Preparation method of fine-grain high-purity aluminum cast ingot
Through pickling, alkaline washing and water washing, and using ultrasonic treatment to adjust the ultrasonic power during the casting process, the problem of excessive grain size of high-purity aluminum ingots is solved, and grain refinement and ingot quality improvement are achieved , suitable for the production of high-purity aluminum sputtering targets.
Patent Information
- Application Number
- CN202410934625.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-01
AI Technical Summary
The existing high-purity aluminum ingots have large grain sizes, which are difficult to meet the purity and tissue performance requirements of the sputtering target.
After the aluminum raw materials are treated with pickling, alkaline washing and water washing, the ultrasonic power is adjusted during the casting process through ultrasonic treatment. The power in the early stage of solidification is higher than that in the later stage. Combined with specific casting and cooling conditions, the grain refinement of the aluminum ingot is achieved.
Effectively refine the grain size of aluminum ingots, improve its performance as a sputtering raw material, reduce the gas content in aluminum liquid, and improve the quality of the ingots.
Smart Images

Figure BDA0004940913390000121 
Figure BDA0004940913390000131
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of high-purity aluminum preparation, and in particular to a method for preparing a fine-grained high-purity aluminum ingot. Background Art
[0002] At present, due to its high electrical conductivity, aluminum is widely used in the field of sputtering targets. It is currently mainly used in the production process of semiconductor chips and TFT liquid crystal display devices through sputtering coating technology. High-purity aluminum sputtering targets and sputtering films have strict requirements in terms of target purity, organizational performance control, and overall quality consistency of target components. The performance of high-purity aluminum sputtering targets directly determines the quality level of metal films. The sputtering efficiency of the target depends on the grain size, and fine grains can effectively improve the sputtering efficiency of the target.
[0003] High-purity aluminum ingots are the basis for manufacturing targets with superior performance. With the improvement of the application performance of high-purity aluminum products and the gradual expansion of their application fields, higher requirements are placed on the quality of high-purity aluminum ingots. Not only must they meet the stringent requirements of downstream products for the purity of high-purity aluminum and impurity elements, but they must also place more stringent requirements on the grain size of high-purity aluminum ingots, that is, they hope that the grain size must be controlled small enough. The high-purity aluminum ingots produced by existing semi-continuous casting have a relatively coarse grain structure in the center of the cross section, which makes it difficult to meet the requirements for fine grains. Since the purity of the high-purity aluminum used in high-purity aluminum sputtering targets needs to meet 5N or above (99.999wt%), grain refinement cannot be achieved by adding grain refiners as in the conventional aluminum alloy production process.
[0004] For example, CN105598398A discloses a method for semi-continuous casting of high-purity aluminum ingots using a fine-grain crystallizer. The fine-grain crystallizer used includes a diverter cover, a main body, a water retaining ring and a lower cover plate. A concave annular groove, a primary cooling crystallization zone and an ingot discharge zone are arranged in the middle of the main body from top to bottom. The diverter cover is fixed to the upper end of the main body by bolts, the lower cover plate is fixed to the lower end of the main body by bolts, and the water retaining ring is clamped in the annular groove of the main body and the lower cover plate to assemble into a fine-grain crystallizer. The total axial height of the fine-grain crystallizer is effectively shortened, and the primary cooling crystallization zone and the ingot discharge zone in the main body form a secondary distribution mechanism, so that the entire aluminum ingot forms a negative temperature gradient region that promotes the production of equiaxed crystals, thereby realizing the equiaxed production of free grains. That is, by changing the structural design of the crystallizer, the melt flow mode can be changed and the growth of free grains inside the ingot can be promoted, the number of grain nucleation can be increased, and the microstructure refinement of the high-purity aluminum ingot can be achieved.
[0005] However, the high-purity aluminum products obtained in the prior art still have the defect of large grain size, which is not conducive to use as sputtering target raw materials. Summary of the invention
[0006] In view of the problems existing in the prior art, the purpose of the present invention is to provide a method for preparing fine-grained high-purity aluminum ingots to solve the problem that high-purity aluminum products still have the defect of large grain size, which is not conducive to use as sputtering target raw materials.
