BOPP (Biaxially-oriented Polypropylene) heat-sealing film with high hot-adhesive strength and preparation method thereof
By using multi-layer structure and water-absorbing materials in the BOPP heat sealing film, the problems of insufficient barrier performance and difficulty in humidity control in the prior art are solved, and higher barrier properties and humidity management are achieved, which extends the shelf life of the product and reduces the cost.
Patent Information
- Application Number
- CN202410908085.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The barrier performance of the existing BOPP heat seal film is limited, making it difficult to effectively control the internal humidity of the packaging, affecting its use and long-term protection.
A high thermal viscosity strength BOPP heat seal film consisting of a barrier layer, an outer surface layer, an intermediate layer and an inner surface layer is used. The barrier layer contains ethyl silicate, sodium methyl silicate and phenyl trichlorosilane, and the outer surface layer contains polypropylene resin and Ethylene-vinyl alcohol copolymer, the intermediate layer is a modified polypropylene film, the inner surface layer is a titanium oxygen modified polypropylene film, and water-absorbing silicone and water-absorbing indicator strips are added to the barrier layer to form the film through melt preparation and stretching process. structure.
It significantly improves the barrier properties and humidity control capabilities of the heat seal film, extends the shelf life of the products in the packaging, and the water absorption indicator bar can intuitively display humidity changes, ensure the quality and safety of the packaging contents, reduce costs and improve the durability of the film. and adjustability.
Smart Images

Figure CN118876541A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of packaging films, in particular to a BOPP heat-sealing film with high hot adhesive strength and a preparation method thereof. Background Art
[0002] BOPP is generally a multi-layer co-extruded film, which is made by co-extruding polypropylene particles into sheets and then stretching them in both the longitudinal and transverse directions. Due to the orientation of the stretched molecules, this film has good physical stability, mechanical strength, air tightness, high transparency and gloss, and is tough and wear-resistant. It is a widely used printing film and is currently widely used in packaging materials for food, medicine and other products.
[0003] For example, the invention patent with the Chinese patent announcement number CN116001397B announces a high heat-adhesive strength BOPP heat-sealing film and its preparation method, which consists of an outer layer, an intermediate layer and an inner layer, and the outer layer is 4-6μm thick, the intermediate layer is 10-15μm thick, and the inner layer is 2-3μm thick, and the components and preparation methods of each layer are provided. This invention solves the problem of low heat-sealing strength of existing BOPP heat-sealing films, and uses silicon-based materials to improve thermal stability, thereby improving the heat-sealing stability of the film and achieving an increase in heat-sealing strength.
[0004] The above solution solves the problem of low heat sealing strength of the existing BOPP heat sealing film and improves the barrier properties of the BOPP heat sealing film. However, the improvement in barrier performance is limited. The humidity changes in the BOPP heat sealing film itself and inside the package are difficult to observe and effectively control, which affects the use, maintenance and long-term protection of the BOPP heat sealing film. Summary of the invention
[0005] The embodiments of the present application provide a high thermal adhesion strength BOPP heat-sealing film and a preparation method thereof, thereby solving the problem of limited improvement in barrier properties of BOPP heat-sealing films in the prior art and further improving the barrier properties of the heat-sealing film.
[0006] The embodiment of the present application provides a high hot adhesive strength BOPP heat-sealing film, which consists of a barrier layer, an outer layer, an intermediate layer and an inner layer, wherein the thickness of the barrier layer is 1-3 μm, the thickness of the outer layer is 2-6 μm, the thickness of the intermediate layer is 10-15 μm, and the thickness of the inner layer is 2-3 μm;
[0007] The barrier layer comprises, by weight, 5-10 parts of ethyl silicate, 3-6 parts of sodium methyl silicate, and 3-6 parts of phenyltrichlorosilane; the outer layer comprises, by weight, 30-40 parts of polypropylene resin and 15-20 parts of ethylene-vinyl alcohol copolymer; the middle layer is a modified polypropylene film, and the proportions by weight are as follows: 40-50 parts of polypropylene resin, 1-3 parts of hydroxy silicone oil, 0.2-0.5 parts of POSS-octahydroxy, 13-20 parts of polyvinyl alcohol, and 3-5 parts of polypropylene grafted hydroxyethyl methacrylate; the inner surface layer adopts titanium oxide modified polypropylene film, and the proportions by weight include: 30-40 parts of polypropylene resin, 2-5 parts of n-butyl titanate, 1-3 parts of cork fiber, 13-15 parts of linear low-density polyethylene, 3-5 parts of xylan, and 1-3 parts of organically modified nano-montmorillonite.
