Selenium-induced defect copper-based sulfur / selenide material as well as preparation method and application thereof
Through the preparation of selenium-induced defective copper-based sulfur/selenide materials, Cu1.96S and CuSe heterojunctions improve the conductivity and cyclic performance of the negative electrode materials of sodium ion battery, and solve the problem of volume expansion and structural stability of the negative electrode materials of sodium ion battery materials. , achieving high energy density and high power density battery performance.
Patent Information
- Application Number
- CN202411364944.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-09-29
AI Technical Summary
The capacity of the negative electrode material of sodium ion batteries rapidly decays due to volume expansion and structural collapse during charging and discharging, and the charge transfer impedance is large, which limits its kinetic process. The existing copper-based chalcogen compounds are complex and costly.
Using selenium-induced defective copper-based sulfur/selenide materials, copper-rich vacancies were formed by co-precipitation of copper acetate and cysteine. Combined with pyrolytic selenization strategy, a high conductivity and Composite materials with electrochemical properties.
The stability of the material structure and high sodium storage capacity are achieved, the rate performance and cycle stability are improved, the first discharge specific capacity can reach 528.43mAh/g, and the 513.42mAh/g is still maintained after 1,000 cycles, which is suitable for high energy density and high Power density sodium ion battery applications.
Smart Images

Figure CN118877924A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sodium ion battery electrode materials, and in particular to a selenium-induced defect copper-based sulfur / selenide material and a preparation method and application thereof. Background Art
[0002] Sodium-ion batteries (SIBs) have the advantages of low cost, abundant sodium resources, stable low-temperature performance, and high safety. They have been studied as the best alternative to lithium-ion batteries. However, the large ionic radius of sodium ions makes them exhibit slow kinetics during charging and discharging, which limits their wide application. As an important component of the battery, the reasonable design of the structure and the improvement of the performance of the negative electrode material can significantly enhance the capacity, rate and cycle performance of sodium-ion batteries.
[0003] Copper-based chalcogenides based on conversion reactions can provide high sodium storage capacity through a multi-electron transfer mechanism, but the formation of Na2S and Na2Se during the charge and discharge process will inevitably lead to volume expansion and structural collapse of the negative electrode material, resulting in rapid capacity decay and shortened battery life. In addition, the inherent semiconductor properties of copper-based chalcogenides will cause large charge transfer impedance and slow ion transport kinetics. In order to solve the problems of volume expansion and low conductivity, reasonable structural design and fine regulation of component optimization are the key to overcoming volume expansion, improving material conductivity, and enhancing sodium storage performance. Structural engineering, vacancy engineering, and interface engineering are considered to be effective strategies to solve the above problems. Reasonable structural design, such as hierarchical structure, hollow structure, core-shell structure, etc., can effectively relieve the stress in the process of sodium embedding of materials, increase the specific surface area of materials, increase their contact area with electrolytes, provide more active sites, and shorten the ion diffusion distance; vacancy engineering, such as cation vacancies and anion vacancies, can regulate the electronic structure of the main material, enhance the conductivity of the material, improve the rate performance, and provide more active sites for sodium storage; interface engineering, such as heterojunction, can introduce new phases into a single phase and form heterojunctions, which can improve electronic conductivity, reduce the sodium ion diffusion energy barrier, and reduce polarization. At present, the copper-based sulfide or selenide negative electrode materials prepared by the above strategy are complex, the raw material cost is high, and they have certain toxicity. Therefore, it is of great significance to prepare copper-based negative electrode materials with high sodium storage activity through simple processes. Summary of the invention
[0004] In order to solve the above problems, the object of the present invention is to provide a selenium-induced defect copper-based sulfur / selenide material and its preparation method and application, the copper-based sulfur / selenide composite material contains copper-rich vacancies 1.96 S and CuSe active sites can improve the conductivity and electrochemical properties of the material.
