3≤8.
[0198] Optionally, the current guiding electrode portion 232 may be in a cylindrical, rectangular or other shape, which is not limited in the present application.
[0199] Optionally, the guide electrode portion 232 may be an integrated structure with the annular electrode portion 231 , or the two may be independent structures connected to each other, which is not limited in the present application.
[0200] One end of the current conducting electrode portion 232 connected to the power source is located outside the furnace body and can be connected to the power source through a connector. At least a portion of the current conducting electrode portion 232 penetrates the furnace body 210 to be connected to the annular electrode portion 231 .
[0201] In the embodiment of the present application, the contact surface area S3 between the guide electrode portion 232 and the annular electrode portion 231 is positively correlated with the cross-sectional area of the guide electrode portion 232 along the extension direction of the material channel 211, that is, the thicker the guide electrode portion 232, the larger S3, and the thinner the guide electrode portion 232, the smaller S3.
[0202] Optionally, in some embodiments, the value range of S3 is 0.15 to 1.1 m. 2 .
[0203] After a lot of experimental verification, S3 is between 0.15 and 1.1 m 2 Within this range, it is beneficial for a large current to pass through the contact surface between the annular electrode portion and the guide electrode portion, so that there is sufficient current density in the electric field.
[0204] Optionally, in some embodiments, the value range of S4 is 0.5 to 7 m. 2 .
[0205] After a lot of experimental verification, S4 is between 0.5 and 7 m 2 Within this range, the annular electrode portion is advantageously provided with a larger current density, thereby ensuring sufficient current density in the electric field.
[0206] When S4 / S3 is too large, for example, S4 is large and S3 is small, the current density through the contact surface S3 is small, and then the current density in the electric field is small, resulting in the inability to reach the temperature required for the graphitization process in the electric field, and the quality of the graphitized product is reduced. When S4 / S3 is too small, the current is prone to bias flow, and the temperature difference in different areas of the electric field is obvious, resulting in poor consistency of the graphitized product, thereby reducing the quality of the graphitized product.
[0207] In the embodiment of the present application, the outer side surface area S4 of the annular electrode portion 231 and the contact surface area S3 between the guide electrode portion 232 and the annular electrode portion 231 satisfy 1.5≤S4 / S3≤8, so that the contact surface area S3 can meet the current density requirement and avoid current deviation, thereby making the temperature required for the graphitization process reach in the electric field, thereby improving the quality of the graphitized product.
[0208] In order to verify whether the above numerical range can improve the quality of graphitized products, relevant evaluation parameters of graphitized products corresponding to different S4 / S3 ratios were measured.
[0209] Test process 6: Different from test process 1, this test uses D2=1350mm, H1=1100mm, and records the graphitization degree of the graphitized product produced by the graphitization furnace at different S4 / S3 ratios. The S4 / S3 ratio and test results are shown in Table 6.
[0210] Table 6
[0211]
[0212]
[0213] It can be seen from Table 6 above that when S3 and S4 satisfy 1.5≤S4 / S3≤8, the graphitization rate of the graphitized product is above 94%, which can improve the quality of the graphitized product and far exceeds the standard value of graphitization degree.
[0214] In some possible implementations, S3 and S4 satisfy 3≤S4 / S3≤5.
[0215] It can be seen from Table 6 above that when S4 and S3 satisfy 3≤S4 / S3≤5, the graphitization rate exceeds 95%, which can further improve the quality of the graphitized product.
[0216] In some possible implementations, continue to refer to Figure 6 Along the radial direction of the material channel 211, the bottom surface of the guide electrode portion 232 can be flush with the bottom surface of the annular electrode portion 231. Along the extension direction of the material channel 211, the height dimension of the annular electrode portion 231 is H2, and the height dimension of the guide electrode portion 232 is H3. H2 and H3 satisfy: 1≤H2 / H3≤4.
[0217] It should be understood that when the material channel 211 is in an inverted shape, Figure 6 Since the furnace body 210 is not completely insulated, an electric field can be generated between the first electrode 220 and the annular electrode portion 231 and between the first electrode 220 and the conductive electrode portion 232. In order to make the electric field more concentrated, so as to heat the material in a centralized manner, the height dimension H2 of the annular electrode portion 231 can be made greater than the height dimension H3 of the conductive electrode portion 232, so that the electric field is formed only between the first electrode 220 and the annular electrode portion 231 as much as possible. Because if H2 is less than H3, that is, the annular electrode portion 231 is lower than the conductive electrode portion 232, an electric field may be formed between the side surfaces of the first electrode 220 and the conductive electrode portion 232, resulting in a larger electric field coverage area and a smaller current density, which is not conducive to the centralized heating of the material and affects the quality of the graphitized product. However, H2 / H3 cannot be too large, that is, the annular electrode portion 231 cannot be too high compared to the conducting electrode portion 232, because although the annular electrode portion 231 is higher than the conducting electrode portion 232, which is beneficial to the formation of an electric field between the first electrode 220 and the annular electrode portion 231, being too high will increase the manufacturing cost of the annular electrode portion 231.
