Battery pole core, preparation method thereof and battery
By using high-energy electromagnetic wave irradiation technology and Ag-coated conductive materials in the battery core, overhang is eliminated, the problem of edge lithium precipitation caused by lithium ion diffusion is solved, and the performance and safety of the battery are improved.
Patent Information
- Application Number
- CN202410858175.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-29
AI Technical Summary
In traditional batteries, the overhang of positive and negative electrode materials causes lithium ions to diffuse, leading to edge lithium precipitation and reducing battery performance and safety.
By using high-energy electromagnetic wave irradiation technology in the battery core, the shapes and positions of the positive and negative active areas completely overlap, eliminating overhang, and using Ag-coated conductive materials and AgBr/I-coated conductive materials to form a conductive network. .
It effectively eliminates overhang, improves the service life and safety performance of the battery, ensures even distribution of lithium ions in the battery, and avoids edge lithium precipitation.
Smart Images

Figure BDA0004919969080000181 
Figure BDA0004919969080000191 
Figure BDA0004919969080000192
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of new energy, and in particular, to a battery core and a preparation method thereof, and a battery. Background Art
[0002] In the design and manufacture of battery cores, the positive and negative electrodes are important components of the core. Regardless of whether it is a wound core or a stacked core, the basic configuration is that the positive and negative electrodes of the sheet structure are bonded together and separated by an electronic insulation layer.
[0003] Positive and negative active materials are attached to the positive and negative electrodes of the sheet structure. Generally, the active materials, conductive agents and binders form porous electrodes together. Among them, the conductive agents are mostly composed of carbon materials, such as carbon black, carbon nanotubes, flake graphite, graphene, etc. For the positive and negative electrode sheets of limited size, it is difficult to align the edges of the positive active materials with the edges of the negative active materials. Generally, the edge of the negative active material will exceed the edge of the positive active material. The length of the exceeding part is the overhang. In the battery core, the overhang is generally greater than 0. However, during the charge and discharge cycle of the battery core, lithium ions will diffuse or migrate in the part of the negative active material where the overhang is greater than 0, so that lithium ions also exist in the negative active material that is not directly facing the positive active material. Over time, the concentration of lithium ions in the positive and negative active materials near the overhang changes, which eventually leads to edge lithium precipitation, reducing the performance and life of the battery, and even causing safety accidents.
[0004] Therefore, how to reduce or even eliminate overhang in batteries to improve battery performance, life and safety is a problem that needs to be solved urgently. Summary of the invention
[0005] The purpose of the present disclosure is to provide a battery pole core and a preparation method thereof and a battery. The overhang of the battery pole core is 0, which solves the problem of edge lithium plating caused by overhang in traditional batteries and effectively improves the service life and safety performance of the battery.
[0006] In order to achieve the above-mentioned object, the present disclosure provides a battery core in a first aspect, wherein the battery core comprises a positive electrode, a negative electrode and an electronic insulation layer;
[0007] The positive electrode comprises a positive electrode current collector and a positive electrode active material layer covering the positive electrode current collector, wherein the positive electrode active material layer comprises a positive electrode active region, and the positive electrode active region contains a positive electrode active material, a first conductive agent and a first binder;
[0008] The negative electrode comprises a negative electrode current collector and a negative electrode active material layer covering the negative electrode current collector, wherein the negative electrode active material layer comprises a negative electrode active region, and the negative electrode active region contains a negative electrode active material, a second conductive agent, and a second binder;
[0009] The negative electrode active material is an Ag-coated negative electrode active material, the first conductive agent and the second conductive agent are each independently Ag and / or Ag-coated conductive material, and the positive projection of the positive electrode active area on the negative electrode active material layer completely overlaps with the negative electrode active area.
[0010] Optionally, the positive electrode active material layer further includes a positive electrode inactive region, and / or the negative electrode active material layer includes a negative electrode inactive region; the positive electrode inactive region and the negative electrode inactive region are not conductive.
[0011] Optionally, the positive electrode inactive region and the negative electrode inactive region independently contain one or more of AgBr, AgI, AgBr-coated conductive material and AgI-coated conductive material.
[0012] Optionally,
[0013] The conductive material in the Ag-coated conductive material is selected from at least one of a granular conductive material, a rod-shaped conductive material and a sheet-shaped conductive material;
[0014] The average diameter of the granular conductive material is 50nm-5μm, preferably, the average diameter is 50nm-500nm;
[0015] The rod-shaped conductive material has a diameter of 3nm-30nm and a length of 1μm-50μm, preferably a diameter of 7nm-15nm and a length of 1μm-5μm;
[0016] The sheet-like conductive material has a thickness of 1 nm to 50 nm and a length of 1 μm to 100 μm, preferably a thickness of 5 nm to 10 nm and a length of 5 μm to 50 μm;
[0017] The Ag-coated conductive material particles include a core and a shell layer coated on the outer surface of the core, and the thickness of the shell layer is 1 nm-1 μm;
[0018] The average particle diameter of the Ag is 20 nm-5 μm, preferably 30 nm-500 nm.
[0019] Optionally, the negative electrode active material is selected from Ag-coated negative electrode active materials, and the negative electrode active material is selected from one or more of carbon materials, transition metal oxides, lithium, aluminum, gallium, indium, silicon, germanium, tin, lithium alloys, aluminum alloys, gallium alloys, indium alloys, silicon alloys, germanium alloys, tin alloys, aluminum oxides, gallium oxides, indium oxides, silicon oxides, germanium oxides and tin oxides.
[0020] Optionally, based on the total weight of the positive electrode active material layer, the content of the first conductive agent is 0.2-30% by weight, preferably 0.5-5% by weight; based on the total weight of the negative electrode active material layer, the content of the second conductive agent is 0.2-30% by weight, preferably 0.5-5% by weight.
[0021] Optionally, the conductive material is one or more of a metal conductor, a non-metal conductor, a carbon material, a conductive polymer material, a conductive semiconductor material, a piezoelectric material and a thermoelectric material, more preferably one or more of carbon black, carbon nanotubes, flaky graphite and graphene.
