Negative plate and battery

By constructing a porous morphology on the surface of the negative electrode sheet of the lithium-ion battery and using oil-based and water-based binders to form depressions, the problem of lithium precipitation in the negative electrode during fast charging is solved, the dynamic performance and cycle life of the battery are improved, and the Fast charging and lifespan compatibility.

CN118867115APending Publication Date: 2024-10-29ZHUHAI COSMX BATTERY CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410848548.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

During the fast charging process of existing lithium-ion batteries, lithium precipitation in the negative electrode leads to capacity attenuation and power loss, and fast charging is difficult to be compatible with life and energy density. The main reason is that the SEI of the graphite negative electrode cannot withstand the mechanical stress caused by fast charging, resulting in structural Exfoliation and electrolyte co-embedding.

Method used

By constructing a porous morphology on the surface of the negative electrode sheet, the first and second active layers composed of oil-based binder and water-based binder are used to form a porous structure of recessed parts and non-depressed parts, thereby improving the electrolyte migration ability and avoiding lithium Metal precipitation.

Benefits of technology

It improves the dynamic performance of the negative electrode, extends the cycle life of the battery, shortens the manufacturing time, reduces the manufacturing cost, improves the fast charging performance and energy density of the battery, avoids the precipitation of lithium metal, and enhances the stability of the pole piece.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118867115A_ABST
    Figure CN118867115A_ABST
Patent Text Reader

Abstract

The invention relates to the field of batteries, and provides a negative plate and a battery, the negative plate comprises a negative current collector, a first active layer coated on the surface of the negative current collector, and a second active layer coated on the surface, far away from the negative current collector, of the first active layer, and the second active layer comprises a concave part and a non-concave part; the first active layer comprises a first negative electrode active material and an oil-based binder, and the second active layer comprises a second negative electrode active material and an aqueous binder; and the content of the oil-based binder in the first active layer is greater than the content of the water-based binder in the second active layer. The negative plate can improve the dynamic performance of the negative electrode, prevents lithium metal from being separated out in the fast charging process of the battery, and improves the fast charging performance of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a negative electrode sheet and a battery. Background Art

[0002] With the rapid development of 3C electronic products, people have put forward higher and higher requirements for the fast charging capabilities of lithium-ion batteries. As a key breakthrough in solving the convenience of charging electric vehicles, breakthroughs in fast charging technology will enhance the user experience of terminal products. Battery fast charging technology has become the core competitiveness of power battery companies to participate in future market competition and is rapidly iterating and innovating. However, from the perspective of battery cell performance, fast charging is difficult to be compatible with life and energy density. At the same time, frequent fast charging will lead to rapid degradation of charging acceptance, energy density, power capacity and other performance. It is generally believed that fast charging is a problem of battery reaction kinetics, involving lithium ion transmission in the electrolyte and lithium ion diffusion in the solid electrode. Other performance is mainly related to material degradation caused by fast charging.

[0003] A large number of studies have shown that negative electrode lithium deposition is the main cause of capacity decay and power loss in lithium-ion batteries. Theoretically, the formation of negative electrode lithium metal is due to the low Coulomb efficiency of lithium metal and the side reaction of metallic lithium with electrolyte solvents. Both reactions will deplete the active Li in the battery that can be deintercalated between the positive and negative electrode materials. + , while consuming a large amount of electrolyte, resulting in a large amount of gas generated inside the battery and causing the SEI to grow out of control. However, in fact, fast charging does not always trigger lithium precipitation, because in normal lithium-ion batteries, the impedance of the graphite negative electrode is much lower than the impedance of the positive electrode. Many studies have shown that the polarization caused by normal fast charging is not enough to drive the potential of the graphite negative electrode to the potential of metallic lithium deposition. Even without the precipitation of metallic lithium, fast charging will still accelerate the capacity decay and impedance growth of the battery. The failure of SEI on the graphite surface is one of the main reasons for the above phenomenon. The main reason is that SEI cannot withstand the mechanical stress caused by the rapid expansion of the graphite particles during fast charging, which leads to the exfoliation of the graphite structure and ultimately leads to the out-of-control growth of SEI; the destruction of SEI will also lead to the solvation of Li + Co-embedding of ions. To address the problem of lithium deposition at the negative electrode, a porous morphology can be constructed on the surface of the negative electrode to achieve rapid migration of the electrolyte, thereby improving the kinetic performance of the negative electrode. How to provide a new negative electrode with a porous surface is an urgent problem to be solved in order to achieve super-fast charging of lithium-ion batteries. Summary of the invention

[0004] The purpose of the present invention is to overcome the above-mentioned problems existing in the prior art and to provide a negative electrode sheet and a battery, wherein the negative electrode sheet can improve the kinetic performance of the negative electrode, avoid lithium metal precipitation during the fast charging process of the battery, and improve the fast charging performance of the battery.

