Semi-solid battery and preparation method thereof
By accurately spraying the curing precursor and performing two curing treatments, the problem of curing unevenness in semi-solid-state batteries is solved, semi-solid-state batteries with high performance and high consistency are achieved, and the development of the preparation process of all-solid-state batteries is promoted.
Patent Information
- Application Number
- CN202410913705.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-10-29
AI Technical Summary
During the in-situ curing electrolyte generation process of existing semi-solid batteries, they are affected by the electrolyte formula, viscosity, infiltration process, and temperature and pressure uniformity, resulting in poor curing consistency, affecting battery performance and consistency, and the traditional liquid injection process is difficult to control. It hinders the performance improvement of batteries and the expansion of all-solid-state batteries.
Using a preparation method that does not require liquid injection, the solid electrolyte layer is formed by accurately spraying and curing the precursor by calculating the three-dimensional hole volume, and curing it twice through ultraviolet light and heating and pressure to ensure that the uniformity of the electrolyte film formation is consistent with the packaging of the battery. sex.
It has realized a semi-solid battery with small internal resistance and high long-term cycle performance, omitting the traditional liquid injection process, promoting the development of all-solid-state battery preparation processes, and improving the overall performance and consistency of the battery.
Smart Images

Figure CN118867412A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a semi-solid battery and a preparation method thereof. Background Art
[0002] Semi-solid-state battery is a new type of battery technology between traditional liquid lithium-ion battery and all-solid-state battery. It combines some characteristics of both types of batteries in order to achieve better performance and safety. A key feature of semi-solid-state battery is the use of solid or semi-solid materials in the positive electrode, negative electrode or electrolyte of the battery, while retaining a portion of liquid electrolyte or gel electrolyte.
[0003] At present, the technical routes adopted by semi-solid batteries are mainly the following: 1. Mix the solid electrolyte with active materials, binders and conductive components to form a slurry, and then apply it to the surface of the current collector to form a composite pole piece mixed with solid electrolyte; 2. Mix the solid electrolyte with binders, lithium salts and other components to form a slurry, and then apply it on the surface of a conventional pole piece composed of active materials, adhesives and conductive components to form a composite pole piece coated with a solid electrolyte; 3. Inject a liquid electrolyte containing polymer monomers, initiators, plasticizers and other components in the injection process, and then initiate monomer polymerization by heating and other means in the subsequent formation process to form an in-situ solidified electrolyte in which the polymer and the liquid electrolyte coexist. Among them, the third in-situ solidification technology route reduces the contact area between the electrolyte and the active material due to the effective binding of the polymer on the liquid electrolyte, which can effectively improve the side reactions at the electrode interface and the safety performance during battery abuse. In addition, the in-situ solidification technology route is highly compatible with the traditional lithium-ion battery production process and has good matching, and mass production can be achieved using existing production lines. Reduce the investment cost of new technology applications.
[0004] However, the in-situ solidified electrolyte generation process is affected by the electrolyte formula, viscosity, infiltration process, and uniformity of temperature and pressure, resulting in poor solidification consistency, which ultimately affects the overall performance and consistency of the battery. For example, after the in-situ solidified electrolyte is injected into the battery cell, the conditions for the solidification reaction need to be precisely controlled, otherwise partial solidification or poor fluidity will occur during the infiltration process, resulting in uneven electrolyte distribution and dry areas in some areas, which seriously affect the performance of the battery cell. In addition, after the infiltration is completed and the curing begins, a clamp is usually used to apply a certain pressure and temperature to the battery cell. The uniformity of the pressure applied to the surface of the battery cell and the uniformity of the temperature distribution will have a huge impact on the curing effect, placing very high demands on the equipment and process, making the actual curing effect difficult to control.
