Composition for secondary battery

By using fluoropolymers with 1,2-vinylidene fluoride structure as binders in secondary batteries, the problems of low binder solubility and gelation in the existing technology are solved, and the efficient formation and formation of electrodes are achieved. Stability improves battery performance and manufacturing efficiency.

CN118872098APending Publication Date: 2024-10-29DAIKIN INDUSTRIES LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380027329.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-23
Filing Date
2023-03-14
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The dissolving capacity of the binder in existing secondary batteries is low, resulting in gelation of the electrode material, affecting the uniformity and performance of the electrode. The gelation phenomenon is particularly serious in cathode active materials containing lithium hydroxide, and When polyvinylidene fluoride is used as a binder, gelation occurs easily and the binder function cannot be fully exerted.

Method used

Using a fluoropolymer with a structure derived from 1,2-vinylidene fluoride as a binder, its excellent solubility can be used to form a suitable secondary battery composition in various general-purpose solvents for electrode formation and electrolyte layers. Formation or membrane formation, improves dispersion, stability and gelation, and reduces drying temperature and time.

Benefits of technology

By using a fluoropolymer with a 1,2-vinylidene fluoride structure as a binder, the low resistance of the electrode surface is improved, the dispersion and stability of the electrode are enhanced, gelation is avoided, and the electrode manufacturing process is simplified. , improving battery performance and efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118872098A_ABST
    Figure CN118872098A_ABST
Patent Text Reader

Abstract

Provided is a composition for a secondary battery using a polymer having a structure derived from 1, 2-difluoroethylene. A composition for secondary batteries, which contains a fluorine-containing polymer and a solvent, and which is characterized in that the fluorine-containing polymer is a polymer that contains a structural unit represented by general formula (1). [chemical] # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a composition for a secondary battery. Background Art

[0002] Fluorine-containing polymers are polymers used in a wide variety of fields. As monomers for producing such polymers, tetrafluoroethylene, vinylidene fluoride, hexafluoropropylene, and the like are known.

[0003] In addition, a method for producing vinylidene fluoride is disclosed in Patent Document 1. In addition, Non-Patent Document 1 discloses the compound and a polymer using the compound.

[0004] On the other hand, it is known to use a fluorine-containing resin such as polyvinylidene fluoride as a binder in electrodes of secondary batteries and the like (Patent Document 2 and the like).

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: International Publication No. 2019 / 216239

[0008] Patent Document 2: Japanese Patent Application Publication No. 2016-25027

[0009] Non-patent literature

[0010] Non-patent document 1: Poly (vinylene fluoride), Synthesis and Properties W.S.Durrell et al. Journal of Polymer Science: Part A Vol.3, P2975-2982 (1965) Summary of the invention

[0011] Problems to be solved by the invention

[0012] An object of the present disclosure is to provide a secondary battery composition using a polymer having a structure derived from vinylidene fluoride.

[0013] Means for solving problems

[0014] The present disclosure relates to a secondary battery composition, which is a secondary battery composition containing a fluorine-containing polymer and a solvent, characterized in that:

[0015] The fluorine-containing polymer is a polymer containing a structural unit represented by the following general formula (1).

[0016] [Chemistry 1]

[0017]

[0018] In the present disclosure, the fluorine-containing polymer may be a polymer further containing a structural unit represented by the following general formula (2).

[0019] [Chemistry 2]

[0020]

[0021] (R1 is hydrogen, fluorine, a partially or fully fluorinated hydrocarbon group having 5 or less carbon atoms, or an OR5 group (R5 group is a partially or fully fluorinated hydrocarbon group having 5 or less carbon atoms.). R2, R3, and R4 are each independently hydrogen or fluorine.)

[0022] The structural unit represented by the general formula (2) is preferably at least one structural unit selected from the group consisting of structural units represented by the following general formulae (3) to (8).

[0023] [Chemistry 3]

[0024]

[0025] The weight average molecular weight of the fluorine-containing polymer is preferably 50,000 to 5,000,000.

[0026] The proportion of the structural unit represented by the general formula (1) in the fluorinated polymer is preferably from 0.1 mol % to 100 mol %.

[0027] The solvent is preferably at least one compound selected from the group consisting of ester compounds, ketone compounds, and amide compounds.

[0028] The above-mentioned composition for secondary batteries is preferably used for electrodes of secondary batteries.

[0029] The secondary battery composition is preferably used for a positive electrode of a secondary battery.

[0030] The secondary battery composition is preferably used for a separator of a secondary battery.

[0031] The present disclosure also relates to a method for forming a layer for a secondary battery, the method comprising the steps of applying a slurry on a substrate and heating and drying the slurry, wherein the slurry contains the composition for a secondary battery.

[0032] The present disclosure also relates to an electrode for a secondary battery, characterized in that it has an active material layer containing a polymer and an active material, wherein the polymer contains a structural unit represented by the following general formula (1).

[0033] [Chemistry 4]

[0034]

[0035] The present disclosure also relates to a solid electrolyte layer for a secondary battery, comprising a polymer and a solid electrolyte, wherein the polymer comprises a structural unit represented by the following general formula (1).

[0036] [Chemistry 5]

[0037]

[0038] The present disclosure also relates to a secondary battery separator, which contains a polymer, wherein the polymer contains a structural unit represented by the following general formula (1).

[0039] [Chemistry 6]

[0040]

[0041] The present disclosure also relates to a secondary battery, characterized by comprising the above-mentioned secondary battery electrode and / or the above-mentioned secondary battery separator.

[0042] Effects of the Invention

[0043] The secondary battery composition of the present disclosure utilizes the advantage that a polymer having a structure derived from vinylidene fluoride has excellent solubility in various general-purpose solvents, and can be suitably used for electrode formation and the like. DETAILED DESCRIPTION

[0044] The present disclosure is described in detail below.

[0045] The present invention discloses a composition for a secondary battery that is preferably used mainly for forming an electrode, an electrolyte layer, or a separator for a secondary battery.

[0046] For example, it is known that in the formation of electrodes and electrolyte layers for sulfide-based solid-state batteries, a slurry containing sulfide-based solid electrolyte particles, a binder and a solvent is applied and dried, and then pressed. In the case of forming a good electrode and electrolyte layer by such a method, the selection of a binder and a solvent used in combination with sulfide-based solid electrolyte particles becomes important. In the case of using sulfide-based solid electrolyte particles, it is necessary to select a substance that does not react with sulfide-based solid electrolyte particles, and the types of solvents that can be used are limited. In addition, in order to prepare a slurry using such a solvent, it is necessary to select a substance that dissolves in the solvent as a binder.

[0047] Therefore, as a binder, it is preferred to use a binder having a suitable solubility in a solvent. However, most of the known binders have a low solubility in a solvent. Therefore, they cannot be fully dissolved in a slurry containing sulfide-based solid electrolyte particles and cannot fully function as a binder.

[0048] In addition, when polyvinylidene fluoride, which is a relatively cheap and general-purpose polymer, is used as the binder, gelation may occur in the slurry. When the binder gels, a uniform slurry cannot be obtained, and thus the function as a binder cannot be exerted.

[0049] Such gelation is particularly prone to occur in slurries using positive electrode active materials containing lithium hydroxide. It is speculated that some oxide-based solid electrolytes are intolerant to moisture and react with moisture in the air to change into lithium hydroxide, forming an alkali component that is the main cause of gelation. In the past, it was known that gelation would also occur in the manufacture of slurries used in the manufacture of electrode materials, and many attempts have been made to improve this.

[0050] In the present disclosure, a secondary battery composition suitable for battery production is obtained by using a fluorine-containing polymer having a structure derived from vinylidene fluoride and having good solubility as a binder.

[0051] In addition, the composition for secondary batteries disclosed in the present invention has excellent dispersibility, stability, gelation, and solid content improvement relative to viscosity. In addition, it is possible to expect low resistance on the electrode surface. Furthermore, since a low boiling point solvent can be used, it has the advantages of lowering the drying temperature and shortening the drying time during the manufacturing process of the electrode, etc.

[0052] The fluorine-containing polymer used in the present disclosure is a polymer having a structure represented by the following general formula (1), and may be a homopolymer or a copolymer.

[0053] [Chemistry 7]

[0054]

[0055] The structure represented by the above general formula (1) is a structure having the following general formula (10):

[0056] [Chemistry 8]

[0057]

[0058] The structure shown in FIG. 1 is obtained by polymerization using 1,2-difluoroethylene as a monomer. 1,2-Difluoroethylene is a known compound, but conventionally, research has been mainly conducted on its use as a refrigerant, and little research has been conducted on its use as a polymerizable monomer.

[0059] In addition, vinylidene fluoride can be used in a general manner to form a copolymer with other monomers, and the copolymerization ratio can be easily changed.

[0060] The fluorine-containing polymer is a polymer consisting only of the structure represented by the general formula (1) or a copolymer having a structural unit represented by the general formula (1).

[0061] It should be noted that 1,2-difluoroethylene has a trans isomer (E isomer) and a cis isomer (Z isomer).

[0062] [Chemistry 9]

[0063]

[0064] Thus, when only the trans isomer is used as the raw material, when only the cis isomer is used as the raw material, and when a mixture thereof is used as the raw material, the stereo configuration thereof is different. The above-mentioned fluorinated polymer may be any one of them. In addition, it may be a mixture of any proportion thereof.

[0065] When the fluorinated polymer is a copolymer, it preferably has a structural unit represented by the following general formula (2) in addition to the structural unit represented by the above general formula (1).

[0066] [Chemistry 10]

[0067]

[0068] (R1 is hydrogen, fluorine, a partially or fully fluorinated hydrocarbon group having 5 or less carbon atoms, or an OR5 group (R5 group is a partially or fully fluorinated hydrocarbon group having 5 or less carbon atoms.). R2, R3, and R4 are each independently hydrogen or fluorine.)

[0069] As the structural unit represented by the general formula (2), there can be mentioned a structure of at least one olefinic monomer which may be substituted with fluorine by a hydrogen atom, a structural unit of at least one propylene monomer which may be substituted with fluorine by a hydrogen atom, a structural unit of at least one butene monomer which may be substituted with fluorine by a hydrogen atom, a structural unit of at least one pentene monomer which may be substituted with fluorine by a hydrogen atom, etc. The fluorinated polymer disclosed in the present invention may also use two or more copolymerized structural units in combination.

[0070] Specific examples of the structure derived from an ethylenic monomer in which at least one hydrogen atom may be substituted with fluorine include vinylidene fluoride, tetrafluoroethylene (TFE), vinyl fluoride, and 1,1,2-trifluoroethylene.

[0071] Examples of the structural unit derived from an acrylic monomer in which at least one hydrogen atom is substituted with fluorine include 1270, 1216, 1252, 1243, 1234, 1225, and 1252.

[0072] Examples of the structural unit derived from a butene monomer in which at least one hydrogen atom may be substituted with fluorine include 1390, 1381, 1372, 1363, 1354, 1345, 1336, 1327, and 1318.

[0073] Examples of the pentylene monomer in which at least one hydrogen atom may be substituted with fluorine include R600, R600a, nonahydrofluoropentene, 1492, 1483, 1474, 1465, 1456, 1447, 1438, 1429, and perfluoropentene.

[0074] It should be noted that these are ASHRAE numbers.

[0075] As the structural unit derived from the propylene monomer in which at least one hydrogen atom is substituted with fluorine, particularly preferred are 1216 (hexafluoropropylene), 1225, 1234, 1243, and 1252 in terms of ASHRAE numbers. Preferred examples of such structural units include structural units represented by the following general formulae (11) to (16).