[0007] To achieve this object, the present invention adopts the following technical solutions:
[0008] The present invention provides a method for preparing a fine-grained high-purity aluminum ingot, the preparation method comprising:
[0009] The aluminum raw material is sequentially subjected to acid washing, alkali washing and water washing to obtain a treated aluminum material;
[0010] The processed aluminum material is sequentially melted, refined and cast to obtain a fine-grained high-purity aluminum ingot;
[0011] Wherein, the casting is assisted by ultrasonic treatment, and the ultrasonic power in the early stage of solidification is greater than the ultrasonic power in the late stage of solidification; the early stage of solidification is when the solidification height is ≤ 0.4 times the ingot length; the late stage of solidification is when the solidification height is greater than 0.4 times the ingot length.
[0012] The preparation method provided by the present invention realizes uniform grain refinement in the obtained aluminum ingot by adopting a specific ultrasonic treatment process in the casting stage, with the grain size being ≤5mm, thereby improving the performance of the ingot as a target sputtering raw material.
[0013] As a preferred technical solution of the present invention, the mass concentration of the acid solution used in the pickling is 5-15%.
[0014] Preferably, the acid solution used in the pickling comprises a nitric acid solution.
[0015] Preferably, the pickling time is 10-30 minutes.
[0016] Preferably, the pickling temperature is 20-30°C.
[0017] As a preferred technical solution of the present invention, the mass concentration of the alkali solution used in the alkali washing is 2-10%.
[0018] Preferably, the alkali solution used in the alkali washing includes potassium hydroxide solution and / or sodium hydroxide solution.
[0019] Preferably, the alkali washing time is 5-20 min.
[0020] Preferably, the temperature of the alkali washing is 20-30°C.
[0021] As a preferred technical solution of the present invention, the water washing time is 10-30 minutes.
[0022] Preferably, the water washing temperature is 20-30°C.
[0023] As a preferred technical solution of the present invention, the melting temperature is 740-800°C.
[0024] As a preferred technical solution of the present invention, the flow rate of argon gas in the refining is 3-6m 3 / h.
[0025] Preferably, the speed during refining is controlled at 400-500 r / min.
[0026] Preferably, the refining time is 1-2 hours.
[0027] As a preferred technical solution of the present invention, the ultrasonic power in the early stage of casting is 1.5-2kW.
[0028] Preferably, the ultrasonic power in the early stage of casting is 1-1.3 kW.
[0029] As a preferred technical solution of the present invention, the frequency of the ultrasound in the casting is 18-25kHz.
[0030] As a preferred technical solution of the present invention, the pouring temperature of the casting is 690-720°C.
[0031] Preferably, the flow rate of the cooling medium in the casting is 200-500 L / min.
[0032] Preferably, the temperature of the cooling medium during the casting is 10-30°C.
[0033] Preferably, the casting speed is 50-100 mm / min.
[0034] As a preferred technical solution of the present invention, the ultrasonic vibration transmission rod in the casting penetrates 150-300 mm below the liquid surface of the aluminum liquid.
[0035] Preferably, when the aluminum liquid level drops during the casting, the ultrasonic vibration transmission rod begins to gradually rise, and the lifting speed is 30-50 mm / min.
[0036] Compared with the prior art solutions, the present invention has the following beneficial effects:
[0037] (1) When the ultrasonic vibration system is working, a large number of cavitation bubbles can be formed. When the sound pressure exceeds a certain threshold, the cavitation bubbles will break, breaking up the crystal grains that have grown and making the grains refined.
[0038] (2) The ultrasonic vibration system can also reduce the gas content in the aluminum liquid, thereby improving the quality of the ingot.