[0005] Patent document CN116960468A proposes to immerse the negative electrode sheet in an electrolyte mixture, prepare a solid electrolyte layer by pulling, and then solidify it by heating or ultraviolet light irradiation to form a solid electrolyte-coated negative electrode sheet. After the above negative electrode sheet and the positive electrode are stacked, they are injected and the subsequent process is carried out. However, it is impossible to achieve accurate quantification by applying the solidified precursor solution to the surface of the electrode sheet by pulling, which may cause excessive coating of the precursor solution and increase the impedance. And the injection process is still required, and the technical expansion to all-solid-state batteries cannot be achieved. The purpose of coating the negative electrode surface with a solid electrolyte is to play the role of electronic insulation of the diaphragm, but in order to ensure a good insulation effect, the thickness of the solid electrolyte is usually very large, which seriously affects the energy density of the battery. Summary of the invention
[0006] The present invention provides a method for preparing a semi-solid battery which does not require liquid injection and can accurately control the film-forming quality and consistency of a solid electrolyte. The present invention also provides a semi-solid battery with small cell internal resistance and high long-term cycle performance.
[0007] The present invention discloses a method for preparing a semi-solid battery, comprising the following steps:
[0008] S1. Prepare positive electrode sheet, negative electrode sheet and separator;
[0009] S2, preparing a curing precursor, and fully mixing a polymer monomer, an initiator, and an electrolyte to form the curing precursor;
[0010] S3, calculating the mass of the required solidified precursor according to the volume of the three-dimensional holes in the positive electrode sheet, the negative electrode sheet and the separator;
[0011] S4, multiplying the calculated mass of the cured precursor by a coefficient to obtain an actual spraying amount, weighing the required mass of the cured precursor, and spraying it evenly onto the positive electrode sheet, the negative electrode sheet, and the separator;
[0012] S5, the precursor to be cured is fully in contact with the diaphragm, and is cured to form a laminated unit;
[0013] S6. Welding, packaging and chemically forming the stacked units to obtain a semi-solid-state battery.
[0014] The positive electrode sheet includes a positive electrode active material, a conductive agent, a binder, and a solvent; the mass ratio of the positive electrode active material, the conductive agent, and the binder is (7-100): (0.1-5): (0.1-5), preferably 95:3:2; the positive electrode active material is preferably one or more of lithium cobalt oxide, lithium manganese oxide, ternary nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium nickel cobalt manganese aluminum oxide, lithium iron phosphate, lithium manganese iron phosphate, and lithium-rich manganese-based; the binder is preferably polyvinylidene fluoride, polytetrafluoroethylene, etc.; the conductive agent is preferably carbon nanotubes, conductive carbon black, etc.; the solvent is preferably N-methylpyrrolidone.
[0015] The negative electrode sheet is composed of a negative electrode active material, a conductive agent, a binder, and a solvent; the mass ratio of the negative electrode active material, the conductive agent, and the binder is (7-100): (0.1-5): (0.1-5), preferably 94:3:3; the negative electrode active material is preferably one or more of graphite, silicon, silicon oxide, silicon carbon, hard carbon, metallic lithium, and metallic lithium alloy; the binder is preferably one or more of carboxymethyl cellulose, styrene-butadiene rubber, polyacrylic acid, and polyacrylonitrile; the conductive agent is preferably carbon nanotubes, conductive carbon black, etc.; the solvent is preferably water or N-methylpyrrolidone.
[0016] The separator is selected from one of polyethylene, polypropylene, polyimide, aramid, and non-woven fabric, or a composite of two of them.
[0017] The surface of the diaphragm may be coated with alumina, boehmite, NASICON, LiPON, LISICON, perovskite, garnet or antiperovskite solid electrolyte; the surface of the diaphragm may also not be coated.
[0018] The positive electrode sheet, the negative electrode sheet and the separator may be mixed with a solid electrolyte, and the solid electrolyte preferably includes NASICON type, LiPON type, LISICON type, perovskite type, garnet type and antiperovskite type. In addition, according to the battery performance requirements, the solid electrolyte in the composite electrode sheet and the composite separator may also be a sulfide and halide solid electrolyte.
[0019] The electrolyte includes a solvent and a lithium salt, and the solvent preferably includes one or more of ethylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, fluoroethylene carbonate, propylene carbonate, butylene carbonate, methyl formate, ethyl formate, propyl formate, butyl formate, ethylene glycol dimethyl ether, tetrahydrofuran, and cyclopentane sulfone.
