Preparation method of color master batch as well as product and application of color master batch

By using specially made pore-size machine die heads and specific additives in the preparation process of masterbatch, the problem of insufficient dispersion of masterbatch in plastic is solved, efficient utilization of toner and product performance is achieved, and production costs and environment are reduced. Influence.

CN118876262AInactive Publication Date: 2024-11-01ZHONGSHAN ZENHE COLOR RESOURCES CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410927789.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing color masterbatch is insufficient in plastics, resulting in degradation of product performance, color deviation and waste of resources, and a large amount of dispersant is required to achieve uniform dispersion, which increases production costs and environmental burden.

Method used

Twin screw extrusion is performed by using a specially made pore-size machine die during the masterbing process, combining the use of specific additives and antioxidants, and pretreating the toner to improve its dispersion, forming small-sized particles or different The shape of color masterbatch increases the contact area with the plastic and shortens the melting time.

Benefits of technology

It improves the utilization rate and color effect of toner, reduces the use of color masterbatch, reduces energy consumption, and achieves uniform melting of color masterbatch and plastic, improving the quality and appearance of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004938741100000071
    Figure BDA0004938741100000071
  • Figure BDA0004938741100000081
    Figure BDA0004938741100000081
Patent Text Reader

Abstract

The invention relates to the technical field of rubber plastics, in particular to a preparation method of a color master batch as well as a product and application of the color master batch. The invention relates to a preparation method of a color master batch. The preparation method comprises the following steps: S01, preparing a machine die head into a machine die head with the aperture of 0.1-1.5 mm; s02, weighing the toner, the auxiliary agent and the carrier, and uniformly mixing the materials in a high-speed stirrer; transferring the mixed material into a double-screw extruder with a replaced die head, and carrying out grain pumping; the auxiliary agent comprises an antioxidant and a dispersing agent; the melt index of the carrier is not less than 3g / 10min.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of rubber and plastics, in particular to a preparation method of a masterbatch and its products and applications. Background Art

[0002] Masterbatches primarily consist of color powder, additives, and a carrier. They typically come in various shapes, including cylindrical, elliptical, spherical, and flake. Masterbatches typically contain a high concentration of color powder. To ensure optimal dispersion within plastics, masterbatch manufacturers employ various methods to improve dispersibility, such as adding dispersants and using high-flow resins as carriers. However, due to the high concentration of color powder in masterbatches, even with the addition of these additives, the quality of the masterbatch and plastic melt in the machine directly impacts product performance.

[0003] Masterbatch manufacturers generally achieve uniform dispersion of masterbatches in plastics. However, this is achieved by adding large amounts of dispersants, increasing the masterbatch's fluidity, and raising machine temperatures, without considering the masterbatch itself. These methods can lead to side effects such as the presence of precipitates, reduced product properties, and color variations. Uniform mixing of masterbatches and plastics requires a large contact surface, a temperature below the melting point of the plastic itself, and good fluidity. Only in this way can the masterbatch mix well with the plastic in a short period of time.

[0004] Furthermore, after fully mixing the masterbatch into the finished product, some of the color powder still agglomerates during the production process, preventing it from being fully effective and thus being "wasted." While theoretically only one part of masterbatch is needed to achieve the desired effect, in reality, 1.1 parts or more is required. This increases costs for manufacturers, but also reduces the amount of masterbatch used, which has a positive impact on environmental protection.

[0005] Therefore, the present invention provides a method for preparing a masterbatch that can improve the dispersibility of the masterbatch, thereby increasing the utilization rate of the toner. The same color effect can be achieved by adding a smaller amount of masterbatch. Furthermore, the method is simple and easy to implement. Summary of the Invention

[0006] In order to solve the above technical problems, the present invention provides a method for preparing a masterbatch, comprising the following steps:

[0007] S01: the die head is made into a die head with an aperture of 0.1-1.5 mm;

[0008] S02 Weigh the color powder, additives, and carrier, and mix them evenly with a high-speed mixer; transfer the mixed materials into a twin-screw extruder with a replaced die head to extract pellets;

[0009] The auxiliary agent comprises an antioxidant and a dispersant;

[0010] The melt index of the carrier is not less than 3g / 10min.

[0011] As an embodiment of the present invention, the dispersant is selected from one or more of liquid wax, PE wax, PP wax, synthetic wax, sodium stearate, zinc stearate, calcium stearate, EBS, epoxidized soybean oil, and soybean oil.