[0039] (3) Use a special ceramic ultrasonic vibration rod (the commonly used vibration rod material is titanium alloy) to prevent contamination of high-purity aluminum liquid. DETAILED DESCRIPTION
[0040] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows:
[0041] This embodiment provides a method for preparing a fine-grained high-purity aluminum ingot, the preparation method comprising:
[0042] The aluminum raw material is sequentially subjected to acid washing, alkali washing and water washing to obtain a treated aluminum material;
[0043] The processed aluminum material is sequentially melted, refined and cast to obtain a fine-grained high-purity aluminum ingot;
[0044] Wherein, the casting is assisted by ultrasonic treatment, and the ultrasonic power in the early stage of solidification is greater than the ultrasonic power in the late stage of solidification; the early stage of solidification is when the solidification height is ≤ 0.4 times the ingot length; the late stage of solidification is when the solidification height is greater than 0.4 times the ingot length.
[0045] In the present invention, the aluminum raw material includes a high-purity aluminum raw material or an ultra-high-purity aluminum raw material, and a high-purity aluminum product or an ultra-high-purity aluminum product can be prepared accordingly.
[0046] In the present invention, the high purity refers to a purity of ≥99.99%.
[0047] In the present invention, the ultra-high purity refers to a purity of 99.9999% or more.
[0048] The mass concentration of the acid solution used in the pickling is 5-15%, for example, it can be 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14% or 15%, etc., but is not limited to the listed values, and other unlisted values within this range also meet the requirements.
[0049] Wherein, the acid solution used in the pickling includes nitric acid solution.
[0050] The pickling time is 10-30 min, for example, 10 min, 15 min, 20 min, 25 min or 30 min, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0051] The pickling temperature is 20-30°C, for example, 20°C, 22°C, 24°C, 26°C, 28°C or 30°C, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0052] Among them, the mass concentration of the alkali solution used in the alkali washing is 2-10%, for example, it can be 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%, etc., but is not limited to the listed values, and other unlisted values within this range also meet the requirements.
[0053] Wherein, the alkali solution used in the alkali washing includes potassium hydroxide solution and / or sodium hydroxide solution.
[0054] The alkali washing time is 5-20 min, for example, it can be 5 min, 6 min, 8 min, 10 min, 12 min, 14 min, 16 min, 18 min or 20 min, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0055] The alkali washing temperature is 20-30°C, for example, 20°C, 22°C, 24°C, 26°C, 28°C or 30°C, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0056] The water washing time is 10-30 min, for example, 10 min, 15 min, 20 min, 25 min or 30 min, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0057] The water washing temperature is 20-30°C, for example, 20°C, 22°C, 24°C, 26°C, 28°C or 30°C, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0058] Wherein, the melting temperature is 740-800°C, for example, it can be 740°C, 745°C, 750°C, 755°C, 760°C, 765°C, 770°C, 775°C, 780°C, 785°C, 790°C, 795°C or 800°C, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0059] The flow rate of argon gas in the refining process is 3-6m 3 / h, for example, 3m 3 / h、3.2m 3 / h、3.4m 3 / h、3.6m 3 / h、3.8m 3 / h、4m 3 / h、4.2m 3 / h、4.4m 3 / h、4.6m 3 / h、4.8m 3 / h、5m 3 / h、5.2m 3 / h、5.4m 3 / h、5.6m 3 / h、5.8m 3 / h or 6m 3 / h, etc., but not limited to the listed values, other values not listed within the range also meet the requirements.
[0060] The speed during refining is controlled to be 400-500 r / min, for example, 400 r / min, 410 r / min, 420 r / min, 430 r / min, 440 r / min, 450 r / min, 460 r / min, 470 r / min, 480 r / min, 490 r / min or 500 r / min, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0061] The refining time is 1-2h, for example, 1h, 1.1h, 1.2h, 1.3h, 1.4h, 1.5h, 1.6h, 1.7h, 1.8h, 1.9h or 2h, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0062] Among them, the ultrasonic power in the early stage of coagulation is 1.5-2kW, for example, it can be 1.5kW, 1.55kW, 1.6kW, 1.65kW, 1.7kW, 1.75kW, 1.8kW, 1.85kW, 1.9kW, 1.95kW or 2kW, but is not limited to the listed values, and other unlisted values within this range also meet the requirements.
