Through sufficient extraction and simple purification process before depolymerization, the problems of insufficient dye extraction and poor color tone in the prior art are solved, and the preparation of PET resin with excellent heat resistance and drying properties is achieved.

CN118871497APending Publication Date: 2024-10-29TORAY INDUSTRIES INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380027595.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-15
Filing Date
2023-03-08
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

In the existing chemical recycling technology, the dyes in the fibers are not fully extracted, resulting in the final PET resin having a worse color tone than that made from unused raw materials, and requiring a high degree of purification process, which affects efficiency.

Method used

The coloring component is fully extracted before the depolymerization process, and the simple purification process of activated carbon treatment, filtration and crystallization is used to obtain the ester monomer (BHET) with excellent color tone, and the heat resistance is improved compared with the unused raw material. sex and dryness.

Benefits of technology

The ester monomer with excellent color tone is obtained through a simple purification process and used to prepare PET resin with excellent heat resistance and drying properties, which solves the problems of poor color tone and complicated purification process in the existing technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005042401800000111
    Figure BDA0005042401800000111
  • Figure BDA0005042401800000121
    Figure BDA0005042401800000121
Patent Text Reader

Abstract

A regenerated polyester resin obtained using a colored PET fabric as a raw material, the regenerated polyester resin being a polyethylene terephthalate resin, the polyethylene terephthalate resin having terephthalic acid residues in an amount of 88-100 mol% with respect to the total acid component, the present invention relates to a polyethylene terephthalate resin which is characterized in that the amount of ethylene glycol residues is 88-100 mol% relative to the total amount of diol components, and the polyethylene terephthalate resin satisfies the following conditions: (1) the diethylene glycol content is 0.1-0.8 mass%, (2) the nitrogen atom content is 0.5-15.0 mass ppm, and (3) the Hunter tone: b value is-10.0-less than 5.0.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a recycled polyester resin obtained by using colored PET cloth as a raw material and a method for obtaining an ester monomer from the colored PET cloth, and mainly relates to a recycled polyester resin obtained by using colored PET cloth as a raw material. Background Art

[0002] So far, a social system of mass production, mass consumption, and mass waste has been maintained, but various adverse effects on the environment, such as the depletion of natural resources and the destruction of nature accompanying resource collection, have been gradually confirmed. Therefore, in order to efficiently use limited resources and continue sustainable development, it is indispensable to build a recycling social system of reuse and recycling resources to minimize the generation of waste and prevent the generated waste from burdening the environment.

[0003] In order to realize such a recycling-oriented social system, it is necessary to build a recycling system such as thermal recycling, material recycling, and chemical recycling. Among them, chemical recycling technology that can recycle waste plastics into raw material monomer units and recycle the obtained recycled monomers into plastic materials of equivalent quality has attracted much attention.

[0004] The need for recycling of polyester fibers, which are used in a wide range of applications because they are inexpensive and have excellent mechanical properties and a dry feel, is also increasing, and various methods have been proposed as chemical recycling technologies.

[0005] For example, Patent Document 1 proposes a chemical recycling technology that uses colored polyethylene terephthalate (PET) fiber clothing to perform depolymerization and evaporation purification of bis(2-hydroxyethyl) terephthalate (BHET) as a monomer after depolymerization.

[0006] Patent Documents 2 and 3 propose a chemical recycling technology that uses a cloth made of colored polyethylene terephthalate fibers and performs dye extraction, depolymerization, and filtration purification using activated carbon.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2020-176258

[0010] Patent Document 2: Japanese Patent Application Publication No. 2005-330444

[0011] Patent Document 3: Japanese Patent Application Publication No. 2005-255963 Summary of the invention

[0012] Problems to be solved by the invention

[0013] However, in the chemical recycling technologies of the above Patent Documents 1 to 3, the pre-extraction of dyes in the fibers is not sufficient. For example, Patent Document 1 has the problem of high purification such as the <BHET evaporation and purification process> disclosed in the examples, and Patent Documents 2 and 3 have the problem of high purification such as molecular distillation in the "distillation treatment" disclosed in the examples. In addition, there is the following problem: Even after such high purification, the hue of the finally obtained PET resin is still inferior to that of the PET resin manufactured from unused raw materials.

[0014] In order to solve the problems of the above prior art, an object of the present invention is to provide a recycled polyester resin that sufficiently extracts coloring components before the depolymerization process, adopts simple purification processes such as activated carbon treatment, filtration, and crystallization after depolymerization, and moreover, uses the ester monomer (BHET) with excellent hue obtained as a raw material, and has excellent heat resistance, drying property, and the same hue as the PET resin manufactured from unused raw materials.

[0015] Means for Solving the Problems

[0016] The above problems are solved by the following [1] to [9].

[0017] [1] A recycled polyester resin obtained from a colored PET fabric as a raw material, the recycled polyester resin being a polyethylene terephthalate resin having the following characteristics (1) to (3), and the terephthalic acid residue of the polyethylene terephthalate resin being 88 mol% or more and 100 mol% or less relative to all acid components, and the ethylene glycol residue being 88 mol% or more and 100 mol% or less relative to all glycol components.

[0018] (1) The content of diethylene glycol is 0.1% by mass or more and less than 0.8% by mass

[0019] (2) The content of nitrogen atoms is 0.5 mass ppm or more and 15.0 mass ppm or less

[0020] (3) Hunter color tone: The b value is -10.0 or more and less than 5.0

[0021] [2] The recycled polyester resin according to the above [1], having the following characteristics (4) and (5).

[0022] (4) Hunter color tone: The L value is 70.0 or more and less than 85.0

[0023] (5) Hunter color tone: The a value is -2.0 or more and 2.0 or less

[0024] [3] The regenerated polyester resin according to [1] above, which has the following characteristics (6) and (7).

[0025] (6) After isothermally holding at 280°C for 5 minutes and rapidly cooling to room temperature at a rate of 100°C / min or more, a temperature rise crystallization temperature observed when heating from 20°C to 280°C at a rate of 16°C / min using a differential scanning calorimeter is 140°C or more and less than 150°C

[0026] (7) After isothermally holding at 280°C for 5 minutes, the crystallization temperature observed when cooling at a heating rate of 16°C / min was higher than 190°C and lower than 205°C

[0027] [4] A polyethylene terephthalate molded article obtained by using the recycled polyester resin described in [1] or [3] above.