[0012] As an embodiment of the present invention, the toner is pre-treated before preparation, and the pre-treatment steps are:

[0013] S01: Dry the commercially available toner in a low-temperature drying oven, grind it, and pass it through a 600-mesh sieve;

[0014] S02: Mix the modifier and ether in a mass ratio of 3:1;

[0015] S03: uniformly mixing the toner prepared in step S01 and the mixture obtained in step S02 under stirring;

[0016] S04 is then stirred and constant temperature evaporated at 35°C to obtain the pre-treated toner.

[0017] As an embodiment of the present invention, the twin-screw extruder process is: 110℃, 125℃, 130℃, 140℃, 145℃, 145℃, 145℃, 145℃, 145℃; the head temperature is 145℃; the feeding screw speed is 350rpm, and the main screw speed is 600rpm.

[0018] As an embodiment of the present invention, the twin-screw extruder process is: 180℃, 190℃, 200℃, 200℃, 205℃, 205℃, 205℃, 205℃, 205℃; the head temperature is 205℃; the feeding screw speed is 190rpm, and the main screw speed is 380rpm.

[0019] As an embodiment of the present invention, the antioxidant comprises two antioxidants, and the melting points of the two antioxidants differ by more than 30°C.

[0020] As an embodiment of the present invention, the antioxidant comprises antioxidant 1010 and antioxidant 168, and the ratio of the antioxidant 1010 and antioxidant 168 is 1:(0.8-1.2).

[0021] As an embodiment of the present invention, the antioxidant comprises antioxidant 1010 and antioxidant 168, and the ratio of the antioxidant 1010 and antioxidant 168 is 1:1.

[0022] The second aspect of the present invention provides a masterbatch prepared by the above-mentioned preparation method.

[0023] As an embodiment of the present invention, the masterbatch is used to prepare rubber resin.

[0024] By adopting the above technical solution, the present invention has the following beneficial effects:

[0025] 1. By processing the die head of the screw extruder, making the die head with a certain aperture and increasing the number of holes, the masterbatch can be prepared into small-sized particles or different shapes; when added through the masterbatch machine, the masterbatch is mixed and melted with the plastic inside the barrel. Because the masterbatch is small in size, its contact area with the plastic is increased, which is conducive to the dispersion of the masterbatch in the plastic; at the same time, the masterbatch melting time can be shortened, the entire product cycle can be shortened, and energy consumption can be reduced.

[0026] 2. When making the masterbatch formula, select specific additives so that the masterbatch can melt better when mixed with the plastic and heated, which is conducive to the dispersion of the masterbatch.

[0027] 3. Selecting a specific material as the masterbatch carrier ensures minimal die pressure during processing, resulting in a masterbatch with a superior appearance and quality. Excessive die pressure can cause plastic backflow, increasing the likelihood of quality issues such as black specks. Only by implementing these steps simultaneously can we achieve a masterbatch with stable quality, beautiful appearance, and excellent performance. DETAILED DESCRIPTION

[0028] The technical solution of the present invention will be described clearly and completely below. Obviously, the embodiments described are only some embodiments of the present invention, not all embodiments. All other embodiments derived by persons of ordinary skill in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.

[0029] Example 1

[0030] The present invention provides a method for preparing a masterbatch, comprising the following steps:

[0031] S1 makes the die head of the 65 machine into a hole with a diameter of 0.8 mm and 50 holes;

[0032] S2 weighs 16 kg of rutile titanium dioxide, 9 kg of LLDPE 6201 (Mobil Exxon, melt index 60 g / 10 min, measured at 190°C / 2.16 kg), 0.2 kg of PP1302 wax (Clariant, dropping point 93°C), and 0.1 kg of antioxidant (antioxidant 1010 and 168 in a 1:1 mass ratio). Mix thoroughly in a high-speed blender. Transfer the blended material to a twin-screw extruder with a replaced die for pelletization. The twin-screw extruder's operating temperature is: 110°C, 125°C, 130°C, 140°C, 145°C, 145°C, 145°C, 145°C, 145°C, 145°C. The die temperature is 145°C. The feed screw speed is 350 rpm, and the main screw speed is 600 rpm. The strands were pelletized through a 3-meter water trough. The pelletizer speed was controlled to produce cylindrical masterbatch 1, approximately 0.8 mm x 1 mm. One kilogram of the prepared masterbatch was weighed and added to 50 kilograms of homopolymer PP using a masterbatch machine. The resulting product was then molded into a 1.5 mm thick product using an injection molding machine. This was labeled A1.