[0218] In the embodiment of the present application, the height dimension H2 of the annular electrode portion 231 and the height dimension H3 of the guide electrode portion 232 satisfy 1≤H2 / H3≤4, which not only takes into account the manufacturing cost of the annular electrode portion 231, but also forms a more concentrated electric field to centrally heat the material, thereby improving the quality of the graphitized product.
[0219] In some possible implementations, H2 and H3 satisfy: 1≤H2 / H3≤1.8.
[0220] A large amount of experimental data shows that the height dimension H2 of the annular electrode portion 231 and the height dimension H3 of the guide electrode portion 232 satisfy 1≤H2 / H3≤1.8, and the graphitization rate can reach more than 93.5%, which can further improve the quality of the graphitized product.
[0221] In some possible implementations, such as Figure 7 As shown, the graphitization furnace 200 may further include a first thermal insulation layer 240 , which is disposed at the innermost side of the furnace body 210 and forms a partial channel section of the material channel 211 .
[0222] The first thermal insulation layer 240 is an insulating thermal insulation layer, and its resistivity is much greater than that of graphite.
[0223] In the above embodiment, by providing the first insulation layer 240, the temperature of the heating zone formed between the first electrode 220 and the second electrode 230 can be insulated, so that the heating zone is maintained in a high temperature range, the graphitization degree of the material is uniform, and the consistency of the graphitized product can be improved.
[0224] In some possible implementations, the thermal conductivity of the first thermal insulation layer 240 is 0.05-5w / mk.
[0225] The greater the thermal conductivity of the material, the better the thermal conductivity and the worse the heat preservation effect. The above embodiment makes the thermal conductivity lower, which can reduce the heat loss of the graphitization furnace 200, thereby improving the energy utilization rate.
[0226] In some possible implementations, the compressive strength of the first thermal insulation layer 240 is 0.1-40 MPa.
[0227] The higher the compressive strength, the less likely the object is to crack and pulverize. By setting the compressive strength of the first thermal insulation layer 240, the first thermal insulation layer 240 can have a higher strength support function, thereby increasing the service life of the graphitization furnace 200.
[0228] In some possible implementations, the temperature resistance of the first thermal insulation layer 240 is 1800-3200°C.
[0229] Temperature resistance refers to the property of an object that will not be damaged or significantly reduce its use value when the external temperature changes. By setting the temperature resistance of the first thermal insulation layer 240, the first thermal insulation layer 240 can have a higher intensity of temperature resistance, thereby increasing the service life of the graphitization furnace.
[0230] In some possible implementations, such as Figure 7 As shown, the graphitization furnace 200 may further include a second thermal insulation layer 250 , which is disposed on a side of the first thermal insulation layer 240 facing the outside of the furnace body 210 .
[0231] The second thermal insulation layer 250 is a carbon thermal insulation layer. By arranging the second thermal insulation layer 250 outside the first thermal insulation layer 240, the temperature of the heating zone formed between the first electrode 220 and the second electrode 230 can be further insulated, so that the heating zone is maintained in a high temperature range, the graphitization degree of the material is uniform, and the consistency of the graphitized product can be further improved.
[0232] In some possible implementations, the thermal conductivity of the second thermal insulation layer 250 is 0.1-20w / mk. A low thermal conductivity can reduce the heat loss of the graphitization furnace 200, thereby improving energy utilization.
[0233] In some possible implementations, the compressive strength of the second thermal insulation layer 250 is 20-60 MPa.
[0234] In the above embodiment, by setting the compressive strength of the second thermal insulation layer 250 , the second thermal insulation layer 250 can have a relatively high-strength supporting effect, thereby increasing the service life of the graphitization furnace 200 .
[0235] In some possible implementations, the temperature resistance of the second thermal insulation layer 250 is 1500-3200°C.
[0236] In the above embodiment, by setting the temperature resistance of the second thermal insulation layer 250 , the second thermal insulation layer 250 can have a higher intensity of temperature resistance, thereby increasing the service life of the graphitization furnace 200 .
[0237] In some possible implementations, the ash content of the second thermal insulation layer 250 is 0.1-10%.
[0238] Ash content refers to the content of other solid elements in an object except carbon graphite. Excessive ash content will affect the quality of the object. By setting the ash content of the second insulation layer 250, the effect of excessive ash content on the quality of the second insulation layer 250 can be reduced, and the service life of the graphitization furnace 200 can be increased.