[0076] [Chemistry 11]

[0077]

[0078] (In the formula, Rf1 to Rf6 represent a fluoromethyl group having 1 to 3 fluorine atoms.)

[0079] Specific examples of the compound having the structure represented by the above general formula include 2,3,3,3-tetrafluoropropylene (HFO-1234yf), (Z or E-)1,3,3,3-tetrafluoropropylene (HFO-1234ze), (Z or E-)1,2,3,3,3-pentafluoropropylene (HFO-1225ye), (Z or E-)1,1,3,3,3-pentafluoropropylene (HFO-1225zc) and (Z or E-)3,3,3-trifluoropropylene (HFO-1243zf).

[0080] The structural unit shown in general formula (2) can also be

[0081] [Chemistry 12]

[0082]

[0083] (R1 to R3 are selected from H and F, and Rf is a fluorinated alkyl group having 1 to 6 carbon atoms).

[0084] The structural unit represented by the general formula (20) is a structural unit derived from a fluorinated vinyl ether compound. The fluorinated vinyl ether compound is not particularly limited, and examples thereof include perfluoromethyl vinyl ether (PMVE) (the following general formula (7)), perfluoroethyl vinyl ether (the following general formula (8)), and perfluoropropyl vinyl ether (the following general formula (9)).

[0085] [Chemistry 13]

[0086]

[0087] Among the structural units represented by the general formula (2) in the copolymer, structural units represented by the following general formulas (3) to (8) are particularly preferably used.

[0088] [Chemistry 14]

[0089]

[0090] The structure represented by the general formula (3) is a structural unit derived from tetrafluoroethylene, and the structure represented by the general formula (4) is a structural unit derived from vinylidene fluoride.

[0091] The structure represented by the general formula (5) is a structural unit derived from hexafluoropropylene (HFP), and the structure represented by the general formula (6) is a structural unit derived from CH2=CFCF3.

[0092] The structure represented by the general formula (7) is a structural unit derived from perfluoro(methyl vinyl ether). The structure represented by the general formula (8) is a structural unit derived from perfluoro(ethyl vinyl ether).

[0093] When the fluorinated polymer is a copolymer, the proportion of the structural unit represented by the general formula (1) is preferably from 0.1 mol % to 99.9 mol %, more preferably from 1 mol % to 99 mol %, further preferably from 10 mol % to 99 mol %.

[0094] In addition, the composition of the above-mentioned fluorine-containing polymer can be measured using an NMR analyzer.

[0095] When the fluorinated polymer is a copolymer, the proportion of the structural unit represented by the general formula (2) is preferably from 0.1 mol % to 99.9 mol %.

[0096] It should be noted that, depending on the composition of the copolymer, it may become a polymer that is difficult to dissolve in a general solvent. For example, the case of copolymerizing TFE etc. is equivalent to this. Therefore, the amount of TFE etc. is preferably less than 60 mol%.

[0097] The fluorinated polymer may have a structural unit derived from a copolymer component other than the structural unit represented by the above general formula (2). The copolymer component is not particularly limited, and examples thereof include chlorotrifluoroethylene, hexafluoroisobutylene, ethylene, propylene, and alkyl vinyl ether.

[0098] The amount of the copolymer components other than the structural unit represented by the general formula (2) is not particularly limited, but is more preferably 99.9 mol % or less, further preferably 99 mol % or less, and most preferably 97 mol % or less.

[0099] The weight average molecular weight of the fluorinated polymer is preferably 50000 to 5000000. The weight average molecular weight within the above range is preferred in terms of thermal decomposition resistance and slurry stability.

[0100] The upper limit is more preferably 3,000,000, and even more preferably 2,000,000. The lower limit is more preferably 80,000, and even more preferably 100,000. In addition, since coating properties depend on molecular weight, the weight average molecular weight is more preferably 120,000 or more.

[0101] The weight average molecular weight disclosed herein is a value measured by gel permeation chromatography (GPC).

[0102] (Polymerization method)

[0103] The fluorine-containing polymer of the present disclosure can be prepared by converting the following general formula (10) into

[0104] [Chemistry 15]

[0105]

[0106] The monomers shown are obtained by a step of polymerizing a part or all of a monomer composition. The compound represented by the above general formula (10) is a known compound and can be produced by the method described in Patent Document 1, for example.

[0107] The method for producing the fluorinated polymer is not particularly limited, and the fluorinated polymer may be produced by any common polymerization method such as solution polymerization, emulsion polymerization, suspension polymerization, etc. The solvent, emulsifier, initiator, etc. used in the polymerization are also not particularly limited, and generally known reagents may be used.

[0108] The fluorinated polymer has excellent solubility in a solvent. The secondary battery composition disclosed herein preferably has the fluorinated polymer dissolved in a solvent to be in a slurry state.

[0109] The fluorinated polymer has good solubility in a general-purpose solvent and is therefore particularly preferred from the viewpoint of cost. Examples of general-purpose solvents capable of dissolving the fluorinated polymer include N-methyl-2-pyrrolidone (NMP), acetone, methyl ethyl ketone, tetrahydrofuran, N,N-dimethylformamide, dimethylacetamide (DMAC), butyl acetate, and the like.

[0110] The solvent used in the present disclosure preferably contains at least one compound selected from the group consisting of ester compounds, ketone compounds, amide compounds, aromatic compounds, aliphatic hydrocarbon compounds, ether compounds and carbonate compounds. Preferably, it is at least one compound selected from the group consisting of ester compounds, ketone compounds and amide compounds. More preferably, it is at least one compound selected from the group consisting of ketone compounds and amide compounds.

[0111] Examples of the ester compound include compounds represented by the following general formula (21).

[0112] General formula (21):

[0113] [Chemistry 16]

[0114]

[0115] (Where R 1 and R 2 are independently H, C1~C 10 A straight-chain or branched aliphatic group, or a C6~C 10 Aromatic groups.)

[0116] In the above general formula (21), R 1 and R 2 are independently H, C1~C 10 A straight-chain or branched aliphatic group, or a C6~C 10 Examples of the aliphatic group include C1 to C 10 alkyl or alkenyl, etc. Specifically, methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, tert-butyl, pentyl, isopentyl, neopentyl, hexyl, heptyl, octyl, nonyl, decyl, vinyl, propenyl, butenyl, etc. are mentioned. Among them, methyl, ethyl, propyl, butyl, etc. are preferred. In addition, phenyl, naphthyl, etc. can be mentioned as aromatic groups.

[0117] Specific examples of the ester compound include ethyl butyrate, butyl butyrate, propyl propionate, butyl methacrylate, and ethyl acetate.

[0118] Examples of the ketone compound include compounds represented by the following general formula (22).

[0119] General formula (22):

[0120] [Chemistry 17]

[0121]

[0122] (Where R 3 and R 4 are independently H, C1~C 10 A straight-chain or branched aliphatic group, or a C6~C 10 Aromatic groups.)

[0123] In the above general formula (22), R 3 and R 4 are independently H, C1~C 10A straight-chain or branched aliphatic group, or a C6~C 10 As an aliphatic group, preferably C1 to C 10 Specifically, methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, tert-butyl, pentyl, isopentyl, neopentyl, hexyl, heptyl, octyl, nonyl, decyl, etc. are mentioned. Among them, methyl or ethyl is preferred, and methyl is more preferred. In addition, phenyl, naphthyl, etc. are mentioned as aromatic groups.

[0124] Specific examples of the ketone compound include acetone and methyl ethyl ketone.

[0125] Examples of the amide compound include compounds represented by the following general formula (23) or (24).

[0126] General formula (23):

[0127] [Chemistry 18]

[0128]

[0129] (Where R 5 H, C1~C 10 A straight-chain or branched aliphatic group, or a C6~C 10 Aromatic groups.)

[0130] General formula (24):

[0131] [Chemistry 19]

[0132]

[0133] (Where R 6 H, C1~C 10 A straight-chain or branched aliphatic group, R 7 H, C1~C 10 A straight-chain or branched aliphatic group, or a C6~C 10 Aromatic groups.)

[0134] In the above general formula (23), R 5 H, C1~C 10 A straight-chain or branched aliphatic group, or a C6~C 10 As aliphatic groups and aromatic groups, with the above R 3 and R 4 The contents described in are the same.

[0135] In the above general formula (24), R 6 H, C1~C 10 A straight-chain or branched aliphatic group, R7 H, C1~C 10 A straight-chain or branched aliphatic group, or a C6~C 10 In addition, the two R 7 As aliphatic groups and aromatic groups, the above R 3 and R 4 The contents described in are the same.

[0136] In the above general formulas (23) and (24), R 5 ~R 7 Preferably, each of the above groups is independently H, methyl or ethyl.

[0137] Specific examples of the amide compound include N-methyl-2-pyrrolidone, dimethylformamide, and dimethylacetamide.

[0138] In the present disclosure, when a sulfide-based solid electrolyte is used, a low-polarity solvent is preferably used. By using a low-polarity solvent, it is preferred that the reaction with the sulfide-based solid electrolyte particles does not easily occur. In the present disclosure, a low-polarity solvent is defined as a solvent having a relative dielectric constant of less than 20 at a frequency of 100 kHz. More preferably, it is less than 10.

[0139] The low polarity solvent is not particularly limited, and examples thereof include n-octane, n-nonane, n-decane, n-butyl ether, diisoamyl ether, ethylbenzene, ethyl acetate, ethyl butyrate, butyl butyrate, propyl propionate, butyl methacrylate, dimethyl carbonate, diethyl carbonate, methyl phenyl ether, cyclopentyl methyl ether, ethylene carbonate, diphenyl ether, fluorobenzene, trifluoromethylbenzene, bistrifluoromethylbenzene, benzene, mercaptan, and the like.

[0140] Among them, at least one solvent selected from the group consisting of propyl propionate, butyl methacrylate, ethyl acetate, ethyl butyrate, and butyl butyrate can be more preferably used. A mixed solvent of two or more of these solvents may be used in combination.

[0141] In the case of making a secondary battery composition in which the fluorinated polymer is dissolved in a solvent, the polymer concentration can be set according to the following uses, preferably 0.5 mass % or more and 90.0 mass % or less. The lower limit of the polymer concentration is more preferably 1.0 mass %, and more preferably 2.5 mass %. The upper limit of the polymer concentration is more preferably 80.0 mass %, and more preferably 75.0 mass %.

[0142] By setting it as this range, stable composition slurry for secondary batteries can be produced.

[0143] In the secondary battery composition disclosed herein, the water content is preferably low, specifically, preferably 1000 ppm or less, more preferably 500 ppm or less, and even more preferably 100 ppm or less.

[0144] The secondary battery composition disclosed in the present invention is used for electrode applications of solid-state batteries, and is also used for electrode applications of secondary batteries containing electrolytes. In addition, it is also used for solid electrolyte layer applications in solid-state batteries. Furthermore, it is also used for diaphragm applications of secondary batteries. According to these applications, the components constituting the electrodes, etc., can be appropriately combined.

[0145] When the electrode is an electrode for a solid-state battery, an electrode active material and a solid electrolyte are further used, and when the electrode is an electrode for a secondary battery containing an electrolyte solution, an electrode active material is further used. A conductive additive and other components may also be used as needed.