[0005] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides a negative electrode sheet, which comprises a negative electrode collector, a first active layer coated on the surface of the negative electrode collector, and a second active layer coated on the first active layer away from the surface of the negative electrode collector, wherein the second active layer comprises a recessed portion and a non-recessed portion; the first active layer comprises a first negative electrode active material, a first conductive agent and an oil-based binder, and the second active layer comprises a second negative electrode active material, a second conductive agent and an aqueous binder; and the content of the oil-based binder in the first active layer is greater than the content of the aqueous binder in the second active layer.

[0006] In some embodiments, a ratio of the thickness of the first active layer to the thickness of the second active layer is 0.1-0.8.

[0007] A second aspect of the present invention provides a battery, comprising the negative electrode sheet described in the first aspect.

[0008] The present invention adopts the above technical solution to achieve the following beneficial effects:

[0009] The present invention contains an oil-based binder in the first active layer and a water-based binder in the second active layer. Without adding additional pore-forming materials and negative doping treatment processes, a negative electrode sheet with a porous structure having the recessed portion is obtained through the physical and chemical properties of the coating itself.

[0010] By constructing a porous structure on the surface of the negative electrode, the electrolyte retention capacity of the battery cell can be effectively improved, the cycle life and capacity retention rate of the battery can be extended; moreover, the electrolyte penetration rate can be accelerated, the aging time in the battery manufacturing process can be shortened, and the manufacturing cost of the battery can be reduced. By constructing a porous structure on the surface of the electrode, the proportion of the non-solid part of the electrode is increased, the expansion process of the electrode is reduced, the expansion ratio of the overall electrode is alleviated, and the risk of battery deformation is reduced.

[0011] The negative electrode kinetic performance of the battery prepared by the negative electrode sheet of the present invention is improved, and lithium metal precipitation is avoided during the fast charging process of the battery, thereby improving the fast charging performance of the battery.

[0012] The endpoints and any values ​​of the range disclosed in this article are not limited to the precise range or value, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Herein, in the absence of special instructions, data ranges include endpoints. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 Shown is a microscope photograph of the surface of the negative electrode sheet after rolling.

[0014] Figure 2 Shown is a scanning electron microscope photograph of the surface of the negative electrode sheet after rolling, and b is an enlarged view of the square area in a.

[0015] Figure 3 The figure shows a partial cross-sectional view of the negative electrode sheet without a recessed portion after rolling.

[0016] Figure 4 Shown is a partial cross-sectional view of the concave portion of the pole piece after rolling.

[0017] Figure 5 Shown are photos of the negative electrode sheet before and after rolling, a is before rolling, and b is after rolling. DETAILED DESCRIPTION

[0018] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0019] Unless otherwise defined, all scientific and technical terms used in the present invention have the same meanings as commonly understood by one of ordinary skill in the art to which the present invention relates.

[0020] A first aspect of the present invention provides a negative electrode sheet, which comprises a negative electrode collector, a first active layer coated on the surface of the negative electrode collector, and a second active layer coated on the first active layer away from the surface of the negative electrode collector, wherein the second active layer comprises a recessed portion and a non-recessed portion; the first active layer comprises a first negative electrode active material, a first conductive agent, and an oil-based binder, and the second active layer comprises a second negative electrode active material, a second conductive agent, and an aqueous binder; and the content of the oil-based binder in the first active layer is greater than the content of the aqueous binder in the second active layer.

[0021] In the present invention, an oil-based binder (such as PVDF) is used in the first active layer, and an aqueous binder is used in the second active layer, that is, the solvent used in the second active layer is a non-solvent of the binder of the first active layer. When the aqueous slurry is applied on the surface of the first active layer to prepare the second active layer, because water is not a good solvent for the oil-based binder, the oil-based binder cannot be wetted by water at all. Due to the local hydrophobic properties, non-wetting areas (such as shrinkage holes) exist, and these non-wetting areas form pits during the drying process of the second active layer. Without adding additional pore-forming materials, a recessed structure is formed on the second active layer, and the method is simple and reduces costs.

[0022] In the present invention, the oil-based binder refers to a binder using organic matter as a solvent, and the corresponding slurry formed is an oil-based slurry. In some embodiments, the oil-based binder includes at least one of polyvinylidene fluoride (PVDF), polyacrylonitrile compounds (PAN), polyimide compounds (PI), perfluorosulfonic acid ionomer compounds (Nafion), polypropylene oxide, polytetrafluoroethylene (PTFE), polymethyl methacrylate (PMMA), polyvinyl butyral (PVB), polyacrylonitrile, polyvinyl chloride, polyvinylidene fluoride-co-hexafluoropropylene, polyethylene imine, polymethyl methacrylate, polyvinyl pyrrolidone, polyvinyl acetate, polyethylene-co-vinyl acetate (EVA), polyarylate, polystyrene acyl p-phenylenediamine polyethylene oxide, polyoxymethylene, SD-3, polyvinyl chloride, polyethylene, polypropylene, epoxy resin and nylon.