[0020] The lithium salt preferably includes one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(oxalatoborate), lithium bis(fluorosulfonyl)imide, and lithium perchlorate.
[0021] Furthermore, in step S2, the polymer monomer is selected from one or more of ester monomers, carbonate monomers, sulfone monomers, isocyanate monomers, amide monomers, nitrile monomers, fluorinated monomers, ether compounds, ether-containing segment oligomers, and siloxanes.
[0022] Furthermore, in step S2, the initiator is selected from one or more of azo initiators, peroxide initiators, anionic and cationic initiators, organic metal compound initiators, and organic phosphorus initiators.
[0023] Furthermore, in step S2, the mass of the polymer monomer: the mass of the electrolyte is 0.01-40%; the mass of the initiator: the mass of the electrolyte is 0.0001-0.4%.
[0024] Furthermore, in step S4, the polymer monomer in the curing precursor sprayed on the positive electrode sheet is an oxidation-resistant polymer monomer; the polymer monomer in the curing precursor sprayed on the negative electrode sheet is a reduction-resistant polymer monomer; and the curing precursor sprayed on the diaphragm is a mixed liquid of the curing precursors sprayed on the positive electrode sheet and the negative electrode sheet.
[0025] In this way, the corresponding positive and negative electrode materials can be matched according to the oxidation and reduction resistance characteristics of the polymer monomers, avoiding the consequences of poor polymerization due to oxidation or reduction of the polymer monomers, which affects the battery performance.
[0026] The oxidation-resistant polymer monomer is selected from one or more of carbonate monomers, sulfone monomers, isocyanate monomers, amide monomers, nitrile monomers, fluorinated monomers, ether compounds, ether-containing segment oligomers, and siloxanes.
[0027] The reduction-resistant polymer monomer is selected from one or more of fluorinated monomers, siloxanes, nitrile monomers, ester monomers, carbonate monomers, sulfone monomers, and amide monomers.
[0028] Furthermore, in step S4, the coefficient by which the mass of the solidified precursor is multiplied is 1.05-1.4.
[0029] Taking into account the loss caused by the diffusion of the solidified precursor in the pores during the actual spraying process, it is common experience that the weight of the solidified precursor calculated above is multiplied by a coefficient as the final amount of solid electrolyte to be sprayed on the electrode or diaphragm.
[0030] Furthermore, in step S5, the curing and molding is performed in two operations. In the first curing, the positive electrode sheet, the negative electrode sheet and the separator are irradiated with ultraviolet light to induce a polymerization reaction; and then the polymerized positive electrode sheet, the negative electrode sheet and the separator are cured for a second time by heating and pressurizing, and compounded to form a laminated unit.
[0031] In the first curing, the polymer monomers polymerize under the initiation of ultraviolet light, forming a sticky polymer on the surface of the positive electrode sheet, the negative electrode sheet and the separator, so that the positive electrode sheet and the negative electrode sheet can be bonded to the separator, avoiding the separator gluing process; the second curing heating and pressurizing treatment completes the assembly of the positive electrode sheet and the negative electrode sheet with the separator, and also completes the secondary polymerization of the positive electrode sheet and the negative electrode sheet with the separator. The polymerization is carried out twice to make the polymerization reaction more uniform and the curing consistency better.
[0032] Furthermore, in step S5, the first curing treatment is irradiation with ultraviolet light of wavelength 200-400nm for 1-300s.
[0033] Furthermore, in step S5, the second curing is performed at 20-80° C. and a pressure of 1-50 PSI.
[0034] The present invention also discloses a semi-solid battery, which is processed by the preparation method of the semi-solid battery as described above, and has a capacity retention rate greater than 94% after 200 cycles.