[0146] The secondary battery composition disclosed in the present invention can be made into a slurry for positive electrode or a slurry for negative electrode. In addition, it can also be made into a slurry for forming a solid electrolyte layer. Among them, when it is made into a slurry for electrode, it also contains active material particles. When it is made into a slurry for electrode of a solid-state battery, it contains active material particles and a solid electrolyte. The active material particles can be made into positive electrode active materials and negative electrode active materials. The secondary battery composition disclosed in the present invention can be more suitable for use as a slurry for a positive electrode using a positive electrode active material.

[0147] Hereinafter, each component for constituting the electrode will be described in detail.

[0148] (Electrode Active Material)

[0149] When the secondary battery composition of the present disclosure is used as a positive electrode slurry, a positive electrode active material is mixed in the slurry. The positive electrode active material can be a positive electrode active material known as a positive electrode active material for a secondary battery. In particular, it is preferred to use a positive electrode active material that can contain / release lithium ions.

[0150] There are no particular limitations on the positive electrode active material as long as it can electrochemically store and release lithium ions. Specifically, it is preferably a material containing lithium and at least one transition metal, such as lithium transition metal composite oxides and lithium-containing transition metal phosphate compounds.

[0151] As transition metals of lithium transition metal composite oxides, V, Ti, Cr, Mn, Fe, Co, Ni, Cu, etc. are preferred. Specific examples of lithium transition metal composite oxides include lithium cobalt composite oxides such as LiCoO2; lithium nickel composite oxides such as LiNiO2; lithium manganese composite oxides such as LiMnO2, LiMn2O4, Li2MnO3; and substances obtained by replacing part of the transition metal atoms serving as the main body of these lithium transition metal composite oxides with other metals such as Al, Ti, V, Cr, Mn, Fe, Co, Li, Ni, Cu, Zn, Mg, Ga, Zr, Si, etc. Specific examples of substances obtained by replacement include, for example, LiNi 0.5 Mn 0.5 O2、LiNi 0.85 Co 0.10 Al 0.05 O2、LiNi 0.82 Co 0.15 Al 0.03 O2、LiNi 0.80 Co 0.15 Al 0.05 O2、LiNi 1 / 3Co 1 / 3 Mn 1 / 3 O2、LiNi 0.80 Co 0.10 Mn 0.10 O2、LiMn 1.8 Al 0.2 O4、LiMn 1.5 Ni 0.5 O4、Li4Ti5O 12 In the positive electrode active material containing Ni, as the ratio of Ni increases, the capacity of the positive electrode active material increases, and thus further improvement in the capacity of the battery can be expected.

[0152] As the transition metal of the lithium-containing transition metal phosphate compound, V, Ti, Cr, Mn, Fe, Co, Ni, Cu and the like are preferred. Specific examples of the lithium-containing transition metal phosphate compound include iron phosphates such as LiFePO4, Li3Fe2(PO4)3, LiFeP2O7, cobalt phosphates such as LiCoPO4, and substances obtained by replacing a part of the transition metal atoms serving as the main body of these lithium-containing transition metal phosphate compounds with other metals such as Al, Ti, V, Cr, Mn, Fe, Co, Li, Ni, Cu, Zn, Mg, Ga, Zr, Nb, Si, etc.

[0153] In particular, LiCoO2, LiNiO2, LiMn2O4, LiNi0.82 Co 0.15 Al 0.03 O2、LiNi 0.80 Co 0.15 Al 0.05 O2、LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, LiFePO4.

[0154] In addition, components in which a substance having a composition different from that of the substance constituting the main positive electrode active material is attached to the surface of these positive electrode active materials may also be used. Examples of the surface-attached substance include oxides such as aluminum oxide, silicon oxide, titanium oxide, zirconium oxide, magnesium oxide, calcium oxide, boron oxide, antimony oxide, and bismuth oxide, sulfates such as lithium sulfate, sodium sulfate, potassium sulfate, magnesium sulfate, calcium sulfate, and aluminum sulfate, and carbonates such as lithium carbonate, calcium carbonate, and magnesium carbonate.

[0155] These surface-attached substances can be attached to the surface of the positive electrode active material by, for example, the following methods: a method of dissolving or suspending the surface-attached substance in a solvent, adding the substance to the positive electrode active material by impregnation and drying; a method of dissolving or suspending the surface-attached substance precursor in a solvent, adding the substance to the positive electrode active material by impregnation and then reacting by heating or the like; a method of adding the substance to the positive electrode active material precursor and simultaneously firing the substance; and the like.

[0156] The amount of the surface-attached substance is preferably 0.1 ppm, more preferably 1 ppm, and further preferably 10 ppm, and the upper limit is preferably 20%, more preferably 10%, and further preferably 5%, relative to the positive electrode active material, by mass. The surface-attached substance can inhibit the oxidation reaction of the non-aqueous electrolyte on the surface of the positive electrode active material and improve the battery life; if the amount of the surface-attached substance is too small, the effect cannot be fully demonstrated; if it is too large, it will hinder the entry and exit of lithium ions, so the resistance may increase.

[0157] The shape of the positive electrode active material particles can use the previously used block, polyhedron, spherical, ellipsoidal, plate-like, needle-like, columnar, etc., wherein the primary particles are preferably agglomerated to form secondary particles, and the shape of the secondary particles is spherical or ellipsoidal. Usually, in an electrochemical element, the active material in the electrode expands and shrinks with its charge and discharge, so it is easy to cause degradation such as destruction of the active material or disconnection of the conductive path caused by the stress. Therefore, compared with a single particle active material that is only a primary particle, when the primary particles are agglomerated to form secondary particles, the stress of expansion and contraction can be alleviated and degradation can be prevented, so it is preferred. In addition, compared with plate-like equiaxially oriented particles, when it is a spherical or ellipsoidal particle, the orientation during electrode molding is less, so the expansion and contraction of the electrode during charge and discharge is also less, and it is also easy to mix evenly with the conductive auxiliary agent when making the electrode, so it is preferred.

[0158] The tap density of the positive electrode active material is usually 1.3 g / cm 3 Above, preferably 1.5 g / cm 3 More preferably, 1.6 g / cm 3 More than, most preferably 1.7g / cm 3 Above. When the tap density of the positive electrode active material is lower than the above lower limit, the amount of dispersion medium required when forming the positive electrode active material layer increases, and the required amount of the conductive auxiliary agent and the binder increases, the filling rate of the positive electrode active material in the positive electrode active material layer is restricted, and the battery capacity may be restricted. By using a metal composite oxide powder with a high tap density, a high-density positive electrode active material layer can be formed. The larger the tap density is, the better, and there is no particular upper limit. However, when the tap density is too large, the diffusion of lithium ions using the non-aqueous electrolyte in the positive electrode active material layer as a medium becomes rate-controlled, and the load characteristics may be easily reduced. Therefore, the tap density is usually 2.5g / cm 3 Below, preferably 2.4 g / cm 3 the following.

[0159] The tap density of the positive electrode active material is defined as follows: a sample is passed through a sieve with a mesh size of 300 μm and falls on a surface of 20 cm 3 In a tapping cell, after filling the cell volume, use a powder density tester (such as Tapdenser manufactured by Seishin Enterprise) to perform 1000 taps with a stroke length of 10 mm. The density is calculated from the volume and weight of the sample at this time and is defined as the tap density.

[0160] The median diameter d50 of the particles of the positive electrode active material (secondary particle diameter in the case where the primary particles agglomerate to form secondary particles) is usually 0.1 μm or more, preferably 0.5 μm or more, more preferably 1 μm or more, and most preferably 3 μm or more, and usually 20 μm or less, preferably 18 μm or less, more preferably 16 μm or less, and most preferably 15 μm or less. If it is lower than the above lower limit, a high bulk density product may not be obtained; if it exceeds the upper limit, the diffusion of lithium in the particles takes time, which may lead to a decrease in battery performance, or when the positive electrode of the battery is made, that is, the positive electrode active material and the conductive aid, binder, etc. are slurried with a solvent and coated into a thin film, problems such as scratching may occur. Here, by mixing two or more positive electrode active materials with different median diameters d50, the filling property during the production of the positive electrode can be further improved.

[0161] It should be noted that the median diameter d50 in the present disclosure is measured using a known laser diffraction / scattering particle size distribution measuring device. When the particle size distribution meter uses LA-920 manufactured by HORIBA, as the dispersion medium used during measurement, a 0.1% by mass sodium hexametaphosphate aqueous solution is used, and after 5 minutes of ultrasonic dispersion, the measured refractive index is set to 1.24 for measurement.

[0162] In the case where the primary particles are agglomerated to form secondary particles, the average primary particle size of the positive electrode active material is usually 0.01 μm or more, preferably 0.05 μm or more, more preferably 0.08 μm or more, most preferably 0.1 μm or more, usually 3 μm or less, preferably 2 μm or less, more preferably 1 μm or less, and most preferably 0.6 μm or less. If the upper limit is exceeded, it is difficult to form spherical secondary particles, which has an adverse effect on the powder filling property or greatly reduces the specific surface area, so the possibility of reduced battery performance such as output characteristics is sometimes increased. On the contrary, if it is lower than the lower limit, crystallization is usually not developed, so problems such as poor reversibility of charge and discharge may occur. It should be noted that the primary particle size is measured by observation using a scanning electron microscope (SEM). Specifically, in a photograph with a magnification of 10,000 times, the longest value of the slice obtained by the left and right boundary lines of the primary particles relative to the straight line in the horizontal direction is obtained for any 50 primary particles, and the average value is obtained, thereby obtaining the primary particle size.

[0163] The BET specific surface area of ​​the positive electrode active material is 0.2 m 2 / g or more, preferably 0.3m 2 / g or more, more preferably 0.4m 2 / g or more, 4.0m 2 / g or less, preferably 2.5m 2 / g or less, more preferably 1.5m2 If the BET specific surface area is smaller than this range, the battery performance is likely to be reduced; if it is larger than this range, the tap density is difficult to increase, and the coating property when the positive electrode active material is formed may be prone to problems.

[0164] The BET specific surface area is defined as follows: using a surface area meter (for example, a fully automatic surface area measuring device manufactured by Okura Riken Co., Ltd.), the sample is pre-dried at 150°C for 30 minutes under nitrogen flow, and then a nitrogen-helium mixed gas precisely adjusted so that the relative pressure of nitrogen relative to atmospheric pressure is 0.3 is used to measure the sample by the nitrogen adsorption BET single-point method based on the gas flow method, and the BET specific surface area is defined using the obtained value.

[0165] As a method for manufacturing positive electrode active materials, a common method for manufacturing inorganic compounds is used. In particular, various methods are considered for preparing spherical or ellipsoidal active materials, for example, the following methods can be cited: a transition metal raw material such as transition metal nitrates and sulfates and raw materials of other elements as necessary are dissolved or crushed and dispersed in a solvent such as water, pH is adjusted under stirring, a spherical precursor is prepared and recovered, and it is dried as needed, and then a Li source such as LiOH, Li2CO3, LiNO3 is added and fired at a high temperature to obtain an active material; a transition metal raw material such as transition metal nitrates, sulfates, hydroxides, oxides and raw materials of other elements as necessary are dissolved or crushed and dispersed in water A method in which a raw material of a transition metal such as a nitrate, sulfate, hydroxide, oxide, etc. is dissolved or crushed and dispersed with a Li source such as LiOH, Li2CO3, LiNO3, and raw materials of other elements as necessary in a solvent such as water, and dried and molded by a spray dryer to make a spherical or ellipsoidal precursor, and then fired at a high temperature to obtain an active material; and the like.