[0008] Furthermore, the barrier layer is prepared from a barrier layer melt, and the preparation method of the barrier layer melt specifically includes:
[0009] S11. Add ether to distilled water and stir evenly at low temperature, let stand and settle to obtain a layered liquid, and then extract the ether layer to obtain aqueous ether; the volume ratio of ether to distilled water is 4-7:1, the low temperature stirring temperature is 2-5 ° C, the stirring speed is 300-600r / min, and the temperature of standing and settling is 8-15 ° C;
[0010] S12. Ethyl silicate and phenyltrichlorosilane are mixed uniformly, and transferred into an aqueous ether solution for low-temperature ultrasonic dispersion for 15-25 min, and the ether is removed by decompression desolventizing to obtain a hydrolyzate; the stirring speed of the uniform mixing is 500-600 r / min, and the temperature is 5-10° C.; the temperature of the low-temperature ultrasonic dispersion is 5-10° C.; the ultrasonic frequency is 40-60 kHz;
[0011] S13. Adding sodium methyl silicate to the hydrolyzate, stirring and mixing at a temperature of melt plasticization to obtain a barrier layer melt;
[0012] The temperature of the melt-plasticization is 230-250° C., and the stirring time of the melt-plasticization is 10-30 min.
[0013] Furthermore, the outer surface layer is prepared from an outer surface layer melt, and the preparation method of the outer surface layer melt specifically includes:
[0014] S21. The polypropylene resin and ethylene-vinyl alcohol copolymer are cryogenically ground to form a powder, and stirred to obtain an outer layer mixture; the cryogenic grinding temperature is 5-10 ° C, the grinding pressure is 0.4-0.6MPa, and the stirring speed is 300-500r / min;
[0015] S22. Add the outer layer mixture into the extruder for melting and plasticization to obtain an outer layer melt.
[0016] Furthermore, the intermediate layer is prepared from an intermediate layer melt, and the preparation method of the intermediate layer melt specifically includes:
[0017] S31. The polypropylene resin and polyvinyl alcohol are ground and crushed to obtain a premixed powder, and the grinding is carried out under a nitrogen atmosphere, the grinding pressure is 0.4-0.8MPa, and the temperature is 15-25°C;
[0018] S32. The polypropylene grafted hydroxyethyl methacrylate, hydroxy silicone oil was added and stirred, and then POSS-octahydroxy was added and dispersed evenly to obtain an intermediate layer mixture;
[0019] S33. Put the intermediate layer mixture into an extruder for melting and plasticization to obtain an intermediate layer melt.
[0020] Furthermore, the inner surface layer is prepared from an inner surface layer melt, and the preparation method of the inner surface layer melt specifically includes:
[0021] S41. The n-butyl titanate and the cork fiber are stirred evenly and allowed to stand for 30-40 minutes to obtain a slurry;
[0022] S42. Adding organic modified nano-montmorillonite and stirring at a constant temperature to form a mixed filler;
[0023] S43. The polypropylene resin, linear low-density polyethylene and xylan were ground and stirred to obtain a mixed powder, and then the mixed filler was added and stirred to form an inner surface mixture;
[0024] S44, adding the inner surface layer mixture into an extruder for melting and plasticization to obtain an inner surface layer melt.
[0025] The method for preparing the above-mentioned high hot adhesive strength BOPP heat-sealing film specifically comprises the following steps:
[0026] S51. The inner surface layer melt, the middle layer melt, the outer surface layer melt and the barrier layer melt are successively placed into the same hanger-shaped die head, and the melt passes through the internal melt flow channel to form a four-layer structure in which the barrier layer covers the outer surface layer, and the melt temperature is 250-260°C;
[0027] S52. The melt of the four-layer structure coming out of the die is cooled by a chilled roller and a water tank to form a four-layer sheet, which is a tape-cast sheet; the sheet from the tape-cast sheet is reheated in a longitudinal stretching device, the preheating temperature is 140 ° C, and then stretched at 130 ° C, the stretching ratio is 4.5-5.0 times; the longitudinally stretched film enters the transverse stretching device, after preheating, stretching, buffering, shaping and cooling, the preheating temperature is 175 ° C, the stretching temperature is 160 ° C, the shaping temperature is 165 ° C, the cooling temperature is 60 ° C, and the transverse stretch ratio is 8-10 times;
[0028] S53. After transverse stretching, the film enters the traction and winding device, and is wound after cooling, edge trimming, thickness measurement and corona treatment to obtain a BOPP film.
[0029] Furthermore, the BOPP heat-sealing film also includes a water-absorbing material; the water-absorbing material replaces the barrier layer material in mass, and the water-absorbing material is 2-4 parts by weight; the water-absorbing material includes water-absorbing silica gel, and the water-absorbing material is pre-heated before being added to make it in a molten state.
[0030] Furthermore, in step S5, a blow molding method is also used to prepare a BOPP heat-sealing film; specifically, the inner surface layer melt, the middle layer melt, the outer surface layer melt, and the barrier layer melt are successively placed into the same hanger-shaped die head to form a four-layer structure; the four-layer structure is placed in a preheated blow molding mold for blow molding; the obtained film is cooled, pulled, and rolled to obtain the BOPP heat-sealing film.
[0031] Furthermore, a water absorption indicator strip is provided on the outer surface of the barrier layer; the water absorption indicator strip comprises a water absorption material;
[0032] The specific preparation process of the water absorption indicator strip is as follows: a pipe for introducing molten water absorption material is set during the blow molding process, and the pipe mouth is attached to the outside of the blown film. When the film is blown, the water absorption material is attached to the outside of the film to obtain a film with a water absorption indicator strip. There is at least one pipe, which is attached to the outside of the film in sequence.