[0063] Among them, the ultrasonic power in the late coagulation stage is 1-1.3kW, for example, it can be 1kW, 1.02kW, 1.04kW, 1.06kW, 1.08kW, 1.1kW, 1.12kW, 1.14kW, 1.16kW, 1.18kW, 1.2kW, 1.22kW, 1.24kW, 1.26kW, 1.28kW or 1.3kW, etc., but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0064] The frequency of the ultrasound in the casting is 18-25 kHz, for example, 18 kHz, 18.5 kHz, 19 kHz, 19.5 kHz, 20 kHz, 20.5 kHz, 21 kHz, 21.5 kHz, 22 kHz, 22.5 kHz, 23 kHz, 23.5 kHz, 24 kHz, 24.5 kHz or 25 kHz, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0065] The casting temperature is 690-720°C, for example, 690°C, 695°C, 700°C, 705°C, 710°C, 715°C or 720°C, etc., but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0066] Wherein, the flow rate of the cooling medium in the casting is 200-500L / min, for example, it can be 200L / min, 220L / min, 240L / min, 260L / min, 280L / min, 300L / min, 320L / min, 340L / min, 360L / min, 380L / min, 400L / min, 420L / min, 440L / min, 460L / min, 480L / min or 500L / min, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0067] Wherein, the temperature of the cooling medium in the casting is 10-30°C, for example, it can be 10°C, 12°C, 14°C, 16°C, 18°C, 20°C, 22°C, 24°C, 26°C, 28°C or 30°C, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0068] In the present invention, the cooling medium used in casting includes water, oil and other commonly used cooling media in the art to achieve cooling and solidification during the casting process.
[0069] Wherein, the casting speed is 50-100 mm / min, for example, it can be 50 mm / min, 55 mm / min, 60 mm / min, 65 mm / min, 70 mm / min, 75 mm / min, 80 mm / min, 85 mm / min, 90 mm / min, 95 mm / min or 100 mm / min, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0070] The ultrasonic vibration transmission rod in the casting is inserted 150-300 mm below the aluminum liquid surface, which can be, for example, but not limited to the listed values. Other values not listed within this range also meet the requirements.
[0071] Among them, when the aluminum liquid level drops during the casting, the ultrasonic vibration rod begins to gradually rise, and the lifting speed is 30-50mm / min, for example, it can be 30mm / min, 32mm / min, 34mm / min, 36mm / min, 38mm / min, 40mm / min, 42mm / min, 44mm / min, 46mm / min, 48mm / min or 50mm / min, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0072] In the present invention, gradually lifting the ultrasonic vibration transmission rod during casting as the casting proceeds means gradually moving the ultrasonic vibration transmission rod out of the aluminum liquid.
[0073] Further, in order to illustrate the grain refinement effect that can be achieved by the high-purity aluminum product obtained by the preparation method provided by the present invention, the following actual example is used for illustration, as follows:
[0074] Example 1
[0075] This embodiment provides a method for preparing a fine-grained high-purity aluminum ingot, the preparation method comprising:
[0076] The aluminum raw material (purity of 99.99%) is sequentially subjected to acid washing, alkali washing and water washing to obtain a treated aluminum material;
[0077] The processed aluminum material is melted, refined and cast in sequence to obtain fine-grained high-purity aluminum ingots (purity is 99.99%);
[0078] The mass concentration of the acid solution used in the pickling is 12%; the acid solution used in the pickling is a nitric acid solution; the pickling time is 20 minutes; the pickling temperature is 25°C;
[0079] The mass concentration of the alkali solution used in the alkali washing is 8%; the alkali solution used in the alkali washing is a sodium hydroxide solution; the alkali washing time is 15 minutes; the alkali washing temperature is 28°C;
[0080] The water washing time is 25 minutes; the water washing temperature is 28°C;
[0081] The melting temperature is 760°C;
[0082] The flow rate of argon gas in the refining is 4m 3 / h; the speed during refining is controlled to be 480r / min; the refining time is 1.5h;
[0083] The pouring temperature of the casting is 700°C; the flow rate of the cooling medium in the casting is 300L / min; the temperature of the cooling medium in the casting is 25°C; the casting speed is 70mm / min; the ultrasonic vibration rod in the casting penetrates 250mm below the aluminum liquid level; when the aluminum liquid level drops in the casting, the ultrasonic vibration rod begins to gradually rise, and the lifting speed is 40mm / min; the casting is assisted by ultrasonic treatment, and the ultrasonic power in the early stage of solidification is greater than the ultrasonic power in the late stage of solidification; the early stage of solidification is that the solidification height is ≤0.4 times the ingot length; the late stage of solidification is that the solidification height is greater than 0.4 times the ingot length; the ultrasonic power in the early stage of solidification is 1.8kW; the ultrasonic power in the late stage of solidification is 1.2kW; the frequency of ultrasound in the casting is 20kHz.