[0023] In the present invention, the water-based binder refers to a water-soluble binder, and the corresponding slurry formed is a water-based slurry. In some embodiments, the water-based binder includes at least one of methyl cellulose (MC), ethyl cellulose (EC), hydroxyethyl cellulose (HEC), carboxymethyl cellulose (CMC), hydroxypropyl cellulose, diacetyl cellulose, styrene-butadiene rubber (SBR), polyvinyl alcohol (PVA), polyacrylate compounds (such as LA series), polyacrylic binders (such as polyacrylic acid (PAA)), sodium alginate (ALG), chitosan (CTS), carboxymethyl chitosan (C-CTS), and water-based acrylic resin.

[0024] In some embodiments, the oil-based binder is different from the water-based binder. The polarity of the oil-based binder is lower than that of the water-based binder. The solvent corresponding to the oil-based binder is an organic solvent, such as N-methylpyrrolidone NMP, and the solvent corresponding to the water-based binder is water.

[0025] In some embodiments, the content of the oil-based binder in the first active layer is 3-20wt%, for example, 3wt%, 5wt%, 8wt%, 10wt%, 12wt%, 14wt%, 16wt%, 18wt%, or 20wt%.

[0026] In some embodiments, the content of the aqueous binder in the second active layer is 0.6-6wt%, such as 0.6wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt%, 5wt%, 5.5wt%, 6wt%. When the content of the aqueous binder is smaller, it is not conducive to the stability of the pole piece, resulting in poor wettability of the pole piece, significantly reduced peeling force, and poor cycle performance and dynamic performance of the battery.

[0027] In some embodiments, the ratio of the content of the oil-based binder in the first active layer to the content of the aqueous binder in the second active layer is 2-20, such as 2, 4, 6, 8, 10, 12, 14, 16, 18, 20. Within this range, holes of good size, depth, and arrangement can be formed, which is beneficial to improve the wetting of the electrode and improve the dynamic performance of the battery. When the ratio is too high and the content of the aqueous binder in the second active layer is too low, the peeling force between the first active layer and the second active layer is reduced, and there is a risk of falling off. According to experimental tests, foil leakage will occur, affecting the production yield of the electrode. When the ratio is too small and the content of the oil-based binder in the first active layer is too low, the holes formed are small and the number is small, and no obvious beneficial effect can be achieved.

[0028] In some embodiments, the thickness ratio of the first active layer to the second active layer is 0.1-0.8, such as 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8. By controlling the thickness ratio of the first active layer to the second active layer and the content of the oil-based binder in the first active layer being greater than the content of the water-based binder in the second active layer, it is possible to obtain pits of suitable size and regular shape, which is beneficial to improve the wettability of the pole piece, improve the peeling strength of the pole piece, alleviate or even inhibit the lithium precipitation of the battery, and improve the cycle performance and dynamic performance of the battery. When the thickness of the first active layer is too small, the second active layer will completely cover the surface of the first active layer due to its large thickness, and basically no surface pits can be formed; when the thickness of the first active layer is too large, large and irregular pits will appear after the second active layer is coated.

[0029] In some embodiments, the thickness of the first active layer is 10-200 μm, such as 10 μm, 20 μm, 40 μm, 60 μm, 80 μm, 100 μm, 120 μm, 140 μm, 160 μm, 180 μm, or 200 μm.

[0030] In some embodiments, the second active layer has a thickness of 100-500 μm, such as 100 μm, 150 μm, 200 μm, 250 μm, 300 μm, 350 μm, 400 μm, 450 μm, or 500 μm.

[0031] In some embodiments, the porosity of the negative electrode sheet is 20%-50%, such as 20%, 25%, 30%, 35%, 40%, 45%, 50%. The method for determining the porosity is described in GB / T 42697-2023.

[0032] In some embodiments, in the second active layer, along the thickness direction of the negative electrode sheet, the projection area of ​​the recessed portion accounts for 10%-35% of the projection area of ​​the non-recessed portion, such as 10%, 15%, 20%, 25%, 30%, 35%; when it is less than this range, there are too few surface pits, and the effect of improving the electrolyte infiltration efficiency and the rate performance cannot be achieved; if the area of ​​the recessed portion accounts for too large a proportion, the amount of lithium ions accommodated by the entire electrode sheet is reduced, affecting the energy density of the battery. It should be understood that the projection is projected along the thickness direction of the electrode sheet, and the projection area of ​​the recessed portion is calculated based on the area formed by the projection of the outer contour of the pit.

[0033] In some embodiments, the recessed portion comprises a contraction-shaped hole, that is, the size of the hole formed by the side wall of the recessed portion decreases from top to bottom or from outside to inside, for example Figure 2 As shown, from Figure 2 It can be seen from Figure b that the bottom and side surfaces of the recessed portion are uneven.

[0034] In some embodiments, the upper sidewall surface of the contraction-shaped hole is a sloped surface, such as Figure 4 As shown, the inclination angle is preferably 10°-70°.