[0028] [5] A method for obtaining an ester monomer using a colored PET fabric, the method comprising the following steps (1) to (3):

[0029] Step (1) is to bring heated EG into contact with a colored PET cloth to extract a coloring component, wherein the step (1) comprises the following steps (a) and (b):

[0030] Step (a), bringing EG vapor into contact with the colored PET fabric,

[0031] Step (b), bringing heated EG at 185° C. or higher into contact with the colored PET fabric;

[0032] Step (2), depolymerizing the PET fabric after the coloring component is extracted using EG to prepare an EG solution containing ester monomers;

[0033] Step (3) is a purification step of purifying the EG solution containing the ester monomer to obtain the ester monomer.

[0034] [6] The method for obtaining an ester monomer according to [5] above, characterized in that the step of purifying the EG solution containing the ester monomer (BHET) obtained by depolymerization to obtain purified BHET only includes the following steps (A) to (D):

[0035] Step (A), removing EG from the depolymerized EG solution containing BHET until the EG content is in the range of 0 mass % to 5 mass % to recover BHET;

[0036] Step (B), after carrying out the steps described in step (A), dissolving the recovered BHET in hot water at 85° C. to 100° C., and performing hot filtration;

[0037] Step (C), after carrying out the step described in step (B), cooling the filtered solution at 85° C. to 100° C. to 30° C. or less to crystallize the ester monomer to recover the ester monomer;

[0038] Step (D) is a step in which, in either step (B) or step (C), the ester monomer is dissolved in hot water and subjected to an activated carbon treatment or an ion exchange treatment.

[0039] [7] The method for obtaining an ester monomer according to [5] or [6] above, wherein the peak area of ​​the coloring component in the obtained ester monomer observed by a spectrophotometer in the range of 450 to 800 nm is 20 or less.

[0040] [8] The method for obtaining an ester monomer according to [5] or [6] above, wherein the PET fabric after the coloring component is extracted is depolymerized using 2.0 parts by mass or more and 10.0 parts by mass or less of EG relative to 1 part by mass of the PET fabric.

[0041] [9] The method for obtaining an ester monomer according to [5] or [6] above, wherein the amount of sulfur atoms contained in 100 parts by mass of the colored PET fabric is 0.01 parts by mass or more and 0.83 parts by mass or less.

[0042] Effects of the Invention

[0043] According to the present invention, a recycled polyester resin can be provided, which uses a colored PET cloth as a raw material, can obtain an ester monomer (BHET) with excellent color tone only by performing a simple purification process such as filtration and crystallization, and by polymerizing the ester monomer, thereby having excellent heat resistance and drying properties compared with PET resins obtained from virgin raw materials according to conventional methods. DETAILED DESCRIPTION

[0044] Hereinafter, the present invention will be described in detail.

[0045] In addition, in this specification, "weight" and "mass", "weight%" and "mass%", and "weight parts" and "mass parts" are respectively treated as synonyms.

[0046] In addition, in this specification, "room temperature" means 25°C.

[0047] A recycled polyester resin obtained using a colored PET cloth as a raw material according to one embodiment of the present invention is a polyethylene terephthalate resin, wherein the polyethylene terephthalate resin has a terephthalic acid residue of 88 mol% to 100 mol% relative to all acid components, and an ethylene glycol residue of 88 mol% to 100 mol% relative to all diol components, and the recycled polyester resin is characterized in that (1) the diethylene glycol content is 0.1 mass% to less than 0.8 mass%, (2) the nitrogen atom content is 0.5 mass ppm to 15.0 mass ppm, and (3) the Hunter color tone: the b value is -10.0 to less than 5.0.

[0048] The present invention aims to provide a PET fiber raw material which is inexpensive and has excellent mechanical properties and a dry feel. Therefore, the recycled polyester resin must be composed of terephthalic acid residues in an amount of 88 mol% to 100 mol% relative to the total acid components, and ethylene glycol residues in an amount of 88 mol% to 100 mol% relative to the total diol components.

[0049] From the perspective of obtaining a PET fiber with higher purity, the constituent ratio of terephthalic acid residues is preferably 90 mol% or more, more preferably 95 mol% or more, further preferably 98 mol% or more, and most preferably 99.5 mol% or more. Similarly, the constituent ratio of ethylene glycol residues is preferably 90 mol% or more, more preferably 95 mol% or more, further preferably 98 mol% or more, and most preferably 99.5 mol% or more.

[0050] The diethylene glycol content in the recycled polyester resin of the present embodiment is 0.1% by mass or more and less than 0.8% by mass. The lower the diethylene glycol content, the higher the softening point and melting point of the PET resin, and the better the heat resistance. Therefore, the diethylene glycol content must be less than 0.8% by mass. From the perspective of further improving heat resistance, it is preferably less than 0.3% by mass, and more preferably less than 0.2% by mass. In addition, diethylene glycol is inevitably generated by side reactions in the process of obtaining PET resin by polycondensation of BHET, so it is difficult to make the content less than 0.1% by mass.

[0051] It should be noted that, when a PET resin is produced from terephthalic acid and ethylene glycol as virgin raw materials by a conventional method, especially without going through a purification step, it is difficult to reduce the diethylene glycol content to less than 0.8% by mass.

[0052] The nitrogen atom content in the recycled polyester resin of the present embodiment is 0.5 mass ppm or more and 15.0 mass ppm or less. The nitrogen atom is derived from the coloring component of the fabric used as the recycled raw material, and is preferably a constituent atom of an amine structure or an azo structure. This time, it was found that, in particular, when less than 0.8 mass % of diethylene glycol is contained and more than 0.5 mass ppm of nitrogen atoms are contained, the slow crystallization rate, which is one of the shortcomings of PET resin, can be improved. Therefore, the nitrogen atom content must be 0.5 mass ppm or more, and from the perspective of further improving the crystallization rate, it is preferably 2.0 mass ppm or more, and more preferably 5.0 mass ppm or more. On the other hand, if the nitrogen atom content becomes excessive, the color tone of the PET resin deteriorates, and in addition, it becomes a disadvantage during fiber molding and the difficulty of high-speed spinning increases. Therefore, the nitrogen atom content must be 15.0 mass ppm or less, and from the perspective of further improving the color tone, it is preferably 10.0 mass ppm or less.

[0053] The nitrogen atom content can be measured using, for example, a trace nitrogen analyzer ND-100 manufactured by Mitsubishi Chemical.

[0054] The Hunter color tone: b value of the recycled polyester resin of the present embodiment is greater than -10.0 and less than 5.0. From the perspective of preventing the blue tone of the fabric from becoming stronger than the target color tone when the fabric is woven after fiber molding and dyed with a dye, the Hunter color tone: b value of the recycled polyester resin must be greater than -10.0. In addition, from the perspective of preventing the yellow tone of the fabric from becoming stronger than the target color tone when the fabric is woven after fiber molding and dyed with a dye, the Hunter color tone: b value of the recycled polyester resin must be less than 5.0, preferably less than 4.5, more preferably less than 4.0, further preferably less than 3.5, and most preferably less than 3.0. In particular, in fiber products, it is particularly important to make the Hunter color tone: b value close to 0 in recycled polyester that is prone to yellowing in order to avoid products dyed with colors other than the yellow system from having a yellow tone.