[0084] Example 2
[0085] This embodiment provides a method for preparing a fine-grained high-purity aluminum ingot, the preparation method comprising:
[0086] The aluminum raw material (purity of 99.99%) is sequentially subjected to acid washing, alkali washing and water washing to obtain a treated aluminum material;
[0087] The processed aluminum material is melted, refined and cast in sequence to obtain fine-grained high-purity aluminum ingots (purity is 99.99%);
[0088] The mass concentration of the acid solution used in the pickling is 8%; the acid solution used in the pickling is a nitric acid solution; the pickling time is 15 minutes; the pickling temperature is 22°C;
[0089] The mass concentration of the alkali solution used in the alkali washing is 5%; the alkali solution used in the alkali washing is potassium hydroxide solution; the alkali washing time is 10 minutes; the alkali washing temperature is 25°C;
[0090] The water washing time is 20 minutes; the water washing temperature is 25°C;
[0091] The melting temperature is 800°C;
[0092] The flow rate of argon gas in the refining is 5m 3 / h; the speed during refining is controlled to be 450r / min; the refining time is 1.4h;
[0093] The pouring temperature of the casting is 710°C; the flow rate of the cooling medium in the casting is 400L / min; the temperature of the cooling medium in the casting is 20°C; the casting speed is 80mm / min; the ultrasonic vibration rod in the casting penetrates 200mm below the aluminum liquid level; when the aluminum liquid level drops in the casting, the ultrasonic vibration rod begins to gradually rise, and the lifting speed is 45mm / min; the casting is assisted by ultrasonic treatment, and the ultrasonic power in the early stage of solidification is greater than the ultrasonic power in the late stage of solidification; the early stage of solidification is the solidification height ≤0.4 times the ingot length; the late stage of solidification is the solidification height >0.4 times the ingot length; the ultrasonic power in the early stage of solidification is 1.7kW; the ultrasonic power in the late stage of solidification is 1.2kW; the frequency of ultrasound in the casting is 22kHz.
[0094] Example 3
[0095] This embodiment provides a method for preparing a fine-grained high-purity aluminum ingot, the preparation method comprising:
[0096] The aluminum raw material (purity of 99.9999%) is sequentially subjected to acid washing, alkali washing and water washing to obtain a treated aluminum material;
[0097] The processed aluminum material is sequentially melted, refined and cast to obtain fine-grained ultra-high purity aluminum ingots (purity of 99.9999%);
[0098] The mass concentration of the acid solution used in the pickling is 5%; the acid solution used in the pickling is a nitric acid solution; the pickling time is 30 minutes; the pickling temperature is 20°C;
[0099] The mass concentration of the alkali solution used in the alkali washing is 2%; the alkali solution used in the alkali washing is a sodium hydroxide solution; the alkali washing time is 20 minutes; the alkali washing temperature is 30°C;
[0100] The water washing time is 10 minutes; the water washing temperature is 30°C;
[0101] The melting temperature is 800°C;
[0102] The flow rate of argon gas in the refining is 6m 3 / h; the speed during refining is controlled to be 400r / min; the refining time is 1h;
[0103] The pouring temperature of the casting is 720°C; the flow rate of the cooling medium in the casting is 500L / min; the temperature of the cooling medium in the casting is 10°C; the casting speed is 100mm / min; the ultrasonic vibration rod in the casting penetrates 150mm below the aluminum liquid level; when the aluminum liquid level drops in the casting, the ultrasonic vibration rod begins to gradually rise, and the lifting speed is 30mm / min; the casting is assisted by ultrasonic treatment, and the ultrasonic power in the early stage of solidification is greater than the ultrasonic power in the late stage of solidification; the early stage of solidification is the solidification height ≤0.4 times the ingot length; the late stage of solidification is the solidification height >0.4 times the ingot length; the ultrasonic power in the early stage of solidification is 2kW; the ultrasonic power in the late stage of solidification is 1.3kW; the frequency of ultrasound in the casting is 25kHz.