[0033] Furthermore, a water-absorbing layer is provided between the outer layer and the barrier layer; the water-absorbing layer comprises a water-absorbing material.
[0034] One or more technical solutions provided in the embodiments of the present application have at least the following technical effects or advantages:
[0035] First, by separating the barrier layer from the outer layer, the outer layer melt removes the internal inorganic three-dimensional structure, and the inorganic three-dimensional structure is covered on the outer layer of the outer layer as a barrier layer. The barrier layer has hydrophobic barrier properties, which can prevent the penetration of external moisture and liquids and protect the internal materials from moisture. The outer layer maintains barrier properties to oxygen and has certain hydrophilicity and hygroscopicity, which can prevent product oxidation, absorb moisture or steam generated inside, and adjust the humidity inside the package, so that the product in the package is in a relatively stable humidity environment, thereby extending the shelf life of the product in the package. It is suitable for products that need both moisture-proof and oxidation-proof or need long-term storage or transportation.
[0036] Secondly, the absorbent silica gel has water-absorbing properties, which can make the barrier layer have the functions of water absorption and water isolation. While blocking external moisture, it can absorb a small amount of moisture generated in the humid environment inside the film to maintain the stability of the internal environment of the package; the absorbent silica gel changes color after absorbing water, which can intuitively indicate humidity changes. The humidity status of the BOPP heat-sealing film itself can be judged by the color change of the absorbent silica gel, so that timely measures can be taken to make adjustments to ensure the quality and safety of the packaging contents; the absorbent silica gel can be reused after dehydration, which reduces costs. The dehydration method is simple, and the water absorption capacity of the silica gel can be restored by heating treatment, thereby extending the service life of the BOPP heat-sealing film.
[0037] Thirdly, the water-absorbing material added in strip form forms a water-absorbing indicator strip on the surface of the membrane. When it absorbs water and changes color, it can very intuitively show the change in humidity. The color change of the water-absorbing indicator strip can be more concentrated and obvious, which is convenient for rapid detection and taking measures.
[0038] Fourthly, adding a water-absorbing layer between the barrier layer and the outer layer can prevent part of the water-absorbing indicator strip from extending through the barrier layer to the outer layer, causing external moisture to penetrate into the film through the extended water-absorbing indicator strip; the existence of the water-absorbing layer can absorb the penetrated moisture, thereby preventing the moisture from further penetrating into the film, thereby improving the waterproof performance of the film; the water-absorbing layer can absorb the penetrated moisture, and the water absorption capacity of the water-absorbing layer enhances the barrier performance of the entire film. Even if there are some tiny holes or defects in the barrier layer, the water-absorbing layer can quickly absorb the penetrated moisture, thereby ensuring that the inside of the film is not affected by moisture and maintaining the overall barrier effect of the film. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 This is a schematic diagram of the preparation process of the water absorption indicator strip according to the third embodiment of the present invention;
[0040] Figure 2 This is a schematic diagram of a BOPP heat-sealing film water absorption indicator strip according to Embodiment 3 of the present invention;
[0041] Figure 3 Schematic cross-sectional view of each layer of the BOPP heat-sealing film according to the third embodiment of the present invention;
[0042] Figure 4 Schematic cross-sectional view of each layer of the BOPP heat-sealing film according to the fourth embodiment of the present invention. DETAILED DESCRIPTION
[0043] To facilitate the understanding of the present invention, the present application will be described more comprehensively below with reference to the relevant drawings; the drawings show preferred embodiments of the present invention, but the present invention can be implemented in many different forms and is not limited to the embodiments described herein; on the contrary, the purpose of providing these embodiments is to enable a more thorough and comprehensive understanding of the disclosed content of the present invention.
[0044] It should be noted that the terms “vertical”, “horizontal”, “up”, “down”, “left”, “right” and similar expressions used in this document are only for illustrative purposes and do not represent the only implementation method.
[0045] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which the present invention belongs; the terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention; the term "and / or" used herein includes any and all combinations of one or more related listed items.