[0033] The rutile titanium dioxide is pre-treated before mixing in a high-speed mixer, and the steps are as follows:

[0034] S01: Dry the commercially available rutile titanium dioxide in a low-temperature drying oven at 30°C to constant weight, then grind and pulverize it through a 600-mesh sieve;

[0035] S02: Mix RBW102 wax and ether in a mass ratio of 1:3;

[0036] S03 uniformly mix the rutile titanium dioxide prepared in step S01 and the mixture obtained in step S02 under stirring;

[0037] S04 is then stirred and constant temperature evaporated at 35° C. to obtain a pre-treated toner. The mass ratio of the rutile titanium dioxide to the ether is 9:1.

[0038] Example 2

[0039] The present invention provides a method for preparing a masterbatch, comprising the following steps:

[0040] A 35-molding die was manufactured with 12 holes and a particle size of 0.5 mm. 12 kg of yellow powder, 13 kg of ABS material, 0.2 kg of antioxidant (antioxidant 1010 and 168 in a 1:1 mass ratio), and 0.2 kg of Licowax OP wax (Clariant, dropping point 96°C) were weighed and mixed in a high-speed blender. The mixed material was transferred to a twin-screw extruder with a new die to produce pellets. The extruder cycle was: 180°C, 190°C, 200°C, 200°C, 205°C, 205°C, 205°C, 205°C, 205°C, 205°C. The die temperature was 205°C. The feed screw speed was 190 rpm, and the main screw speed was 380 rpm. The pellets were hot-cut into 0.5 x 1 mm oval pellets and cooled to room temperature via a 5-meter-long air-cooling zone to produce the masterbatch. Weigh 1.5 kg of the prepared masterbatch and add it to 50 kg of ABS material using a masterbatch machine. Use an injection molding machine to form a 1.5 mm thick product. Mark it as A2.

[0041] The rutile titanium dioxide is pre-treated before mixing in a high-speed mixer, and the steps are as follows:

[0042] S01 Dry the commercially available yellow powder in a 30°C low-temperature drying oven to constant weight, then grind and pulverize it through a 600-mesh sieve;

[0043] S02: Mix RBW102 wax and ether in a mass ratio of 1:3;

[0044] S03: uniformly mixing the yellow powder prepared in step S01 and the mixture obtained in step S02 under stirring;

[0045] S04 is then stirred and constant temperature evaporated at 35°C to obtain the pre-treated toner, wherein the mass ratio of the yellow powder to ether is 9:1.

[0046] Example 3

[0047] The present invention provides a method for preparing a masterbatch, comprising the following steps:

[0048] S1 makes the die head of the 65 machine into a hole with a diameter of 0.8 mm and 50 holes;

[0049] S2 weighs 16 kg of rutile titanium dioxide, 9 kg of LLDPE 6201 (Mobil Exxon, melt index 60 g / 10 min, measured at 190°C / 2.16 kg), 0.2 kg of PP1302 wax (Clariant, dropping point 93°C), and 0.1 kg of antioxidant (antioxidant 1010 and 168 in a 1:1 mass ratio). Mix thoroughly in a high-speed blender. Transfer the blended material to a twin-screw extruder with a replaced die for pelletization. The twin-screw extruder's operating temperature is: 110°C, 125°C, 130°C, 140°C, 145°C, 145°C, 145°C, 145°C, 145°C, 145°C. The die temperature is 145°C. The feed screw speed is 350 rpm, and the main screw speed is 600 rpm. The strands are pelletized through a 3-meter water trough. The pelletizer speed is controlled to produce cylindrical masterbatches (approximately 0.8 mm x 1 mm). One kilogram of the prepared masterbatch is weighed and added to 50 kilograms of homopolymer PP using a masterbatch machine. The resulting product is then molded into a 1.5 mm thick product using an injection molding machine. Label it A3.

