Composite current collector and preparation method and application thereof

By using composite current collectors in lithium batteries, using a carbon material skeleton and a metal conductive layer to form a porous structure, the problem of reduced energy density of metal-based current collectors and poor mechanical strength of non-metal-based current collectors is solved, achieving high mechanical strength and electrical conductivity. performance, improving the cycle and safety performance of the battery.

CN118867261APending Publication Date: 2024-10-29SVOLT ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410859962.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing metal-based current collectors reduce battery energy density, and non-metal-based current collectors have poor mechanical strength, making it difficult to limit the formation of lithium dendrites and the volume change of lithium metal anodes.

Method used

A composite current collector is used, including a carbon material skeleton and a metal conductive layer. A porous structure is formed by plating conductive metal and lithiophilic material layers to improve mechanical strength and conductive properties and limit the generation of lithium dendrites.

Benefits of technology

It achieves high mechanical strength, low density and excellent electrical conductivity, limits the formation of lithium dendrites and the volume change of lithium metal anode, and improves the cycle performance and safety performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118867261A_ABST
    Figure CN118867261A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of batteries, in particular to a composite current collector and a preparation method and application thereof. The composite current collector comprises a composite matrix layer and a lithium-loving material layer located on the surface of the composite matrix layer, and the composite matrix layer comprises a carbon material framework and a metal conductive layer located on the surface of the carbon material framework; the composite current collector has a porous structure. The composite current collector has high mechanical strength, low density and high specific surface area, and can limit the generation of lithium dendrites; the lithium-loving material layer can ensure the lithium metal compounding effect in the preparation of the negative plate and has better adaptability; in addition, the three-dimensional structure pores can limit the volume change of the lithium metal negative electrode in the cycle process, and the cycle performance of the battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of battery technology, and in particular to a composite current collector and a preparation method and application thereof. Background Art

[0002] Since the birth of lithium batteries, researchers have been considering how to introduce lithium metal anodes into lithium batteries. This is because lithium metal anodes have extremely high discharge capacity, extremely low redox potential, and are the metals with the lowest density in nature. However, lithium metal anodes are very likely to produce lithium dendrites due to uneven lithium deposition during the cycle, which in turn will develop a series of safety issues.

[0003] At present, the modification of lithium metal negative electrodes includes electrolyte additives, solid electrolytes and three-dimensional current collector structure design. Among them, since the SEI film will be continuously regenerated during the cycle, the electrolyte additives will be continuously consumed, thus making its modification effect ineffective. In addition, there is currently no effective way to solve the interfacial impedance of solid electrolyte materials, which also limits its further application. Currently, the commonly used three-dimensional current collector structures are metal-based and non-metal-based. The high density of metal-based current collectors will reduce the overall energy density of the battery. The mechanical strength of non-metal-based current collectors is average and it is very easy to collapse during the cycle.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] One object of the present invention is to provide a composite current collector to solve the technical problems that the metal-based current collector of the prior art will reduce the energy density of the battery and the non-metal-based current collector has poor mechanical strength. The composite current collector of the present invention has high mechanical properties, large specific surface area, good conductivity, can limit the formation of lithium dendrites, and limit the volume change of the lithium metal negative electrode during the cycle.

[0006] Another object of the present invention is to provide a method for preparing a composite current collector, which is simple and easy to implement, and the obtained composite current collector has excellent comprehensive properties.

[0007] Another object of the present invention is to provide a negative electrode sheet.

[0008] Another object of the present invention is to provide a battery.

[0009] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0010] A composite current collector comprises a composite matrix layer and a lithium-philic material layer located on the surface of the composite matrix layer, wherein the composite matrix layer comprises a carbon material skeleton and a metal conductive layer located on the surface of the carbon material skeleton; the composite current collector has a porous structure.

[0011] In some embodiments, the lithiophilic material layer comprises zinc oxide.

[0012] In some implementations, the conductive layer is made of copper.

[0013] In some implementations, the thickness L2 of the metal conductive layer satisfies: 0<L2<20μm.

[0014] In some embodiments, the specific surface area S of the composite current collector satisfies: 50m 2 / g≤S≤2000m 2 / g.