[0104] Example 4
[0105] This embodiment provides a method for preparing a fine-grained high-purity aluminum ingot, the preparation method comprising:
[0106] The aluminum raw material (purity of 99.9999%) is sequentially subjected to acid washing, alkali washing and water washing to obtain a treated aluminum material;
[0107] The processed aluminum material is sequentially melted, refined and cast to obtain fine-grained ultra-high purity aluminum ingots (purity of 99.9999%);
[0108] The mass concentration of the acid solution used in the pickling is 15%; the acid solution used in the pickling is a nitric acid solution; the pickling time is 10 minutes; the pickling temperature is 30°C;
[0109] The mass concentration of the alkali solution used in the alkali washing is 10%; the alkali solution used in the alkali washing is a potassium hydroxide solution and a sodium hydroxide solution with a mass ratio of 1:1; the alkali washing time is 5 minutes; the alkali washing temperature is 20°C;
[0110] The water washing time is 30 minutes; the water washing temperature is 20°C;
[0111] The melting temperature is 740°C;
[0112] The flow rate of argon gas in the refining is 3m 3 / h; the speed during refining is controlled to be 500r / min; the refining time is 2h;
[0113] The frequency of ultrasound in the casting is 18kHz; the pouring temperature of the casting is 690℃; the flow rate of the cooling medium in the casting is 200L / min; the temperature of the cooling medium in the casting is 30℃; the casting speed is 50mm / min; the ultrasonic vibration rod in the casting penetrates 300mm below the aluminum liquid level; when the aluminum liquid level drops in the casting, the ultrasonic vibration rod begins to gradually rise, and the lifting speed is 50mm / min; the casting is assisted by ultrasonic treatment, and the ultrasonic power in the early stage of solidification is greater than the ultrasonic power in the late stage of solidification; the early stage of solidification is the solidification height ≤0.4 times the ingot length; the late stage of solidification is the solidification height >0.4 times the ingot length; the ultrasonic power in the early stage of solidification is 1.5kW; the ultrasonic power in the late stage of solidification is 1kW; the frequency of ultrasound in the casting is 18kHz.
[0114] Comparative Example 1
[0115] The only difference from Example 1 is that no ultrasonic treatment is performed during casting.
[0116] Comparative Example 2
[0117] The only difference from Example 1 is that the ultrasonic power in the early stage of coagulation is less than the ultrasonic power in the late stage of coagulation, that is, the ultrasonic power in the early stage of coagulation is 1.2 kW; the ultrasonic power in the late stage of coagulation is 1.8 kW.
[0118] Comparative Example 3
[0119] The only difference from Example 1 is that the ultrasonic power during the coagulation process is fixed at 1.2 kW.
[0120] Comparative Example 4
[0121] The only difference from Example 1 is that the ultrasonic power during the coagulation process is fixed at 0.8 kW.
[0122] Comparative Example 5
[0123] The only difference from Example 1 is that the casting speed is 40 mm / min.
[0124] Comparative Example 6
[0125] The only difference from Example 1 is that the flow rate of the cooling medium in the casting is 150 L / min.
[0126] The grain size of the aluminum products obtained in the embodiment and the comparative example was tested in accordance with GB / T3246.2-2012. At the same time, an oxygen, nitrogen and hydrogen analyzer (LECO) was used to measure the H content in the aluminum products obtained in the embodiment and the comparative example. During casting, hydrogen will not have time to escape and form pore defects. These defects will be inherited from the ingot to the target material, which can easily cause abnormal discharge during the use of the target material.