[0046] Embodiment 1: The present application discloses a high hot adhesive strength BOPP heat-sealing film, specifically, composed of a barrier layer, an outer surface layer, an intermediate layer and an inner surface layer, wherein the thickness of the barrier layer is 1-3 μm, the thickness of the outer surface layer is 2-6 μm, the thickness of the intermediate layer is 10-15 μm, and the thickness of the inner surface layer is 2-3 μm;
[0047] The barrier layer comprises, by weight, 5-10 parts of ethyl silicate, 3-6 parts of sodium methyl silicate, and 3-6 parts of phenyltrichlorosilane;
[0048] S1. The barrier layer is prepared from a barrier layer melt, and the preparation method of the barrier layer melt specifically includes:
[0049] S11. Add ether to distilled water and stir evenly at low temperature, let stand to settle to obtain a layered liquid, and then extract the ether layer to obtain aqueous ether;
[0050] The volume ratio of ether to distilled water is 4-7:1, the low temperature stirring temperature is 2-5°C, the stirring speed is 300-600r / min, and the temperature of static sedimentation is 8-15°C;
[0051] S12. The ethyl silicate and phenyltrichlorosilane were mixed evenly, and transferred into an aqueous ether solution for low temperature ultrasonic dispersion for 15-25 min, and the ether was removed by decompression desolventizing to obtain a hydrolyzate;
[0052] The stirring speed for uniform mixing is 500-600 r / min, and the temperature is 5-10°C; the temperature for low-temperature ultrasonic dispersion is 5-10°C; and the ultrasonic frequency is 40-60kHz;
[0053] S13. Adding sodium methyl silicate to the hydrolyzate, stirring and mixing at a temperature of melting and plasticization to form an inorganic three-dimensional structure to obtain a barrier layer melt;
[0054] The temperature of the melt-plasticization is 230-250°C, and the stirring time of the melt-plasticization is 10-30min;
[0055] The outer layer comprises, by weight, 30-40 parts of polypropylene resin and 15-20 parts of ethylene-vinyl alcohol copolymer;
[0056] S2. The outer layer is prepared from an outer layer melt, and the preparation method of the outer layer melt specifically includes:
[0057] S21. The polypropylene resin and ethylene - vinyl alcohol copolymer are cryogenically ground to form a powder, and stirred to obtain an outer layer mixture;
[0058] The temperature of the cryogenic grinding is 5-10°C, the grinding pressure is 0.4-0.6MPa, and the stirring speed is 300-500r / min;
[0059] S22. The outer layer mixture is added to the extruder and melted and plasticized to obtain an outer layer melt;
[0060] The temperature of the extruder is 230-240-250-240-240°C;
[0061] The middle layer is a modified polypropylene film, and the proportions by mass are as follows: 40-50 parts of polypropylene resin, 1-3 parts of hydroxy silicone oil, 0.2-0.5 parts of POSS-octahydroxy, 13-20 parts of polyvinyl alcohol, and 3-5 parts of polypropylene grafted hydroxyethyl methacrylate;
[0062] S3. The intermediate layer is prepared from an intermediate layer melt, and the preparation method of the intermediate layer melt specifically includes:
[0063] S31. The polypropylene resin and polyvinyl alcohol are ground and crushed to obtain a premixed powder, and the grinding is carried out under a nitrogen atmosphere, the grinding pressure is 0.4-0.8MPa, and the temperature is 15-25°C;
[0064] S32. The polypropylene grafted hydroxyethyl methacrylate, hydroxy silicone oil was added and stirred, and then POSS-octahydroxy was added and dispersed evenly to obtain an intermediate layer mixture;
[0065] The stirring speed is 500-800r / min;
[0066] S33. The intermediate layer mixture is placed in an extruder and melted and plasticized to obtain an intermediate layer melt;
[0067] The temperature of the extruder is 240°C-250°C-260°C-250°C-230°C;
[0068] The inner surface layer adopts titanium oxide modified polypropylene film, and the proportion by mass includes: 30-40 parts of polypropylene resin, 2-5 parts of n-butyl titanate, 1-3 parts of cork fiber, 13-15 parts of linear low-density polyethylene, 3-5 parts of xylan, and 1-3 parts of organic modified nano-montmorillonite;
[0069] S4. The inner surface layer is prepared from an inner surface layer melt, and the preparation method of the inner surface layer melt specifically includes:
[0070] S41. The n-butyl titanate and the cork fiber are stirred evenly and allowed to stand for 30-40 minutes to obtain a slurry;
[0071] The stirring speed for uniform stirring is 300-500r / min, the static atmosphere is an air atmosphere with a water vapor volume ratio of 5%, and the temperature is 40-50°C;
[0072] S42. Adding organic modified nano-montmorillonite and stirring at a constant temperature to form a mixed filler;
[0073] The temperature of the constant temperature stirring is 120-130°C;
[0074] S43. The polypropylene resin, linear low-density polyethylene and xylan were ground and stirred to obtain a mixed powder, and then the mixed filler was added and stirred to form an inner surface mixture;
[0075] The grinding temperature is 0.5-0.8MPa and the temperature is 5-10°C;
[0076] S44, adding the inner surface layer mixture into an extruder for melting and plasticization to obtain an inner surface layer melt;
[0077] The temperature of the extruder is 230°C-250°C-260°C-240°C-240°C;
[0078] S5. A method for preparing a BOPP heat-sealing film, comprising:
[0079] S51. The inner surface layer melt, the middle layer melt, the outer surface layer melt and the barrier layer melt are successively placed into the same hanger-shaped die head, and the melt passes through the internal melt flow channel to form a four-layer structure in which the barrier layer covers the outer surface layer, and the melt temperature is 250-260°C;
[0080] S52. The melt of the four-layer structure coming out of the die is cooled by a chilled roller and a water tank to form a four-layer sheet. The process is a tape cast sheet; the sheet from the tape cast sheet is reheated in a longitudinal stretching device, the preheating temperature is 140 ° C, and then stretched at 130 ° C, and the stretching ratio is 4.5-5.0 times; the longitudinally stretched film enters the transverse stretching device, after preheating, stretching, buffering, shaping and cooling, the preheating temperature is 175 ° C, the stretching temperature is 160 ° C, the shaping temperature is 165 ° C, the cooling temperature is 60 ° C, and the transverse stretch ratio is 8-10 times;
[0081] S53. After transverse stretching, the film enters the traction and winding device, and is wound after cooling, edge trimming, thickness measurement and corona treatment to obtain a BOPP film.