[0055] The Hunter Color: L value of the recycled polyester resin of the present embodiment is preferably 70.0 or more and less than 85.0. From the perspective of suppressing the lack of vividness of the fabric compared to the target color tone when the fabric is woven after fiber molding and dyed with a dye, the Hunter Color: L value of the recycled polyester resin is preferably 70.0 or more, more preferably 73.0 or more, further preferably 75.0 or more, particularly preferably 76.0 or more, and most preferably 77.0 or more. In addition, the Hunter Color: L value of the recycled polyester resin can be made less than 85.0, especially without adding fluorescent whitening materials, so the Hunter Color: L value of the recycled polyester resin is preferably less than 85.0.

[0056] The Hunter color: a value of the recycled polyester resin of the present embodiment is preferably not less than -2.0 and not more than 2.0. From the perspective of preventing the green tone of the fabric from becoming stronger than the target color tone when the fabric is woven after fiber molding and dyed with a dye, the Hunter color: a value of the recycled polyester resin is preferably not less than -2.0, and more preferably not less than -1.5. In addition, from the perspective of preventing the red tone of the fabric from becoming stronger than the target color tone when the fabric is woven after fiber molding and dyed with a dye, the Hunter color: a value of the recycled polyester resin is preferably not more than 2.0, and more preferably not more than 0.

[0057] Hunter color tone of recycled polyester resin: L value, a value, b value can be measured, for example, by filling pellets of recycled polyester resin into a quartz dish with a height of 20 mm and using a colorimeter SM Color Computer Model SM-T45 manufactured by Suga Test Instruments Co., Ltd. in the transmitted light mode.

[0058] In the case of the recycled polyester resin of the present embodiment, after being isothermally maintained at 280°C for 5 minutes and rapidly cooled to room temperature at a rate of 100°C / min or more, the temperature rise crystallization temperature observed when heated from 20°C to 280°C at a temperature rise rate of 16°C / min using a differential scanning calorimeter is preferably 140°C or more and less than 150°C. The lower the crystallization temperature, the faster the crystallization during the drying process proceeds, and the adhesion of the resin pellets to each other can be suppressed. From the above-mentioned viewpoints, the temperature rise crystallization temperature is preferably less than 150°C, more preferably 147°C or less, and further preferably 145°C or less. On the other hand, an excessively low temperature of the temperature rise crystallization temperature indicates that there is an excessive amount of foreign matter that becomes a crystal nucleus material in the resin, and the difficulty of high-speed spinning during fiber molding becomes high. Therefore, the temperature rise crystallization temperature is preferably 140°C or more, and more preferably 143°C or more.

[0059] For the recycled polyester resin of the present embodiment, after being isothermally maintained at 280°C for 5 minutes, the temperature drop crystallization temperature observed when cooling at a heating rate of 16°C / min is preferably higher than 190°C and lower than 205°C. The higher the temperature drop crystallization temperature, the more crystals are produced when the molten resin is water-cooled and solidified in the form of strips and processed into pellets after polycondensation of the PET resin, and the adhesion of the resin pellets to each other during the drying process can be suppressed. From the above-mentioned aspects, the temperature drop crystallization temperature is preferably higher than 190°C, and more preferably higher than 193°C. On the other hand, an excessively high temperature of the temperature drop crystallization temperature indicates that there is an excessive amount of foreign matter that becomes a crystal nucleus material in the resin, and the difficulty of high-speed spinning during fiber molding becomes high. Therefore, the temperature drop crystallization temperature is preferably lower than 205°C, more preferably lower than 203°C, and further preferably lower than 200°C.

[0060] The regenerated polyester resin of the present embodiment is preferably 253° C. or higher and 258° C. or lower when the regenerated polyester resin is isothermally maintained at 280° C. for 5 minutes, rapidly cooled to room temperature at a rate of 100° C. / min or higher, and then heated from 20° C. to 280° C. at a temperature increase rate of 16° C. / min using a differential scanning calorimeter. From the viewpoint of heat resistance, it is preferred that a large amount of diethylene glycol or a dicarboxylic acid or diol component copolymerizable with PET is contained so that the melting point is 253° C. or higher. On the other hand, in high-purity polyethylene terephthalate, it is not difficult to design the melting point to be 258° C. or lower, so the melting point is preferably 258° C. or lower.

[0061] The recycled polyester resin of the present embodiment can be made into a recycled polyester composition containing resin additives such as a pigment for coloring and an antioxidant according to the purpose of use. For example, titanium oxide particles can be included as a pigment, and by including titanium oxide particles, barrier properties can be imparted when processed into clothing products. As an antioxidant, for example, [pentaerythritol-tetrakis (3-(3,5-di-tert-butyl-4-hydroxyphenol) propionate)] (IR1010 manufactured by BASF (Ilganox (registered trademark) 1010)) which can be obtained cheaply can be exemplified.

[0062] The recycled polyester resin of this embodiment is preferably used as a processed product such as a bottle, a film, or a fiber by melt molding. In particular, by reprocessing the recycled PET cloth into a fiber product, and recycling it again after use by consumers, it is possible to reduce the amount of petroleum used in the production of polyester fibers and reduce the environmental load in the incineration of waste clothing. Therefore, the use as a fiber product is particularly preferred. However, as long as it is a processed product, the use is not limited.

[0063] When producing the recycled polyester resin of this embodiment, the fabric used as the recycled raw material is a colored PET (polyethylene terephthalate) fabric. The coloring component in the colored PET fabric is a disperse dye, a cationic dye or a pigment, preferably a disperse dye or a cationic dye.

[0064] When the recycled polyester resin of the present embodiment is produced, as the PET component in the colored PET cloth, a dicarboxylic acid component other than terephthalic acid and a diol component other than ethylene glycol (EG) may be contained as a copolymer component.

[0065] When producing the recycled polyester resin of the present embodiment, as a dicarboxylic acid component other than terephthalic acid, dicarboxylic acids such as isophthalic acid, naphthalene dicarboxylic acid, 4,4'-diphenyl dicarboxylic acid, cyclohexane dicarboxylic acid, and 5-sulfoisophthalic acid and their ester-forming derivatives can be copolymerized. From the aspect that cationic dyes can be used, a resin obtained by copolymerizing dicarboxylic acids of 5-sulfoisophthalic acid and their ester-forming derivatives can also be preferably used.