[0015] The method for preparing the composite current collector as described above comprises the following steps:

[0016] (a) coating the surface of the porous polymer layer with a conductive metal to form a metal conductive layer to obtain a composite layer;

[0017] (b) immersing the composite layer in a lithium-philic solution;

[0018] (c) heat treating the impregnated composite layer to obtain a three-dimensional composite current collector;

[0019] In some embodiments, the material of the polymer layer includes at least one of polypropylene, polyethylene terephthalate and polyimide.

[0020] In some embodiments, the porosity of the polymer layer is 10% to 80%.

[0021] In some embodiments, the thickness L1 of the porous polymer layer satisfies: 0<L1<20 μm.

[0022] In some embodiments, the plating includes evaporation and / or water electroplating.

[0023] In some embodiments, before the plating, the method further comprises: depositing a metal seed layer on the surface of the porous polymer layer by magnetron sputtering; and performing the plating after the metal seed layer reaches 20 to 100 nm.

[0024] In some embodiments, the lithiophilic solution comprises a zinc salt solution; the anion of the zinc salt is a complex anion or an organic acid radical. In some embodiments, the zinc salt solution comprises one or more of zinc acetate and zinc sulfate.

[0025] In some embodiments, the concentration of the lithiophilic solution is 0.01 to 1 mol / L.

[0026] In some embodiments, the immersion time is 0.5 to 5 hours.

[0027] In some embodiments, the heat treatment includes a drying process and a sintering process;

[0028] In some embodiments, during the heat treatment, the drying temperature is 20 to 60° C., and the drying time is 0.5 to 5 hours.

[0029] In some embodiments, during the heat treatment, the sintering temperature is 300 to 800° C., and the sintering time is 1 to 15 hours.

[0030] In some embodiments, during the heat treatment, the atmosphere of the sintering treatment is a protective gas.

[0031] A negative electrode sheet comprises the composite current collector and a lithium metal layer located on the surface of the composite current collector.

[0032] A battery comprises the negative electrode sheet.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] (1) The composite current collector of the present invention has both high mechanical strength and low density. Compared with the current collector with a pure metal skeleton, it has a lighter density, which can reduce the impact on the energy density of the lithium metal battery. Compared with the non-metallic current collector, it has high mechanical strength and can meet the use requirements of the lithium metal negative electrode. The composite current collector has a high specific surface area and can limit the formation of lithium dendrites. The lithium-philic material layer can ensure better adaptability during the lithium metal composite process. In addition, due to the restraining effect of the three-dimensional structure pores, the volume change of the lithium metal negative electrode during the cycle can also be limited.

[0035] (2) The preparation method of the composite current collector of the present invention comprises stretching the polymer base film to obtain a uniform microporous structure, and plating a conductive metal to form a metal conductive layer to improve the conductive performance. The two can be coordinated to obtain a composite matrix layer with high mechanical strength, low density and good conductivity; the surface of the composite matrix layer is further modified to obtain a material layer with lithium affinity, which is beneficial to the composite effect of lithium metal in the subsequent preparation process of the negative electrode sheet while ensuring the comprehensive performance of the composite current collector, so as to improve the mechanical properties and electrochemical properties of the negative electrode sheet.

[0036] (3) The battery of the present invention has excellent cycle performance and safety performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0038] Figure 1 is a schematic diagram of the cross-sectional structure of the composite current collector of the present invention;

[0039] Figure 2 A schematic diagram of depositing lithium metal on the composite current collector of the present invention;

[0040] Figure 3 It is a comparison chart of the cycle capacity retention rate of the batteries of Example 6 of the present invention and Comparative Example 1;

[0041] Figure 4 It is a comparison chart of the cycle capacity retention rate of the batteries of Example 7 of the present invention and Comparative Example 2.

[0042] Reference numerals:

[0043] 1-composite matrix layer, 101-carbon material skeleton, 102-metal conductive layer, 2-lithium-philic material layer. DETAILED DESCRIPTION

[0044] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.

[0045] According to one aspect of the present invention, the present invention relates to a composite current collector, comprising a composite matrix layer and a lithium-philic material layer located on the surface of the composite matrix layer, wherein the composite matrix layer comprises a carbon material skeleton and a metal conductive layer located on the surface of the carbon material; the composite current collector has a porous structure.