[0035] In some embodiments, the depth of the recessed portion is less than or equal to the thickness of the second active layer.

[0036] In some embodiments, the ratio L / S of the long diameter L to the short diameter S of the projection of the recessed portion is 1-2. When L / S is too large, it means that the formed pits are poor (the ideal state is densely distributed circular pits). There are two situations. One is that the coating of the upper layer is too thick, resulting in most of the formed pits being covered, and the remaining pits being partially covered, resulting in a large aspect ratio of the pits; the other situation is that when the thickness of the upper layer is small, the shrinkage cavity during the wet film formation process is particularly serious, forming large-area pits with very irregular contours. Among them, the long diameter L is the size of the longest line segment that can be obtained by two points in the outer contour of the recessed portion, and the short diameter S is the size of the shortest line segment that can be obtained by two points in the outer contour diameter of the recessed portion.

[0037] In some embodiments, the first negative electrode active material and the second active material each independently include a carbon-based material and / or a non-carbon-based material.

[0038] In some embodiments, the carbon-based material includes at least one of graphite (such as natural graphite, artificial graphite, and mesophase carbon spheres), amorphous carbon (such as coke, mesophase carbon microspheres, carbon fiber, epoxy resin, phenolic resin, etc.), doped carbon (such as carbon materials doped with elements such as boron, phosphorus, and silicon), and nanocarbon materials (such as carbon nanotubes, graphene, etc.).

[0039] In some embodiments, the non-carbon-based materials include silicon-based materials, conductive polymers (such as polyacetylene and polypyrrole), metals (such as lithium, tin, aluminum, zirconium and titanium), metal oxides (such as titanium oxide, lithium-titanium oxide, tin-based oxides, etc.), metal alloys (such as alloys composed of at least two metals among lithium, tin, aluminum, zirconium, manganese and titanium, such as lithium-tin alloys, lithium-aluminum alloys, lithium-aluminum-manganese alloys), titanium-based materials (such as lithium titanate (Li4Ti5O 12 , LTO), titanium niobate (TiNb2O7, TNO) and TiO2, etc.), tin-based materials (such as tin-carbon composite materials) and at least one of nitrides (such as Li3FeN2, Cu3N).

[0040] In some embodiments, the silicon-based material may be silicon, silicon oxide (SiO x ), silicon-carbon composite materials (for example, carbon particles coated with silicon and / or silicon carbide on the surface, silicon particles or silicon oxide particles coated with carbon and / or silicon carbide on the surface, and silicon carbide), and silicon alloys (for example, silicon-aluminum alloys, silicon-lithium alloys, silicon-nickel alloys, silicon-ferrosilicon alloys, silicon-titanium alloys, silicon-manganese alloys, silicon-copper alloys, silicon-tin alloys), etc.

[0041] In some embodiments, the first conductive agent and the second conductive agent each independently include at least one of conductive carbon black, acetylene black (AB), Ketjen black (KB), carbon nanotubes (CNTs), graphite, nanocarbon fiber (VGCF), superconducting carbon, carbon dots, graphene, polyacetylene, polyaniline, polypyridine, polythiophene, polythiourea, indium tin oxide, and polyphenylene derivatives. Conductive carbon black is, for example, SUPER PLi (SP) and EnsacoTM. Graphite can be graphite KS6, graphite KS15, graphite SFG15, and graphite SFG6.

[0042] In some embodiments, in the first active layer, the content of the first negative electrode active material is 75-96wt%, such as 75wt%, 80wt%, 85wt%, 90wt%, 95wt%, 96wt%; the content of the first conductive agent is 1-5wt%, such as 1wt%, 2wt%, 3wt%, 4wt%, 5wt%.

[0043] In some embodiments, in the second active layer, the content of the second negative electrode active material is 89-98.9wt%, such as 89wt%, 90wt%, 92wt%, 94wt%, 96wt%, 98wt%, 98.9wt%; the content of the second conductive agent is 0.5-5wt%, such as 0.5wt%, 1wt%, 2wt%, 3wt%, 4wt%, 5wt%.

[0044] In some embodiments, the surface density of the first active layer is 4-15 mg cm -2 .

[0045] In some embodiments, the surface density of the second active layer is 10-25 mg cm -2 .

[0046] In some embodiments, the negative electrode current collector is a single current collector or a composite current collector.

[0047] In some embodiments, the material of the single current collector includes at least one of copper, lithium, titanium, nickel, stainless steel, carbon black, graphene, carbon fiber, and carbon nanotubes.

[0048] In some embodiments, the composite current collector comprises a polymer layer and a coating layer located on the surface of the polymer layer.

[0049] In some embodiments, the material of the polymer layer includes at least one of polyimide (PI), polyethylene terephthalate (PET), and polypropylene (PP).

[0050] In some embodiments, the material of the coating includes at least one of copper, lithium, titanium, nickel, stainless steel, carbon black, graphene, carbon fiber, and carbon nanotubes.