[0050] Example 4

[0051] The present invention provides a method for preparing a masterbatch, comprising the following steps:

[0052] S1 makes the die head of the 65 machine into a hole with a diameter of 0.8 mm and 50 holes;

[0053] S2 weighs 16 kg of rutile titanium dioxide, 9 kg of LLDPE 6201 (Mobil Exxon, melt index 60 g / 10 min, measured at 190°C / 2.16 kg), 0.2 kg of RBW102 wax, and 0.1 kg of antioxidant (antioxidant 1010 and 168 in a 1:1 mass ratio). Mix thoroughly in a high-speed blender. Transfer the blended material to a twin-screw extruder with a replaced die for pelletizing. The twin-screw extruder's operating temperature is: 110°C, 125°C, 130°C, 140°C, 145°C, 145°C, 145°C, 145°C, 145°C, 145°C. The die temperature is 145°C. The feed screw speed is 350 rpm, and the main screw speed is 600 rpm. The strands were pelletized through a 3-meter water trough. The pelletizer speed was controlled to produce cylindrical masterbatches approximately 0.8 mm x 1 mm in diameter. One kilogram of the prepared masterbatch was weighed and added to 50 kilograms of homopolymer PP using a masterbatch machine. The resulting product was then molded into a 1.5 mm thick product using an injection molding machine. Label it A4.

[0054] The rutile titanium dioxide is pre-treated before mixing in a high-speed mixer, and the steps are as follows:

[0055] S01: Dry the commercially available rutile titanium dioxide in a low-temperature drying oven at 30°C to constant weight, then grind and pulverize it through a 600-mesh sieve;

[0056] S02: Mix PP1302 wax and ether in a mass ratio of 1:3;

[0057] S03 uniformly mix the rutile titanium dioxide prepared in step S01 and the mixture obtained in step S02 under stirring;

[0058] S04 is then stirred and constant temperature evaporated at 35° C. to obtain a pre-treated toner. The mass ratio of the rutile titanium dioxide to the ether is 9:1.

[0059] Example 5

[0060] The same procedure as in Example 1 was used, except that the die head of the 65-molding machine was replaced with a standard die head with a 0.25 mm aperture and 16 holes. The resulting masterbatch had a standard color masterbatch size of 0.25 x 0.3 mm. 1.2 kg of the prepared masterbatch was weighed and added to 50 kg of homopolymer PP using a masterbatch machine. A 1.5 mm thick product was then produced using an injection molding machine. This was labeled A5.

[0061] Example 6

[0062] The present invention provides a method for preparing a masterbatch, comprising the following steps:

[0063] S1 makes the die head of the 65 machine into a hole with a diameter of 0.8 mm and 50 holes;

[0064] S2 weighs 16 kg of rutile titanium dioxide, 9 kg of ExxonMobil LLDPE LL6101RQ, 0.2 kg of PP1302 wax (Clariant, dropping point 93°C), and 0.1 kg of antioxidant (antioxidant 1010 and 168 in a 1:1 mass ratio). Mix thoroughly in a high-speed blender. The blended material is then transferred to a twin-screw extruder with a modified die to produce pellets. The extruder's operating temperature is 110°C, 125°C, 130°C, 140°C, 145°C, 145°C, 145°C, 145°C, 145°C, and 145°C. The die temperature is 145°C. The feed screw speed is 350 rpm, and the main screw speed is 600 rpm. The pelletizer is then passed through a 3-meter water trough and pelletized. The pelletizer speed is controlled to produce cylindrical masterbatch 1 approximately 0.8 mm x 1 mm. Weigh 1 kg of the prepared masterbatch and add it to 50 kg of homopolymer PP using a masterbatch machine. Use an injection molding machine to form a 1.5 mm thick product. Mark it as A6.

[0065] The rutile titanium dioxide is pre-treated before mixing in a high-speed mixer, and the steps are as follows:

[0066] S01: Dry the commercially available rutile titanium dioxide in a low-temperature drying oven at 30°C to constant weight, then grind and pulverize it through a 600-mesh sieve;

[0067] S02: Mix RBW102 wax and ether in a mass ratio of 1:3;

[0068] S03 uniformly mix the rutile titanium dioxide prepared in step S01 and the mixture obtained in step S02 under stirring;

[0069] S04 is then stirred and constant temperature evaporated at 35° C. to obtain a pre-treated toner. The mass ratio of the rutile titanium dioxide to the ether is 9:1.

[0070] Performance testing:

[0071] Test 1: Test the physical properties of the masterbatches of Examples 1 to 6, including: specific gravity (g / cm 3 ), melt flow rate (g / 10min), and residual value on ignition (%). Specific gravity was tested according to GB / T 1033; melt flow rate was tested according to GB / T 3682. Ten sets of data were tested for each formulation, and the average results were taken. The results are shown in Table 1.