[0166] It should be noted that the positive electrode active material may be used alone, or two or more positive electrode active materials having different compositions or different powder properties may be used in any combination and ratio.

[0167] When the secondary battery composition of the present disclosure is used as a negative electrode slurry, a negative electrode active material is mixed into the slurry. As the negative electrode active material, a known negative electrode active material for a secondary battery can be used.

[0168] The negative electrode active material is not particularly limited, and examples thereof include materials selected from lithium metal, artificial graphite, graphite carbon fiber, resin-fired carbon, pyrolysis vapor-grown carbon, coke, mesocarbon microbeads (MCMB), furfuryl alcohol resin-fired carbon, polyacene, pitch-based carbon fiber, vapor-grown carbon fiber, natural graphite, and carbon containing carbonaceous materials such as non-graphitizable carbon, silicon-containing compounds such as silicon and silicon alloys, Li4Ti5O 12 Among them, a substance containing at least a part of a carbonaceous material or a silicon-containing compound can be particularly preferably used.

[0169] In the present disclosure, the amount of active material particles in the electrode slurry is preferably 1% to 99.0% by mass relative to the total solid content of the slurry. The above lower limit is more preferably 10% by mass, and more preferably 20% by mass. The above upper limit is more preferably 98% by weight, and more preferably 97% by mass. By mixing in the above ratio, the active material layer contains the active material in the above ratio.

[0170] (Conductive additive)

[0171] In the present disclosure, the slurry for an electrode may further contain a conductive auxiliary agent as necessary.

[0172] The conductive aid used in the present invention is not particularly limited as long as it can improve the conductivity in the target electrode, and examples thereof include carbon black such as acetylene black and Ketjen black; carbon fibers such as multi-walled carbon nanotubes, single-walled carbon nanotubes, carbon nanofibers and vapor grown carbon fibers (VGCF); metal powders such as SUS powder and aluminum powder, etc.

[0173] When a conductive aid is used, the conductive aid is generally used in a solid content of the electrode slurry containing 0.01% by mass or more, preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and generally used in a solid content of 50% by mass or less, preferably 30% by mass or less, and more preferably 15% by mass or less. If the content is lower than this range, the conductivity is sometimes insufficient. On the contrary, if the content is higher than this range, the battery capacity is sometimes reduced.

[0174] The slurry may contain materials other than the above-mentioned materials. However, when the volume of the entire slurry is 100% by mass, the content of the material is preferably 8% by mass or less, and more preferably 4% by mass or less.

[0175] (Solid Electrolyte)

[0176] The solid electrolyte used in the secondary battery composition of the present disclosure may be a sulfide-based solid electrolyte or an oxide-based solid electrolyte. In particular, when a sulfide-based solid electrolyte is used, there is an advantage of having flexibility.

[0177] Examples of the sulfide-based solid electrolyte include lithium ion conductive inorganic solid electrolytes having a composition represented by the following formula (1).

[0178] Li a1 M b1 P c1 S d1 A e1 (1)

[0179] In the formula, M represents an element selected from B, Zn, Sn, Si, Cu, Ga, Sb, Al and Ge. A represents an element selected from I, Br, Cl and F. a1 to e1 represent the composition ratio of each element, and a1:b1:c1:d1:e1 satisfies 1 to 12:0 to 5:1:2 to 12:0 to 10. a1 is preferably 1 to 9, more preferably 1.5 to 7.5. b1 is preferably 0 to 3, more preferably 0 to 1. d1 is preferably 2.5 to 10, more preferably 3.0 to 8.5. e1 is preferably 0 to 5, more preferably 0 to 3.

[0180] In the present disclosure, the sulfide-based solid electrolyte preferably contains lithium. The sulfide-based solid electrolyte containing lithium is used for solid-state batteries using lithium ions as carriers, and is particularly preferred from the perspective of electrochemical devices having high energy density.

[0181] As described below, the composition ratio of each element can be controlled by adjusting the blending amount of the raw material compound when producing the sulfide-based solid electrolyte.

[0182] The sulfide-based solid electrolyte may be amorphous (glass), crystallized (glass ceramic), or only partially crystallized. For example, Li-PS-based glass containing Li, P, and S, or Li-PS-based glass ceramic containing Li, P, and S may be used.

[0183] Sulfide-based solid electrolytes can be manufactured, for example, by reacting at least two or more raw materials including lithium sulfide (Li2S), phosphorus sulfide (e.g., phosphorus pentasulfide (P2S5)), elemental phosphorus, elemental sulfur, sodium sulfide, hydrogen sulfide, lithium halide (e.g., LiI, LiBr, LiCl) and sulfides of the elements represented by M above (e.g., SiS2, SnS, GeS2).

[0184] As specific examples of sulfide-based solid electrolytes, examples of raw material combinations are shown below. Examples include Li2S-P2S5-LiCl, Li2S-P2S5-H2S, Li2S-P2S5-H2S-LiCl, Li2S-LiI-P2S5, Li2S-LiI-Li2O-P2S5, Li2S-LiBr-P2S5, Li2S-Li2O-P2S5, Li2S-Li3PO4-P2S5, Li2S-P2S5-P2O5, Li2S-P2S5-SiS2, Li2S-P2S5-SiS2-LiCl, Li2S-P2S5-SnS, Li2S-P2S5-Al2S3, Li2S- S-GeS2, Li2S-GeS2-ZnS, Li2S-Ga2S3, Li2S-GeS2-Ga2S3, Li2S-GeS2-P2S5, Li2S-GeS2-Sb2S5, Li2S-GeS2-Al2S3, Li2S-SiS2, Li2 S-Al2S3, Li2S-SiS2-Al2S3, Li2S-SiS2-P2S5, Li2S-SiS2-P2S5-LiI, Li2S-SiS2-LiI, Li2S-SiS2-Li4SiO4, Li2S-SiS2-Li3PO4, Li 10 GeP2S 12 etc. However, there is no limitation on the mixing ratio of each raw material.

[0185] The oxide-based solid electrolyte is preferably a compound containing oxygen atoms (O), having ion conductivity of a metal belonging to Group 1 or Group 2 of the periodic table, and having electron insulating properties.

[0186] As specific examples of compounds, for example, Li xa La ya TiO3[xa=0.3~0.7, ya=0.3~0.7](LLT), Li xb La yb Zr zb M bb mb O nb (M bb is at least one element selected from the group consisting of Al, Mg, Ca, Sr, V, Nb, Ta, Ti, Ge, In, and Sn, xb satisfies 5≤xb≤10, yb satisfies 1≤yb≤4, zb satisfies 1≤zb≤4, mb satisfies 0≤mb≤2, and nb satisfies 5≤nb≤20. ), Li xc B yc M cc zc O nc (M ccis at least one element selected from C, S, Al, Si, Ga, Ge, In, and Sn, xc satisfies 0≤xc≤5, yc satisfies 0≤yc≤1, zc satisfies 0≤zc≤1, and nc satisfies 0≤nc≤6. ), Li xd (Al,Ga) yd (Ti,Ge) zd Si ad P md O nd (where 1≤xd≤3, 0≤yd≤1, 0≤zd≤2, 0≤ad≤1, 1≤md≤7, 3≤nd≤13), Li (3-2xe) M ee xe D ee O(xe represents a number greater than 0 and less than 0.1, M ee Represents a divalent metal atom. ee represents a halogen atom or a combination of two or more halogen atoms. ), Li xf Si yf O zf (1≤xf≤5,0 <yf≤3、1≤zf≤10)、Li xg S yg O zg (1≤xg≤3,0 <yg≤2、1≤zg≤10)、Li3BO3-Li2SO4、Li2O-B2O3-P2O5、Li2O-SiO2、Li6BaLa2Ta2O 12 、Li3PO (4-3 / 2w) N w (w satisfies w<1) and has a LISICON (Lithium super ionic conductor) type crystal structure 3.5 Zn 0.25 GeO4, La with perovskite crystal structure 0.55 Li 0.35 TiO3, LiTi2P3O with NASICON (Natrium superionic conductor) crystal structure 12 , Li 1+xh+yh (Al,Ga) xh (Ti,Ge) 2- xh Si yh P 3-yh O 12 (where 0≤xh≤1, 0≤yh≤1), Li7La3Zr2O with garnet crystal structure 12(LLZ) and the like. In addition, ceramic materials in which LLZ has been elementally substituted are also known. For example, it is preferred to use a material containing at least one element selected from the group consisting of Mg, Al, Si, Ca (calcium), Ti, V (vanadium), Ga (gallium), Sr, Y (yttrium), Nb (niobium), Sn (tin), Sb (antimony), Ba (barium), Hf (hafnium), Ta (tantalum), W (tungsten), Bi (bismuth) and lanthanide elements. In addition, for LLZ, it is more preferred to use an LLZ-based ceramic material in which at least one element of Mg (magnesium) and A (A is at least one element selected from the group consisting of Ca (calcium), Sr (strontium), and Ba (barium)) has been substituted. In addition, phosphorus compounds containing Li, P and O are also preferred. Examples include lithium phosphate (Li3PO4), LiPON in which a portion of the oxygen in lithium phosphate is replaced with nitrogen, and LiPOD 1 (D 1 is at least one selected from Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zr, Nb, Mo, Ru, Ag, Ta, W, Pt, Au, etc. In addition, LiA 1 ON(A 1 is at least one selected from Si, B, Ge, Al, C, Ga, etc.) and the like.

[0187] The oxide-based solid electrolyte preferably contains a lanthanoid element. An oxide-based solid electrolyte containing a lanthanoid element is particularly preferred in terms of good Li ion conductivity.

[0188] The oxide-based solid electrolyte is preferably a garnet-type ion-conductive oxide. Selecting a substance having such a structure is preferred in terms of good Li ion conductivity.

[0189] The volume average particle size of the solid electrolyte is not particularly limited, but is preferably 0.01 μm or more, more preferably 0.03 μm or more. The upper limit of the volume average particle size is preferably 100 μm or less, more preferably 50 μm or less.

[0190] It should be noted that the average particle size of the solid electrolyte particles is measured in the following order. The solid electrolyte particles are diluted and adjusted to a 1% dispersion using water (heptane is used in the case of substances unstable to water) in a 20 ml sample bottle. The diluted dispersed sample is irradiated with 1 kHz ultrasound for 10 minutes and then used in the test immediately. Using the dispersion sample, 50 data acquisitions are performed using a laser diffraction / scattering particle size distribution analyzer LA-920 (manufactured by HORIBA) at a temperature of 25°C using a quartz cell for measurement to obtain the volume average particle size. For other detailed conditions, refer to the description of JIS Z 8828: 2013 "Particle Size Analysis-Dynamic Light Scattering Method" as needed. Five samples are prepared for each level, and the average value is adopted.

[0191] Regarding the content of the solid electrolyte in the solid component of the solid electrolyte composition, when considering the reduction of the interface resistance when used for a solid secondary battery and the maintenance of the reduced interface resistance, in the solid component 100% by mass, it is preferably 3% by mass or more, more preferably 4% by mass or more, and particularly preferably 5% by mass or more in the electrode. As the upper limit of the content of the solid electrolyte, from the same aspect, it is preferably 99% by mass or less, more preferably 90% by mass or less, and particularly preferably 80% by mass or less. In addition, it is preferably 50% by mass or more, more preferably 60% by mass or more, and particularly preferably 70% by mass or more in the solid electrolyte layer disposed between the positive electrode and the negative electrode. As the upper limit of the content of the solid electrolyte, from the same aspect, it is preferably 99.9% by mass or less, more preferably 99.8% by mass or less, and particularly preferably 99.7% by mass or less. The above-mentioned solid electrolyte can be used alone or in combination with two or more.