[0035] The present invention constructs in-situ cured positive electrode sheets, negative electrode sheets and diaphragms in advance, and accurately controls the amount of solid electrolyte required for coating according to the pores of the positive electrode sheets, negative electrode sheets and diaphragms, and adopts a thermal composite stacking assembly method to solve the problems of uneven curing, poor wettability, poor cell consistency, etc. caused by in-situ curing in the traditional injection process. In addition, the present invention can omit the injection process in the traditional lithium-ion battery production process, laying the foundation for expansion to the all-solid-state battery preparation process. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 The present invention is a flow chart of a method for preparing a semi-solid-state battery. DETAILED DESCRIPTION
[0037] The following will describe the implementation methods of the present application in detail with the accompanying drawings and examples, so that the implementation process of how the present application uses technical means to solve technical problems and achieve technical effects can be fully understood and implemented accordingly. Based on the examples in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.
[0038] The reagents, methods and equipment used in this application are conventional reagents, methods and equipment in this technical field. Unless otherwise specified, the reagents and materials used in this application are commercially available. Figure 1 As shown, the preparation of the semi-solid-state battery is as follows.
[0039] Example 1
[0040] (1) The solid component mass ratio is LiNi 0.9Co 0.05 Mn 0.05 O2: polyvinylidene fluoride: carbon black: carbon nanotubes = 95:2:2:1 and N-methylpyrrolidone were mixed and homogenized, and the positive electrode sheet was obtained after coating, drying and rolling; the solid components were mixed and homogenized with water and N-methylpyrrolidone in a mass ratio of graphite: silicon carbon: carboxymethyl cellulose: styrene butadiene rubber: carbon black: carbon nanotubes = 74:20:1:2:2:1, and the negative electrode sheet was obtained after coating, drying and rolling. The separator is a 9μm PE film, and 2μm boehmite is coated on the front and back sides.
[0041] (2) Add pentaerythritol tetraacrylate and azobisisobutyronitrile to 1.5 mol / L lithium hexafluorophosphate, fluoroethylene carbonate / diethyl carbonate / dimethyl carbonate (volume ratio 3:5:2) + 2 wt% vinylene carbonate + 1 wt% lithium difluorooxalate borate electrolyte and stir and mix thoroughly to form a curing precursor liquid. The mass ratio of pentaerythritol tetraacrylate to the mass ratio of the electrolyte is 10%, and the mass ratio of azobisisobutyronitrile to the electrolyte is 0.1%.
[0042] (3) The porosity of the positive electrode sheet obtained in step (1) was measured by mercury intrusion method to be 25%, the pore volume was 0.86 mL, the density of the solidified precursor was 1.3 g / mL, and the mass of the solidified precursor solution required was 1.29 g (the coefficient here is 1.15). The porosity of the negative electrode sheet obtained in step (2) was measured by the same method to be 30%, the pore volume was 0.94 mL, and the mass of the solidified precursor solution required was 1.47 g (the coefficient here is 1.2), the porosity of the diaphragm was 50%, the pore volume was 0.12 mL, and the mass of the solidified precursor solution required was 0.17 g (the coefficient here is 1.1).
[0043] (4) The solidified precursor liquid obtained in step (2) is uniformly sprayed onto the positive electrode sheet, the negative electrode sheet and the separator obtained in step (1) according to the weight calculated in step (3).
[0044] (5) After standing for 300 seconds, the positive electrode sheet, the negative electrode sheet and the separator were irradiated with ultraviolet light with a wavelength of 260 nm for 120 seconds.
[0045] (6) The positive electrode sheet, negative electrode sheet and separator obtained in step (5) are thermally composited and assembled into a battery cell at a temperature of 60° C. and a pressure of 30 PSI.
[0046] (7) After welding and packaging, a semi-solid-state battery is obtained.
[0047] Example 2
[0048] (1) The solid component mass ratio is LiNi 0.9 Co 0.05 Mn 0.05O2: polyvinylidene fluoride: carbon black: carbon nanotubes = 95:2:2:1 and N-methylpyrrolidone were mixed and homogenized, and the positive electrode sheet was obtained after coating, drying and rolling; the solid components were mixed and homogenized with water and N-methylpyrrolidone in a mass ratio of graphite: silicon carbon: carboxymethyl cellulose: styrene butadiene rubber: carbon black: carbon nanotubes = 74:20:1:2:2:1, and the negative electrode sheet was obtained after coating, drying and rolling. The separator is a 9μm PE film, and 2μm boehmite is coated on the front and back sides.