[0022] A second aspect of the present disclosure provides a method for preparing a battery core, the method comprising:
[0023] S1. Assembling a positive electrode, a negative electrode and an electronic insulating layer into an electrode core to be dried, wherein the positive electrode comprises a positive electrode current collector and a positive electrode active material slurry layer coated on the positive electrode current collector, and the negative electrode comprises a negative electrode current collector and a negative electrode active material slurry layer coated on the negative electrode current collector;
[0024] The positive electrode active material slurry layer contains a positive electrode active material, a first conductive agent precursor and a first binder; the negative electrode active material slurry layer contains a negative electrode active material precursor, a second conductive agent precursor and a second binder; the precursor of the negative electrode active material is a negative electrode active material coated with AgBr and / or a negative electrode active material coated with AgI; the first conductive agent precursor and the second conductive agent precursor are each independently one or more of AgBr, AgI, AgBr coated conductive material and AgI coated conductive material;
[0025] S2. Under optional negative pressure or vacuum conditions, irradiate the main surface of the electrode core to be dried with high-energy electromagnetic waves to form a positive electrode active area with the positive electrode active material slurry layer and a negative electrode active area with the negative electrode active material slurry layer, and dry the electrode core to obtain a dried electrode core;
[0026] The positive electrode active area contains a positive electrode active material, a first conductive agent and a first binder, and the negative electrode active area contains a negative electrode active material, a second conductive agent and a second binder; the negative electrode active material is a negative electrode active material coated with Ag, and the first conductive agent and the second conductive agent are each independently Ag and / or Ag-coated conductive material; the positive electrode active area's orthographic projection on the negative electrode active material layer completely overlaps with the negative electrode active area;
[0027] S3, injecting liquid, forming, aging and volume separation of the dried electrode core.
[0028] Optionally, step S2 comprises: using high-energy electromagnetic waves to vertically irradiate the main surface of the electrode core to be dried; the frequency of the high-energy electromagnetic waves is 3×10 16 Hz-3×10 22 Hz, wavelength is less than 10nm, and the radiation power is 1kW-1000kW; preferably, the frequency is 3×10 16 Hz-3×10 20 Hz, wavelength is 0.001nm-10nm, and ray power is 10kW-100kW.
[0029] Optionally, the precursor of the negative electrode active material is one or more of an Ag-coated negative electrode active material, an AgBr-coated negative electrode active material and an AgI-coated negative electrode active material; the negative electrode active material is selected from one or more of a carbon material, a transition metal oxide, lithium, aluminum, gallium, indium, silicon, germanium, tin, a lithium alloy, an aluminum alloy, a gallium alloy, an indium alloy, a silicon alloy, a germanium alloy, a tin alloy, an aluminum oxide, a gallium oxide, an indium oxide, a silicon oxide, a germanium oxide and a tin oxide.
[0030] A third aspect of the present disclosure provides a battery, comprising the battery core provided by the first aspect of the present disclosure or the battery core prepared by the method provided by the second aspect of the present disclosure.
[0031] Through the above technical solution, the overhang in the battery core of the present invention is 0, which solves the problem of lithium deposition at the edge of the negative electrode caused by overhang in traditional batteries, and effectively improves the service life and safety performance of the battery. The method disclosed in the present invention is simple and easy to implement. By irradiating the core to be aged with high-energy electromagnetic waves, a core with the same shape and consistent position of the positive electrode active area and the negative electrode active area can be prepared, so that the overhang in the battery core is 0.
[0032] Other features and advantages of the present disclosure will be described in detail in the following detailed description. DETAILED DESCRIPTION
[0033] The specific embodiments of the present disclosure are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present disclosure, and are not used to limit the present disclosure.
[0034] A first aspect of the present disclosure provides a battery core, the battery core comprising a positive electrode, a negative electrode and an electronic insulation layer; the positive electrode comprises a positive electrode collector and a positive electrode active material layer coated on the positive electrode collector, the positive electrode active material layer comprises a positive electrode active area, the positive electrode active area contains a positive electrode active substance, a first conductive agent and a first binder; the negative electrode comprises a negative electrode collector and a negative electrode active material layer coated on the negative electrode collector, the negative electrode active material layer comprises a negative electrode active area, the negative electrode active area contains a negative electrode active substance, a second conductive agent and a second binder; wherein the negative electrode active substance is a negative electrode active material coated with Ag, the first conductive agent and the second conductive agent are each independently Ag and / or Ag-coated conductive material; the positive electrode active area is completely overlapped by an orthographic projection of the negative electrode active area on the negative electrode active material layer.
[0035] The orthographic projection of the positive electrode active area on the negative electrode active material layer in the battery core of the present disclosure completely overlaps with the negative electrode active area, which means that the distance between the edge of the orthographic projection of the positive electrode active area on the negative electrode active material layer and the corresponding edge of the negative electrode active area is 0-100μm, that is, the difference in shape and position of the corresponding positive electrode active area and negative electrode active area can be ignored and can be considered to be exactly the same, so that the overhang is 0, which effectively solves the problem of lithium deposition at the edge of the negative electrode caused by the existence of overhang, so that the battery has a better service life and safety performance. In the present disclosure, the distance between the edge of the orthographic projection of the positive electrode active area and the corresponding edge of the negative electrode active area can be determined by cutting the core along the thickness direction and then using the elemental analysis function of SEM on the cross section to determine the edge position of the Br and / or I elements of the positive electrode, and determine the edge position of the Br and / or I elements of the negative electrode.
[0036] In a specific embodiment of the present disclosure, the positive electrode active material layer further includes a positive electrode inactive region, and / or the negative electrode active material layer includes a negative electrode inactive region; the positive electrode inactive region and the negative electrode inactive region are non-conductive. In this embodiment, the positive electrode inactive region and the negative electrode inactive region are transmission networks without electronic conductivity, which do not participate in the electrochemical reaction of the lithium-ion battery, while the positive electrode active region and the negative electrode active region are transmission networks with electronic conductivity. Through this structure, it is possible to achieve an absolute alignment of the positive electrode active region and the negative electrode active region, so that the overhang in the lithium-ion battery is 0.