[0082] The technical solutions in the above embodiments of the present application have at least the following technical effects or advantages:
[0083] The barrier layer is formed by the hydrolysis products of ethyl silicate, sodium methyl silicate and phenyltrichlorosilane. The hydrolysis products of these silicon-based materials can form a large number of hydroxyl structures, which are cross-linked and shrunk during the melting process to form an inorganic three-dimensional structure network with strong barrier properties. When the inorganic three-dimensional structure is covered on the outer layer of the outer layer, it can form an independent, dense and uniform barrier layer, thereby directly blocking the penetration of oxygen and water vapor and improving the barrier capacity.
[0084] The barrier layer covering the outer layer can improve the surface smoothness and scratch resistance of the film. At the same time, it can provide structural support for the entire film. The barrier layer has high mechanical properties and strong stability. When covered on the outer layer, it can enhance the stability of the entire film structure, enhance the mechanical properties of the film, and improve the tensile strength, tear strength and wear resistance, thereby improving the overall durability of the film.
[0085] By separating the barrier layer from the outer layer, the outer layer melt removes the internal inorganic three-dimensional structure, and the inorganic three-dimensional structure is covered on the outer layer of the outer layer as a barrier layer. The barrier layer has hydrophobic barrier properties, which can prevent the penetration of external moisture and liquids and protect the internal materials from moisture. The outer layer maintains oxygen barrier properties and has certain hydrophilicity and hygroscopicity, which can prevent product oxidation, absorb moisture or steam generated inside, and adjust the humidity inside the package, so that the product in the package is in a relatively stable humidity environment, thereby extending the shelf life of the product in the package. It is suitable for products that need both moisture and oxidation protection or need long-term storage or transportation.
[0086] Silicon-based materials have high thermal stability. The barrier layer covering the outer layer can enhance the heat resistance of the film. During the heat sealing process, the outer barrier layer can enhance the stability of the film at high temperatures and maintain the integrity of the heat sealing area, thereby improving the heat sealing strength of the film.
[0087] The improved film structure has expanded the application scope of BOPP heat-sealing film and can meet the packaging needs of a variety of products. The adjustment of the film structure has increased the adaptability of BOPP heat-sealing film. By separating the barrier layer from the outer layer, the thickness and performance of each layer can be more accurately controlled, enhancing the adjustability and processing adaptability of the film structure and improving production flexibility.
[0088] Embodiment 2: Embodiment 1 above improves the barrier performance and thermal stability of the BOPP heat-sealing film by separating the barrier layer from the outer layer, and expands the application scope of the BOPP heat-sealing film. In order to improve the barrier performance of the barrier layer, further optimization is made on the basis of Embodiment 1.
[0089] The barrier layer also includes a water-absorbing material; the water-absorbing material replaces the barrier layer material by mass, and the water-absorbing material is 2-4 parts by weight; the water-absorbing material includes water-absorbing silica gel, and the water-absorbing material is preheated before being added to make it in a molten state;
[0090] Specifically, in step S13, sodium methyl silicate is added to the hydrolyzate, and water-absorbing silica gel is added at the same time, and the mixture is stirred and mixed evenly at a melting and plasticizing temperature to form a water-absorbing silica gel barrier layer melt;
[0091] The water-absorbing silica gel is preheated to 250-280°C before being added to make the water-absorbing silica gel in a molten state, the temperature of the melt-plasticization is 230-250°C, and the stirring time of the melt-plasticization is 10-30 minutes;
[0092] In step S51, the inner surface layer melt, the middle layer melt, the outer surface layer melt and the water-absorbing silicone barrier layer melt are successively placed into the same hanger-shaped die head, and the melt passes through the internal melt flow channel to form a four-layer structure in which the barrier layer covers the outer surface layer. The melt temperature is set to 250-260°C.
[0093] The technical solutions in the above embodiments of the present application have at least the following technical effects or advantages:
[0094] The addition of water-absorbing silica gel further enhances the barrier properties of the barrier layer. The silica gel material itself has elasticity and water resistance. When it is combined with the barrier layer, it can form a denser barrier network, thereby further enhancing the ability to prevent the penetration of substances such as oxygen and moisture.
[0095] Water-absorbing silica gel has water-absorbing properties, which can make the barrier layer have the functions of water absorption and water isolation. While blocking external moisture, it can absorb a small amount of moisture generated in the humid environment inside the film to maintain the stability of the internal environment of the package; the water-absorbing silica gel changes color after absorbing water, which can intuitively indicate humidity changes. The humidity status of the BOPP heat-sealing film itself can be judged by the color change of the water-absorbing silica gel, so that timely measures can be taken to make adjustments to ensure the quality and safety of the packaging contents; the water-absorbing silica gel can be reused after dehydration, which reduces costs. The dehydration method is simple, and the water absorption capacity of the silica gel can be restored by heating treatment, thereby extending the service life of the BOPP heat-sealing film;
[0096] The water-absorbing silica gel is tightly combined with the barrier layer in the molten state, which can enhance the sealing strength during the heat sealing process and improve the sealing and reliability of the heat sealing film. At the same time, the addition of water-absorbing silica gel can increase the flexibility of the BOPP heat sealing film, improve the crease resistance and tear resistance, make it easy to operate and adapt to products of different shapes during the packaging process, and increase the durability of the film.