[0005] In order to achieve the above object, the present invention discloses a method for preparing a selenium-induced defect copper-based sulfur / selenide material, comprising the following steps: (1) Dissolve copper acetate (Cu(CH3COO)2•H2O) in water to prepare solution A, dissolve cysteine in water, and after cysteine is completely dissolved, add NaOH solution to adjust the pH value of the cysteine solution to alkaline to obtain solution B, then add solution A to solution B, and stir the reaction in a constant temperature water bath. After the reaction is completed, centrifuge the obtained mixed solution, discard the upper layer of liquid, obtain the lower layer of precipitate, and wash the precipitate with water for multiple times by centrifugation, and then vacuum dry to obtain Cys-Cu precursor; (2) Place the Cys-Cu precursor in porcelain boat A and the selenium powder in porcelain boat B. Then place porcelain boat B in the upstream of a double-temperature zone tubular furnace and porcelain boat A in the downstream of the double-temperature zone tubular furnace. Heat the mixture to a certain temperature under an inert atmosphere and keep the temperature constant for a period of time. After the temperature is constant, cool the mixture naturally to room temperature to obtain a selenium-induced defective copper-based sulfur / selenide material.
[0006] Furthermore, in step (1), the molar concentration of copper acetate in solution A is 0.02-0.06 mol / L, and the molar concentration of cysteine in solution B is 0.01-0.02 mol / L; the speed of centrifugal separation is 5000-10000 rpm, and the time of each centrifugal separation is 3-8 minutes; and the drying temperature is 50-80°C.
[0007] Furthermore, in step (1), the water used is deionized water; the concentration of the NaOH solution is 1-4 mol / L, the volume of the added NaOH solution is 5-15 mL, the pH value of solution B is 8-12; the temperature of the constant temperature water bath is 20-40°C, and the stirring reaction time is 0.2-30 hours; Furthermore, in step (2), the mass ratio of the Cys-Cu precursor to the selenium powder is 1:1 to 1:6.
[0008] Furthermore, in step (2), the heating rate is 2-5°C / min, the temperature is raised to 300-600°C, the constant temperature time is 1-5 hours, and the inert atmosphere is N2 atmosphere.
[0009] The invention also discloses a selenium-induced defect copper-based sulfur / selenide material obtained according to the preparation method and application of the selenium-induced defect copper-based sulfur / selenide material as a negative electrode material for a sodium ion battery.
[0010] Furthermore, the selenium-induced defective copper-based sulfur / selenide material contains Cu 1.96 S and CuSe, and Cu 1.96 A homologous heterojunction is formed between S and CuSe.
[0011] The present invention uses copper acetate as a metal source and cysteine as an organic ligand to form a new metal organic framework compound through simple coprecipitation, and then uses the new metal organic framework compound as a precursor and combines it with a pyrolysis selenization strategy to prepare a copper-based sulfur / selenide composite material with abundant copper vacancies. The composite material can be used as a negative electrode material for sodium ion batteries. 1.96 S and Cu 1.96 Formation of S / CuSe heterojunction, vacancy-rich Cu 1.96 S has higher conductivity and high chemical activity, and the homologous heterojunction Cu 1.96 The built-in electric field constructed at the S / CuSe interface can improve the surface reaction kinetics of the electrode material, accelerate the electron transfer rate, and thus improve the sodium storage performance of the material.