[0046] The composite current collector of the present invention has the advantages of both the mechanical strength of metals and the low density of non-metals, has a high specific surface area, and can limit the generation of lithium dendrites; the lithium-philic material layer can ensure better adaptability during the lithium metal composite process; in addition, due to the restraining effect of the three-dimensional structural pores, it can also limit the volume change of the lithium metal negative electrode during the cycle process.

[0047] In some embodiments, the lithium-philic material layer comprises zinc oxide. The use of zinc oxide in the present invention is more conducive to the lithium metal compounding in the process of preparing the negative electrode sheet, thereby improving the electrical performance of the negative electrode sheet.

[0048] In some implementations, the conductive layer is made of copper.

[0049] In some embodiments, the thickness L2 of the metal conductive layer satisfies: 0<L2<20μm, for example, 1μm, 2μm, 5μm, 6μm, 8μm, 10μm, 12μm, 15μm, 18μm, 20μm, etc., or any range value between the two.

[0050] The polymer layer and the metal conductive layer of the present invention have suitable thicknesses, thereby ensuring that the composite current collector has both light weight and excellent mechanical properties.

[0051] In some embodiments, the negative electrode current collector has a porous structure at the microscopic level.

[0052] In some embodiments, the specific surface area S of the composite current collector satisfies: 50m 2 / g≤S≤2000m 2 / g, for example 50m 2 / g, 80m 2 / g、100m 2 / g, 200m 2 / g、300m 2 / g, 400m 2 / g、500m 2 / g、600m 2 / g、700m 2 / g、800m 2 / g、900m 2 / g、1000m 2 / g、1200m 2 / g、1400m 2 / g、1500m 2 / g、1600m 2 / g、1800m 2 / g, 2000m 2 / g, etc., or any range value between the two. The composite current collector of the present invention has a high specific surface area. During the electrode reaction, the speed of electron transfer is faster than the liquid phase mass transfer speed of lithium ions in the electrolyte, and the current density of the electrode is closely related to the electron transfer step. According to the current density formula j=I / S (j is the current density, I is the current, and S is the electrode surface), when the current I remains unchanged, increasing the electrode surface area S can effectively reduce the current density, thereby achieving the effect of limiting the formation of lithium dendrites.

[0053] According to another aspect of the present invention, the present invention also relates to a method for preparing the composite current collector as described above, comprising the following steps:

[0054] (a) coating the surface of the porous polymer layer with a conductive metal to form a metal conductive layer to obtain a composite layer; (b) immersing the composite layer in a lithium-philic solution; (c) subjecting the immersed composite layer to a high-temperature heat treatment to obtain a three-dimensional composite current collector.

[0055] The preparation method of the composite current collector of the present invention comprises the following steps: stretching the polymer base film to obtain a uniform microporous structure, and plating a conductive metal to form a metal conductive layer to improve the conductive performance. The two can be coordinated to obtain a composite matrix layer with high mechanical strength, light weight and good conductivity; the surface of the composite matrix layer is further modified to obtain a material layer with lithium affinity, which is beneficial to the composite effect of lithium metal in the subsequent preparation process of the negative electrode sheet on the basis of ensuring the comprehensive performance of the composite current collector, so as to improve the mechanical properties and electrochemical properties of the negative electrode sheet.

[0056] In some embodiments, the material of the porous polymer layer includes at least one of polypropylene (PP), polyethylene terephthalate (PET) and polyimide (PI). The polymer layer of the present invention can select any one of the above, or a combination of at least two, such as a combination of polypropylene and polyethylene terephthalate, a combination of polyethylene terephthalate and polyimide, a combination of polypropylene, polyethylene terephthalate and polyimide, etc. The porosity is 10% to 80%, such as 10%, 20%, 30%, 40%, 50%, 60%, 70% or 80%, etc. The porous polymer layer is subsequently subjected to high temperature heat treatment to form the above-mentioned carbon material skeleton.

[0057] In some embodiments, the thickness L1 of the porous polymer layer satisfies: 0<L1<20μm, for example 1μm, 2μm, 5μm, 6μm, 8μm, 10μm, 12μm, 15μm, 18μm, 20μm, etc., or any range between the two.

[0058] In some embodiments, the plating includes evaporation and / or water electroplating. The present invention uses conventional evaporation and / or water electroplating to obtain a metal conductive layer of suitable thickness to ensure conductive properties.