[0097] The addition of water-absorbing silica gel enables BOPP heat-sealing film to be used in areas that require humidity control and moisture-proof protection, such as food, medicine, chemicals, and electronic products, expanding the scope of use of BOPP heat-sealing film.
[0098] Embodiment 3: Embodiment 2 above adds water-absorbing silica gel into the barrier layer, so that the barrier layer has both water-absorbing and water-isolating functions, thereby expanding the application scope of BOPP heat-sealing film. In order to improve the barrier performance of the barrier layer, further optimization is made on the basis of Embodiment 2.
[0099] Specifically, in step S13, sodium methyl silicate is added to the hydrolyzate, and the mixture is stirred and mixed evenly at a temperature of melting and plasticization to form a barrier layer;
[0100] The temperature of the melt-plasticization is 230-250°C, and the stirring time of the melt-plasticization is 10-30min;
[0101] like Figure 1-3 As shown, in step S5, a blow molding method is also used to prepare a BOPP heat-sealing film;
[0102] Specifically, the inner surface layer melt, the middle layer melt, the outer surface layer melt and the barrier layer melt are successively placed into the same hanger-shaped die head to form a four-layer structure; the four-layer structure is placed into a preheated blow molding mold for blow molding; the obtained film is cooled, pulled and rolled to obtain a BOPP heat-sealed film;
[0103] Wherein, a water absorption indicator strip is also provided on the outer surface of the barrier layer; the water absorption indicator strip comprises a water absorption material;
[0104] The specific preparation process of the water absorption indicator strip is as follows: a pipe for introducing molten water absorption material is set during the blow molding process, and the pipe mouth is attached to the outside of the blown film. When the film is blown, the water absorption material is attached to the outside of the film to obtain a film with a water absorption indicator strip. There is at least one pipe, which is attached to the outside of the film in sequence.
[0105] The technical solutions in the above embodiments of the present application have at least the following technical effects or advantages:
[0106] The water-absorbing material added in strip form forms a water-absorbing indicator strip on the surface of the film. When it absorbs water and changes color, it can very intuitively show the change in humidity. Compared with the case where the water-absorbing silica gel and the barrier layer are mixed in Example 2, the color change of the water-absorbing indicator strip can be more concentrated and obvious, which is convenient for rapid discovery and taking measures;
[0107] Since the water absorption indicator strips are attached to the outside of the film in strip form, these strip areas can form local barrier reinforcement areas. When the film is attacked by moisture or water, the water absorption indicator strips can quickly absorb and display, while providing a barrier effect in these areas;
[0108] Adding water-absorbing materials in strips can reduce the overall amount of silica gel used. The water absorption indicator strips are concentrated in specific strip areas instead of being dispersed throughout the barrier layer. This allows the film to have water absorption indicators and maintain barrier effects while reducing costs and improving production efficiency.
[0109] The existence of the water absorption indicator strip enables the film to be clearly and conveniently located at the problem area according to the discoloration degree and discoloration area of the water absorption indicator strip, so that the film can be partially replaced or processed, making the film easy to monitor and maintain;
[0110] By adjusting the position and number of water absorption indicator strips, it can flexibly adapt to different packaging needs and humidity environments. For example, the number of silica gel strips can be increased in areas where higher humidity is expected to meet different production needs, increasing the flexibility and adjustability of film production, thereby expanding the scope of use of the film;
[0111] By adding a moisture absorption indicator strip, BOPP heat sealing film can be applied to more moisture-sensitive product packaging, such as food, medicine, electronic products, etc., making the application of BOPP heat sealing film in the packaging industry more extensive and flexible.
[0112] Embodiment 4: Embodiment 3 above adds water-absorbing material in strip form to form water-absorbing indicator strips, making the film color more intuitive and rapid, while improving the adjustability of film production. In order to improve the barrier properties of the film, further optimization is made on the basis of Embodiment 3.
[0113] like Figure 4As shown, in step S5, the inner surface layer melt, the middle layer melt, the outer surface layer melt, the water absorbing layer melt, and the barrier layer melt are successively put into the same hanger-shaped die to form a five-layer structure;
[0114] Wherein, a water-absorbing layer is provided between the outer layer and the barrier layer; the water-absorbing layer comprises a water-absorbing material, and the water-absorbing material comprises water-absorbing silica gel.
[0115] The technical solutions in the above embodiments of the present application have at least the following technical effects or advantages:
[0116] The film is composed of an inner surface layer, an intermediate layer, an outer surface layer, a water-absorbing layer, a barrier layer, and water-absorbing indicator strips distributed on the barrier layer in sequence; the water-absorbing layer is added between the barrier layer and the outer surface layer to prevent part of the water-absorbing indicator strips from extending through the barrier layer to the outer surface layer, causing external moisture to penetrate into the film through the extended water-absorbing indicator strips; the existence of the water-absorbing layer can absorb the penetrated moisture, thereby preventing the moisture from further penetrating into the film, thereby improving the waterproof performance of the film;
[0117] The water-absorbing layer can absorb the penetrated water. The water-absorbing capacity of the water-absorbing layer enhances the barrier performance of the entire film. Even if there are some tiny holes or defects in the barrier layer, the water-absorbing layer can quickly absorb the penetrated water to ensure that the inside of the film is not affected by moisture and maintain the overall barrier effect of the film.