[0037] In a specific embodiment of the present disclosure, the positive electrode inactive area and the negative electrode inactive area independently contain one or more of AgBr, AgI, AgBr-coated conductive materials and AgI-coated conductive materials. By using the technical solution of the present disclosure, the positive and negative active areas that are aligned in an absolute sense are opened up in the positive and negative electrode inactive areas, which is achieved by using high-energy electromagnetic waves to irradiate AgBr and / or AgI and other photosensitive coating materials. During the photosensitive reaction, AgBr and / or AgI decompose to produce Ag particles that can conduct the electronic conductivity network, activating the electronic conductivity of the entire core, and truly achieving the feat of zero overhang for lithium-ion batteries.
[0038] In a specific embodiment of the present disclosure, the Ag-coated conductive material particles include a core and an outer shell layer coated on the outer surface of the core, and the thickness of the outer shell layer is 1 nm-1 μm.
[0039] In one embodiment, the conductive material in the Ag-coated conductive material is selected from at least one of a granular conductive material, a rod-shaped conductive material and a sheet-shaped conductive material. In a specific embodiment, the granular conductive material includes but is not limited to carbon black and graphite, and the average diameter of the granular conductive material is 50nm-5μm, preferably, the average diameter is 50nm-500nm. In another specific embodiment, the rod-shaped conductive material is but is not limited to carbon nanotubes, and the diameter of the rod-shaped conductive material is 3nm-30nm, and the length is 1μm-50μm, preferably, the diameter is 7nm-15nm, and the length is 1μm-5μm. In another specific embodiment, the sheet-shaped conductive material includes but is not limited to graphene, and the thickness of the sheet-shaped conductive material is 1nm-50nm, and the length is 1μm-100μm, preferably, the thickness is 5nm-10nm, and the length is 5μm-50μm. In this embodiment, the particles of the Ag-coated conductive material include a core and a shell layer coated on the outer surface of the core, and the thickness of the shell layer is 1nm-1μm.
[0040] In one embodiment, the average particle diameter of the Ag is 20 nm-5 μm, preferably 30-500 nm.
[0041] The Ag and / or Ag-coated conductive materials of the above-mentioned sizes are of appropriate sizes, so the conductive network formed by them has good conductivity, so that the battery including the battery pole core of the present disclosure has a longer service life and better safety performance. In the present disclosure, the diameter, thickness, and length of the Ag-coated conductive material are detected by SEM morphology detection method. The average particle diameter of the granular conductive material is obtained by using the SEM morphology detection method to detect the diameters of 50 granular conductive materials in the field of view and calculate the average value. The thickness of the outer shell layer is detected by FIB manufacturing particle cross-section combined with SEM morphology detection method. The average particle diameter of Ag is detected by SEM morphology detection method.
[0042] According to the present disclosure, the negative electrode active material can be a negative electrode active material conventionally used by those skilled in the art, and can be directly commercially available or prepared by methods well known to those skilled in the art. In a preferred embodiment of the present disclosure, the negative electrode active material is selected from one or more of carbon materials, transition metal oxides, lithium, aluminum, gallium, indium, silicon, germanium, tin, lithium alloys, aluminum alloys, gallium alloys, indium alloys, silicon alloys, germanium alloys, tin alloys, aluminum oxides, gallium oxides, indium oxides, silicon oxides, germanium oxides, and tin oxides.
[0043] In a specific embodiment of the present disclosure, the Ag-coated negative electrode active material also has a core-shell structure, which includes an inner core and an outer shell coated on the outer surface of the inner core, the thickness of the outer shell layer is 20nm-1μm, and the average particle diameter of the Ag-coated negative electrode active material is 50nm-100μm.
[0044] In the present disclosure, the thickness of the outer shell layer of the Ag-coated conductive material can be detected by using a FIB method to manufacture a particle cross section combined with a SEM morphology detection method, and the average particle diameter of the Ag-coated negative electrode active material can be obtained by using a SEM morphology detection method to detect the diameters of 50 Ag-coated negative electrode active material particles within the field of view and calculate the average value.
[0045] According to the present disclosure, the content of the first conductive agent and the second conductive agent can vary in a wide range. In a specific embodiment, based on the total weight of the negative electrode active material layer, the content of the second conductive agent is 0.2-30% by weight, preferably 0.5-5% by weight; based on the total weight of the positive electrode active material layer, the content of the first conductive agent is 0.2-30% by weight, preferably 0.5-5% by weight. Within the above content range, the content of the first conductive agent and the second conductive agent is appropriate, and the battery has better service life and safety performance.
[0046] According to the present disclosure, the thickness of the active material layer is not specifically limited and can be selected according to actual needs. In a specific embodiment, the thickness of the positive electrode active material layer and the thickness of the negative electrode active material layer can be independently 50-500 μm, preferably 100-300 μm.
[0047] According to the present disclosure, the positive electrode active material can be well known to those skilled in the art. In a specific embodiment of the present disclosure, the positive electrode active material can be selected from but not limited to LiCoO2, LiNiO2, LiCo x Ni 1-x O2(0≤x≤1), LiCo x Ni 1-x-y Al y O2(0≤x≤1,0≤y≤1), LiMn2O4, LiFe x Mn y M z O4 (M is at least one of Al, Mg, Ga, Cr, Co, Ni, Cu, Zn and Mo, 0≤x≤1, 0≤y≤1, 0≤z≤1, x+y+z=1), Li 1+x L 1-y-z M y N z O2 (L, M, N is at least one of Li, Co, Mn, Ni, Fe, Al, Mg, Ga, Ti, Cr, Cu, Zn, Mo, F, I, S and B, -0.1≤x≤0.2, 0≤y≤1, 0≤z≤1, 0≤y+z≤1), LiFePO4, Li3V2(PO4)3, Li3V3(PO4)3, LiVPO4F, Li2CuO2, Li5FeO4, and metal sulfides and oxides such as TiS2, V2S3, FeS, FeS2, LiMS x (M is at least one transition metal element such as Ti, Fe, Ni, Cu, Mo, 1≤x≤2.5), TiO2, Cr3O8, V2O5, MnO2, etc.
[0048] According to the present disclosure, the first binder and the second binder may also be well known to those skilled in the art. In a specific embodiment of the present disclosure, the first binder and the second binder are each independently selected from one or more of polythiophene, polypyrrole, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polystyrene, polyacrylamide, ethylene-propylene-diene copolymer resin, styrene-butadiene rubber, polybutadiene, fluororubber, polyethylene oxide, polyvinyl pyrrolidone, polyester resin, acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol, carboxypropyl cellulose, ethyl cellulose, sodium carboxymethyl cellulose (CMC) and styrene-butadiene latex (SBR).