[0051] A second aspect of the present invention provides a battery, comprising the negative electrode sheet described in the first aspect.

[0052] In some embodiments, the battery is a lithium-ion battery.

[0053] The battery may be a liquid electrolyte battery, a semi-solid battery, or an all-solid battery.

[0054] The components of the battery other than the negative electrode (such as the positive electrode, separator, electrolyte, aluminum-plastic film, etc.) can all be conventionally selected in the art.

[0055] In some embodiments, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer coated on at least one side of the positive electrode current collector, and the positive electrode active material layer includes a positive electrode active material, a conductive agent, and a binder. The type of the conductive agent can refer to the first aspect, and the type of the binder can refer to the oil-based binder.

[0056] The positive electrode active material may be selected conventionally in the art, for example, the positive electrode active material comprises at least one of lithium cobalt oxide (LCO), nickel cobalt manganese ternary material (NCM), nickel cobalt aluminum ternary material (NCA), nickel cobalt manganese aluminum quaternary material (NCMA), lithium iron phosphate (LFP), lithium manganese phosphate (LMP), lithium vanadium phosphate (LVP), lithium manganese oxide (LMO), lithium nickel oxide, nickel manganese oxide binary material, lithium-rich manganese-based and lithium iron manganese phosphate. The positive electrode active material may also include doped and / or coated positive electrode active materials.

[0057] In some embodiments, the mass percentage of each component in the positive electrode active material layer is: 80-99.5wt% of positive electrode active material, 0.25-10wt% of conductive agent, and 0.25-10wt% of binder.

[0058] If there is no special explanation, other options of the lithium battery are conventional options in the art. The battery can be assembled in a conventional manner in the art.

[0059] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0060] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.

[0061] The present invention is described in detail below in conjunction with specific embodiments, which are used to understand but not to limit the present invention.

[0062] Morphology measurement: Microscope and SEM are mainly used for observation and analysis of the surface morphology and cross-section of the negative electrode sheet. The SEM model is JSN-7001F produced in Japan, with an acceleration voltage of 0.5 to 30 kV and a magnification of 250,000 to 1 million times.

[0063] Example 1

[0064] (1) Positive electrode

[0065] Lithium cobalt oxide, conductive carbon black and PVDF (model HSV900) were mixed evenly in a mass ratio of 95.2:3:1.8, dissolved in N-methylpyrrolidone, and stirred evenly to form a positive electrode slurry with a solid content of 70wt%. The slurry was evenly coated on an aluminum foil, and then dried, rolled, and cut into positive electrode sheets.

[0066] (2) Negative electrode

[0067] First active layer: Graphite, carbon nanotubes and oil-based binder PVDF are mixed evenly in a mass ratio of 88.7:1.3:10 (i.e., in the first active layer, the binder content N1 is 10wt%), added to NMP, stirred evenly to prepare a negative electrode slurry with a solid content of 50wt%, evenly coated on copper foil, and dried. The thickness T1 of the first active layer is 50μm, and the surface density is 5.85mg cm -2 .

[0068] Second active layer: Graphite, carbon nanotubes and aqueous binder polyacrylic acid PAA were mixed evenly in a mass ratio of 97.5:1.5:1 (i.e., in the second active layer, the binder content N2 was 1wt%), added to deionized water, stirred evenly to prepare a negative electrode slurry with a solid content of 50wt%, and evenly coated on the first active layer, dried, rolled, and cut to prepare a negative electrode sheet. The thickness of the second active layer was 200μm and the surface density was 15.35mg cm -2 .

[0069] like Figure 5 As shown in Figures a and b in Figure 2, there are multiple pits on the surface of the negative electrode sheet before and after rolling. Figure 1 As shown, the outer contour of the pit in the negative electrode sheet after rolling is circular or quasi-circular. Figure 2 Figure a shows a scanning electron microscope photo of the surface of the negative electrode sheet after rolling. Figure 2 Figure b shows a scanning electron microscope photo of the square area (depression) on the surface of the negative electrode sheet after rolling. Figure 4 The partial cross-sectional view of the concave portion of the pole piece after rolling shows that the concave portion contains shrinkage-shaped holes, that is, the size of the holes formed by the side walls of the concave portion decreases from the outside to the inside, and the bottom and side surfaces of the concave portion are uneven. The upper side wall surface of some shrinkage-shaped holes is a slope surface with an inclination angle in the range of 10°-70°. Figure 3 The figure shows a partial cross-sectional view of the negative electrode sheet after rolling without a depressed portion. The first active layer and the second active layer of the negative electrode sheet contain a large number of pores. According to the measurement, the porosity of the negative electrode sheet is 38.2%.

[0070] Specific parameters of the negative electrode sheet and the recessed portion are shown in Table 1, wherein the thickness of the first active layer is T1, the thickness of the second active layer is T2, the content of the binder in the first active layer is N1, the content of the binder in the second active layer is N2, the depth of the recessed portion is a, the ratio of the projected area of ​​the recessed portion to the non-recessed portion is R, and the ratio of the major diameter L to the minor diameter S of the projection of the recessed portion is L / S.