[0059] In some embodiments, before the plating, the method further includes: depositing a metal seed layer on the surface of the polymer layer by magnetron sputtering. The metal seed is applied to the skeleton of the polymer layer by magnetron sputtering, which has strong adhesion and is beneficial to the subsequent plating effect, ensuring the composite effect of the metal conductive layer and the polymer layer, and improving the mechanical strength and conductive properties of the composite matrix layer. The subsequent plating process begins after the metal seed layer reaches 20-100nm (for example, 20nm, 30nm, 40nm, 50nm, 60nm, 80nm or 100nm, etc.).

[0060] In some embodiments, the lithiophilic solution includes a zinc salt solution; the anion of the zinc salt is a complex anion or an organic acid radical.

[0061] In some embodiments, the concentration of the lithiophilic solution is 0.01 to 1 mol / L, such as 0.01 mol / L, 0.02 mol / L, 0.05 mol / L, 0.1 mol / L, 0.5 mol / L, 0.8 mol / L, 1 mol / L, etc., or any range between the two. A lithiophilic solution of appropriate concentration is more conducive to surface modification of the composite substrate layer.

[0062] In some embodiments, the immersion time is 0.5 to 5 hours, for example, but not limited to 0.5 hours, 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, 4 hours or 5 hours, or any range between the two. The present invention adopts a suitable immersion treatment time to ensure the treatment effect and improve the mechanical properties, conductive properties and lithium affinity of the composite current collector.

[0063] In some embodiments, the heat treatment includes a drying process and a sintering process.

[0064] In some embodiments, the drying temperature is 20-60°C, for example, but not limited to 20°C, 25°C, 30°C, 40°C, 50°C, 55°C, 60°C, etc., or any range between the two. The drying time is 0.5-5h, for example, but not limited to 0.5h, 1h, 1.5h, 2h, 3h, 4h, 5h, etc., or any range between the two. The drying process is performed to remove moisture.

[0065] In some embodiments, the temperature of the sintering treatment is 300 to 800°C, for example, it can be but not limited to 300°C, 400°C, 500°C, 600°C, 700°C or 800°C, or any range between the two. The sintering treatment time is 1 to 15h, for example, 1h, 2h, 3h, 4h, 5h, 6h, 8h, 10h, 11h, 12h, 13h, 15h, or any range between the two. The sintering treatment atmosphere is a protective gas, such as nitrogen, argon, helium, etc. The present invention adopts a suitable sintering treatment temperature and time to ensure the formation of the lithium-philic material layer and to ensure the mechanical properties and electrical properties of the composite current collector.

[0066] According to another aspect of the present invention, the present invention also relates to a negative electrode sheet, comprising the composite current collector and a lithium metal layer located on the surface of the composite current collector.

[0067] The negative electrode sheet of the invention has excellent mechanical properties and electrical properties.

[0068] According to another aspect of the present invention, the present invention also relates to a battery, comprising the negative electrode sheet.

[0069] The battery of the present invention has excellent cycle performance, rate performance and safety performance.

[0070] The following is further explained in conjunction with specific embodiments and comparative examples.

[0071] Example 1

[0072] This embodiment provides a method for preparing a composite current collector, comprising the following steps:

[0073] (a) The polymer base film is stretched to obtain a polymer layer with a porous structure. The thickness of the polymer layer is L1 = 9 μm. The material of the polymer layer is polyethylene terephthalate, and the porosity is 65%.

[0074] (b) depositing a metal copper seed layer on the surface of the polymer layer by magnetron sputtering, the metal seed layer reaching 50 nm, and then electroplating conductive metal copper to form a metal conductive layer 102, the thickness of the metal conductive layer 102 is 500 nm, to obtain a composite layer.

[0075] (c) placing the composite layer in a lithiophilic solution (zinc acetate solution) for immersion treatment, the concentration of the lithiophilic solution is 0.5 mol / L, and the immersion treatment time is 2.5 h.

[0076] (d) The impregnated material is heat-treated, and the heat treatment includes drying and sintering in sequence. The drying temperature is 40°C, the drying time is 2 hours, the sintering temperature is 300°C, the sintering time is 7 hours, and the sintering atmosphere is argon. A lithium-philic material layer 2 is formed, and the polymer layer forms a carbon material skeleton 101. The carbon material skeleton 101 and the metal conductive layer 102 form a composite matrix layer 1 to obtain a composite current collector.