[0049] According to the present disclosure, the conductive material in the Ag-coated conductive material can be a material that uses electrons as a conductor of carriers; preferably, the conductive material can include but is not limited to one or more of a metal conductor, a non-metal conductor, a carbon material, a conductive polymer material, a conductive semiconductor material, a piezoelectric material and a thermoelectric material, and more preferably one or more of carbon black, carbon nanotubes, flaky graphite and graphene.
[0050] The present disclosure does not specifically limit the type of current collector, and the current collector is selected from metal foil or alloy foil. In a specific embodiment of the present disclosure, the positive electrode current collector and the negative electrode current collector are each independently selected from metal foil, metal / polymer layer composite current collector, alloy foil, etc. Preferably, the metal foil includes copper, titanium, aluminum, platinum, iridium, ruthenium, nickel, tungsten, tantalum, gold or silver foil, and the alloy foil includes stainless steel, or an alloy containing at least one element of copper, titanium, aluminum, platinum, iridium, ruthenium, nickel, tungsten, tantalum, gold and silver. Optionally, the alloy foil is composed of the above elements as the main component. The metal foil may further contain doping elements, and the doping elements include but are not limited to one or more of platinum, ruthenium, iron, cobalt, gold, copper, zinc, aluminum, magnesium, palladium, rhodium, silver and tungsten.
[0051] In one embodiment of the present disclosure, the electronic insulating layer includes an electrolyte and a diaphragm. The electrolyte may contain a lithium salt, an organic solvent and an additive. The lithium salt is one or more of common lithium salts such as LiBF4, LiPF6, LiClO4, LiTFSI, LiFSI, LiBOB, LiODFB, etc. The organic solvent is one or more of organic solvents such as carbonates, carboxylates / ethers, sulfur-containing organic solvents, nitriles, phosphorus series and silicon series, and the additive is one or more of carbonates, sulfur series, silane esters and lithium salts. The diaphragm can be one or more of those known to those skilled in the art. In a specific embodiment, the diaphragm can be selected from but not limited to PP, PE, PI, PET, PVdF, PPTA, MPIA and various composite films.
[0052] In another specific embodiment of the present disclosure, the electronic insulating layer includes a solid electrolyte, and the solid electrolyte is one or more of an oxide solid electrolyte, a sulfide solid electrolyte, a chloride solid electrolyte, a solid polymer electrolyte, and a lithium salt having lithium ion transport capability.
[0053] The second aspect of the present disclosure provides a method for preparing a battery core, the method comprising: S1, assembling a positive electrode, a negative electrode and an electronic insulating layer into a core to be dried, the positive electrode comprising a positive electrode collector and a positive electrode active material slurry layer coated on the positive electrode collector, the negative electrode comprising a negative electrode collector and a negative electrode active material slurry layer coated on the negative electrode collector; wherein the precursor of the negative electrode active material is a negative electrode active material coated with AgBr and / or a negative electrode active material coated with AgI; the positive electrode active material slurry layer contains a positive electrode active material, a first conductive agent precursor and a first binder; the negative electrode active material slurry layer contains a precursor of a negative electrode active material, a second conductive agent precursor and a second binder; the first conductive agent precursor and the second conductive agent precursor are each independently AgBr, AgI, AgBr coated conductive material and One or more of AgI-coated conductive materials; S2. Under optional negative pressure or vacuum conditions, high-energy electromagnetic waves are used to irradiate the main surface of the dried electrode core so that the positive active material slurry layer forms a positive active area, and the negative active material slurry layer forms a negative active area and is dried to obtain a dried electrode core; wherein the positive active area contains a positive active substance, a first conductive agent and a first binder, and the negative active area contains a negative active substance, a second conductive agent and a second binder; the negative active substance is a negative active material coated with Ag, and the first conductive agent and the second conductive agent are each independently Ag and / or Ag-coated conductive materials; the positive active area on the negative active material layer is completely overlapped with the negative active area; S3. The dried electrode core is injected, formed, aged and volume separated.
[0054] According to the present disclosure, the main surface of the pole core to be dried refers to the surface opposite to the positive electrode and the negative electrode. In the method disclosed in the present disclosure, the pole core to be dried is irradiated with high-energy electromagnetic waves to decompose AgBr into Ag and Br, AgI into Ag and I, AgBr-coated conductive material into Br and Ag-coated conductive material, AgI-coated conductive material into I and Ag-coated conductive material, wherein the Ag-coated conductive material and Ag single substance serve as conductive agents and form a structure in which the positive projection of the positive electrode active area on the negative electrode active material layer completely overlaps with the negative electrode active area, that is, the shape and position of the positive electrode active area and the negative electrode active area are exactly the same, so that a battery pole core with an overhang of 0 can be prepared. The method disclosed in the present disclosure is simple and easy to implement, and solves the problem of lithium deposition at the edge of the negative electrode caused by overhang in batteries prepared by traditional methods, and effectively improves the service life and safety performance of the battery.
[0055] In a preferred specific embodiment of the present disclosure, step S2 includes: irradiating the main surface of the electrode core to be dried with high-energy electromagnetic waves vertically. In this preferred embodiment, the electron path of the required area is activated by cleverly irradiating the main surface of the electrode core to be dried with high-energy electromagnetic waves vertically. The activated positive electrode active area and negative electrode active area are activated by light at a vertical angle, so the overhang in an absolute sense can be 0, that is, the positive projection of the positive electrode active area on the negative electrode active material layer is absolutely completely overlapped with the negative electrode active area, there is no offset error, and the straight distance between the edge of the positive projection of the positive electrode active area and the corresponding edge of the negative electrode active area is 0. The method is simple and easy, and the overhang of the prepared battery electrode core is 0.
[0056] In a specific embodiment of the present disclosure, the frequency of the high energy electromagnetic wave is 3×10 16 Hz-3×10 22 Hz, wavelength is less than 10nm, and the radiation power is 1kW-1000kW; preferably, the frequency is 3×10 16 Hz-3×10 20 Hz, wavelength is 0.001nm-10nm, and ray power is 10kW-100kW. Under the above conditions, the parameters of high-energy electromagnetic waves are suitable, and AgBr can be decomposed into Ag and Br, AgI can be decomposed into Ag and I, AgBr-coated conductive materials can be decomposed into Br and Ag-coated conductive materials, and AgI-coated conductive materials can be decomposed into I and Ag-coated conductive materials, so as to efficiently prepare a battery core with an overhang of 0.