[0071] (3) Electrolyte

[0072] In the electrolyte, the electrolyte salt is 1 mol / L lithium hexafluorophosphate, the organic solvent is a mixture of EC, DEC and EMC in a mass ratio of 2:3:5, and the additive is 5 wt% fluoroethylene carbonate.

[0073] (4) Battery assembly

[0074] The prepared positive electrode sheet, the polyethylene porous separator and the prepared negative electrode sheet are stacked in sequence, wound to obtain a winding core, and then packaged, injected, formed and sorted to make a battery.

[0075] Example 2 and Comparative Example 1

[0076] The operation was carried out according to the method described in Example 1, except that the content of the oil-based binder in the first active layer was different, as shown in Table 1.

[0077] Among them, in the comparative example 1 group, due to the small value of N1 / N2, the number of pits on the surface of the negative electrode sheet is small and the holes are also small, or even the pits cannot be formed. As N1 increases, the proportion of pits gradually increases.

[0078] Example 3 Group

[0079] The operation was performed according to the method described in Example 1, except that the thicknesses of the first active layer and the second active layer were different, as shown in Table 1.

[0080] In Example 3g, the thickness of the first active layer is too small, and the coating thickness of the second active layer is too large, which makes T1 / T2 too small, and the number of pits on the surface of the prepared negative electrode sheet is small and the size is also small, and the total area of ​​the pits accounts for a small proportion; in Example 3h, the thickness of the first active layer is too large, which makes T1 / T2 too large. After the second active layer is coated, larger pits will appear, and the depth of the pits is close to the thickness of the second active layer, and L / S is large, mostly in the range of 3-4.

[0081] Example 4

[0082] The operation was carried out according to the method described in Example 1, except that the thicknesses of the first active layer and the second active layer were different and the content of the oil-based binder in the first active layer was different from the content of the water-based binder in the second active layer, as shown in Table 1.

[0083] Table 1

[0084] serial number <![CDATA[T1 / μm]]> <![CDATA[T2 / μm]]> <![CDATA[T1 / T2]]> <![CDATA[N1 / wt%]]> <![CDATA[N2 / wt%]]> <![CDATA[N1 / N2]]> R Negative electrode porosity / % Example 1 50 200 0.25 10 1 10 30.2% 38.2 Example 2a * * * 15 1 15 28.1% 34.9 Example 2b * * * 10 2 5 29.5% 35.6 Example 2c * * * 20 1 20 29.7% 32.5 Example 2d * * * 5 1 5 26.1% 28.3 Example 2e * * * 10 0.8 12.5 27.2% 28.5 Comparative Example 1a * * * 5 5 1 3.2% 26.5 Comparative Example 1b * * * 3 5 0.6 2.5% 25.7 Comparative Example 1c * * * 1 5 0.2 1.4% 24.4 Example 3a * 100 0.5 * * * 28.5% 35.5 Example 3b * 300 0.17 * * * 22.9% 34.6 Example 3c * 400 0.13 * * * 21.4% 32.5 Example 3d 25 * 0.13 * * * 19.9% 30.6 Example 3e 75 * 0.38 * * * 27.8% 36.1 Example 3f 100 * 0.5 * * * 20.4% 31.4 Example 3g 15 235 0.06 * * * 4.6% 27.1 Example 3h 150 100 1.5 * * * 15.8% 28.0 Example 4 100 150 0.67 15 5 3 26.4% 33.2

[0085] Note: "*" indicates the same as Example 1.

[0086] Example 5 Group

[0087] The operation was carried out according to the method described in Example 1, except that the types of aqueous binders and / or oily binders used in the negative electrode sheets were different, as shown in Table 2.

[0088] Table 2

[0089] serial number Oil-based adhesive Water-based adhesive Example 1 PVDF PAA Example 5a Polyimide compounds (PI) * Example 5b Polyacrylonitrile compounds (PAN) * Example 5c * Polyvinyl alcohol (PVA) Example 5d * Polyvinylpyrrolidone (PVP)

[0090] Note: "*" indicates the same as Example 1.

[0091] Test Case

[0092] The performance of the negative electrode sheets and batteries prepared in the embodiments and preparation examples was evaluated, and the specific evaluation method is as follows.

[0093] (1) Electrolyte infiltration test method:

[0094] The electrode is infiltrated by the dripping method. The electrode to be tested is placed on a flat surface, 20 μL of electrolyte is sucked with a pipette, and dropped vertically on the surface of the electrode. A stopwatch is used to record the time. The time taken for the electrolyte to completely infiltrate the electrode is recorded as the electrolyte infiltration rate of the electrode, in units of s / 20 μL.

[0095] Method for determining the electrolyte retention amount: the weight of the battery cell before injection is W0, the weight of the battery cell after injection is W1, and the electrolyte retention amount = (W1-W0).