[0049] (2) Add maleic anhydride and azobisisobutyronitrile to 1.5mol / L lithium hexafluorophosphate, fluoroethylene carbonate / diethyl carbonate / dimethyl carbonate (volume ratio 3:5:2) + 2wt% vinylene carbonate + 1wt% lithium difluorooxalate borate electrolyte and stir and mix thoroughly to form a positive electrode curing precursor liquid. Among them, the mass ratio of maleic anhydride to the mass ratio of the electrolyte is 5%, and the mass ratio of azobisisobutyronitrile to the electrolyte is 0.05%. Add polyethylene glycol and azobisisobutyronitrile to 1.5mol / L lithium hexafluorophosphate, fluoroethylene carbonate / diethyl carbonate / dimethyl carbonate (volume ratio 3:5:2) + 2wt% vinylene carbonate + 1wt% lithium difluorooxalate borate electrolyte and stir and mix thoroughly to form a negative electrode curing precursor liquid. Among them, the mass ratio of polyethylene glycol to the mass ratio of the electrolyte is 5%, and the mass ratio of azobisisobutyronitrile to the electrolyte is 0.05%. The positive electrode curing precursor liquid and the negative electrode curing precursor liquid are mixed in a mass ratio of 1:1, and the obtained precursor liquids are mixed to obtain a diaphragm curing precursor liquid.
[0050] (3) The porosity of the positive electrode sheet obtained in step (1) was measured by mercury intrusion method to be 25%, the pore volume was 0.86 mL, and the mass of the required solidified precursor solution was 1.29 g (the coefficient here is 1.15). The porosity of the negative electrode sheet obtained in step (2) was measured by the same method to be 30%, the pore volume was 0.94 mL, and the mass of the required solidified precursor solution was 1.47 g (the coefficient here is 1.2), the porosity of the diaphragm was 50%, the pore volume was 0.12 mL, and the mass of the required solidified precursor solution was 0.17 g (the coefficient here is 1.1).
[0051] (4) The positive electrode curing precursor liquid obtained in step (2) is uniformly sprayed onto the composite positive electrode sheet obtained in step (1) according to the weight calculated in step (3). The negative electrode curing precursor liquid obtained in step (2) is uniformly sprayed onto the composite negative electrode sheet obtained in step (1) according to the weight calculated in step (3). The diaphragm curing precursor liquid obtained in step (2) is uniformly sprayed onto the diaphragm according to the weight calculated in step (3).
[0052] (5) After standing for 300 seconds, the positive electrode sheet, negative electrode sheet and separator are irradiated with ultraviolet light for 120 seconds.
[0053] (6) The positive electrode sheet, negative electrode sheet and separator obtained in step (5) are thermally composited and assembled into a battery cell at a temperature of 60° C. and a pressure of 30 PSI.
[0054] (7) After welding, packaging and formation, the semi-solid-state battery is completed.
[0055] Comparative Example 1
[0056] (1) The solid component mass ratio is LiNi 0.9 Co 0.05 Mn 0.05 O2: polyvinylidene fluoride: carbon black: carbon nanotubes = 95:2:2:1 and N-methyl pyrrolidone were mixed and homogenized, and the positive electrode sheet was obtained after coating, drying and rolling. The solid components were mixed and homogenized with water and N-methyl pyrrolidone in a mass ratio of graphite: silicon carbon: carboxymethyl cellulose: styrene butadiene rubber: carbon black: carbon nanotubes = 74:20:1:2:2:1, and the negative electrode sheet was obtained after coating, drying and rolling. The separator is a 9μm PE film, and 2μm boehmite is coated on the front and back. The obtained positive and negative electrode sheets and separators are assembled into a battery cell.
[0057] (2) Add pentaerythritol tetraacrylate and azobisisobutyronitrile to 1.5 mol / L lithium hexafluorophosphate, fluoroethylene carbonate / diethyl carbonate / dimethyl carbonate (volume ratio 3:5:2) + 2 wt% vinylene carbonate + 1 wt% lithium difluorooxalate borate electrolyte and stir and mix thoroughly to form a curing precursor liquid. The mass ratio of pentaerythritol tetraacrylate to the mass of the electrolyte is 10%, and the mass ratio of azobisisobutyronitrile to the electrolyte is 0.1%.