[0192] In addition, the solid content (solid content) in this specification refers to the component which does not disappear by volatilization or evaporation when drying treatment is performed at 170° C. for 6 hours in a nitrogen atmosphere. Typically, it refers to the components other than the above-mentioned dispersion medium.

[0193] The total mass of the slurry is set to 100% by mass, and the content ratio of the solvent is preferably 10% by mass or more and 90% by mass or less. If the content ratio of the solvent is less than 10% by mass, the content ratio of the solvent is too small, so the binder, active material, etc. are not dissolved in the solvent, and it is possible to form an obstacle to the formation of the layer of the secondary battery. On the other hand, if the content ratio of the solvent exceeds 90% by mass, the content ratio of the solvent is too much, so it is possible to be difficult to control the basis weight (coating). The content ratio of the solvent when the total mass of the slurry is set to 100% by mass is more preferably 20% by mass or more and 70% by mass or less, and more preferably 25% by mass or more and 65% by mass or less.

[0194] The slurry preferably contains 0.1 to 9.5 parts by mass of the fluorinated polymer as a binder relative to the total mass of the solid component in the slurry. If the binder is too little, the adhesion in the electrode layer and the adhesion between the negative electrode layer and the collector are poor when the electrode is made, and the processing of the electrode may become difficult. If the binder is too much, the resistance of the electrode increases, and a solid-state battery with sufficient performance may not be obtained.

[0195] In the present disclosure, in the process of making the above-mentioned slurry, the amount of solid components (electrode active material, solid electrolyte and binder) relative to the solvent is not particularly limited, for example, it is preferred that the solid component in the slurry is 30% by mass or more and 75% by mass or less. If it is such a solid component ratio, it is easier to manufacture an electrode or a solid electrolyte layer. The lower limit of the solid component ratio is more preferably 50% by mass or more, and the upper limit of the solid component ratio is more preferably 70% by mass or less.

[0196] In the process of preparing the above-mentioned slurry, the above-mentioned components are mixed to form a slurry. The mixing order of the components is not particularly limited, and the components can be added to a solvent and mixed. However, from the perspective of obtaining a slurry in which a binder is dissolved, it is preferably mixed by the following method.

[0197] In the step of preparing the slurry, it is preferred that a binder solution is prepared by dissolving the binder in the solvent in advance, and then the solution is mixed with other materials.

[0198] In the present disclosure, the slurry is preferably prepared according to the following steps.

[0199] (1) The above-mentioned binder is added to a solvent to obtain a binder solution containing the binder.

[0200] (2) In the case of electrode slurry, the binder solution obtained in (1), the separately prepared positive electrode active material or negative electrode active material, and the solid electrolyte as required are added to the solvent and stirred to obtain an "electrode slurry" in which the active material, binder, etc. are dispersed in the solvent. Further solvent is added and a dispersion treatment using a stirrer or the like is carried out to prepare an "electrode slurry" of a specified viscosity in a state in which the electrode active material, solid electrolyte, and binder are highly dispersed in the solvent. In step (2), a conductive auxiliary agent may be added as required.

[0201] (3) In the case of a slurry for a solid electrolyte layer, the binder solution obtained in (1) and a separately prepared solid electrolyte are added to a solvent, and a dispersion treatment using a stirrer or the like is carried out, thereby obtaining a "slurry for a solid electrolyte layer" in which the solid electrolyte and the binder are highly dispersed in the solvent. Further, a solvent is added, and a dispersion treatment using a stirrer or the like is carried out, thereby being able to prepare a "slurry for a solid electrolyte layer" of a predetermined viscosity in a state in which the solid electrolyte and the binder are highly dispersed in the solvent. In step (3), a conductive auxiliary agent may be added as needed.

[0202] Like this, by adding binder, electrode active material and / or solid electrolyte in stages and implementing successive dispersion treatment, it is possible to easily obtain a slurry in which each component is highly dispersed in a solvent. The situation of adding any component (conductive aid etc.) other than these is also the same, preferably while implementing successive dispersion treatment while adding.

[0203] However, even when a binder, an electrode active material, a solid electrolyte, and optional components are added to a solvent at once and dispersed at once, a slurry can be obtained.

[0204] It should be noted that the above-mentioned stirrer can be cited as an example of a form of dispersion treatment. In addition, dispersion using a homogenizer and the like are also conceivable.

[0205] In the step of preparing the slurry, the mixing ratio of the binder, the electrode active material and / or the solid electrolyte may be any mixing ratio that appropriately functions when forming each layer, and a known mixing ratio may be adopted.

[0206] The slurry may be used to form an electrode for a secondary battery and / or an electrolyte layer for a solid-state battery.

[0207] The method for producing the secondary battery electrode is not particularly limited, and can be carried out by (1) preparing a substrate, (2) preparing a slurry, and (3) applying the slurry to form the secondary battery electrode.

[0208] Hereinafter, the above steps (1) to (3) will be described in order.

[0209] Step (1) Step of preparing a substrate

[0210] The substrate used in the present disclosure is not particularly limited as long as it has a flat surface to which the slurry can be applied. The substrate may be in the form of a plate or a sheet. In addition, the substrate may be pre-made or may be a commercially available product.

[0211] The substrate used in the present disclosure can be used for a secondary battery after forming an electrode for a secondary battery and / or an electrolyte layer for a solid battery, or it may not be a material for a secondary battery. As an example of a substrate used in a secondary battery, for example, electrode materials such as a collector, solid electrolyte layer materials such as a solid electrolyte membrane, etc. can be cited. It is also possible to use an electrode for a secondary battery and / or an electrolyte layer for a solid battery obtained by using the slurry disclosed in the present disclosure as a substrate, and further form an electrode for a secondary battery and / or an electrolyte layer for a solid battery here.

[0212] As a substrate that does not become a material of a secondary battery, transfer substrates such as transfer sheets and transfer substrates can be cited. After the secondary battery electrode and / or solid-state battery electrolyte layer formed on the transfer substrate are joined to the secondary battery electrode and / or solid-state battery electrolyte layer by thermocompression bonding, the transfer substrate is peeled off, so that the secondary battery electrode can be formed on the solid electrolyte layer. In addition, after the secondary battery electrode formed on the transfer substrate is joined to the collector by thermocompression bonding, the transfer substrate is peeled off, so that the secondary battery electrode can be formed on the electrode collector.

[0213] Step (2) Step of preparing slurry

[0214] This step can be performed according to the above-mentioned method for preparing the slurry.

[0215] Step (3) Step of applying the slurry to form an electrode for a secondary battery or an electrolyte layer for a solid-state battery

[0216] This step is a step of applying the slurry on at least one surface of the substrate to form an electrode for a secondary battery or an electrolyte layer for a solid-state battery.

[0217] The secondary battery electrode or the solid-state battery electrolyte layer may be formed on only one surface of the substrate or may be formed on both surfaces of the substrate.

[0218] The coating method and drying method of the slurry can be appropriately selected. For example, the coating method includes spraying, screen printing, doctor blade, bar coating, roll coating, gravure printing, die coating, and the like.

[0219] Examples of the drying method include reduced pressure drying, heating drying, reduced pressure heating drying, etc. The specific conditions for reduced pressure drying and heating drying are not limited and may be appropriately set.

[0220] The amount of slurry applied varies depending on the composition of the slurry, the intended use of the secondary battery electrode, etc., but is 5 mg / cm in a dry state. 2 ~30mg / cm 2The thickness of the secondary battery electrode is not particularly limited, but may be approximately 10 μm to 250 μm.

[0221] The present disclosure also relates to an electrode for a secondary battery, characterized in that it has an active material layer containing a polymer and an active material, wherein the polymer contains a structural unit represented by general formula (1). In the case of an electrode for a solid-state secondary battery, the active material layer further contains a solid electrolyte.

[0222] The secondary battery electrode may further include a current collector and a lead connected to the current collector in addition to the active material layer.

[0223] The thickness of the active material layer used in the present disclosure varies depending on the intended use of the secondary battery, but is preferably 10 μm to 250 μm, particularly preferably 20 μm to 200 μm, and most preferably 30 μm to 150 μm.

[0224] The current collector used in the present disclosure is not particularly limited as long as it has the function of collecting the above-mentioned active material layer. As the material of the positive electrode current collector, for example, aluminum, SUS, nickel, iron, titanium, chromium, gold, platinum, zinc, etc. can be cited, among which aluminum and SUS are preferred. In addition, as the shape of the positive electrode current collector, for example, foil, plate, mesh, etc. can be cited, among which foil is preferred.

[0225] The secondary battery positive electrode disclosed herein exhibits excellent adhesive force by setting the content of the binder to 0.5 to 10 mass % of the secondary battery positive electrode (preferably the electrode active material layer), and a secondary battery using the positive electrode exhibits high output.

[0226] The negative electrode current collector used in the present disclosure is not particularly limited as long as it has the function of collecting current from the negative electrode active material layer.

[0227] As the material of the negative electrode collector, for example, chromium, SUS, nickel, iron, titanium, copper, cobalt and zinc etc. can be mentioned, among which copper, iron and SUS are preferred. In addition, as the shape of the negative electrode collector, for example, foil, plate, mesh etc. can be mentioned, among which foil is preferred.

[0228] The secondary battery negative electrode disclosed herein exhibits excellent adhesive force by setting the content of the binder to 0.5 to 10 mass % of the secondary battery negative electrode (preferably the electrode active material layer), and the sulfide-based solid-state battery using the negative electrode exhibits high output.

[0229] In addition, the present disclosure also relates to a solid electrolyte layer comprising a polymer and a solid electrolyte, wherein the polymer comprises a structural unit represented by the general formula (1). The solid electrolyte used may be the solid electrolyte described above.

[0230] The secondary battery composition of the present disclosure may also be made into a slurry for a separator.

[0231] The present disclosure also relates to a separator for a secondary battery, comprising a polymer, wherein the polymer comprises a structural unit represented by the general formula (1).

[0232] Hereinafter, the separator will be described in detail.

[0233] The diaphragm disclosed in the present invention is preferably composed of a porous substrate and a composite porous membrane formed on the porous substrate. The composite porous membrane preferably comprises the fluorinated polymer and at least one inorganic particle selected from the group consisting of metal oxide particles and metal hydroxide particles. The composite porous membrane preferably further comprises organic particles.

[0234] The content of the fluorine-containing polymer in the composite porous membrane is preferably 50% by mass or less.

[0235] If it exceeds 50 mass %, the porosity in the composite porous membrane decreases excessively, and the ion permeation function as a separator may not be exhibited.

[0236] The content of the fluorine-containing polymer in the composite porous membrane is preferably 1 mass % or more because the bonding between the inorganic particles is insufficient and the mechanical properties of the composite porous membrane may be significantly reduced.

[0237] The content of the fluorinated polymer in the composite porous membrane is more preferably 45% by mass or less, further preferably 40% by mass or less, more preferably 2% by mass or more, further preferably 3% by mass or more, particularly preferably 4% by mass or more.