[0239] In some possible implementations, such as Figure 7As shown, the graphitization furnace further includes a third thermal insulation layer 260 , which is disposed on a side of the second thermal insulation layer 250 facing the outside of the furnace body 210 .
[0240] By providing the third thermal insulation layer 260 outside the second thermal insulation layer 250, the energy loss of the first thermal insulation layer 240 and the second thermal insulation layer 250 can be reduced, thereby improving energy utilization and thermal insulation effect.
[0241] In some possible embodiments, the third insulation layer 260 contains more than 30% alumina. In the above embodiment, by providing the third insulation layer 260 with alumina material, the third insulation layer 260 can have a certain anti-oxidation function, thereby improving the service life of the graphitization furnace 200.
[0242] In some possible implementations, the compressive strength of the third thermal insulation layer 260 is 5 to 60 MPa.
[0243] In the above embodiment, by setting the compressive strength of the third thermal insulation layer 260 , the third thermal insulation layer 260 can have a relatively high-strength supporting effect, thereby increasing the service life of the graphitization furnace.
[0244] In some possible implementations, the third thermal insulation layer 260 has a temperature resistance of 1000-2000° C. In the above implementations, by setting the temperature resistance of the third thermal insulation layer 260, the third thermal insulation layer 260 can have a higher intensity of temperature resistance, thereby increasing the service life of the graphitization furnace.
[0245] The present application also provides a battery production system, including the graphitization furnace 200 in any of the above embodiments, and the graphitization furnace 200 is used to produce negative electrode graphite materials for batteries.
[0246] It is understandable that the battery production system may include, in addition to the graphitization furnace 200 for producing the negative electrode graphite material of the battery, related equipment for producing other battery materials.
[0247] The battery production system may be a battery production line, and a plurality of devices in the battery production line may be arranged in the same centralized location, or may also be arranged in separate different locations.
[0248] Although the present application has been described with reference to preferred embodiments, various modifications may be made thereto and parts thereof may be replaced with equivalents without departing from the scope of the present application. In particular, the various technical features mentioned in the various embodiments may be combined in any manner as long as there are no structural conflicts. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.
Claims
1. A graphitization furnace, characterized in that: include: A furnace body (210), wherein a material channel (211) is provided in the furnace body (210); a first electrode (220), at least a portion of the first electrode (220) being located in the material channel (211); a second electrode (230) having a polarity opposite to that of the first electrode, comprising an annular electrode portion (231), the annular electrode portion (231) being protrudingly disposed on an inner wall (2111) of the material channel (211) along a radial direction of the material channel (211) and surrounding a partial channel section of the material channel (211); Along the extension direction of the material channel (211), the distance between the end surface of the first electrode (220) and the first plane is H1, the inner diameter of the annular electrode portion (231) is D1, and H1 and D1 satisfy: 0.5≤H1 / D1≤5; The first plane is the plane where the surface (2311) of the annular electrode portion (231) facing the first electrode (220) is located.
2. The graphitization furnace according to claim 1, characterized in that: H1 and D1 satisfy: 0.8≤H1 / D1≤1.
5.
3. The graphitization furnace according to claim 1 or 2, characterized in that: The value range of H1 is 350~3000mm.
4. The graphitization furnace according to claim 1 or 2, characterized in that: The value range of D1 is 430~2400mm.
5. The graphitization furnace according to any one of claims 1 to 4, characterized in that: The outer diameter of the annular electrode portion (231) is D2, and D1 and D2 satisfy: 1.17≤D2 / D1≤3.
6. The graphitization furnace according to claim 5, characterized in that: D1 and D2 satisfy: 1.24≤D2 / D1≤2.
51.
7. The graphitization furnace according to claim 5 or 6, characterized in that: The value range of D2 is 580~2750mm.
8. The graphitization furnace according to any one of claims 1 to 7, characterized in that: Along the radial direction of the material channel (211), the thickness dimension of the annular electrode portion (231) is T, and H1 and T satisfy: 0.6≤H1 / T≤7.
4.
9. The graphitization furnace according to claim 8, characterized in that: H1 and T satisfy: 0.81≤H1 / T≤5.
10. The graphitization furnace according to claim 8 or 9, characterized in that: The value range of T is 130~1500mm.
11. The graphitization furnace according to any one of claims 1 to 10, characterized in that: The first electrode (220) is a cylindrical electrode, the diameter of the first electrode (220) is D3, and D3 and D1 satisfy: 1≤D1 / D3≤3.
4.
12. The graphitization furnace according to claim 11, characterized in that: D3 and D1 satisfy: 1≤D1 / D3≤2.
13. The graphitization furnace according to claim 11 or 12, characterized in that: The value range of D3 is 350~1200mm.
14. The graphitization furnace according to any one of claims 1 to 13, characterized in that: The first electrode (220) is a cylindrical electrode, the diameter of the first electrode (220) is D3, and D3 and H1 satisfy: 0.7≤H1 / D3≤4.