[0066] When the recycled polyester resin of the present embodiment is produced, when dicarboxylic acid of 5-sulfoisophthalic acid and its ester-forming derivative are copolymerized as the PET component in the colored PET cloth, the copolymerization amount is preferably 0.06 mol% or more and 5.0 mol% or less relative to the total dicarboxylic acid components from the viewpoint of excellent color tone of the obtained recycled polyester resin. As the upper limit, from the viewpoint of more excellent color tone, it is more preferably 3.5 mol% or less, and further preferably 2.0 mol% or less.

[0067] In the present embodiment, from the perspective of excellent color tone of the obtained recycled polyester resin, the sulfur atom content in the colored PET fabric is preferably 0.01 parts by mass or more and 0.83 parts by mass or less relative to 100 parts by mass of the colored PET fabric, and from the perspective of more excellent color tone, it is more preferably 0.59 parts by mass or less, and further preferably 0.33 parts by mass or less. The sulfur atom content in the colored PET fabric can be measured using a fluorescent X-ray analyzer (model: 3270) manufactured by Rigaku Denki Co., Ltd. after the colored fabric is melt-molded into a plate at 260°C.

[0068] When producing the recycled polyester resin of the present embodiment, as the diol component other than EG in the colored PET cloth, a diol compound such as propylene glycol, butanediol, tetramethylene glycol, hexamethylene glycol, diethylene glycol, cyclohexanedimethanol, neopentyl glycol, polypropylene glycol, and their ester-forming derivatives can be copolymerized. Preferably, EG accounts for 80 mol% or more of all diol components.

[0069] As a method for producing the recycled polyester resin of the present embodiment, from the perspective of being able to provide a recycled polyester resin having excellent color tone, heat resistance, and drying properties, a method for obtaining an ester monomer (BHET) using a colored PET cloth can be preferably adopted. This method is a method for obtaining an ester monomer comprising the following steps (1) to (3).

[0070] Step (1), bringing heated EG into contact with a colored PET cloth to extract a coloring component, the step (1) comprising steps (a) and (b):

[0071] Step (a), bringing EG vapor into contact with the colored PET fabric,

[0072] Step (b), bringing heated EG at 185° C. or higher into contact with the colored PET fabric;

[0073] Step (2), depolymerizing the PET fabric after the coloring component is extracted using EG to prepare an EG solution containing ester monomers;

[0074] Step (3) is a purification step of purifying the EG solution containing the ester monomer to obtain the ester monomer.

[0075] In the method for producing the recycled polyester resin of the present embodiment, from the viewpoint of obtaining BHET and PET resins having excellent color tones, it is preferred to include the following step (1) of bringing the colored PET cloth into contact with heated EG to extract the coloring component in advance before depolymerizing the colored PET cloth to obtain the ester monomer.

[0076] As a pre-extraction step of the coloring component, a step of bringing heated EG into contact with the colored PET fabric is included in the step (a) of bringing EG vapor into contact with the colored PET fabric; and the step (b) of bringing heated EG at 185°C or higher into contact with the colored PET fabric. By bringing the heated EG into contact with the colored PET fabric, the PET fiber structure of the colored PET fabric is relaxed, and the extraction of the coloring component becomes easy. By further bringing the heated EG at 185°C or higher into contact, the coloring component is extracted from the relaxed PET fiber.

[0077] From the viewpoint of the ease of extraction of the coloring component, the heated EG is more preferably 187°C or higher. The upper limit temperature is not specified, but from the viewpoint that it can be carried out under normal pressure, it is preferably 198°C or lower, and more preferably 190°C or lower. By applying this extraction step, the nitrogen atom content in the recycled polyester resin can be easily controlled within the range of 0.5 mass ppm or higher and 15.0 mass ppm or lower, and in addition, the Hunter color: b value in the recycled polyester resin can be easily controlled within the range of -10.0 or higher and less than 5.0.

[0078] In the method for producing the recycled polyester resin of the present embodiment, (a) contact with EG vapor and (b) contact with heated EG at 185° C. or higher can be implemented as independent steps, preferably in the order of (a) followed by (b), but can also be implemented simultaneously. As a method for implementing them simultaneously, a reflow method that can bring pure EG into contact with the colored PET cloth and can also reduce the amount of EG used is suitable.

[0079] In the method for producing the recycled polyester resin of the present embodiment, the extraction time of the coloring component of the colored PET cloth is preferably 15 minutes or more, more preferably 30 minutes or more, and even more preferably 60 minutes or more. From the perspective of preventing the embrittlement of the colored PET cloth, the upper limit time is preferably within 150 minutes. Regarding the time distribution when (a) and (b) are not performed simultaneously, the ratio of (a) to (b): (a) / (b) is preferably in the range of 1 / 9 to 5 / 5.

[0080] In the method for producing the recycled polyester resin of the present embodiment, the following step (2) is included: the PET cloth after the coloring component is extracted is depolymerized with EG to prepare an EG solution containing ester monomers. The depolymerization is preferably performed by adding 2.0 parts by mass or more and 10.0 parts by mass or less of EG to 1 part by mass of the PET cloth, and performing the depolymerization at 190° C. or more and 210° C. or less for 1.0 hour or more and 6.0 hours or less at normal pressure. By performing the depolymerization, an EG solution containing ester monomers (BHET) can be obtained.

[0081] In the method for producing the recycled polyester resin of the present embodiment, if the amount of EG added during depolymerization is less than 2.0 parts by mass relative to 1 part by mass of PET cloth, the molecular weight of the obtained BHET becomes large, and therefore the yield in the purification process performed thereafter deteriorates and the efficiency decreases. The amount of EG added is more preferably 2.3 parts by mass or more relative to 1 part by mass of PET cloth, and more preferably 2.5 parts by mass or more. In addition, even if more than 10.0 parts by mass of EG is added, the effect obtained is the same, so it is not preferred from the perspective of cost. From the perspective of cost, it is more preferably 8.0 parts by mass or less, and more preferably 6.0 parts by mass or less.

[0082] In the method for producing the regenerated polyester resin of the present embodiment, the temperature during depolymerization is preferably 190° C. to 210° C., and is more preferably 200° C. or higher from the perspective of shortening the depolymerization time. In addition, from the perspective of efficiently performing depolymerization, it is preferably performed by adding sodium hydroxide or sodium carbonate in a range of 0.5% by mass to 2.0% by mass relative to 100% by mass of BHET.

[0083] In the method for producing the recycled polyester resin of the present embodiment, from the perspective of being able to provide a recycled polyester resin having excellent color tone, heat resistance, and drying properties, the BEHT purification method can be suitably adopted, wherein the step of purifying the EG solution containing the ester monomer (BHET) obtained by depolymerization to obtain purified BHET only includes the following steps (A) to (D).