[0057] According to the present disclosure, when the first conductive agent precursor and / or the second conductive agent precursor is AgBr and / or AgBr-coated conductive material, high-energy electromagnetic waves are vertically irradiated on the main surface of the dry pole core to directly extract the liquid Br element formed by the decomposition of AgBr. When the first conductive agent precursor and / or the second conductive agent precursor is AgI and / or AgI-coated conductive material, high-energy electromagnetic waves are vertically irradiated on the main surface of the dry pole core under negative pressure or vacuum to extract the gaseous I element formed by the decomposition of AgI. In a preferred embodiment, under negative pressure or vacuum, at a temperature of 25-110°C, the gaseous I element formed by the decomposition of AgI is extracted. In step S2, the negative pressure is a gas pressure state lower than normal pressure (i.e., one atmospheric pressure commonly known as atmospheric pressure). In the present disclosure, the pressure of the negative pressure is 0.1-60kPa, and the vacuum degree of the vacuum is 40-101kPa.
[0058] According to the present disclosure, the negative electrode active material can be a negative electrode active material conventionally used by those skilled in the art, and can be directly commercially purchased or prepared by methods well known to those skilled in the art. In a preferred embodiment of the present disclosure, the negative electrode active material is selected from one or more of carbon materials, transition metal oxides, lithium and alloys thereof, aluminum, gallium, indium, silicon, germanium, tin and alloys and oxides thereof.
[0059] According to the present disclosure, AgBr-coated negative electrode conductive materials, AgI-coated negative electrode conductive materials, AgBr-coated negative electrode active materials and AgI-coated negative electrode active materials can be prepared by methods well known to those skilled in the art, for example, solid phase coating, solvent reaction method, magnetron sputtering, physical vapor deposition (PVD), chemical vapor deposition (CVD) and atomic layer deposition (ALD) can be used, preferably solid phase coating method and solvent reaction method. The specific steps of the above methods are well known to those skilled in the art and will not be repeated here.
[0060] According to the present disclosure, the positive electrode active material and can be well known to those skilled in the art. In a specific embodiment of the present disclosure, the positive electrode active material is selected from but not limited to LiCoO2, LiNiO2, LiCo x Ni 1-x O2(0≤x≤1), LiCo x Ni 1-x-y Al y O2(0≤x≤1,0≤y≤1), LiMn2O4, LiFe x Mn y M z O4 (M is at least one of Al, Mg, Ga, Cr, Co, Ni, Cu, Zn and Mo, 0≤x≤1, 0≤y≤1, 0≤z≤1, x+y+z=1), Li 1+x L 1-y-z M y N z O2 (L, M, N is at least one of Li, Co, Mn, Ni, Fe, Al, Mg, Ga, Ti, Cr, Cu, Zn, Mo, F, I, S and B, -0.1≤x≤0.2, 0≤y≤1, 0≤z≤1, 0≤y+z≤1), LiFePO4, Li3V2(PO4)3, Li3V3(PO4)3, LiVPO4F, Li2CuO2, Li5FeO4, and metal sulfides and oxides such as TiS2, V2S3, FeS, FeS2, LiMS x (M is at least one transition metal element such as Ti, Fe, Ni, Cu, Mo, 1≤x≤2.5), TiO2, Cr3O8, V2O5, MnO2, etc.
[0061] According to the present disclosure, the first binder and the second binder are well known to those skilled in the art. In a specific embodiment, the first binder and the second binder are each independently selected from one or more of polythiophene, polypyrrole, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polystyrene, polyacrylamide, ethylene-propylene-diene copolymer resin, styrene-butadiene rubber, polybutadiene, fluororubber, polyethylene oxide, polyvinyl pyrrolidone, polyester resin, acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol, carboxypropyl cellulose, ethyl cellulose, sodium carboxymethyl cellulose (CMC) and styrene-butadiene latex (SBR).
[0062] According to the present disclosure, the conductive material contains a conductor whose carriers are electrons, preferably one or more of a metal conductor, a non-metal conductor, a carbon material, a conductive polymer material, a conductive semiconductor material, a piezoelectric material and a thermoelectric material, and more preferably one or more of carbon black, carbon nanotubes, flaky graphite and graphene.
[0063] The present disclosure does not specifically limit the type of current collector, and the current collector is selected from metal foil or alloy foil. In a specific embodiment of the present disclosure, the positive electrode current collector and the negative electrode current collector are each independently selected from metal foil, metal / polymer layer composite current collector, alloy foil, etc. Preferably, the metal foil includes copper, titanium, aluminum, platinum, iridium, ruthenium, nickel, tungsten, tantalum, gold or silver foil, and the alloy foil includes stainless steel, or an alloy containing at least one element of copper, titanium, aluminum, platinum, iridium, ruthenium, nickel, tungsten, tantalum, gold and silver. Optionally, the alloy foil is composed of the above elements as the main component. The metal foil may further contain doping elements, and the doping elements include but are not limited to one or more of platinum, ruthenium, iron, cobalt, gold, copper, zinc, aluminum, magnesium, palladium, rhodium, silver and tungsten.
[0064] The present disclosure does not specifically limit the form of the electrolyte, and the electrolyte can be a solid electrolyte or an electrolyte. In a specific embodiment, the electrolyte contains a lithium salt, an organic solvent and an additive, the lithium salt is one or more of common lithium salts such as LiBF4, LiPF6, LiClO4, LiTFSI, LiFSI, LiBOB, LiODFB, etc., the organic solvent is one or more of organic solvents such as carbonates, carboxylates / ethers, sulfur-containing organic solvents, nitriles, phosphorus series and silicon series, and the additive is one or more of carbonates, sulfur series, silane esters and lithium salts. In another specific embodiment of the present disclosure, the solid electrolyte is one or more of an oxide solid electrolyte, a sulfide solid electrolyte, a chloride solid electrolyte, a solid polymer electrolyte and a lithium salt having lithium ion transmission capability.