[0077] The cross-sectional structure diagram of the composite current collector is shown in Figure 1 shown.

[0078] Example 2

[0079] This embodiment provides a method for preparing a composite current collector, comprising the following steps:

[0080] (a) The polymer base film is stretched to obtain a polymer layer with a porous structure. The thickness of the polymer layer is L1 = 15 μm. The material of the polymer layer is polyimide and the porosity is 70%.

[0081] (b) depositing a metal copper seed layer on the surface of the polymer layer by magnetron sputtering, the metal seed layer reaching 50 nm, and then evaporating conductive metal copper to form a metal conductive layer 102, the thickness of the metal conductive layer 102 is 800 nm, to obtain a composite layer.

[0082] (c) placing the composite layer in a lithiophilic solution (zinc acetate solution) for immersion treatment, the concentration of the lithiophilic solution is 1 mol / L, and the immersion treatment time is 0.5 h.

[0083] (d) The impregnated material is heat-treated, and the heat treatment includes drying and sintering in sequence. The drying temperature is 60°C, the drying time is 0.5 h, the sintering temperature is 350°C, the sintering time is 6 h, and the sintering atmosphere is argon. A lithium-philic material layer 2 is formed, and the polymer layer forms a carbon material skeleton 101. The carbon material skeleton 101 and the metal conductive layer 102 form a composite matrix layer 1 to obtain a composite current collector.

[0084] Example 3

[0085] This embodiment provides a method for preparing a composite current collector, comprising the following steps:

[0086] (a) The polymer base film is stretched to obtain a polymer layer with a porous structure. The thickness of the polymer layer is L1 = 20 μm. The material of the polymer layer is polyethylene terephthalate, and the porosity is 50%.

[0087] (b) depositing a metal copper seed layer on the surface of the polymer layer by magnetron sputtering, the metal seed layer reaching 50 nm, and then evaporating conductive metal copper to form a metal conductive layer 102, the thickness of the metal conductive layer 102 is 600 nm, to obtain a composite layer.

[0088] (c) placing the composite layer in a lithiophilic solution (zinc acetate solution) for immersion treatment, the concentration of the lithiophilic solution is 0.8 mol / L, and the immersion treatment time is 1 hour.

[0089] (d) The impregnated material is heat-treated, and the heat treatment includes drying and sintering in sequence. The drying temperature is 50°C, the drying time is 1.5 hours, the sintering temperature is 400°C, the sintering time is 5 hours, and the sintering atmosphere is argon. A lithium-philic material layer 2 is formed, and the polymer layer forms a carbon material skeleton 101. The carbon material skeleton 101 and the metal conductive layer 102 form a composite matrix layer 1 to obtain a composite current collector.

[0090] Example 4

[0091] This embodiment provides a method for preparing a composite current collector, comprising the following steps:

[0092] (a) The polymer base film is stretched to obtain a polymer layer with a porous structure, wherein the thickness of the polymer layer is L1=15 μm, and the polymer layer is a composite laminate of polypropylene and polyethylene terephthalate, with a thickness ratio of 1:4 and a porosity of 60%.

[0093] (b) depositing a metal copper seed layer on the surface of the polymer layer by magnetron sputtering, the metal seed layer reaching 80 nm, and then evaporating conductive metal copper to form a metal conductive layer 102, the thickness of the single-side metal conductive layer 102 being 700 nm, to obtain a composite layer.

[0094] (c) The composite layer is placed in a lithiophilic solution (zinc acetate solution) for immersion treatment, the concentration of the lithiophilic solution is 0.6 mol / L, and the immersion treatment time is 1.5 h.

[0095] (d) The impregnated material is heat-treated, and the heat treatment includes drying and sintering in sequence. The drying temperature is 45°C, the drying time is 2 hours, the sintering temperature is 450°C, the sintering time is 4 hours, and the sintering atmosphere is argon. A lithium-philic material layer 2 is formed, and the polymer layer forms a carbon material skeleton 101. The carbon material skeleton 101 and the metal conductive layer 102 form a composite matrix layer 1 to obtain a composite current collector.

[0096] Example 5

[0097] This embodiment provides a method for preparing a composite current collector, comprising the following steps:

[0098] (a) The polymer base film is stretched to obtain a polymer layer with a porous structure, wherein the thickness of the polymer layer is L1=16 μm, and the polymer layer is a composite laminate of polyimide and polyethylene terephthalate, with a thickness ratio of 1:3 and a porosity of 40%.