[0096] (2) Pole peel strength measurement:

[0097] The negative electrode sheet was cut into test specimens of 20×100mm size for later use; the side of the electrode sheet to be tested was adhered with double-sided tape and compacted with a pressure roller to make it fit the electrode sheet completely; the other side of the double-sided tape of the specimen was adhered to the stainless steel surface, and one end of the specimen was bent in the opposite direction with a bending angle of 180°; the high-speed rail tensile testing machine was used for testing, one end of the stainless steel was fixed to the clamp below the tensile testing machine, and the bent end of the specimen was fixed to the clamp above, the angle of the specimen was adjusted to ensure that the upper and lower ends were in a vertical position, and then the specimen was stretched at a speed of 50mm / min until the negative electrode slurry was completely peeled off from the substrate, the displacement and force during the process were recorded, and the force when the force was balanced was considered to be the peel strength of the electrode sheet.

[0098] (3) Battery performance test:

[0099] The initial capacity of the battery is recorded as C0, and the initial thickness is recorded as t0. At 25°C, the lithium-ion battery is charged to 4.45V at a constant current of 0.5C, then charged to a current of 0.05C at a constant voltage of 4.45V, left to stand for 5 minutes, and then discharged to a different cut-off voltage of 3.0V at a constant current of 1C, left to stand for 2 minutes, which is considered a cycle. According to the above cycle, after 300 cycles, the discharge capacity of the battery is recorded as C1, and the thickness is recorded as t1. The capacity retention rate and cycle expansion rate of the battery are calculated as follows:

[0100] Battery capacity retention rate = C1 / C0*100%;

[0101] Thickness expansion ratio = (actual thickness - initial thickness) / initial thickness × 100%.

[0102] (4) Lithium deposition area ratio

[0103] The test temperature is 0°C, and the full batteries prepared in the embodiments and comparative examples are charged to 4.45V at a constant current of 0.7C, charged to 0.05C at a constant voltage, and discharged to 3.0V at 0.5C after standing for 5 minutes. Then, a 0.7C charge / 0.5C discharge cycle test is performed, and after 20 cycles, the battery cells are removed and disassembled to observe the lithium precipitation phenomenon.

[0104] The judgment is made based on the state of the fully charged electrode when it is disassembled, where a golden electrode indicates no lithium deposition, and a gray electrode indicates lithium deposition. The degree of lithium deposition is determined based on the ratio of the area of ​​lithium deposited (gray) on the fully charged electrode to the area of ​​the entire electrode. The color of the electrode without lithium deposition is used as a reference, and the lithium deposition area is calculated by the ratio of the grayscale values ​​of the photograph of the disassembled electrode. For example, the color information can be extracted and calculated using Photoshop software.

[0105] (5) Battery EIS test:

[0106] The frequency range is generally 10–2~105Hz, with an amplitude of 5mv / s. The test equipment is Zahner, model Zennium Pro. First, select the EIS mode, enter the parameter setting interface, select different modes of impedance test, set the test frequency range, starting frequency point, frequency test sequence, sampling interval, etc., and obtain the results of charge transfer resistance (Rct) and Warburg impedance (Zw).

[0107] The results of the above tests are shown in Table 3.

[0108] Table 3

[0109]

[0110]

[0111] As can be seen from Table 3, in the negative electrode sheet of the present invention, by controlling the type and content of the binder in the first active layer and the second active layer, a concave portion of a certain area can be constructed on the surface of the negative electrode sheet, which can improve the liquid retention capacity and peeling strength of the negative electrode sheet, effectively improve the kinetic performance of the negative electrode, improve the rate performance of the battery, alleviate or even completely inhibit the occurrence of lithium precipitation, and can also reduce the cycle expansion rate of the battery, improve the capacity retention rate of the battery and extend the cycle life of the battery. In the case of preferably further controlling the thickness ratio of the first active layer and the second active layer, the performance of the electrode sheet and the battery can be further improved.

[0112] It should be noted that, in this article, the terms "comprise", "include" or any other variant thereof are intended to cover non-exclusive inclusion, so that the process, method, article or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise one..." do not exclude the presence of other identical elements in the process, method, article or device including the element. In addition, it should be pointed out that the scope of the methods and devices in the embodiments of the present application is not limited to performing functions in the order shown or discussed, and may also include performing functions in a substantially simultaneous manner or in reverse order according to the functions involved, for example, the described method may be performed in an order different from that described, and various steps may also be added, omitted, or combined. In addition, the features described with reference to certain examples may be combined in other examples.

[0113] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A negative electrode sheet, characterized in that: The negative electrode sheet comprises a negative electrode current collector, a first active layer coated on the surface of the negative electrode current collector, and a second active layer coated on the first active layer away from the surface of the negative electrode current collector, wherein the second active layer comprises a depressed portion and a non-depressed portion; the first active layer comprises a first negative electrode active material and an oil-based binder, and the second active layer comprises a second negative electrode active material and an aqueous binder; the content of the oil-based binder in the first active layer is greater than the content of the aqueous binder in the second active layer.