[0084] Step (A) of removing EG from the depolymerized EG solution containing BHET until the amount of EG is in the range of 0 parts by mass or more and 5 parts by mass or less, thereby recovering BHET.

[0085] Step (B), after carrying out the steps described in step (A), the recovered BHET is dissolved in hot water at 85°C or higher and 100°C or lower, and hot filtration is performed.

[0086] Step (C), after carrying out the step described in step (B), cooling the filtered solution at 85°C to 100°C to 30°C or less to crystallize the ester monomer to recover the ester monomer

[0087] Step (D): in either step (B) or step (C), the ester monomer is dissolved in hot water and then treated with activated carbon or ion exchange.

[0088] It should be noted that the ion exchange treatment refers to exposing a target solution to an ion exchange membrane or an ion exchange resin.

[0089] In the method for producing the recycled polyester resin of the present embodiment, it is preferred to perform the following step (step (A)): remove EG from the depolymerized BHET until the EG content is in the range of 0 mass % to 5 mass %. If the EG content in BHET is more than 5 mass %, the yield will deteriorate in the subsequent hot filtration step and crystallization step, which is not preferred.

[0090] As the step of removing EG from the depolymerized BHET, any of the following methods may be employed.

[0091] The first method is a reprecipitation step, that is, the EG solution of BHET obtained by depolymerization is added dropwise to water adjusted to 20°C or less to obtain a turbid solution, and then BHET containing impurities is recovered using a filter. From the perspective of increasing the yield, the water temperature is preferably 15°C or less, and more preferably 10°C or less.

[0092] The second method is a distillation removal step, that is, EG contained in the EG solution obtained by depolymerization is removed by distillation to increase the concentration.

[0093] The reprecipitation step is preferably used because the obtained recycled polyester resin has excellent color tone, heat resistance, and drying properties.

[0094] In the method for producing the recycled polyester resin of the present embodiment, in order to remove impurities (metal compounds represented by titanium oxide, inorganic compounds represented by silica gel, etc.) contained in the colored PET cloth, it is preferable to adopt a hot water dissolution step and a hot filtration step (step (B)). Water can be added dropwise to the recovered BHET obtained in the EG removal step, heated to 85°C or more and 100°C or less, and passed through a filter, thereby obtaining a transparent high-temperature aqueous solution in which BHET is dissolved.

[0095] In the method for manufacturing the regenerated polyester resin of the present embodiment, it is preferred to have the following adsorption step: adding an adsorbent such as activated carbon or an ion exchange membrane / ion exchange resin to the transparent high-temperature aqueous solution after the filtration step to remove impurities in the aqueous solution. That is, it is preferred to have a step (step (D)) of performing an activated carbon treatment or an ion exchange treatment in a state where the ester monomer is dissolved in hot water. From the perspective of being able to adsorb independently of the structure of the coloring component, an activated carbon treatment step is more preferred. In addition, in the case where it is known that most of the coloring components come from cationic dyes, ion exchange treatment can also be appropriately used.

[0096] When exposed to activated carbon, etc., a method of passing liquid through a column filled with activated carbon, etc. or directly adding activated carbon, etc. to the solution can be appropriately adopted. When a column is used, for example, when a 2.5% BHET aqueous solution is passed through, the passing time is preferably 10 minutes or more, preferably 30 minutes or more, and most preferably 60 minutes or more from the aspect of improving the removal rate of impurities. On the other hand, from the aspect of not deteriorating the BHET yield, the passing time is preferably within 180 minutes, more preferably within 120 minutes, and most preferably within 90 minutes.

[0097] In addition, in the case where activated carbon or the like is directly added to the solution and an adsorption treatment is performed for 60 to 90 minutes, the addition amount is preferably added in the range of 1% by mass or more and 65% by mass or less relative to BHET. From the aspect of improving the removal rate of impurities, the addition amount of activated carbon or the like is more preferably 3% by mass or more, further preferably 5% by mass or more, and most preferably 10% by mass or more. In addition, from the aspect of suppressing the amount of BHET attached to the activated carbon and improving the yield, the addition amount of activated carbon or the like is more preferably 40% by mass or less, further preferably 30% by mass or less, and most preferably 20% by mass or less. After the adsorption treatment is implemented, by passing it through the filter, a transparent high-temperature aqueous solution in which impurities and adsorbents such as activated carbon are removed can be obtained, but this is not necessary depending on the type of adsorbent.

[0098] In the method for producing the regenerated polyester resin of the present embodiment, it is preferred to have a crystallization step of cooling the transparent high-temperature aqueous solution after the adsorption treatment to separate the solid components of the ester monomers and perform solid-liquid separation. Specifically, it is preferred to have a step (step (C)) of cooling the filtered solution at 85° C. to 100° C. to 30° C. or less to crystallize and recover the ester monomers.

[0099] The method for producing the regenerated polyester resin of the present embodiment preferably includes a step (step (D)) of subjecting the transparent high-temperature aqueous solution before the crystallization step to the activated carbon treatment or ion exchange treatment.

[0100] It should be noted that the step of performing the activated carbon treatment or ion exchange treatment (step (D)) is preferably performed in any one of the filtration step (step (B)) and the crystallization step (step (C)).

[0101] In the method for producing the recycled polyester resin of the present embodiment, by carrying out the above-mentioned purification step, a high-quality ester monomer (BHET) with excellent color tone can be obtained. The obtained high-quality ester monomer can be polymerized in the presence of a polymerization catalyst according to a known PET polymerization method, thereby producing high-quality PET with excellent color tone, heat resistance, and drying properties.

[0102] The light absorption intensity of the coloring component in the ester monomer obtained by the method for producing the recycled polyester resin of the present embodiment can be evaluated using a spectrophotometer, and the peak area observed in the wavelength region of 450 to 800 nm can be set to 20 or less. From the perspective of obtaining high-quality BHET and PET resins with a small amount of light absorption, it is more preferably 15 or less, more preferably 10 or less, particularly preferably 5 or less, and most preferably 0.5 or less. It should be noted that the detection lower limit is 0.1.

[0103] In the method for producing the recycled polyester resin of the present invention, the absorbance intensity evaluation using a spectrophotometer is performed as follows. Regarding the sample preparation used in the evaluation, a mixed solvent of water and hexafluoroisopropanol (1:4) is prepared, and a solution containing 10% by mass of BHET is prepared using the mixed solvent, and the integrated value of the absorbance intensity at 450 to 800 nm is calculated in a wavelength scanning mode using a spectrophotometer, for example, a spectrophotometer U3010 manufactured by Hitachi High Tech Science Co., Ltd.