[0065] According to the present disclosure, the diaphragm may be well known to those skilled in the art. In a specific embodiment of the present disclosure, the diaphragm may be selected from but not limited to PP, PE, PI, PET, PVdF, PPTA, MPIA and various composite films.
[0066] According to the present disclosure, the present disclosure does not impose any specific restrictions on the specific conditions for drying in step S2. Drying can be carried out in equipment familiar to those skilled in the art. In a specific embodiment of the present disclosure, the drying conditions include: a temperature of 90-150°C and a time of 120 min-24 h.
[0067] A third aspect of the present disclosure provides a battery, comprising the battery core provided by the first aspect of the present disclosure or the battery core prepared by the method provided by the second aspect of the present disclosure.
[0068] The present disclosure is further illustrated below by way of examples, but the present disclosure is not limited thereby.
[0069] Unless otherwise specified in the examples and comparative examples, the raw materials used were commercially available.
[0070] The AgI or AgBr coated graphite used in the embodiment can be prepared by solid phase coating method, solvent reaction method, ALD (atomic layer deposition) method, magnetron sputtering, PVD (physical vapor deposition), CVD (chemical vapor deposition), wherein the ALD method is to use atomic layer deposition equipment to select appropriate parameters for coating, the coating thickness is thin, and the time efficiency is low. The specific method is well known to technicians in this field and will not be repeated here.
[0071] AgI solid coating method: AgI (particle size 100nm) and graphite are fully mixed at a weight ratio of 1:50, added to a shear force particle mixer, and AgI particles with different hardness are uniformly coated on the graphite surface using appropriate shear force at a certain speed. The average particle diameter of the AgI-coated graphite is 2μm and the shell layer thickness is 50nm.
[0072] AgBr solvent reaction method: a certain amount of hexadecyltrimethylammonium bromide and 1500mL of deionized water are added to form a transparent solution, 1000g of graphite is added, the container is placed in an ice water bath, 1060mL of 0.1mol / L AgNO3 solution is slowly added dropwise while the bottom layer is continuously stirred, the reaction is carried out in the dark for 24h, the solution is filtered and the obtained product is washed with deionized water and ethanol, and freeze-dried in the dark to obtain graphite uniformly coated with AgBr particles. The average particle diameter of the AgBr-coated graphite is 2μm, and the shell thickness is 50nm.
[0073] In the following embodiments, the electrode core is cut along the thickness direction and then the element analysis function of SEM is used to determine the edge position of the Br and / or I element of the positive electrode, and the edge position of the Br and / or I element of the negative electrode is determined, so as to detect the distance between the edge of the positive projection of the positive electrode active area and the corresponding edge of the negative electrode active area, that is, the size of the overhang.
[0074] Example 1
[0075] S1. 35 g of AgBr with an average particle diameter of 300 nm, 20 g of binder PVdF, 1000 g of lithium iron phosphate and 650 mL of solvent NMP are mixed to obtain a positive electrode slurry, and the positive electrode slurry is coated on a positive electrode current collector and dried to obtain a positive electrode. The positive electrode has a thickness of 150 μm based on the total weight of the positive electrode active material layer, and the content of the conductive agent is 1.9 wt %;
[0076] 35g of AgBr with an average particle diameter of 300nm, 20g of binder SBR, 1000g of AgBr-coated graphite and 2000mL of water were mixed to obtain a negative electrode slurry, and the negative electrode slurry was coated on a negative electrode current collector and dried to obtain a negative electrode. The thickness of the negative electrode active material layer in the negative electrode was 120μm based on the total weight of the negative electrode active material layer, and the content of the conductive agent was 1.9wt%;
[0077] The positive electrode, the separator and the negative electrode are stacked in sequence to obtain the electrode core to be dried.
[0078] S2. Under a negative pressure of 1 kPa, high-energy electromagnetic waves are vertically irradiated on the main surface of the electrode core to be dried, so that the positive electrode active material slurry layer forms a positive electrode active area, and the negative electrode active material slurry layer forms a negative electrode active area and is dried to obtain a dried electrode core; wherein the frequency of the high-energy electromagnetic waves is 3×10 17 Hz, wavelength is 1nm, power is 50kW;
[0079] S3, injecting liquid, forming, aging and dividing the capacity of the dried electrode core to obtain a battery electrode core.
[0080] The battery core includes a positive electrode, a negative electrode, an electrolyte and a separator; wherein the positive electrode includes a positive electrode current collector and a positive electrode active material layer covering the positive electrode current collector, the positive electrode active material layer includes a positive electrode active region, and the positive electrode active region contains lithium iron phosphate, Ag and PVdF; the negative electrode includes a negative electrode current collector and a negative electrode active material layer covering the negative electrode current collector, the negative electrode active material layer includes a negative electrode active region, and the negative electrode active region contains Ag, Ag-coated graphite and SBR. wherein the first conductive agent contained in the positive electrode active region is Ag, with an average particle diameter of 150nm and a shell thickness of 50nm; the second conductive agent contained in the negative electrode active region is Ag, with an average particle diameter of 150nm and a shell thickness of 50nm.
[0081] The distance between the edge of the positive electrode active area and the corresponding edge of the negative electrode active area is 1 μm, and it is determined that the positive electrode active area on the negative electrode active material layer completely overlaps with the negative electrode active area. The parameters of the battery core are shown in Table 1.
[0082] Example 2
[0083] The battery core was prepared by the same method as in Example 1, except that in step S1, 20 g of AgI-coated carbon black (for the positive electrode) with an average particle diameter of 150 nm was used instead of AgBr, 20 g of AgI-coated carbon black (for the negative electrode) with an average particle diameter of 150 nm was used instead of AgBr, and 1000 g of AgI-coated graphite was used instead of AgBr-coated graphite.
[0084] In the prepared battery core, the positive electrode active area contains lithium iron phosphate, Ag-coated carbon black and PVdF, and the content of the conductive agent carbon black in the positive electrode is 1.9 weight percent based on the total weight of the positive electrode active material layer; the negative electrode active area contains Ag-coated carbon black, PVdF and Ag-coated graphite, and the content of the conductive agent Ag-coated carbon black in the negative electrode is 1.9 weight percent based on the total weight of the negative electrode active material layer. The average particle diameter of the Ag-coated carbon black in the positive electrode active area is 150 nm, and the shell layer thickness is 30 nm; the average particle diameter of the Ag-coated carbon black in the negative electrode active area is 150 nm, and the shell layer thickness is 30 nm.