[0099] (b) depositing a metal copper seed layer on the surface of the polymer layer by magnetron sputtering, the metal seed layer reaching 100 nm, and then evaporating conductive metal copper to form a metal conductive layer 102, the thickness of the metal conductive layer 102 is 700 nm, to obtain a composite layer.

[0100] (c) placing the composite layer in a lithiophilic solution (zinc salt solution) for immersion treatment, the concentration of the lithiophilic solution is 0.6 mol / L, and the immersion treatment time is 1.5 h.

[0101] (d) The impregnated material is heat-treated, and the heat treatment includes drying and sintering in sequence. The drying temperature is 45°C, the drying time is 2 hours, the sintering temperature is 400°C, the sintering time is 4 hours, and the sintering atmosphere is argon. A lithium-philic material layer 2 is formed, and the polymer layer forms a carbon material skeleton 101. The carbon material skeleton 101 and the metal conductive layer 102 form a composite matrix layer 1 to obtain a composite current collector.

[0102] Example 6

[0103] A method for preparing a negative electrode sheet, comprising:

[0104] In an inert environment, lithium metal is heated to 200° C. to make it molten, and the molten lithium metal is slowly poured onto the surface of the composite current collector prepared in Example 1. After the lithium metal is completely infiltrated, a lithium metal layer is formed after cooling. The thickness of the lithium metal layer is consistent with that of the three-dimensional composite current collector, and a negative electrode sheet is obtained.

[0105] A method for preparing a battery includes: assembling a negative electrode sheet and a positive electrode sheet, a separator and an electrolyte into a button battery, wherein the method for preparing the positive electrode sheet includes: the separator is a PE-based film; the electrolyte is 1M LiPF6 dissolved in a mixed solution of DMC, DEC and EC in a volume ratio of 1:1:1.

[0106] Example 7

[0107] A method for preparing a negative electrode sheet comprises the following steps:

[0108] Metal lithium is electroplated on the surface of the composite current collector in Example 2, and the thickness of the lithium metal layer is consistent with that of the composite current collector, thereby obtaining a negative electrode sheet.

[0109] Schematic diagram of lithium metal deposition on composite current collector Figure 2 shown.

[0110] The preparation method of the battery in this embodiment adopts the negative electrode sheet in this embodiment, and other conditions are the same as those in Example 6.

[0111] Example 8

[0112] A method for preparing a negative electrode sheet, which is different from Example 7 in that the composite current collector in Example 3 is used.

[0113] The preparation method of the battery in this embodiment adopts the negative electrode sheet in this embodiment, and other conditions are the same as those in Example 6.

[0114] Example 9

[0115] A method for preparing a negative electrode sheet, which is different from Example 7 in that the composite current collector in Example 4 is used.

[0116] The preparation method of the battery in this embodiment adopts the negative electrode sheet in this embodiment, and other conditions are the same as those in Example 6.

[0117] Example 10

[0118] A method for preparing a negative electrode sheet, which is different from Example 7 in that the composite current collector in Example 5 is used.

[0119] The preparation method of the battery in this embodiment adopts the negative electrode sheet in this embodiment, and other conditions are the same as those in Example 6.

[0120] Comparative Example 1

[0121] A negative electrode sheet adopts lithium metal foil.

[0122] The preparation method of the battery in this comparative example adopts the negative electrode sheet in this comparative example, and other conditions are the same as those in Example 6.

[0123] Comparative Example 2

[0124] A current collector is made of copper foil, and the thickness of the composite current collector is the same as that of the composite current collector of Example 7.

[0125] A method for preparing a negative electrode sheet comprises: using the current collector of this comparative example, and other conditions are the same as those of Example 7.

[0126] The preparation method of the battery in this comparative example adopts the negative electrode sheet in this comparative example, and other conditions are the same as those in Example 6.

[0127] Comparative Example 3

[0128] The preparation method of the composite current collector of this comparative example comprises the following steps:

[0129] (a) The polymer base film is stretched to obtain a polymer layer with a porous structure. The thickness of the polymer layer is L1 = 9 μm, and the material of the polymer layer is polyethylene terephthalate.