[0238] The composite porous membrane comprises at least one inorganic particle selected from the group consisting of metal oxide particles and metal hydroxide particles. The content of the inorganic particles is preferably 50% to 99% by mass in the composite porous membrane. If the content of the inorganic particles is within the above range, a separator having a composite porous membrane with a pore size and porosity that does not hinder the permeation of lithium ions can be obtained. Furthermore, a separator with high heat resistance and little shrinkage due to heat can be achieved.

[0239] The content of the inorganic particles in the composite porous membrane is more preferably 55 mass % or more, further preferably 60 mass % or more, more preferably 98 mass % or less, further preferably 97 mass % or less, particularly preferably 96 mass % or less.

[0240] The average particle size of the inorganic particles is preferably 20 μm or less, more preferably 10 μm or less, and even more preferably 5 μm or less. The lower limit of the average particle size is preferably 0.001 μm.

[0241] The above average particle size is a value measured using a transmission electron microscope, a laser particle size distribution analyzer, or the like.

[0242] The metal oxide particles are preferably metal oxides other than alkali metals and alkaline earth metals, and more preferably at least one selected from the group consisting of aluminum oxide, silicon oxide, titanium oxide, vanadium oxide and copper oxide, from the perspective of improving the ion conductivity and shutdown effect of the separator.

[0243] The average particle size of the metal oxide particles is preferably 20 μm or less, more preferably 10 μm or less, and even more preferably 5 μm or less. The lower limit of the average particle size is preferably 0.001 μm.

[0244] The above average particle size is a value measured using a transmission electron microscope.

[0245] Particularly preferred metal oxide particles are aluminum oxide particles or silicon oxide particles having an average particle size of 5 μm or less, from the viewpoint of excellent ion conductivity.

[0246] The content of the metal oxide particles is preferably 50% to 99% by mass in the composite porous membrane. If the content of the metal oxide particles is within the above range, a separator having a composite porous membrane having a pore size and porosity that does not hinder the permeation of lithium ions can be obtained. Furthermore, a separator having high heat resistance and little shrinkage due to heat can be achieved.

[0247] The content of the metal oxide particles in the composite porous membrane is more preferably 55 mass % or more, further preferably 60 mass % or more, more preferably 98 mass % or less, further preferably 97 mass % or less, particularly preferably 96 mass % or less.

[0248] The metal hydroxide particles are preferably hydroxides of alkali metals or alkaline earth metals, and more preferably at least one selected from the group consisting of magnesium hydroxide, calcium hydroxide, aluminum hydroxide, chromium hydroxide, zirconium hydroxide and nickel hydroxide, from the perspective of improving the ion conductivity and shutdown effect of the separator.

[0249] The average particle size of the metal hydroxide particles is preferably 20 μm or less, more preferably 10 μm or less, and even more preferably 5 μm or less. The lower limit of the average particle size is preferably 0.001 μm.

[0250] The above average particle size is a value measured using a transmission electron microscope.

[0251] The content of the metal hydroxide particles is preferably 50% to 99% by mass in the composite porous membrane. If the content of the metal hydroxide particles is within the above range, a separator having a composite porous membrane with a pore size and porosity that does not hinder the permeation of lithium ions can be obtained. Furthermore, a separator with high heat resistance and little shrinkage due to heat can be achieved.

[0252] The content of the metal hydroxide particles in the composite porous membrane is more preferably 55% by mass or more, further preferably 60% by mass or more, and more preferably 98% by mass or less, further preferably 97% by mass or less.

[0253] The composite porous membrane preferably further includes organic particles. The organic particles are preferably non-conductive cross-linked polymers, more preferably cross-linked polystyrene, cross-linked polymethacrylate, or cross-linked acrylate.

[0254] The average particle size of the organic particles is preferably 20 μm or less, more preferably 10 μm or less, and even more preferably 5 μm or less. The lower limit of the average particle size is preferably 0.001 μm.

[0255] The above average particle size is a value measured using a transmission electron microscope.

[0256] The content of the organic particles in the composite porous membrane is preferably 0 to 49% by mass. When the content of the organic particles is within the above range, a separator having a laminated composite porous membrane having a pore diameter and porosity that does not hinder lithium ion permeation can be obtained.

[0257] The content of the organic particles in the composite porous membrane is more preferably 2% by mass or more, further preferably 5% by mass or more, and more preferably 37% by mass or less, further preferably 35% by mass or less.

[0258] The composite porous membrane may contain other components in addition to the fluorine-containing polymer, inorganic particles, and organic particles. Examples of the other components include other resins, rubbers, and the like.

[0259] Preferred resins for use together include, for example, one or more of polyacrylate, polymethacrylate, polyacrylonitrile, polyamide-imide, polyvinylidene fluoride (PVdF), and VdF / HEP copolymer resins.

[0260] Preferred rubbers for use include, for example, one or more of VdF / HFP copolymer rubber, VdF / TFE / HFP copolymer rubber, acrylic rubber, etc. These rubbers may be crosslinked or not.

[0261] As the resin or rubber used in combination, acrylic rubber is particularly preferred from the perspective of improving ion conductivity; in addition, VdF / HFP copolymer rubber, VdF / TFE / HFP copolymer rubber, and VdF / HFP resin are preferred from the perspective of improving ion conductivity and improving oxidation resistance.

[0262] In the VdF / HFP copolymer rubber, the VdF unit / HFP unit is preferably in a molar ratio of 80 / 20 to 65 / 35.

[0263] In the VdF / TFE / HFP copolymer rubber, the molar ratio of VdF unit / HFP unit / TFE unit is preferably 80 / 5 / 15 to 60 / 30 / 10.

[0264] In the VdF / HFP resin, the VdF unit / HFP unit is preferably in a molar ratio of 98 / 2 to 85 / 15.

[0265] The melting point of the VdF / HFP resin is preferably 100°C to 200°C.

[0266] The amount of other resin or rubber mixed is preferably 400 parts by mass or less, more preferably 200 parts by mass or less, and further preferably 150 parts by mass or less, based on 100 parts by mass of the fluorinated polymer. The lower limit varies depending on the intended effect, but is about 10 parts by mass.

[0267] The composite porous membrane is preferably provided on a porous substrate, and more preferably provided directly on the porous substrate.

[0268] In addition, the composite porous membrane may be arranged only on one side of the porous substrate or on both sides. In addition, the composite porous membrane may be arranged in a manner that covers the entire porous substrate on which the composite porous membrane is arranged, or may be arranged in a manner that covers only a portion of the porous substrate.

[0269] The weight of the composite porous membrane is preferably 0.5 g / m2 when the composite porous membrane is formed only on one side of the porous substrate. 2 ~50.0g / m 2 If it is less than 0.5g / m 2 If the thickness is more than 50.0 g / m 2 When the composite porous membrane is formed on both the surface and the back of the porous substrate, the weight of the fluorinated polymer is preferably 0.1 g / m 2 ~6.0g / m 2 .

[0270] The porous substrate is a substrate having pores or voids inside. As such a substrate, porous sheets formed of fibrous materials such as microporous membranes or nonwoven fabrics, paper sheets, or composite porous membranes obtained by laminating one or more other porous layers on these microporous membranes or porous sheets can be cited. It should be noted that the microporous membrane is a membrane having a large number of micropores inside, a structure formed by connecting these micropores, and gas or liquid can pass from one surface to another.

[0271] The material constituting the porous substrate can be any material of an organic material or an inorganic material having electrical insulation. In particular, from the perspective of imparting a shutdown function to the substrate, a thermoplastic resin is preferably used as the constituent material of the substrate. Here, the so-called shutdown function refers to the function that when the battery temperature rises, the thermoplastic resin dissolves and blocks the pores of the porous substrate, thereby blocking the movement of ions and preventing thermal runaway of the battery. As a thermoplastic resin, a thermoplastic resin having a melting point of less than 200°C is suitable, and polyolefins are particularly preferred.

[0272] As a porous substrate using polyolefin, a polyolefin microporous membrane is suitable. As a polyolefin microporous membrane, a polyolefin microporous membrane having sufficient mechanical properties and ion permeability and suitable for existing non-aqueous secondary battery separators can be used. Moreover, from the aspect of having the above-mentioned shutdown function, the polyolefin microporous membrane preferably includes polyethylene.

[0273] The weight average molecular weight of the polyolefin is preferably 100,000 to 5,000,000. If the weight average molecular weight is less than 100,000, it may be difficult to ensure sufficient mechanical properties. In addition, if the weight average molecular weight is greater than 5,000,000, there may be cases where the shutdown characteristics deteriorate or molding becomes difficult.

[0274] Such a polyolefin microporous film can be manufactured, for example, by the following method. That is, a method for forming a microporous film by sequentially implementing the following steps can be cited: (i) a process of extruding a molten polyolefin resin from a T-die and forming a sheet, (ii) a process of crystallizing the sheet, (iii) a process of stretching the sheet, and (iv) a process of heat-treating the sheet. In addition, a method for forming a microporous film by sequentially implementing the following steps can also be cited: (i) a polyolefin resin is melted together with a plasticizer such as liquid paraffin, extruded from a T-die and cooled to form a sheet, (ii) a process of stretching the sheet, (iii) a process of extracting the plasticizer from the sheet, and (iv) a process of heat-treating the sheet.

[0275] As a porous sheet composed of fibrous materials, a porous sheet composed of the following fibrous materials or a mixture of these fibrous materials can be used, wherein the above-mentioned fibrous materials are composed of polyesters such as polyethylene terephthalate, polyolefins such as polyethylene or polypropylene, aromatic polyamides or polyimides, polyether sulfones, polysulfones, polyether ketones, polyether imides and other heat-resistant polymers.

[0276] The porous substrate may be a composite porous substrate in which a functional layer is further laminated.

[0277] From the aspect that further functions can be added by the functional layer, the above-mentioned composite porous substrate is preferred. As the functional layer, for example, from the aspect of imparting heat resistance, a porous layer composed of a heat-resistant resin or a porous layer composed of a heat-resistant resin and an inorganic filler can be used. As the heat-resistant resin, one or more heat-resistant polymers selected from aromatic polyamides, polyimides, polyether sulfones, polysulfones, polyether ketones and polyether imides can be cited. As inorganic fillers, metal oxides such as aluminum oxide or metal hydroxides such as magnesium hydroxide can be appropriately used. It should be noted that, as a composite method, a method of coating a functional layer on a porous sheet, a method of bonding with an adhesive, a method of performing thermal compression bonding, etc. can be cited.

[0278] As the porous substrate in the present disclosure, among the above, it is preferable that the porous substrate is composed of at least one resin selected from the group consisting of polyethylene, polypropylene, polyimide, polyamide, polyethylene terephthalate, polyester and polyacetal.

[0279] In the present disclosure, from the viewpoint of obtaining good mechanical properties and internal resistance, the film thickness of the porous substrate is preferably in the range of 5 μm to 50 μm.

[0280] The diaphragm disclosed in the present invention can be manufactured by laminating the composite porous membrane on the porous substrate. There is no particular limitation on the lamination method, and a known method can be used. Specifically, the following methods are preferred: a method in which the fluorinated polymer, inorganic particles and other components as necessary are dissolved or dispersed in a solvent or water, and the resulting solution or dispersion is roll-coated on a porous substrate; a method in which a porous substrate is immersed in the solution or dispersion; a method in which the solution or dispersion is applied to a porous substrate and further immersed in an appropriate coagulation liquid for production.

[0281] Alternatively, a film composed of the composite porous film may be prepared in advance, and the film may be laminated by laminating the film with a porous substrate, etc. As a method for preparing a film composed of the composite porous film, the following method may be exemplified: the fluorine-containing polymer, the inorganic particles, and other components as necessary are dissolved or dispersed in a solvent, the obtained solution or dispersion is cast on a film having a smooth surface such as a polyester film or an aluminum film, and then peeled off.