[0104] The present invention also provides a polyethylene terephthalate molded product obtained by using the recycled polyester resin of this embodiment. For example, the recycled polyester resin of this embodiment can be melt-molded to form fibers, thereby providing a polyethylene terephthalate molded product, which can be suitably used for general clothing applications, sportswear applications, bedding applications, and interior decoration applications.

[0105] Example

[0106] The present invention will be described in more detail below with reference to Examples and Comparative Examples. It should be noted that the present invention is not limited to the Examples and Comparative Examples.

[0107] A. Analysis of the color tone of fabrics and BHET

[0108] The sample was placed with a black calibration plate as a background using a spectrocolorimeter CM-3700d manufactured by Minolta, and the hue L* value, a* value, and b* value were measured.

[0109] B. Coloring ingredient content

[0110] A mixed solvent of water and hexafluoroisopropanol (HFIP) (1:4) was prepared, and the sample concentration was adjusted to 10 wt % using the mixed solvent. If the sample was difficult to dissolve, it was dissolved in HFIP before preparing the mixed solvent, and then water was added.

[0111] After preparing the sample solution, the absorbance intensity at 450 to 800 nm was measured in a wavelength scan mode using a spectrophotometer U3010 manufactured by Hitachi High-Tech Science & Technology Co., Ltd., and the integrated value (peak area) of the absorbance intensity was calculated.

[0112] C. Analysis of sulfur atom content (S content) in colored fabrics

[0113] The sulfur atom content in the colored fabric was measured by melt-molding the colored fabric into a sheet at 260° C. using a fluorescent X-ray analyzer (model: 3270) manufactured by Rigaku Corporation.

[0114] D. Color tone analysis of polyester resin pellets

[0115] The pellets were filled in a quartz dish with a height of 20 mm, and Hunter color tone: L value, a value, and b value were measured in the transmitted light mode using a colorimeter SM Color Computer Model SM-T45 manufactured by Suga Test Instruments Co., Ltd.

[0116] E. Nitrogen atomic content (N atomic weight) analysis

[0117] The nitrogen atom content in the recycled polyester resin was measured using a Mitsubishi Chemical micro nitrogen analyzer, model ND-100. The sample was introduced into the device, thermal analysis / oxidation was performed, and the generated nitrogen monoxide was measured using chemiluminescence. The electric furnace temperature was set to 800°C (thermal decomposition part) / 900°C (catalyst part), the main oxygen flow rate was 300mL / min, the secondary oxygen flow rate was 300mL / min, and the argon flow rate was 400mL / min. Quantification was performed based on a standard curve prepared using a pyridine standard solution.

[0118] F. Diethylene glycol (DEG) quantity analysis

[0119] 2-aminoethanol was used as a solvent and 1,6-hexanediol was added as an internal standard to the recycled polyester resin, and the mixture was decomposed at 260°C. After cooling, methanol was added, and then the mixture was neutralized with an acid, and the precipitate was filtered. The filtrate was measured using a gas chromatograph GC-14B manufactured by Shimadzu Corporation.

[0120] G. Analysis of carboxyl terminal group

[0121] 0.5 g of recycled polyester resin was accurately weighed, 40 ml of o-cresol was added, dissolved at 90°C, and titrated with 0.04 N potassium hydroxide ethanol solution, thereby calculating the amount in units of eq / ton. The same operation was repeated 5 times, and the amount of carboxyl terminal groups was the value obtained by rounding off the first decimal place of the simple average value.

[0122] H. Intrinsic Viscosity (IV) Analysis

[0123] The recycled polyester resin was dissolved in an o-chlorophenol solvent to adjust the concentrations to 0.5 g / dL, 0.2 g / dL, and 0.1 g / dL. The relative viscosity (ηr) of the solution at the obtained concentration C at 25°C was measured using an Ubbelohde viscometer, and (ηr-1) / C was plotted against C. The obtained results were extrapolated to a concentration of 0 to obtain the intrinsic viscosity.

[0124] I. Crystallization temperature and melting point analysis

[0125] About 5 mg of the recycled polyester resin was weighed and measured using a differential scanning calorimeter (DSC) Q2000 manufactured by TA Instruments to measure the rising temperature crystallization temperature, the falling temperature crystallization temperature and the melting point. The measurement was performed three times for each sample and the average value was taken as the measured value.

[0126] It should be noted that the heating crystallization temperature is obtained by isothermally maintaining the sample at 280°C for 5 minutes, then immediately taking the sample out onto an iron plate that has been cooled to room temperature, thereby rapidly cooling the sample to room temperature at a rate of more than 100°C / min, and then using the above-mentioned differential scanning calorimeter to measure the temperature observed when heating from 20°C to 280°C at a heating rate of 16°C / min.

[0127] The temperature drop crystallization temperature is obtained by isothermally maintaining at 280° C. for 5 minutes and then measuring the temperature observed when cooling at a temperature increase rate of 16° C. / min.

[0128] J. Drying evaluation

[0129] The polyester resin was quenched and solidified from the molten state in the form of strips with a diameter of 0.7 mm or more and 2.0 mm or less, and 1.5 g of cylindrical recycled polyester resin pellets cut into a height of 2.0 mm or more and 4.0 mm or less were put into a test tube with an inner diameter of 14 mm. In this state, the pellets were subjected to a crystallization treatment at 170°C for 30 minutes in air, and then cooled to room temperature. After cooling, the test tube was covered with a rubber stopper, and after vigorous up and down vibration mixing 5 times, the pellets were taken out, and the weight of the unfused pellets that were not bonded to each other was measured, and the weight % of the unfused pellets relative to the total weight was calculated. The dryness of the pellets with a calculated value of 35% by weight or more and 100% by weight or less was recorded as "S", the dryness of the pellets with a calculated value of 30% by weight or more and less than 35% by weight was recorded as "A", and the dryness of the pellets with a calculated value of 0% by weight or more and less than 30% by weight was recorded as "B".

[0130] K. Composition analysis of copolyester

[0131] The composition (type / copolymerization amount of dicarboxylic acid / diol components) of the polyester composition can be analyzed by using "AL-400" manufactured by JEOL Ltd. as a nuclear magnetic resonance apparatus (NMR), using 1,1,1,3,3,3-hexafluoro-2-propanol-D2 (deuterated HFIP) as a deuterated solvent, with a sample concentration of 50 mg of the measurement sample in 1 mL of the deuterated solvent, and setting the cumulative number of times to 128. It was confirmed that the polyesters obtained in the examples described in the present invention are all composed of terephthalic acid residues in an amount of 95 mol% or more and 100 mol% or less relative to the total acid components and ethylene glycol residues in an amount of 95 mol% or more and 100 mol% or less relative to the total diol components.