[0058] (3) Injecting the solidified precursor liquid obtained in step (2) into the battery cell during the liquid injection process.
[0059] (4) After standing for 48 hours, the semi-solid-state battery was cured at 60°C for 12 hours.
[0060] Comparative Example 2
[0061] (1) The solid component mass ratio is LiNi 0.9 Co 0.05 Mn 0.05 O2: polyvinylidene fluoride: carbon black: carbon nanotubes = 95:2:2:1 and N-methyl pyrrolidone were mixed and homogenized, and the positive electrode sheet was obtained after coating, drying and rolling. The solid component mass ratio of graphite: silicon carbon: carboxymethyl cellulose: styrene butadiene rubber: carbon black: carbon nanotubes = 74:20:1:2:2:1 was mixed and homogenized with water and N-methyl pyrrolidone, and the negative electrode sheet was obtained after coating, drying and rolling. The separator was a 9μm PE film, and 2μm boehmite was coated on the front and back sides.
[0062] (2) Maleic anhydride, polyethylene glycol and azobisisobutyronitrile are added to 1.5 mol / L lithium hexafluorophosphate, fluoroethylene carbonate / diethyl carbonate / dimethyl carbonate (volume ratio 3:5:2) + 2 wt% vinylene carbonate + 1 wt% lithium difluorooxalate borate electrolyte and stirred and mixed to form a solidified precursor liquid. Among them, the mass ratio of maleic anhydride to the mass ratio of the electrolyte is 5%, the mass ratio of polyethylene glycol to the mass ratio of the electrolyte is 5%, and the mass ratio of azobisisobutyronitrile to the mass ratio of the electrolyte is 0.05%.
[0063] (3) The porosity of the positive electrode sheet obtained in step (1) was measured by mercury intrusion method to be 25%, the pore volume was 0.86 mL, and the mass of the required solidified precursor solution was 1.29 g (the coefficient here is 1.15). The porosity of the negative electrode sheet was measured by the same method to be 30%, the pore volume was 0.94 mL, and the mass of the required solidified precursor solution was 1.47 g (the coefficient here is 1.2), the porosity of the diaphragm was 50%, the pore volume was 0.12 mL, and the mass of the required solidified precursor solution was 0.17 g (the coefficient here is 1.1).
[0064] (4) The solidified precursor liquid obtained in step (2) is uniformly sprayed onto the positive electrode sheet, negative electrode sheet and separator obtained in step (1) according to the weight calculated in step (3).
[0065] (5) After standing for 300 seconds, the obtained positive electrode sheet, negative electrode sheet and separator were irradiated with ultraviolet light for 120 seconds.
[0066] (6) The positive electrode sheet, negative electrode sheet and separator obtained in step (5) are thermally composited and assembled into a battery cell at a temperature of 60° C. and a pressure of 30 PSI.
[0067] (8) After welding, packaging and formation, the semi-solid-state battery is completed.
[0068] Comparative Example 3
[0069] (1) The solid component mass ratio is LiNi 0.9 Co 0.05 Mn 0.05 O2: polyvinylidene fluoride: carbon black: carbon nanotubes = 95:2:2:1 and N-methylpyrrolidone were mixed and homogenized, and the positive electrode sheet was obtained after coating, drying and rolling; the solid components were mixed and homogenized with water and N-methylpyrrolidone in a mass ratio of graphite: silicon carbon: carboxymethyl cellulose: styrene butadiene rubber: carbon black: carbon nanotubes = 74:20:1:2:2:1, and the negative electrode sheet was obtained after coating, drying and rolling. The separator is a 9μm PE film, and 2μm boehmite is coated on the front and back sides.