[0130] (b) depositing a metal copper seed layer on the surface of the polymer layer by magnetron sputtering, and then evaporating conductive metal copper to form a metal conductive layer 102 with a thickness of 500 nm to obtain a composite current collector.

[0131] The method for preparing the negative electrode sheet provided in this comparative example comprises: using the composite current collector of this comparative example, and other conditions are the same as those in Example 7.

[0132] The preparation method of the battery in this comparative example adopts the negative electrode sheet in this comparative example, and other conditions are the same as those in Example 6.

[0133] Experimental example

[0134] The batteries of each embodiment and comparative example were subjected to charge and discharge cycle tests at a current density of 150 mA / g, and the cycle capacity retention rate test results are shown in Table 1. Figure 3 The comparison of the cycle capacity retention rate of the battery of Example 7 of the present invention and Comparative Example 2 is shown in FIG. Figure 4 shown.

[0135] Table 1 Battery cycle performance test results

[0136]

[0137]

[0138] The composite current collector of the present invention has both high mechanical strength and low density, and can limit the generation of lithium dendrites; the lithium-philic material layer can ensure better adaptability during the lithium metal composite process; the three-dimensional structural pores can also limit the volume change of the lithium metal negative electrode during the cycle process, and the obtained battery has excellent cycle performance. As shown in Table 1, the batteries of various embodiments of the present invention have a high capacity retention rate. The capacity retention rate of the batteries of Comparative Examples 1 to 3 is poor.

[0139] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A composite current collector, characterized in that: It comprises a composite matrix layer and a lithium-philic material layer located on the surface of the composite matrix layer, wherein the composite matrix layer comprises a carbon material skeleton and a metal conductive layer located on the surface of the carbon material skeleton; and the composite current collector has a porous structure.

2. The composite current collector according to claim 1, characterized in that: Contains at least one of the following features (1) to (2): (1) The lithium-philic material layer comprises zinc oxide; (2) The conductive layer is made of copper.

3. The composite current collector according to claim 1, characterized in that: The thickness L2 of the metal conductive layer satisfies: 0<L2<20μm.

4. The composite current collector according to claim 1, characterized in that: The specific surface area S of the composite current collector satisfies: 50m 2 / g≤S≤2000m 2 / g.

5. The method for preparing a composite current collector according to any one of claims 1 to 4, characterized in that: The following steps are involved: (a) coating the surface of the porous polymer layer with a conductive metal to form a metal conductive layer to obtain a composite layer; (b) immersing the composite layer in a lithium-philic solution; (c) heat treating the impregnated composite layer to obtain a three-dimensional composite current collector.

6. The method for preparing a composite current collector according to claim 5, characterized in that: Contains at least one of the following features (1) to (5): (1) The material of the porous polymer layer includes at least one of polypropylene, polyethylene terephthalate and polyimide; (2) The porosity of the porous polymer layer is 10% to 80%; (3) The thickness L1 of the porous polymer layer satisfies: 0<L1<20 μm; (4) The plating includes evaporation and / or water electroplating; (5) Before the plating, the method further comprises: depositing a metal seed layer on the surface of the porous polymer layer by magnetron sputtering; and performing the plating after the metal seed layer reaches 20 to 100 nm.

7. The method for preparing a composite current collector according to claim 5, characterized in that: Contains at least one of the following features (1) to (3): (1) The lithiophilic solution comprises a zinc salt solution; the anion of the zinc salt is a complex anion or an organic acid radical; (2) The concentration of the lithium-philic solution is 0.01 to 1 mol / L; (3) The immersion time is 0.5 to 5 hours.

8. The method for preparing a composite current collector according to claim 5, characterized in that: Contains at least one of the following features (1) to (4): (1) The heat treatment includes drying and sintering; (2) During the heat treatment, the drying temperature is 20 to 60° C. and the drying time is 0.5 to 5 hours; (3) During the heat treatment, the sintering temperature is 300 to 800° C. and the sintering time is 1 to 15 hours; (4) During the heat treatment process, the sintering atmosphere is a protective gas.

9. A negative electrode sheet, characterized in that: The invention comprises the composite current collector according to any one of claims 1 to 4, and a lithium metal layer located on the surface of the composite current collector.

10. A battery, characterized in that: Including the negative electrode sheet as claimed in claim 9.