2. The negative electrode sheet according to claim 1, characterized in that: In the first active layer, the content of the oil-based binder is 3-20wt%; and / or In the second active layer, the content of the aqueous binder is 0.6-6wt%; and / or The ratio of the content of the oil-based binder in the first active layer to the content of the water-based binder in the second active layer is 2-20.

3. The negative electrode sheet according to claim 1 or 2, characterized in that: The ratio of the thickness of the first active layer to the thickness of the second active layer is 0.1-0.8; and / or The thickness of the first active layer is 10 μm-200 μm; and / or The thickness of the second active layer is 100 μm-500 μm; and / or The porosity of the negative electrode sheet is 20%-50%.

4. The negative electrode sheet according to any one of claims 1 to 3, characterized in that: In the second active layer, along the thickness direction of the negative electrode sheet, the projected area of ​​the recessed portion accounts for 10%-35% of the projected area of ​​the non-recessed portion; and / or The recessed portion comprises a contraction-shaped hole, the upper sidewall surface of the contraction-shaped hole is a slope surface, and the inclination angle is preferably 10°-70°; Preferably, the ratio L / S of the long diameter L to the short diameter S of the projection of the concave portion is 1-2; Preferably, the depth of the recessed portion is less than or equal to the thickness of the second active layer.

5. The negative electrode sheet according to any one of claims 1 to 4, characterized in that: The oil-based binder comprises at least one of polyvinylidene fluoride, polyacrylonitrile compounds, polyimide compounds, perfluorosulfonic acid ionomer compounds, polypropylene oxide, polytetrafluoroethylene, polymethyl methacrylate, polyvinyl butyral, polyacrylonitrile, polyvinyl chloride, polyvinylidene fluoride-co-hexafluoropropylene, polyethylene imine, polymethyl methacrylate, polyvinyl pyrrolidone, polyvinyl acetate, polyethylene-co-vinyl acetate, polyarylate, polyphenylene acyl paraphenylenediamine polyethylene oxide, polyoxymethylene, SD-3, polyvinyl chloride, polyethylene, polypropylene, epoxy resin and nylon; and / or The water-based binder includes at least one of methyl cellulose, ethyl cellulose, hydroxyethyl cellulose, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, styrene-butadiene rubber, polyvinyl alcohol, polyacrylate compounds, polyacrylic acid binders, sodium alginate, chitosan, carboxymethyl chitosan, and water-based acrylic resin.

6. The negative electrode sheet according to any one of claims 1 to 5, characterized in that: The first negative electrode active material and the second active material each independently comprise a carbon-based material and / or a non-carbon-based material; Preferably, the carbon-based material comprises at least one of graphite, amorphous carbon, doped carbon, and nanocarbon material; Preferably, the non-carbon-based material includes at least one of a silicon-based material, a conductive polymer, a metal, a metal oxide, a metal alloy, a titanium-based material, a tin-based material, and a nitride.

7. The negative electrode sheet according to any one of claims 1 to 6, characterized in that: The first active layer further comprises a first conductive agent; and / or The second active layer further comprises a second conductive agent; Preferably, the first conductive agent and the second conductive agent each independently include at least one of conductive carbon black, acetylene black, Ketjen black, carbon nanotubes, graphite, nanocarbon fibers, superconducting carbon, carbon dots, graphene, polyacetylene, polyaniline, polypyridine, polythiophene, polythiourea, indium tin oxide and polyphenylene derivatives.

8. The negative electrode sheet according to any one of claims 1 to 7, characterized in that: In the first active layer, the content of the first negative electrode active material is 75-96wt%, and the content of the first conductive agent is 1-5wt%; and / or In the second active layer, the content of the second negative electrode active material is 89-98.9wt%, and the content of the second conductive agent is 0.5-5wt%.

9. The negative electrode sheet according to any one of claims 1 to 8, characterized in that: The negative electrode current collector is a single current collector or a composite current collector; Preferably, the material of the single current collector comprises at least one of copper, lithium, titanium, nickel, stainless steel, carbon black, graphene, carbon fiber and carbon nanotube; Preferably, the composite current collector comprises a polymer layer and a coating layer located on the surface of the polymer layer; More preferably, the material of the polymer layer comprises at least one of polyimide, polyethylene terephthalate, and polypropylene; More preferably, the material of the coating comprises at least one of copper, lithium, titanium, nickel, stainless steel, carbon black, graphene, carbon fiber and carbon nanotube.

10. A battery, characterized in that: The battery comprises the negative electrode sheet according to any one of claims 1 to 9.

Citation Information

Cited By

  • Negative composite electrode of lithium ion battery, preparation of negative composite electrode and lithium ion battery

    CN119517933A

  • Preparation method of sodium-ion battery negative electrode plate with composite coating and application of sodium-ion battery negative electrode plate

    CN120767293A