[0118] The water-absorbing layer and the water-absorbing indicator strip work together to form the effect of indicating moisture and double barrier. The water-absorbing indicator strip can absorb and indicate the presence of moisture. The water-absorbing layer, as an additional barrier, can absorb moisture that has penetrated the barrier layer and prevent it from further penetrating into the film, thereby keeping the film dry and further improving the barrier capacity and reliability of the film.
[0119] The water-absorbing layer is located between the barrier layer and the outer layer, forming an additional barrier. The silicone material itself has good elasticity and water resistance. The water-absorbing layer can further enhance the film's barrier ability to oxygen, moisture and other substances, and improve the protection effect on the packaging contents.
[0120] The water-absorbing layer not only enhances the barrier effect, but also gives the film the ability to absorb water. While blocking external moisture, it can absorb a small amount of moisture that may be generated inside the package, thereby maintaining the stability of the internal environment of the package, so that it can be applied to products that require humidity control.
[0121] The water-absorbing material is tightly combined with the barrier layer and the outer layer in the molten state. The water-absorbing layer can enhance the sealing strength during the heat-sealing process, thereby improving the sealing and reliability of the heat-sealing film. The presence of the water-absorbing layer can increase the flexibility and tear resistance of the heat-sealing area; the water-absorbing layer can increase the flexibility and crease resistance of the BOPP heat-sealing film, making it more durable during packaging, transportation and storage, and reducing damage caused by folding or bending.
[0122] The comparative example adopts the method of announcement number CN116001397B to prepare BOPP heat-sealing film;
[0123] The examples 1 to 4 and the comparative example were tested. The test temperature of water vapor transmission rate and oxygen transmission rate was 38°C and the relative humidity was 90%. The heat sealing temperature of the heat sealing strength test was 130°C and the heat sealing time was 3 seconds. The test results are shown in the following table:
[0124]
[0125] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A high hot adhesive strength BOPP heat-sealing film, characterized in that: It consists of a barrier layer, an outer layer, an intermediate layer and an inner layer, wherein the thickness of the barrier layer is 1-3 μm, the thickness of the outer layer is 2-6 μm, the thickness of the intermediate layer is 10-15 μm, and the thickness of the inner layer is 2-3 μm; The barrier layer comprises, by weight, 5-10 parts of ethyl silicate, 3-6 parts of sodium methyl silicate, and 3-6 parts of phenyltrichlorosilane; the outer layer comprises, by weight, 30-40 parts of polypropylene resin and 15-20 parts of ethylene-vinyl alcohol copolymer; the middle layer is a modified polypropylene film, and the proportions by weight are as follows: 40-50 parts of polypropylene resin, 1-3 parts of hydroxy silicone oil, 0.2-0.5 parts of POSS-octahydroxy, 13-20 parts of polyvinyl alcohol, and 3-5 parts of polypropylene grafted hydroxyethyl methacrylate; the inner surface layer adopts titanium oxide modified polypropylene film, and the proportions by weight include: 30-40 parts of polypropylene resin, 2-5 parts of n-butyl titanate, 1-3 parts of cork fiber, 13-15 parts of linear low-density polyethylene, 3-5 parts of xylan, and 1-3 parts of organically modified nano-montmorillonite.
2. A high hot adhesive strength BOPP heat-sealing film as claimed in claim 1, characterized in that: The barrier layer is prepared from a barrier layer melt, and the preparation method of the barrier layer melt specifically includes: S11. Add ether to distilled water and stir evenly at low temperature, let stand and settle to obtain a layered liquid, and then extract the ether layer to obtain aqueous ether; the volume ratio of ether to distilled water is 4-7:1, the low temperature stirring temperature is 2-5 ° C, the stirring speed is 300-600r / min, and the temperature of standing and settling is 8-15 ° C; S12. Ethyl silicate and phenyltrichlorosilane are mixed uniformly, and transferred into an aqueous ether solution for low-temperature ultrasonic dispersion for 15-25 min, and the ether is removed by decompression desolventizing to obtain a hydrolyzate; the stirring speed of the uniform mixing is 500-600 r / min, and the temperature is 5-10° C.; the temperature of the low-temperature ultrasonic dispersion is 5-10° C.; the ultrasonic frequency is 40-60 kHz; S13. Add sodium methyl silicate to the hydrolyzate, stir and mix evenly at a melting and plasticizing temperature to obtain a barrier layer melt; the melting and plasticizing temperature is 230-250° C., and the stirring time of the melting and plasticizing is 10-30 min.