7.
15. The graphitization furnace according to claim 14, characterized in that: D3 and H1 satisfy: 0.7≤H1 / D3≤2.
16. The graphitization furnace according to any one of claims 1 to 15, characterized in that: Along the radial direction of the material channel (211), the cross-sectional area of the first electrode (220) is S1, the cross-sectional area of the annular electrode portion (231) is S2, and S1 and S2 satisfy: 0.8≤S2 / S1≤18.
17. The graphitization furnace according to claim 16, characterized in that: S1 and S2 satisfy: 1.2≤S2 / S1≤12.
18. The graphitization furnace according to claim 16 or 17, characterized in that: The value range of S1 is 0.12~1.2m 2 .
19. The graphitization furnace according to claim 16 or 17, characterized in that: The value range of S2 is 0.15~2.5m 2 .
20. The graphitization furnace according to any one of claims 1 to 19, characterized in that: The second electrode (230) further includes a current-conducting electrode portion (232); One end of the current-conducting electrode portion (232) is connected to the annular electrode portion (231), and the other end is connected to a power source; The contact surface area between the guide electrode portion (232) and the annular electrode portion (231) is S3, the outer surface area of the annular electrode portion (231) is S4, and S3 and S4 satisfy: 1.5≤S4 / S3≤8.
21. The graphitization furnace according to claim 20, characterized in that: S3 and S4 satisfy: 3≤S4 / S3≤5.
22. The graphitization furnace according to claim 20 or 21, characterized in that: The value range of S3 is 0.15~1.1m 2 .
23. The graphitization furnace according to claim 20 or 21, characterized in that: The value range of S4 is 0.5~7m 2 .
24. The graphitization furnace according to any one of claims 20 to 23, characterized in that: Along the radial direction of the material channel (211), the bottom surface of the guide electrode portion (232) is flush with the bottom surface of the annular electrode portion (231); Along the extension direction of the material channel (211), the height dimension of the annular electrode portion (231) is H2, and the height dimension of the guide electrode portion (232) is H3, and H2 and H3 satisfy: 1≤H2 / H3≤4.
25. The graphitization furnace according to claim 24, characterized in that: H2 and H3 satisfy: 1≤H2 / H3≤1.
8.
26. The graphitization furnace according to claim 24 or 25, characterized in that: The value range of H2 is 400~2000mm.
27. The graphitization furnace according to claim 24 or 25, characterized in that: The value range of H3 is: 350~1200mm.
28. The graphitization furnace according to any one of claims 1 to 27, characterized in that: The graphitization furnace further comprises a first heat-insulating layer (240), which is arranged at the innermost side of the furnace body (210) and forms a partial channel section of the material channel (211).
29. The graphitization furnace according to claim 28, characterized in that: The thermal conductivity of the first thermal insulation layer (240) is 0.05-5w / mk; or The compressive strength of the first thermal insulation layer (240) is 0.1-40 MPa; or The first thermal insulation layer (240) has a temperature resistance of 1800 to 3200°C.
30. The graphitization furnace according to claim 28 or 29, characterized in that: The graphitization furnace further comprises a second thermal insulation layer (250) disposed on a side of the first thermal insulation layer (240) facing the outside of the furnace body (210).
31. The graphitization furnace according to claim 30, characterized in that: The thermal conductivity of the second thermal insulation layer (250) is 0.1-20w / mk; or The compressive strength of the second thermal insulation layer (250) is 20-60 MPa; or The second thermal insulation layer (250) has a temperature resistance of 1500-3200° C.; or The ash content of the second thermal insulation layer (250) is 0.1-10%.
32. The graphitization furnace according to claim 30 or 31, characterized in that: The graphitization furnace further comprises a third thermal insulation layer (260) disposed on a side of the second thermal insulation layer (250) facing the outside of the furnace body (210).
33. The graphitization furnace according to claim 32, characterized in that: The third thermal insulation layer (260) contains more than 30% alumina; or The compressive strength of the third thermal insulation layer (260) is 5 to 60 MPa; or The third thermal insulation layer (260) has a temperature resistance of 1000-2000°C.
34. A battery production system, characterized in that: include: The graphitization furnace according to any one of claims 1 to 33, wherein the graphitization furnace is used to produce negative electrode graphite material for a battery.
Citation Information
Patent Citations
Vertical high temperature continuous graphitizing furnace
CN101786619A
Ultra-high temperature purification furnace for scattered carbon material
CN108046235A
Electro-calcining high temperature graphitization furnace
CN109081336A
Aluminum electrolysis waste cathode treatment device and method
CN113324418A
Vertical graphitization furnace
CN114166013A
Cited By
Graphitization furnace and battery production equipment
CN119554867A