[0132] (Example 1)

[0133] For a PET cloth containing 0.3 parts by weight of titanium oxide, dyeing was performed with the dye TERASIL BLACK WW-KSN at a concentration of 6% owf (130°C, 45 minutes), and the resulting black PET cloth was cut into 1 cm squares. 1000 g of EG was placed in a 2L four-necked flask, and a glass tube containing 15 g of the cut black PET cloth was connected. Furthermore, a serpentine condenser was connected to the upper part of the connected glass tube. The set temperature of EG was set to 210°C, and heating was started. EG was refluxed for 30 minutes, and the dye was extracted. The temperature of the liquid EG refluxed in the serpentine condenser was 185°C.

[0134] The PET fabric after the dye extraction was washed with water and then dried, and 10 g of the fabric was placed in a 1 L three-necked flask. 55 g of EG was further added, and the mixture was stirred and depolymerized at an EG temperature of 200° C. for 5.5 hours.

[0135] When the depolymerized solution dropped to 100° C. or less, it was added dropwise to 500 mL of water adjusted to 10° C. or less to obtain a turbid solution. The obtained turbid solution was filtered with a 4 μ filter to obtain BHET containing impurities as a solid component.

[0136] The obtained BHET containing impurities was added to hot water at 95°C and filtered again using a 1.6μ filter. To the obtained transparent filtrate, 10% by weight of Osaka Gas Chemichrome activated carbon was added relative to the BHET containing impurities, and the mixture was heated and stirred. After 1 hour, the activated carbon was removed using a 1.0μ filter. The obtained transparent filtrate was cooled to below 20°C, and BHET was crystallized and solid-liquid separated to obtain purified BHET as a solid component.

[0137] 100 g of purified BHET obtained by performing the above operation multiple times was used as a raw material and melted at 250° C. Then, 0.005 wt % of cobalt acetate tetrahydrate and phosphoric acid, 0.03 wt % of antimony trioxide, and 0.3 wt % of titanium oxide particles were added. EG was removed by reduced pressure distillation while heating and stirring at 290° C., thereby polymerizing to obtain PET with an intrinsic viscosity (IV) of 0.65.

[0138] (Example 2)

[0139] A PET cloth copolymerized with sodium sulfonyl isophthalate (SSIA) having a sulfur atomic weight of 0.83 parts by weight and containing 0.3 parts by weight of titanium oxide was used, and dyeing was performed using the dye Nichilon Black TR 200% at a concentration of 4% owf (120°C, 60 minutes), and the dye extraction time was set to 150 minutes. The same procedure as in Example 1 was performed except that the dye extraction time was set to 150 minutes.

[0140] (Example 3)

[0141] In Example 1, the same procedures as in Example 1 were carried out except that 4.5 g of EG was additionally added in order to increase the melting rate at 250° C. when the purified BHET was polymerized.

[0142] (Examples 4 to 6)

[0143] The same procedure as in Example 1 was carried out except that the dye extraction conditions in the decolorization step of Example 1 and the adsorption treatment during the BHET purification were changed as shown in Table 1.

[0144] (Example 7)

[0145] The same procedures as in Example 1 were carried out except that the dyeing concentration described in Example 1 was lowered to obtain a gray green body and the dye extraction conditions in the decolorization step were changed as described in Table 1.

[0146] (Example 8)

[0147] The same procedures as in Example 1 were carried out except that a PET cloth copolymerized with sodium sulfoisophthalate having a sulfur atomic weight of 0.01 parts by weight and containing 0.3 parts by weight of titanium oxide was used.

[0148] (Example 9)

[0149] A PET cloth copolymerized with sodium sulfonate isophthalate having a sulfur atomic weight of 0.83 parts by weight and containing 0.3 parts by weight of titanium oxide was used, and dyeing was performed using the dye Nichilon Black TR 200% at a concentration of 4% owf (120°C, 60 minutes). The dye extraction time was set to 150 minutes, and the adsorbent used in the purification treatment was changed from activated carbon to ion exchange resin AMBERLITE IR120BH manufactured by Organo Co., Ltd. The same procedures as in Example 1 were followed except for this.

[0150] (Comparative Example 1)

[0151] The same procedures as in Example 1 were carried out except that dye extraction before depolymerization was not carried out and treatment with an adsorbent such as activated carbon was not carried out during the BHET purification treatment.

[0152] In Comparative Example 1, the Hunter color b value of the polymer was 5 or more, and the color tone was not suitable for fiber use.

[0153] (Comparative Example 2)

[0154] The same procedures as in Example 1 were carried out except that the PET fabric was used without being dyed and that the BHET purification treatment was not performed using an adsorbent such as activated carbon.

[0155] In Comparative Example 2, the nitrogen atom content was less than 0.5 mass ppm, and the drying property was poor.

[0156] (Comparative Example 3)

[0157] The same procedures as in Example 2 were carried out except that dye extraction before depolymerization was not carried out and treatment with an adsorbent such as activated carbon was not carried out during the BHET purification treatment.

[0158] In Comparative Example 3, the Hunter color b value of the polymer was 5 or more, and the color tone was not suitable for fiber use.

[0159] (Comparative Example 4)

[0160] In Example 2, the same procedures as in Example 2 were carried out except that the PET fabric was used directly without being dyed and that the BHET purification treatment was not performed using an adsorbent such as activated carbon.

[0161] In Comparative Example 4, the nitrogen atom content was less than 0.5 mass ppm, and the drying property was poor.

[0162] (Comparative Example 5)

[0163] In the dye extraction step before depolymerization of Example 1, the cut black PET cloth was placed in a three-necked flask and decolorized in EG heated to 180° C., and the same procedure as in Example 1 was performed except that the BHET purification treatment was not performed using an adsorbent such as activated carbon.

[0164] In Comparative Example 5, the color tone of the polymer deteriorated due to the change in the decolorization method.

[0165] (Comparative Example 6)

[0166] In the dye extraction process before depolymerization of Example 1, a distillation tube is connected to the glass tube containing the colored PET cloth instead of a serpentine condenser, so that EG vapor is refluxed into the flask from the serpentine condenser connected to the other part of the four-necked flask. During the BHET purification treatment, treatment with adsorbent materials such as activated carbon is not carried out. Other than this, the process is carried out in the same manner as in Example 1.

[0167] In Comparative Example 6, the color tone of the polymer deteriorated due to the change in the decolorization method.

[0168] (Comparative Examples 7 and 8)

[0169] The dye extraction conditions of Example 1 were changed as shown in Table 2, and the same procedures as in Example 1 were performed except that the treatment using an adsorbent such as activated carbon was not performed during the purification treatment.