[0282] The solvent is preferably an amide solvent such as dimethylacetamide (DMAC); a ketone solvent such as acetone; a cyclic ether solvent such as tetrahydrofuran, etc. Alternatively, the fluorinated polymer and other components as required may be dispersed in water for use.

[0283] When the solution or dispersion containing the fluorinated polymer and the inorganic particles is aqueous, it may be prepared by mixing with a thickener (stabilizer) for adjusting the viscosity.

[0284] Examples of the thickener (stabilizer) include carboxyalkyl cellulose, alkyl cellulose, and hydroxyalkyl cellulose.

[0285] As a method for forming the composite porous membrane on the porous substrate, it is preferred to apply a slurry coating liquid containing the fluorinated polymer, the inorganic particles, water, etc. on the porous substrate by a known method and then dry the slurry coating liquid. The slurry coating liquid may contain the organic particles, thickener, etc.

[0286] The slurry coating liquid preferably contains 0.5 to 25 mass % of the fluorinated polymer, more preferably 1 mass % or more, and more preferably 20 mass % or less. The concentration of the fluorinated polymer can be adjusted by the mixing ratio of the fluorinated polymer, inorganic particles and water.

[0287] The slurry coating liquid preferably contains 1 to 60 mass % of the inorganic particles, more preferably 2 mass % or more, and more preferably 55 mass % or less. The concentration of the inorganic particles can be adjusted by the mixing ratio of the fluorinated polymer, the inorganic particles and water.

[0288] When the slurry coating liquid contains organic particles, it preferably contains 1 mass % to 60 mass %, more preferably 2 mass % or more, and more preferably 55 mass % or less. The concentration of the organic particles can be adjusted by the mixing ratio of the fluorinated polymer, the inorganic particles and water.

[0289] When the slurry coating liquid contains a thickener, it is preferable that the thickener is contained in an amount of 0.1% by mass to 20% by mass. The concentration of the thickener can be adjusted by the amount of the thickener added to the slurry coating liquid.

[0290] The present disclosure also relates to a secondary battery, characterized in that it comprises the above-mentioned secondary battery electrode and / or secondary battery separator. The secondary battery is preferably a lithium ion battery.

[0291] Among them, the secondary solid-state battery is a solid-state battery comprising a positive electrode, a negative electrode, and a solid electrolyte layer interposed between the positive electrode and the negative electrode, and the positive electrode and / or the negative electrode preferably contains the above-mentioned fluorine-containing polymer.

[0292] The positive electrode and negative electrode used in the secondary battery of the present disclosure are the same as the above-mentioned electrodes for the secondary battery. Hereinafter, the solid electrolyte layer, the separator and the battery case which are suitable for use in the secondary battery of the present disclosure will be described in detail.

[0293] The solid electrolyte layer used in the secondary battery of the present disclosure is not particularly limited, and preferably contains the above-mentioned solid electrolyte. The above-mentioned solid electrolyte layer of the present disclosure can also be used. The solid electrolyte layer used in the secondary battery of the present disclosure is preferably a layer composed of a sulfide-based solid electrolyte.

[0294] The secondary battery of the present disclosure may include a separator between the positive electrode and the negative electrode. Examples of the separator include the separator of the present disclosure, porous films such as polyethylene and polypropylene, and nonwoven fabrics such as nonwoven fabrics made of resins such as polypropylene and nonwoven fabrics made of glass fiber.

[0295] The secondary battery of the present disclosure may further include a battery case. The shape of the battery case used in the present disclosure is not particularly limited as long as it can accommodate the above-mentioned positive electrode, negative electrode, electrolyte layer, etc. Specifically, cylindrical, square, button-shaped, laminated, etc. can be cited. It should be noted that the shape and structure of the positive electrode, negative electrode, and separator can be changed according to the shape of each battery.

[0296] For example, a method for manufacturing a solid-state battery is a method for manufacturing a solid-state battery having a positive electrode, a negative electrode, and a solid electrolyte layer between the positive electrode and the negative electrode, and the method may include the following steps: a step of preparing the solid electrolyte layer; a step of preparing a slurry by mixing the positive or negative electrode active material, a solid electrolyte, a binder, and a solvent or a dispersion medium; and a step of manufacturing a solid-state battery by applying the slurry on one surface of the solid electrolyte layer to form a positive electrode and forming the negative electrode on the other surface of the solid electrolyte layer.

[0297] Example

[0298] The present disclosure will be specifically described below based on Examples. In the following Examples, "parts" and "%" mean "parts by mass" and "% by mass" respectively, unless otherwise specified.

[0299] (Method for producing fluorinated polymer)

[0300] (Monomer represented by general formula (10))

[0301] The 1,2-difluoroethylene E-form used in the following examples has a purity of 99.9% by mass or more. It should be noted that the purity is 99.9% by mass, as confirmed by GC / MS without the presence of impurity peaks. It should be noted that the monomer was prepared according to the example of Patent Document 1 and separated by preparative gas chromatography, thereby obtaining a high-purity monomer.

[0302] (Polymerization method)

[0303] The polymerization of the polymer was carried out by the polymerization method according to each of the following synthesis examples.

[0304] The obtained polymer was evaluated based on the following evaluation criteria.

[0305] (Dimethylacetamide (DMAC) solubility)

[0306] 0.9 g of DMAC was added to 0.1 g of the resin obtained in each synthesis example, and the mixture was stirred using a stirrer. If no residue was observed after 1 hour, the mixture was considered dissolved.

[0307] (Composition Analysis)

[0308] The copolymer composition is measured by a solution NMR method or a melt NMR method.

[0309] <Solution NMR method>

[0310] Measurement device: Varian VNMRS400

[0311] Resonance frequency: 376.04 (Sfrq)

[0312] Pulse width: 30°

[0313] <Melting NMR method>

[0314] Measurement device: AVANCE300 manufactured by Bruker Japan

[0315] Resonance frequency: 282.40[MHz]

[0316] Pulse width: 45°

[0317] (Molecular weight)

[0318] [Weight average molecular weight (Mw)]

[0319] The molecular weight was calculated based on the results of the GPC method using standard polystyrene as a reference. The measurement was performed by the following method depending on the type of polymer.

[0320] GPC equipment: TOSOH HLC-8020

[0321] Column: Shodex GPC806M 2, GPC801, 802 1 each

[0322] Developing solvent: tetrahydrofuran [THF]

[0323] Sample concentration: 0.1 mass%

[0324] Measuring temperature: 40℃

[0325] GPC equipment: TOSOH AS-8010, CO-8020 and SIMADZURID-10A

[0326] Column: GMHHR-H 3

[0327] Developing solvent: dimethylformamide [DMF]

[0328] Sample concentration: 0.05 mass%

[0329] Measuring temperature: 40℃

[0330] (Melting Point)

[0331] The measurement can be performed using a differential scanning calorimeter according to ASTM D 4591. Specifically, the copolymer is thermally measured using a differential scanning calorimeter RDC220 (manufactured by Seiko Instruments) at a heating rate of 10°C / min, and the maximum value in the obtained heat of fusion curve is defined as the melting point.

[0332] (Slurry stability test)

[0333] The slurry viscosity of the mixed solution immediately after preparation and the slurry viscosity 5 days after preparation were measured, and the stability of the slurry was evaluated based on the following calculation formula. The slurry viscosity was measured using a B-type viscometer (TV-10M, manufactured by Toki Sangyo Co., Ltd.) at 25°C, rotor No. M4, and a rotation speed of 6 rpm. The value after 10 minutes from the start of the measurement was used as the slurry viscosity of the mixed solution.

[0334] Stability of slurry (%) = viscosity of the mixed solution 3 days after preparation / viscosity of the mixed solution immediately after preparation × 100

[0335] In addition, in the examples and comparative examples, the following positive electrode active materials and conductive additives were used.

[0336] NMC622:LiNi 0.6 Mn 0.2 Co 0.2 O2

[0337] AB: Acetylene Black

[0338] Polymer Synthesis Example 1

[0339] After introducing 1,330 g of deionized water and 0.67 g of methylcellulose into an autoclave with an internal volume of 1.8 liters, the autoclave was fully purged with vacuum nitrogen. After that, the autoclave was vacuum degassed, and the temperature was raised to 45°C in 1.5 hours with 250 g of 1,2-difluoroethylene E-body, 1 ml of methanol and 2 g of di-n-propyl peroxydicarbonate in the vacuum autoclave. After maintaining at 45°C for 3 hours, 4 g of di-n-propyl peroxydicarbonate was further introduced. After that, 45°C was maintained for 4 hours. The maximum pressure reached during this period was 2.7 MPaG. After that, the pressure was released and returned to atmospheric pressure, and the reaction product was washed with water and dried to obtain 198 g of fluororesin powder.

[0340] The melting point is 198.3℃.

[0341] Polymer Synthesis Example 2

[0342] The stainless steel autoclave with an internal volume of 1.8L was fully replaced with vacuum nitrogen. After that, the autoclave was vacuum degassed, and 1000g of HFE-347pc-f, 197g of 1,2-difluoroethylene E-body, and 128g of vinylidene fluoride (VdF) were introduced into the vacuum autoclave, and then the autoclave was heated to 25°C. Next, 10.5g of 8% di(ω-hydro-dodecafluoroheptanoyl) peroxide (hereinafter referred to as "DHP") perfluorohexane solution was added into the autoclave to start polymerization. The pressure at the beginning was 1.04MPaG. In order to maintain the polymerization pressure, a mixed gas of 1,2-difluoroethylene / VdF=86.0 / 14.0 (mol%) was introduced, and the temperature in the autoclave was maintained at 25°C for 6.3 hours, and then the pressure was released and returned to atmospheric pressure. The reaction product was washed with water and dried to obtain 86g of fluororesin powder. The obtained resin contained vinylidene fluoride and VdF at a molar % ratio of 86.1 / 13.9.

[0343] The melting point is 197.9℃.

[0344] Polymer Synthesis Example 3

[0345] The stainless steel autoclave with an internal volume of 1.8L was fully replaced with vacuum nitrogen. After that, the autoclave was vacuum degassed, and 1000g of HFE-347pc-f, 70g of 1,2-difluoroethylene E body, and 250g of VdF were introduced into the autoclave in a vacuum state, and then the autoclave was heated to 25°C. Next, 7.0g of 8% DHP perfluorohexane solution was added into the autoclave to start polymerization. The pressure at the beginning was 1.40MPaG. In order to maintain the polymerization pressure, a mixed gas of 1,2-difluoroethylene / VdF=54.0 / 46.0 (mol%) was introduced, and the temperature in the autoclave was maintained at 25°C for 6.2 hours, and then the pressure was released and returned to atmospheric pressure. The reaction product was washed with water and dried to obtain 91g of fluororesin powder. The obtained resin contained 1,2-difluoroethylene and VdF in a molar ratio of 53.3 / 46.7.

[0346] The melting point is 180.0℃.