[0127] Table 1
[0128]
[0129]
[0130] It can be seen from Table 1 in combination with Example 1 and Comparative Example 1 that when ultrasonic treatment is not applied, the ingot grain size is larger, and the H content of the early and late ingots is higher; when the ultrasonic vibration system is working, a large number of cavitation bubbles can be formed, and the cavitation bubbles will break under a sound pressure exceeding a certain threshold, breaking the crystal grains that have been crystallized and grown, so that the grains are refined. The ultrasonic vibration system can also reduce the gas content in the aluminum liquid, thereby improving the quality of the ingot. It can be found from Example 1 and Comparative Example 2 that after reducing the early ultrasonic power, the H content of the early ingot increases, but the grain size does not change much. This is because the water vapor in the flow channel refractory material at the beginning of casting is high, and the molten aluminum reacts with the water vapor to increase the hydrogen content, so the H content of the early ingot is greater than the H content in the later period. It can be found from Example 1 and Comparative Example 3 that when the early ultrasonic frequency is small, the H content is high; it can be found from Example 1 and Comparative Example 4 that when the ultrasonic frequency is less than 1kW, the grain refinement effect will deteriorate, and the H content is high.
[0131] It is stated that the present invention illustrates the detailed structural features of the present invention through the above embodiments, but the present invention is not limited to the above detailed structural features, that is, it does not mean that the present invention must rely on the above detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
[0132] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0133] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0134] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A method for preparing a fine-grained high-purity aluminum ingot, characterized in that: The preparation method comprises: The aluminum raw material is sequentially subjected to acid washing, alkali washing and water washing to obtain a treated aluminum material; The processed aluminum material is sequentially melted, refined and cast to obtain a fine-grained high-purity aluminum ingot; Wherein, the casting is assisted by ultrasonic treatment, and the ultrasonic power in the early stage of solidification is greater than the ultrasonic power in the late stage of solidification; the early stage of solidification is when the solidification height is ≤ 0.4 times the ingot length; the late stage of solidification is when the solidification height is greater than 0.4 times the ingot length.
2. The preparation method according to claim 1, characterized in that: The mass concentration of the acid solution used in the pickling is 5-15%; Preferably, the acid solution used in the pickling comprises a nitric acid solution; Preferably, the pickling time is 10-30min; Preferably, the pickling temperature is 20-30°C.
3. The preparation method according to claim 1 or 2, characterized in that: The mass concentration of the alkali solution used in the alkali washing is 2-10%; Preferably, the alkali solution used in the alkali washing includes potassium hydroxide solution and / or sodium hydroxide solution; Preferably, the alkali washing time is 5-20min; Preferably, the temperature of the alkali washing is 20-30°C.
4. The preparation method according to any one of claims 1 to 3, characterized in that: The washing time is 10-30min; Preferably, the water washing temperature is 20-30°C.
5. The preparation method according to any one of claims 1 to 4, characterized in that: The melting temperature is 740-800°C.
6. The preparation method according to any one of claims 1 to 5, characterized in that: The flow rate of argon gas in the refining is 3-6m 3 / h; Preferably, the speed during refining is controlled at 400-500r / min; Preferably, the refining time is 1-2 hours.
7. The preparation method according to any one of claims 1 to 6, characterized in that: The ultrasonic power in the early stage of coagulation is 1.5-2kW; Preferably, the ultrasonic power in the late coagulation stage is 1-1.3 kW.
8. The preparation method according to any one of claims 1 to 7, characterized in that: The frequency of ultrasound in the casting is 18-25 kHz.
9. The preparation method according to any one of claims 1 to 8, characterized in that: The casting temperature is 690-720°C; Preferably, the flow rate of the cooling medium in the casting is 200-500 L / min; Preferably, the temperature of the cooling medium in the casting is 10-30°C; Preferably, the casting speed is 50-100 mm / min.
10. The preparation method according to any one of claims 1 to 9, characterized in that: During the casting, the ultrasonic vibration transmission rod penetrates 150-300 mm below the aluminum liquid surface; Preferably, when the aluminum liquid level drops during the casting, the ultrasonic vibration transmission rod begins to gradually rise, and the lifting speed is 30-50 mm / min.
Citation Information
Cited By
Aluminum cast ingot and preparation method thereof
CN119870389A