[0170] In Comparative Examples 7 and 8, the Hunter color b value of the polymer was 5 or more, and the color tone was not suitable for fiber use.

[0171] (Comparative Example 9)

[0172] The purification treatment in Example 8 was carried out in the same manner as in Example 8, except that the treatment using an adsorbent such as activated carbon was not performed.

[0173] In Comparative Example 9, the Hunter color b value of the polymer was 5 or more, and the color tone was not suitable for fiber use.

[0174] (Comparative Example 10)

[0175] The purification treatment in Example 2 was carried out in the same manner as in Example 2, except that the treatment using an adsorbent such as activated carbon was not performed.

[0176] In Comparative Example 10, the Hunter color b value of the polymer was 5 or more, and the color tone was not suitable for fiber use.

[0177] (Comparative Example 11)

[0178] In Example 1, the same procedures as in Example 1 were carried out except that 9.0 g of EG was additionally added in order to increase the melting rate at 250° C. when the purified BHET was polymerized.

[0179] In Comparative Example 11, the diethylene glycol content exceeded 0.8% by weight, and the heat resistance and drying properties were poor.

[0180] (Comparative Example 12)

[0181] Using terephthalic acid and ethylene glycol derived from petroleum (naphtha), PET having an intrinsic viscosity (IV) of 0.65 was obtained by polymerization through esterification reaction and polycondensation reaction by a known method. As additives used in the polymerization, cobalt acetate tetrahydrate and phosphoric acid were each 0.005% by weight, antimony trioxide was 0.03% by weight, and titanium oxide particles were 0.3% by weight.

[0182] In Comparative Example 12, PET was synthesized from terephthalic acid and ethylene glycol via an esterification reaction. Therefore, the diethylene glycol content was higher than 0.8% by weight, and the heat resistance and drying properties were poor.

[0183] [Table 1]

[0184]

[0185] [Table 2]

[0186]

[0187] In the above, various embodiments are described with reference to the accompanying drawings, but it is needless to say that the present invention is not limited to the examples described. It is obvious that those skilled in the art can think of various variations or modifications within the scope of the claims, and it can be understood that they also belong to the technical scope of the present invention. In addition, the various constituent elements in the above embodiments can also be arbitrarily combined without departing from the scope of the invention.

[0188] It should be noted that this application is based on the Japanese patent application (Japanese Patent Application No. 2022-039894) filed on March 15, 2022, and its contents are incorporated into this application as a reference.

[0189] Industrial Availability

[0190] In the present invention, a recycled polyester resin having excellent color tone can be obtained using recycled PET cloth as a raw material. The PET resin has excellent heat resistance and drying properties compared to PET resins obtained from virgin raw materials according to conventional methods. The PET resin can be melt-molded into fibers, thereby being suitably used for general clothing applications, sportswear applications, bedding applications, and interior decoration applications.

Claims

1. A recycled polyester resin obtained by using a colored PET cloth as a raw material, The recycled polyester resin is a polyethylene terephthalate resin having the following characteristics (1) to (3), wherein the polyethylene terephthalate resin has terephthalic acid residues accounting for 88 mol% to 100 mol% relative to all acid components, and ethylene glycol residues accounting for 88 mol% to 100 mol% relative to all diol components, (1) The diethylene glycol content is 0.1% by mass or more and less than 0.8% by mass, (2) a nitrogen atom content of 0.5 mass ppm or more and 15.0 mass ppm or less, (3) Hunter tone: the b value is greater than -10.0 and less than 5.

0.

2. The recycled polyester resin according to claim 1, which has the following characteristics (4) and (5): (4) Hunter tone: L value is greater than 70.0 and less than 85.0, (5) Hunter tone: the a value is greater than -2.0 and less than 2.

0.

3. The recycled polyester resin according to claim 1, which has the following characteristics (6) and (7): (6) after isothermally holding at 280°C for 5 minutes and rapidly cooling to room temperature at a rate of 100°C / min or more, using a differential scanning calorimeter, when heating from 20°C to 280°C at a rate of 16°C / min, the observed temperature of crystallization is 140°C or more and less than 150°C, (7) After isothermally holding at 280°C for 5 minutes, the temperature drop crystallization temperature observed when cooling at a heating rate of 16°C / min was higher than 190°C and not higher than 205°C.

4. A polyethylene terephthalate molded article obtained by using the recycled polyester resin according to claim 1 or 3.

5. A method for obtaining an ester monomer, which is a method for obtaining an ester monomer using a colored PET cloth, the method comprising the following steps (1) to (3): Step (1) is to bring heated EG into contact with a colored PET cloth to extract a coloring component, wherein the step (1) comprises the following steps (a) and (b): Step (a), bringing EG vapor into contact with the colored PET fabric, Step (b), bringing heated EG at 185° C. or higher into contact with the colored PET fabric; Step (2), depolymerizing the PET fabric after the coloring component is extracted using EG to prepare an EG solution containing ester monomers; Step (3) is a purification step of purifying the EG solution containing the ester monomer to obtain the ester monomer.

6. The method for obtaining an ester monomer according to claim 5, characterized in that: The process of purifying the EG solution containing the ester monomer, namely BHET, obtained by depolymerization to obtain purified BHET only includes the following steps (A) to (D): Step (A), removing EG from the depolymerized EG solution containing BHET until the EG content is in the range of 0 mass % to 5 mass % to recover BHET; Step (B), after carrying out the steps described in step (A), dissolving the recovered BHET in hot water at 85° C. to 100° C., and performing hot filtration; Step (C), after carrying out the step described in step (B), cooling the filtered solution at 85° C. to 100° C. to 30° C. or less to crystallize the ester monomer to recover the ester monomer; Step (D) is a step in which, in either step (B) or step (C), the ester monomer is dissolved in hot water and subjected to an activated carbon treatment or an ion exchange treatment.

7. The method for obtaining an ester monomer according to claim 5 or 6, characterized in that: The amount of the coloring component in the obtained ester monomer was 20 or less in terms of the peak area observed by a spectrophotometer in the range of 450 to 800 nm.

8. The method for obtaining an ester monomer according to claim 5 or 6, characterized in that: The PET cloth from which the coloring component has been extracted is depolymerized with 2.0 parts by mass or more and 10.0 parts by mass or less of EG relative to 1 part by mass of the PET cloth.

9. The method for obtaining an ester monomer according to claim 5 or 6, characterized in that: The amount of sulfur atoms contained in 100 parts by mass of the colored PET cloth is 0.01 parts by mass or more and 0.83 parts by mass or less.