[0347] Polymer Synthesis Example 4

[0348] The interior of a glass-lined stainless steel autoclave with an internal volume of 4.1 L was fully replaced with vacuum nitrogen. After that, the autoclave was vacuum degassed, and after 2300 g of HFE-347pc-f, 41 g of 1,2-difluoroethylene E body, and 436 g of VdF were introduced into the vacuum autoclave, the autoclave was heated to 25°C. Next, 14.0 g of 8% DHP perfluorohexane solution was added into the autoclave to start polymerization. The pressure at the beginning was 1.11 MPaG. In order to maintain the polymerization pressure, a mixed gas of 1,2-difluoroethylene / VdF=25.0 / 75.0 (mol%) was introduced, and the temperature in the autoclave was maintained at 25°C for 3.3 hours, and then the pressure was released and returned to atmospheric pressure. The reaction product was washed with water and dried to obtain 104 g of fluororesin powder. The obtained resin contained vinylidene fluoride and VdF in a ratio of 24.2 / 75.8 in terms of mol %.

[0349] The melting point is 161.7℃.

[0350] Polymer Synthesis Example 5

[0351] The interior of a glass-lined stainless steel autoclave with an internal volume of 4.1 L was fully replaced with vacuum nitrogen. After that, the autoclave was vacuum degassed, and after 2300 g of HFE-347pc-f, 27 g of 1,2-difluoroethylene E body, and 423 g of VdF were introduced into the vacuum autoclave, the autoclave was heated to 25°C. Next, 14.0 g of 8% DHP perfluorohexane solution was added into the autoclave to start polymerization. The pressure at the beginning was 1.06 MPaG. In order to maintain the polymerization pressure, a mixed gas of 1,2-difluoroethylene / VdF=16.0 / 84.0 (mol%) was introduced, and the temperature in the autoclave was maintained at 25°C for 3.4 hours, and then the pressure was released and returned to atmospheric pressure. The reaction product was washed with water and dried to obtain 125 g of fluororesin powder. The obtained resin contained vinylidene fluoride and VdF in a molar % ratio of 16.5 / 83.5.

[0352] The melting point is 162.4℃.

[0353] Polymer Synthesis Example 6

[0354] The autoclave with an internal volume of 0.5 liters was fully purged with vacuum nitrogen. After that, the autoclave was degassed in vacuum, and 150 g of HFE-347pc-f, 23 g of 1,2-difluoroethylene E-body, and 4 g of tetrafluoroethylene were introduced into the autoclave in a vacuum state, and then the autoclave was heated to 28°C. Next, 2.0 g of 8% DHP perfluorohexane solution was added into the autoclave to start polymerization. The polymerization pressure at the beginning was 0.5 MPaG. In order to maintain the polymerization pressure, a mixed gas of 1,2-difluoroethylene E-body / tetrafluoroethylene = 85 / 15 (mol%) was introduced, and the temperature in the autoclave was maintained at 28°C for 5 hours and 15 minutes, and then the pressure was released and returned to atmospheric pressure. The reaction product was washed with water and dried to obtain 12.2 g of fluororesin powder. The obtained resin contains 1,2-difluoroethylene E-body and tetrafluoroethylene in a molar ratio of 85.5 / 14.5.

[0355] The melting point is 210.0℃.

[0356] Polymer Synthesis Example 7

[0357] The autoclave with an internal volume of 0.5 liters was fully purged with vacuum nitrogen. After that, the autoclave was vacuum degassed, and after 150 g of HFE-347pc-f, 6.8 g of 1,2-difluoroethylene E-form, and 20 g of tetrafluoroethylene were introduced into the autoclave in a vacuum state, the autoclave was heated to 28°C. Next, 1.5 g of 8% DHP perfluorohexane solution was added into the autoclave to start polymerization. The polymerization pressure at the beginning was 0.5 MPaG. In order to maintain the polymerization pressure, a mixed gas of 1,2-difluoroethylene E-form / tetrafluoroethylene = 42 / 58 (mol%) was introduced, and the temperature in the autoclave was maintained at 28°C for 1 hour and 50 minutes, and then the pressure was released and returned to atmospheric pressure. The reaction product was washed with water and dried to obtain 13.1 g of fluororesin powder. The obtained resin contained 1,2-difluoroethylene E-form and tetrafluoroethylene in a molar ratio of 42.4 / 57.6.

[0358] The melting point is 246.5℃.

[0359] Polymer Synthesis Example 8

[0360] 40 g of R-225 and 0.43 g of 8% DHP perfluorohexane solution were added to a 100 ml stainless steel (SUS) autoclave, cooled to dry ice temperature, purged with nitrogen, and then 3.0 g of hexafluoropropylene (HFP) and 5.2 g of 1,2-difluoroethylene E were added. The mixture was shaken at 25°C for 13.0 hours using an oscillator. The product was dried to obtain 2.41 g of a fluororesin. The obtained resin contained 1,2-difluoroethylene E and HFP in a molar ratio of 99.2 / 0.8.

[0361] The melting point is 188.5 degrees.

[0362] Polymer Synthesis Example 9

[0363] After introducing 600g of deionized water and 0.3g of methylcellulose into an autoclave with an internal volume of 1.8 liters, the autoclave was fully replaced with vacuum nitrogen. After that, the autoclave was vacuum degassed, and after introducing 150g of perfluorooctacyclobutane, 100g of HFP, and 64g of 1,2-difluoroethylene E body into the autoclave in a vacuum state, the autoclave was heated to 35°C. Next, 1.5g of di-n-propyl peroxycarbonate was added to the autoclave to start polymerization. The polymerization pressure at the beginning was 1.16MPaG. After maintaining the temperature in the autoclave at 35°C for 7 hours, the pressure was released and returned to atmospheric pressure, and the reaction product was washed with water and dried to obtain 17g of fluororesin powder. The obtained resin contains 1,2-difluoroethylene E body and HFP in a molar ratio of 94.9 / 5.1.

[0364] The melting point is 151.2 degrees.

[0365] Polymer Synthesis Example 10

[0366] 40 g of R-225 and 0.43 g of 8% DHP perfluorohexane solution were added to a 100 ml stainless steel (SUS) autoclave, cooled to dry ice temperature, and replaced with nitrogen. Then, 3.0 g of 2,3,3,3-tetrafluoropropylene (HFO-1234yf) and 9.1 g of 1,2-difluoroethylene E were added, and the mixture was shaken at 25°C for 11.8 hours using an oscillator. The product was dried to obtain 1.81 g of a fluororesin. The obtained resin contained 1,2-difluoroethylene E and HFO-1234yf in a molar ratio of 96.5 / 3.5.

[0367] The melting point is 205.9℃.

[0368] Polymer Synthesis Example 11

[0369] 40 g of R-225 and 0.43 g of 8% DHP perfluorohexane solution were added to a 100 ml stainless steel (SUS) autoclave, cooled to dry ice temperature, purged with nitrogen, and then 20.9 g of HFO-1234yf and 3.8 g of 1,2-difluoroethylene E were added, and shaken at 25°C for 13.2 hours using an oscillator. The product was dried to obtain 1.23 g of a fluororesin. The obtained resin contained 1,2-difluoroethylene E and HFO-1234yf in a molar ratio of 16.3 / 83.7.

[0370] No melting point.

[0371] Polymer Synthesis Example 12

[0372] 40 g of R-225 and 0.42 g of 8% DHP perfluorohexane solution were added to a 100 ml stainless steel (SUS) autoclave, cooled to dry ice temperature, purged with nitrogen, and then 6.0 g of perfluoromethyl vinyl ether (PMVE) and 10.2 g of 1,2-difluoroethylene E-form were added, and shaken at 25°C for 13.2 hours using an oscillator. The product was dried to obtain 3.0 g of a fluororesin. The obtained resin contained E-form and PMVE in a molar ratio of 95.3 / 4.5.

[0373] The melting point is 173.3 degrees.

[0374] (Preparation of composition for secondary battery)

[0375] The polymers of Synthesis Examples 1 to 12 were used as binders, NMC622 was used as a positive electrode active material, AB was used as a conductive aid, and DMAC was used as a solvent. The mixture was mixed using a stirrer in a mass ratio of active material / conductive aid / binder / solvent of 72.8 / 1.1 / 1.1 / 25 to obtain a mixed solution. The mixed solution was allowed to stand at room temperature to evaluate the slurry stability of the mixed solution.

[0376] The results are shown in Table 1.

[0377] (Electrode Preparation)

[0378] The obtained mixed solution was evenly coated on one side of a positive electrode collector (aluminum foil with a thickness of 20 μm), and after the DMAC was completely volatilized, a roller press was used to apply a pressure of 10 tons to press, thereby preparing a positive electrode having a positive electrode material layer and a positive electrode collector. The coating properties of the positive electrode material layer on the positive electrode collector are shown in Table 1.

[0379] Evaluation of coating properties was performed by visual inspection based on the following criteria.

[0380] 〇···Electrodes with smooth surfaces can be produced without any problems.

[0381] △···Can be used to make electrodes, but the surface is rough.

[0382] ×···The electrode was able to be produced, but part of it was cracked.

[0383]

[0384] Industrial Applicability

[0385] The secondary battery composition of the present disclosure can be suitably used for forming an electrode of a secondary battery, etc., taking advantage of the excellent solubility of the polymer having a structure derived from vinylidene fluoride in various organic solvents.

Claims

1. A composition for a secondary battery, comprising a fluorinated polymer and a solvent, wherein: The fluorine-containing polymer is a polymer containing a structural unit represented by the following general formula (1): [Chemistry 1] 2. The secondary battery composition according to claim 1, wherein The fluorine-containing polymer is a polymer further comprising a structural unit represented by the following general formula (2): [Chemistry 2] R1 is hydrogen, fluorine, a partially or fully fluorinated hydrocarbon group having 5 or less carbon atoms, or an OR5 group, and the R5 group is a partially or fully fluorinated hydrocarbon group having 5 or less carbon atoms; R2, R3, and R4 are each independently hydrogen or fluorine.

3. The secondary battery composition according to claim 2, wherein The structural unit represented by the general formula (2) is at least one structural unit selected from the group consisting of structural units represented by the following general formulae (3) to (8), [Chemistry 3] 4. The secondary battery composition according to any one of claims 1 to 3, wherein The weight average molecular weight of the fluorine-containing polymer is 50,000 to 5,000,000.

5. The secondary battery composition according to any one of claims 1 to 4, wherein The proportion of the structural unit represented by the general formula (1) in the fluorine-containing polymer is 0.1 mol % to 100 mol %.

6. The secondary battery composition according to any one of claims 1 to 5, wherein The solvent is at least one compound selected from the group consisting of ester compounds, ketone compounds, and amide compounds. 7 . The secondary battery composition according to claim 1 , which is for use in an electrode of a secondary battery. 8 . The secondary battery composition according to claim 1 , which is for a positive electrode of a secondary battery. 9 . The secondary battery composition according to claim 1 , which is for a separator of a secondary battery.

10. A method for forming a layer for a secondary battery, the method comprising the steps of applying a slurry to a substrate and heating and drying the slurry, wherein: The slurry contains the secondary battery composition according to any one of claims 1 to 9.

11. An electrode for a secondary battery, characterized in that: The invention has an active material layer containing a polymer and an active material, wherein the polymer contains a structural unit represented by the following general formula (1): [Chemistry 4] 12. A solid electrolyte layer for a secondary battery, comprising a polymer and a solid electrolyte, wherein the polymer comprises a structural unit represented by the following general formula (1): [Chemistry 5] 13. A secondary battery separator, comprising a polymer, wherein the polymer comprises a structural unit represented by the following general formula (1): [Chemistry 6] 14. A secondary battery, characterized in that: A secondary battery electrode according to claim 11 and / or a secondary battery separator according to claim 13 is provided.