[0085] The detection shows that the distance between the edge of the positive electrode active region's orthographic projection and the corresponding edge of the negative electrode active region is 1 μm, and it is determined that the orthographic projection of the positive electrode active region on the negative electrode active material layer completely overlaps with the negative electrode active region.
[0086] Example 3
[0087] The battery pole core is prepared by the same method as in Example 1, except that, in step S1, 65gAgBr-coated carbon nanotubes (for the positive electrode, the carbon nanotubes have a length of 1μm-5μm and a diameter of 7nm-15nm) are used instead of AgBr, and 65gAgBr-coated graphene (for the negative electrode, the graphene has a length of 5μm-50μm and a thickness of 1nm-10nm) is used instead of AgBr.
[0088] In the prepared battery core, the positive electrode active area contains Ag-coated carbon nanotubes, PVdF and lithium iron phosphate, and the content of the conductive agent Ag-coated carbon nanotubes in the positive electrode is 6 weight% based on the total weight of the positive electrode active material layer; in the negative electrode, the negative electrode active area contains Ag-coated graphene, Ag-coated graphite and SBR, and the content of the conductive agent Ag-coated graphene in the negative electrode is 6 weight% based on the total weight of the negative electrode active material layer.
[0089] The detection shows that the distance between the edge of the positive electrode active region's orthographic projection and the corresponding edge of the negative electrode active region is 1 μm, and it is determined that the orthographic projection of the positive electrode active region on the negative electrode active material layer completely overlaps with the negative electrode active region.
[0090] Example 4
[0091] The battery core was prepared by the same method as in Example 1, except that, in step S1, 1.5 g of AgBr with an average particle diameter of 300 nm, 20 g of PVdF, 1000 g of lithium iron phosphate and 650 mL of solvent NMP were mixed to obtain a positive electrode slurry, the thickness of the positive electrode active material layer was 200 μm, and the content of the conductive agent was 0.15 wt %;
[0092] 1.5 g of AgBr with an average particle diameter of 300 nm, 20 g of SBR, 1000 g of AgBr-coated graphite and 2000 mL of water were mixed to obtain a negative electrode slurry, the thickness of the negative electrode active material layer was 150 μm, and the content of the conductive agent was 0.15 wt %.
[0093] In the battery core, the first conductive agent contained in the positive electrode active area is Ag, and the average particle diameter is 150nm; the second conductive agent contained in the negative electrode active area is Ag, and the average particle diameter is 150nm.
[0094] The detection shows that the distance between the edge of the positive electrode active region's orthographic projection and the corresponding edge of the negative electrode active region is 1 μm, and it is determined that the orthographic projection of the positive electrode active region on the negative electrode active material layer completely overlaps with the negative electrode active region.
[0095] Example 5
[0096] The battery core is prepared by the same method as in Example 1, except that in step S1, the average particle diameter of the first conductive agent AgBr is 1.5 μm, and the average particle diameter of the second conductive agent AgBr is 1.5 μm.
[0097] In the battery core, the first conductive agent contained in the positive electrode active area is Ag, and the average particle diameter is 1 μm; the second conductive agent contained in the negative electrode active area is Ag, and the average particle diameter is 1 μm.
[0098] It was detected that the distance between the edge of the positive electrode active region's orthographic projection and the corresponding edge of the negative electrode active region was 2 μm, and it was determined that the orthographic projection of the positive electrode active region on the negative electrode active material layer completely overlapped with the negative electrode active region.
[0099] Comparative Example 1
[0100] 20 g of carbon black, 20 g of PVdF, 1000 g of lithium iron phosphate and 650 mL of NMP were mixed to obtain a positive electrode slurry, and the positive electrode slurry was coated on a positive electrode current collector and dried to obtain a positive electrode, the thickness of the positive electrode active material layer was 200 μm, and the content of the conductive agent was 1.9 wt %;
[0101] 20 g of carbon black, 20 g of SBR, 1000 g of graphite and 2000 mL of water were mixed to obtain a negative electrode slurry, and the negative electrode slurry was coated on a negative electrode current collector and dried to obtain a negative electrode, wherein the thickness of the negative electrode active material layer was 150 μm, and the content of the conductive agent was 1.9 wt %;
[0102] The positive electrode, polypropylene PP and negative electrode are stacked in sequence and injected with electrolyte, and then the electrode core is obtained through formation, aging and capacity separation. The overhang of the battery electrode core is found to be greater than 100μm through testing, that is, the overhang is not zero.
[0103] Comparative Example 2
[0104] The battery core is prepared by the same method as in Example 1, except that in step S1, the negative electrode active material is replaced by graphite.
[0105] In the negative electrode of the prepared battery core, the negative electrode active area contains Ag, graphite and SBR. Graphite is directly used as the negative electrode active material in the negative electrode. The graphite has electronic conductivity so that the overhang is greater than 100 μm, that is, the overhang is not zero.
[0106] Test Case
[0107] The battery cores prepared in the examples and comparative examples were tested using the following method:
[0108] Take 20 batteries prepared in each embodiment and comparative example, and perform charge and discharge cycle test on the secondary battery performance detection device at 1C rate under 318±1K. The steps are as follows: leave for 30 minutes; charge at constant voltage until 3.8V / 0.1C is cut off; leave for 30 minutes; discharge at constant current until 2.0V, which is 1 cycle. Repeat this step 500 times, and the cycle is terminated. Compare the initial capacity ratio of the battery (with embodiment 1 as the denominator, that is, the initial capacity of each embodiment and comparative example / the initial capacity of embodiment 1) and the capacity retention rate, take the average value for each group, and then disassemble the battery to determine whether there is edge lithium deposition. The obtained cycle life and safety performance are shown in Table 2.
[0109] Table 1
[0110]
[0111]
[0112] ※ Distance: Distance refers to the distance between the edge of the positive projection of the positive active area and the corresponding edge of the negative active area.
[0113] Table 2
[0114]
[0115] As can be seen from Table 2, the overhang of the battery core prepared by the method disclosed in the present invention is 0, which solves the problem of edge lithium plating caused by overhang in traditional batteries and effectively improves the service life and safety performance of the battery.