[0070] (2) Add pentaerythritol tetraacrylate and azobisisobutyronitrile to 1.5 mol / L lithium hexafluorophosphate, fluoroethylene carbonate / diethyl carbonate / dimethyl carbonate (volume ratio 3:5:2) + 2 wt% vinylene carbonate + 1 wt% lithium difluorooxalate borate electrolyte and stir and mix thoroughly to form a curing precursor liquid. The mass ratio of pentaerythritol tetraacrylate to the mass ratio of the electrolyte is 10%.
[0071] (3) The positive electrode sheet, negative electrode sheet and separator obtained in step (1) are immersed in the solidified precursor solution prepared in step (2) for 40 hours respectively, and then the positive and negative electrode sheets and separator are pulled out of the solidified precursor solution at a speed of 2 cm / min.
[0072] (4) After standing for 300 seconds, the positive electrode sheet, negative electrode sheet and separator are irradiated with ultraviolet light for 120 seconds.
[0073] (5) The positive electrode sheet, negative electrode sheet and separator obtained in step (4) are thermally composited and assembled into a battery cell at a temperature of 60° C. and a pressure of 30 PSI.
[0074] (6) After welding, packaging and formation, the semi-solid-state battery is completed.
[0075] The situation of mixing solid electrolytes into the positive electrode sheets and negative electrode sheets is similar to the above embodiment. The solid electrolytes in a preferred proportion can be added during the process of configuring the solidified precursor, and this embodiment will not be described in detail.
[0076] Performance Testing:
[0077] The semi-solid batteries obtained in Examples 1-2 and Comparative Examples 1-3 were subjected to HPPC and cycle tests. The HPPC test conditions were 50% SOC, room temperature discharge for 10s, and a discharge current of 3C. The cycle test conditions were 45°C, and the charge and discharge rates were all 1C. The test results are shown in the following table.
[0078] Table 1 Semi-solid-state battery performance test results
[0079] project Cell internal resistance@25℃,50%SOC,10s Capacity retention after 200 cycles Example 1 2.3~2.4mΩ 94.2% Example 2 1.9~2.0mΩ 96.7% Comparative Example 1 2.5~3.2mΩ 92.5% Comparative Example 2 2.3~2.9mΩ 93.0% Comparative Example 3 3.0~3.5mΩ 87.6%
[0080] Result analysis:
[0081] As shown in Table 1, the internal resistance and cycle performance of the battery cells of Examples 1 and 2 are better than those of Comparative Examples 1 and 2, indicating that the method of constructing in-situ cured positive electrode sheets, negative electrode sheets and separators in advance according to the present invention can significantly improve battery performance.
[0082] The consistency of the data of Examples 1 and 2 on the internal resistance of the battery cells is significantly better than that of Comparative Examples 1 and 2, indicating that the method of constructing in-situ cured positive electrode sheets, negative electrode sheets and separators in advance can significantly enhance the consistency of the semi-solid battery cells.
[0083] The internal resistance and cycle performance of the battery cell of Example 2 are significantly better than those of Example 1, indicating that the design of different polymer monomers for different polarities of the positive and negative electrodes can effectively improve the performance of the battery.
[0084] The internal resistance and cycle performance of the battery cell of Example 2 are significantly better than those of Comparative Example 2, indicating that the same polymer monomer and initiator formula design, assembling the polymer monomer and initiator compatible with the positive electrode separately, and assembling the polymer monomer and initiator compatible with the negative electrode separately, can effectively improve the performance of the battery.
[0085] By comparing the test results of Example 1 and Comparative Example 3, it can be seen that the method of first dipping and then pulling to compound the solid electrolyte on the surface of the pole piece will significantly increase the impedance of the battery and deteriorate the cycle performance. The main reason is that the dipping and pulling method cannot accurately control the film quality and uniformity of the solid electrolyte. Too much solid electrolyte coated on the surface of the pole piece will hinder the conduction of ions and electrons, thereby affecting the impedance of the battery.
[0086] Comparing Example 1 with Comparative Example 1, two curings can improve the uniformity of the polymerization reaction, thereby improving the consistency of film formation. Poor film formation consistency will lead to uneven current density and stress distribution on the surface of the pole piece during the battery cycle, thereby affecting the long-term cycle performance of the battery.