[0072] Test 2: Test the color difference between A1 and A6 using a D65 illuminant and a 10° reflected light source. Ten sets of data were tested for each formulation, and the average results were taken. See Table 2 for the results.

[0073] Test 3: Comparison of physical properties of A1-A6. Ten sets of data were tested for each formulation, and the results were averaged. See Table 3 for the results.

[0074] Table 1 Test results of performance test 1

[0075] Example proportion Melt flow rate Residual value after combustion Example 1 1.203 132.4 64.1% Example 2 1.356 31.8 40.51% Example 3 1.211 117.8 64.05% Example 4 1.208 149.2 64.06% Example 5 1.205 133.1 64.09% Example 6 1.211 64.2 64.02%

[0076] Table 2 Test results of performance test 2

[0077] Example DL* Da* Db* Example 1 96.15 -0.63 1.29 Example 2 62.55 -0.22 58.08 Example 3 96.07 -0.64 1.24 Example 4 96.24 -0.62 1.26 Example 5 95.92 -0.62 1.32 Example 6 96.97 -0.59 1.27

[0078] Table 3 Test results of performance test 3

[0079]

[0080]

[0081] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the above embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a masterbatch, It is characterized in that Here are the steps: S01: the die head is made into a die head with an aperture of 0.1-1.5 mm; S02 weighs the color powder, additives and carrier, and mixes them evenly with a high-speed mixer; transfers the mixed materials into a twin-screw extruder with a replaced die head to extract pellets; The auxiliary agent comprises an antioxidant and a dispersant; The melt index of the carrier is not less than 3 g / 10 min.

2. A method for preparing a masterbatch according to claim 1, It is characterized in that The dispersant is selected from one or more of liquid wax, PE wax, PP wax, synthetic wax, sodium stearate, zinc stearate, calcium stearate, EBS, epoxidized soybean oil, and soybean oil.

3. A method for preparing a masterbatch according to claim 1, It is characterized in that The toner is pre-treated before preparation, and the pre-treatment steps are: S01 Dry the commercially available toner in a low-temperature drying oven, grind it and pass it through a 600-mesh sieve; S02: Mix the modifier and ether in a mass ratio of 3:1; S03, mixing the toner prepared in step S01 and the mixture obtained in step S02 uniformly under stirring; S04 is then stirred at 35°C to evaporate the solvent at a constant temperature to obtain the pre-treated toner.

4. A method for preparing a masterbatch according to claim 1, It is characterized in that The twin-screw extruder process is: 110°C, 125°C, 130°C, 140°C, 145°C, 145°C, 145°C, 145°C, 145°C, 145°C; the head temperature is 145°C; the feed screw speed is 350rpm, and the main engine screw speed is 600rpm.

5. A method for preparing a masterbatch according to claim 1, It is characterized in that The twin-screw extruder process is: 180°C, 190°C, 200°C, 200°C, 205°C, 205°C, 205°C, 205°C, 205°C; the head temperature is 205°C; the feed screw speed is 190rpm, and the main engine screw speed is 380rpm.

6. A method for preparing a masterbatch according to claim 1, It is characterized in that The antioxidant comprises two antioxidants, and the melting points of the two antioxidants differ by more than 30°C.

7. A method for preparing a masterbatch according to claim 6, It is characterized in that The antioxidant comprises antioxidant 1010 and antioxidant 168, and the ratio of the antioxidant 1010 and antioxidant 168 is 1:(0.8-1.2).

8. A method for preparing a masterbatch according to claim 7, It is characterized in that The antioxidant comprises antioxidant 1010 and antioxidant 168, and the ratio of the antioxidant 1010 and antioxidant 168 is 1:

1.

9. A masterbatch, It is characterized in that The compound is prepared by the preparation method according to any one of claims 1 to 8.

10. A masterbatch according to claim 9, It is characterized in that Used in the preparation of rubber resin.

Citation Information

Patent Citations

  • Functional white masterbatch and preparation method thereof

    CN105542292A

  • Weather-resistant color master batch and preparation method thereof

    CN114249935A

  • Ultra-fine color master batch pre-dispersion for non-woven fabric and preparation method of ultra-fine color master batch pre-dispersion

    CN114634638A

  • High-concentration, precipitation-resistant and antistatic flame-retardant color master batch and preparation method thereof

    CN116376170A

  • A masterbatch homocline filtering mechanism for injection molding machine shower nozzle

    CN205929140U