[0116] The preferred embodiments of the present disclosure are described in detail above; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.
[0117] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.
[0118] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.
Claims
1. A battery core, characterized in that: The battery core comprises a positive electrode, a negative electrode and an electronic insulation layer; The positive electrode comprises a positive electrode current collector and a positive electrode active material layer covering the positive electrode current collector, wherein the positive electrode active material layer comprises a positive electrode active region, and the positive electrode active region contains a positive electrode active material, a first conductive agent and a first binder; The negative electrode comprises a negative electrode current collector and a negative electrode active material layer covering the negative electrode current collector, wherein the negative electrode active material layer comprises a negative electrode active region, and the negative electrode active region contains a negative electrode active material, a second conductive agent, and a second binder; The negative electrode active material is an Ag-coated negative electrode active material, the first conductive agent and the second conductive agent are each independently Ag and / or Ag-coated conductive material, and the positive projection of the positive electrode active area on the negative electrode active material layer completely overlaps with the negative electrode active area.
2. The battery core according to claim 1, wherein: The positive electrode active material layer further includes a positive electrode inactive region, and / or the negative electrode active material layer includes a negative electrode inactive region; the positive electrode inactive region and the negative electrode inactive region are not conductive.
3. The battery core according to claim 2, wherein: The positive electrode inactive region and the negative electrode inactive region independently contain one or more of AgBr, AgI, AgBr-coated conductive material and AgI-coated conductive material.
4. The battery core according to claim 1, wherein: The conductive material in the Ag-coated conductive material is selected from at least one of a granular conductive material, a rod-shaped conductive material and a sheet-shaped conductive material; The average diameter of the granular conductive material is 50nm-5μm, preferably, the average diameter is 50nm-500nm; The rod-shaped conductive material has a diameter of 3nm-30nm and a length of 1μm-50μm, preferably a diameter of 7nm-15nm and a length of 1μm-5μm; The sheet-like conductive material has a thickness of 1 nm to 50 nm and a length of 1 μm to 100 μm, preferably a thickness of 5 nm to 10 nm and a length of 5 μm to 50 μm; The Ag-coated conductive material particles include a core and a shell layer coated on the outer surface of the core, and the thickness of the shell layer is 1 nm-1 μm; The average particle diameter of the Ag is 20 nm-5 μm, preferably 30 nm-500 nm.
5. The battery core according to claim 1, wherein: The negative electrode active material is selected from one or more of carbon materials, transition metal oxides, lithium, aluminum, gallium, indium, silicon, germanium, tin, lithium alloys, aluminum alloys, gallium alloys, indium alloys, silicon alloys, germanium alloys, tin alloys, aluminum oxides, gallium oxides, indium oxides, silicon oxides, germanium oxides and tin oxides.
6. The battery core according to claim 1, wherein: Based on the total weight of the positive electrode active material layer, the content of the first conductive agent is 0.2-30% by weight, preferably 0.5-5% by weight; based on the total weight of the negative electrode active material layer, the content of the second conductive agent is 0.2-30% by weight, preferably 0.5-5% by weight.
7. The battery core according to claim 1, wherein: The conductive material is one or more of a metal conductor, a non-metal conductor, a carbon material, a conductive polymer material, a conductive semiconductor material, a piezoelectric material and a thermoelectric material, and more preferably one or more of carbon black, carbon nanotubes, graphite and graphene.
8. A method for preparing a battery core, characterized in that: The method includes: S1. Assembling a positive electrode, a negative electrode and an electronic insulating layer into an electrode core to be dried, wherein the positive electrode comprises a positive electrode current collector and a positive electrode active material slurry layer coated on the positive electrode current collector, and the negative electrode comprises a negative electrode current collector and a negative electrode active material slurry layer coated on the negative electrode current collector; The positive electrode active material slurry layer contains a positive electrode active material, a first conductive agent precursor and a first binder; the negative electrode active material slurry layer contains a negative electrode active material precursor, a second conductive agent precursor and a second binder; the precursor of the negative electrode active material is a negative electrode active material coated with AgBr and / or a negative electrode active material coated with AgI; the first conductive agent precursor and the second conductive agent precursor are each independently one or more of AgBr, AgI, AgBr coated conductive material and AgI coated conductive material; S2. Under optional negative pressure or vacuum conditions, high-energy electromagnetic waves are used to irradiate the surface of the electrode core to be dried, so that the positive electrode active material slurry layer forms a positive electrode active area, and the negative electrode active material slurry layer forms a negative electrode active area, and then drying is performed to obtain a dried electrode core; The positive electrode active area contains a positive electrode active material, a first conductive agent and a first binder, and the negative electrode active area contains a negative electrode active material, a second conductive agent and a second binder; the negative electrode active material is a negative electrode active material coated with Ag, and the first conductive agent and the second conductive agent are each independently Ag and / or Ag-coated conductive material; the positive electrode active area's orthographic projection on the negative electrode active material layer completely overlaps with the negative electrode active area; S3, injecting liquid, forming, aging and volume separation of the dried electrode core.
9. The method according to claim 8, wherein: Step S2 includes: using high-energy electromagnetic waves to vertically irradiate the main surface of the electrode core to be dried; the frequency of the high-energy electromagnetic waves is 3×10 16 Hz-3×10 22 Hz, wavelength is less than 10nm, and the radiation power is 1kW-1000kW; preferably, the frequency is 3×10 16 Hz-3×10 20 Hz, wavelength is 0.001nm-10nm, and ray power is 10kW-100kW.
10. The method according to claim 8, wherein: The negative electrode active material is selected from one or more of carbon materials, transition metal oxides, lithium, aluminum, gallium, indium, silicon, germanium, tin, lithium alloys, aluminum alloys, gallium alloys, indium alloys, silicon alloys, germanium alloys, tin alloys, aluminum oxides, gallium oxides, indium oxides, silicon oxides, germanium oxides and tin oxides.
11. A battery, characterized in that: The battery comprises the battery core according to any one of claims 1 to 7 or the battery core prepared by the method according to any one of claims 8 to 10.
Citation Information
Cited By
Garnet-type solid-state electrolyte powder, method for preparing the same, and lithium-ion cell using the same