[0087] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a semi-solid-state battery, It is characterized in that The following steps are involved: S1. Prepare positive electrode sheet, negative electrode sheet and separator; S2, preparing a curing precursor, and fully mixing a polymer monomer, an initiator, and an electrolyte to form the curing precursor; S3, calculating the mass of the required solidified precursor according to the volume of the three-dimensional holes in the positive electrode sheet, the negative electrode sheet and the separator; S4, multiplying the calculated mass of the cured precursor by a coefficient to obtain an actual spraying amount, weighing the required mass of the cured precursor, and spraying it evenly onto the positive electrode sheet, the negative electrode sheet, and the separator; S5, the precursor to be cured is fully in contact with the diaphragm, and is cured to form a laminated unit; S6. Welding, packaging and chemically forming the stacked units to obtain a semi-solid-state battery.
2. A method for preparing a semi-solid battery according to claim 1, It is characterized in that In step S2, the polymer monomer is selected from one or more of ester monomers, carbonate monomers, sulfone monomers, isocyanates, amide monomers, nitrile monomers, fluorinated monomers, ether compounds, ether-containing segment oligomers, and siloxanes.
3. A method for preparing a semi-solid battery according to claim 2, It is characterized in that In the step S2, the initiator is selected from one or more of azo initiators, peroxide initiators, anionic and cationic initiators, organic metal compound initiators, and organic phosphorus initiators.
4. A method for preparing a semi-solid battery according to claim 3, It is characterized in that In the step S2, the mass of the polymer monomer: the mass of the electrolyte is 0.01-40%; the mass of the initiator: the mass of the electrolyte is 0.0001-0.4%.
5. The method for preparing a semi-solid battery according to claim 2, It is characterized in that In step S4, the polymer monomer in the curing precursor sprayed on the positive electrode sheet is an oxidation-resistant polymer monomer; the polymer monomer in the curing precursor sprayed on the negative electrode sheet is a reduction-resistant polymer monomer; and the curing precursor sprayed on the diaphragm is a mixed liquid of the curing precursors sprayed on the positive electrode sheet and the negative electrode sheet.
6. The method for preparing a semi-solid battery according to claim 1, It is characterized in that In the step S4, the coefficient by which the mass of the solidified precursor is multiplied is 1.05-1.
4.
7. The method for preparing a semi-solid battery according to claim 1, It is characterized in that In step S5, curing and molding is performed in two steps. In the first curing, the positive electrode sheet, the negative electrode sheet and the separator are irradiated with ultraviolet light to induce polymerization reaction. Then, the polymerized positive electrode sheet, the negative electrode sheet and the separator are cured for the second time by heating and pressurizing to form a laminated unit.
8. A method for preparing a semi-solid battery according to claim 7, It is characterized in that In the step S5, the first curing treatment is irradiation with ultraviolet light of wavelength 200-400nm for 1-300s.
9. A method for preparing a semi-solid battery according to claim 8, It is characterized in that In step S5, the second curing is performed at 20-80° C. and a pressure of 1-50 PSI.
10. A semi-solid-state battery, It is characterized in that The semi-solid battery is manufactured by the preparation method of any one of claims 1 to 9, and the capacity retention rate after 200 cycles is greater than 94%.
Citation Information
Patent Citations
High-capacity and high-safety diaphragm-free semi-solid battery and preparation method thereof
CN116960468A
Preparation method of gel-phase polymer lithium battery and gel-phase polymer lithium battery
CN104868165A
Preparation method of positive plate or negative plate for solid-state battery, positive plate or negative plate for solid-state battery and solid-state battery
CN111799514A
Integrated all-solid-state battery and preparation method thereof
CN114335705A
In-situ polymerization solid-state battery with multi-layer structure electrolyte and preparation method of in-situ polymerization solid-state battery
CN114335716A
Cited By
Method and system for improving wettability of battery cell electrolyte
CN119650873A
Preparation method of in-situ solid-state battery structure
CN120341225A
A method of fabricating an in-situ solid state battery structure
CN120341225B
Whole-domain integrated gel semi-solid battery and preparation method thereof
CN120473574A