3. A high hot adhesive strength BOPP heat-sealing film as claimed in claim 1, characterized in that: The outer surface layer is prepared from an outer surface layer melt, and the preparation method of the outer surface layer melt specifically includes: S21. The polypropylene resin and ethylene-vinyl alcohol copolymer are cryogenically ground to form a powder, and stirred to obtain an outer layer mixture; the cryogenic grinding temperature is 5-10 ° C, the grinding pressure is 0.4-0.6MPa, and the stirring speed is 300-500r / min; S22. Add the outer layer mixture into the extruder for melting and plasticization to obtain an outer layer melt.
4. A high hot adhesive strength BOPP heat-sealing film as claimed in claim 1, characterized in that: The intermediate layer is prepared from an intermediate layer melt, and the preparation method of the intermediate layer melt specifically includes: S31. The polypropylene resin and polyvinyl alcohol are ground and crushed to obtain a premixed powder, and the grinding is carried out under a nitrogen atmosphere, the grinding pressure is 0.4-0.8MPa, and the temperature is 15-25°C; S32. The polypropylene grafted hydroxyethyl methacrylate, hydroxy silicone oil was added and stirred, and then POSS-octahydroxy was added and dispersed evenly to obtain an intermediate layer mixture; S33. Put the intermediate layer mixture into an extruder for melting and plasticization to obtain an intermediate layer melt.
5. The high hot adhesive strength BOPP heat-sealing film according to claim 1, characterized in that: The inner surface layer is prepared from an inner surface layer melt, and the preparation method of the inner surface layer melt specifically includes: S41. The n-butyl titanate and the cork fiber are stirred evenly and allowed to stand for 30-40 minutes to obtain a slurry; S42. Adding organic modified nano-montmorillonite and stirring at a constant temperature to form a mixed filler; S43. The polypropylene resin, linear low-density polyethylene and xylan were ground and stirred to obtain a mixed powder, and then the mixed filler was added and stirred to form an inner surface mixture; S44, adding the inner surface layer mixture into an extruder for melting and plasticization to obtain an inner surface layer melt.
6. A method for preparing a high hot adhesive strength BOPP heat-sealing film according to any one of claims 1 to 5, characterized in that: The specific steps include: S51. The inner surface layer melt, the middle layer melt, the outer surface layer melt and the barrier layer melt are successively placed into the same hanger-shaped die head, and the melt passes through the internal melt flow channel to form a four-layer structure in which the barrier layer covers the outer surface layer, and the melt temperature is 250-260°C; S52. The melt of the four-layer structure coming out of the die is cooled by a chilled roller and a water tank to form a four-layer sheet, which is a tape-cast sheet; the sheet from the tape-cast sheet is reheated in a longitudinal stretching device, the preheating temperature is 140 ° C, and then stretched at 130 ° C, the stretching ratio is 4.5-5.0 times; the longitudinally stretched film enters the transverse stretching device, after preheating, stretching, buffering, shaping and cooling, the preheating temperature is 175 ° C, the stretching temperature is 160 ° C, the shaping temperature is 165 ° C, the cooling temperature is 60 ° C, and the transverse stretch ratio is 8-10 times; S53. After transverse stretching, the film enters the traction and winding device, and is wound after cooling, edge trimming, thickness measurement and corona treatment to obtain a BOPP film.
7. The method for preparing a BOPP heat-sealing film with high hot adhesive strength according to claim 6, characterized in that: The BOPP heat-sealing film also includes a water-absorbing material; the water-absorbing material replaces the barrier layer material in mass, and the water-absorbing material accounts for 2-4 parts by weight; the water-absorbing material includes water-absorbing silica gel, and the water-absorbing material is pre-heated before being added to make it in a molten state.
8. The method for preparing a BOPP heat-sealing film with high hot adhesive strength according to claim 7, characterized in that: In step S5, a blow molding method is also used to prepare a BOPP heat-sealing film; specifically, the inner surface layer melt, the middle layer melt, the outer surface layer melt, and the barrier layer melt are successively placed into the same hanger-shaped die head to form a four-layer structure; the four-layer structure is placed in a preheated blow molding mold for blow molding; the obtained film is cooled, pulled, and rolled to obtain the BOPP heat-sealing film.
9. The method for preparing a BOPP heat-sealing film with high hot adhesive strength according to claim 8, characterized in that: A water absorption indicator strip is also provided on the outer surface of the barrier layer; the water absorption indicator strip comprises a water absorption material; The specific preparation process of the water absorption indicator strip is as follows: a pipe for introducing molten water absorption material is set during the blow molding process, and the pipe mouth is attached to the outside of the blown film. When the film is blown, the water absorption material is attached to the outside of the film to obtain a film with a water absorption indicator strip. There is at least one pipe, which is attached to the outside of the film in sequence.
10. The method for preparing a BOPP heat-sealing film with high hot adhesive strength according to claim 9, characterized in that: A water absorbing layer is arranged between the outer layer and the barrier layer; the water absorbing layer comprises a water absorbing material.
Citation Information
Patent Citations
A high thermal tack strength BOPP heat-sealing film and its preparation method
CN116001397B
Microwave water-blocking and oxygen-blocking BOPP (Biaxially-oriented Polypropylene) film and preparation method thereof
CN115847978A
BOPP (Biaxially-oriented Polypropylene) heat-sealing film with high hot-adhesive strength and preparation method thereof