[0012] Compared with the prior art, the present invention has the following beneficial effects: (1) The preparation method proposed in the present invention utilizes the advantages of the novel metal organic framework compound precursor and fully utilizes the advantages of the ligands in the precursor being rich in heteroatoms such as S / N. The target product is obtained by only two steps of precursor preparation and pyrolysis and selenization. The obtained material has a stable structure, high yield, strong repeatability and excellent performance, which provides an option for exploring large-scale synthesis of sodium ion battery negative electrode materials with high rate characteristics and long cycle life. (2) The present invention only utilizes the rapid chelation of metal ions and organic ligands, has low raw material cost and low toxicity, adopts a simple mild co-precipitation and vapor phase selenization method, has a short process flow, is simple and easy to implement, has low equipment requirements, and has a short production cycle, and has great application potential; (3) The selenium-induced defect copper-based sulfur / selenide composite material obtained by the preparation method of the present invention not only improves the conductivity of the material, accelerates the migration speed of sodium ions and shortens the electron diffusion distance, but also the formation of a heterogeneous structure creates more active sites for the adsorption of sodium ions, thereby effectively improving the sodium storage capacity and rate performance of the material; (4) When the selenium-induced defect copper-based sulfur / selenide composite material obtained by the preparation method of the present invention is used as a negative electrode material for a sodium ion battery, it is tested at a current density of 1A / g, and the initial discharge capacity can reach 528.43mAh / g. After 1000 cycles, the discharge capacity is still as high as 513.42mAh / g, showing excellent cycle performance; even after 1000 cycles at a current density of 5A / g, the discharge capacity can still be maintained at 207.7mAh / g; in the rate performance test at different current densities, the material still shows a good capacity retention rate. The above test results show that this selenium-induced defect copper-based sulfur / selenide composite material is not only endowed with high sodium storage performance, but also has excellent rate characteristics, and is a potential application material for high energy density and high power density sodium ion batteries; (5) The present invention combines rapid co-precipitation and pyrolysis selenization strategies to construct vacancy-rich copper-based sulfide and copper-based sulfide / selenide heterojunction composite materials with multiple active sites, which significantly improves the material structure and performance, and enhances the electrochemical properties of this type of negative electrode material, including material conductivity, structural stability, sodium storage capacity, cycle stability and rate performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 The SEM images of the Cys-Cu-30min precursor prepared in Example 1 and the Cys-Cu-24h precursor prepared in Example 2, wherein Figures (a), (b), and (c) are of the Cys-Cu-30min precursor, and Figures (d), (e), and (f) are of the Cys-Cu-24h precursor; Figure 2 The Cu prepared in Example 1 1.96 S / CuSe-30min composite material and Cu prepared in Example 2 1.96 SEM images of S / CuSe-24h composite materials, where (a), (b), and (c) are Cu 1.96 S / CuSe-30min, Figures (d), (e), and (f) are Cu 1.96 S / CuSe-24h; Figure 3 is a SEM image of the Cu2S-30min-thermal composite material prepared in Comparative Example 1; Figure 4 is the BET diagram of the Cys-Cu-30min precursor prepared in Example 1; Figure 5 1 is the XRD pattern of the Cys-Cu-30min precursor prepared in Example 1 and the Cys-Cu-24h precursor prepared in Example 2; Figure 6 The Cu prepared in Example 1 1.96S / CuSe-30min, Cu prepared in Example 2 1.96 XRD patterns of the Cu2S-30min-thermal composites prepared by S / CuSe-24h and Comparative Example 1; Figure 7 The Cu prepared in Example 1 1.96 S / CuSe-30min, Cu prepared in Example 2 1.96 EIS graphs of the sodium ion battery with S / CuSe-24h and Cu2S-30min-thermal composite materials prepared in Comparative Example 1 as negative electrodes before and after 5 cycles at a current density of 1A / g, where Figure (a) is before the cycle and Figure (b) is after 5 cycles; Figure 8 The Cu prepared in Example 1 1.96 S / CuSe-30min, Cu prepared in Example 2 1.96 Cyclic performance curves of sodium ion batteries with S / CuSe-24h, Cu2S-30min-hot prepared in Comparative Example 1, and Cu2S-24h-hot composite materials prepared in Comparative Example 2 as negative electrodes at a current density of 1A / g; Fig. 9 The Cu prepared in Example 1 1.96 Cyclic performance curve of sodium-ion battery with S / CuSe-30min material as negative electrode at current density of 5A / g; Fig.10 The Cu prepared in Example 1 1.96 S / CuSe-30min, Cu prepared in Example 2 1.96 Rate performance curves of sodium ion batteries with negative electrodes of S / CuSe-24h, Cu2S-30min-hot prepared in Comparative Example 1, and Cu2S-24h-hot composite materials prepared in Comparative Example 2, respectively; Fig.11 The Cu prepared in Example 1 1.96 Cycling performance curve of the full battery assembled with S / CuSe-30min anode and sodium nickel iron manganese oxide cathode at a current density of 0.5 A / g. DETAILED DESCRIPTION
[0014] In order to better understand the content of the present invention, the present invention will be further described below in conjunction with specific embodiments and drawings. The following embodiments are implemented based on the technology of the present invention, and detailed implementation methods and operating steps are given, but the protection scope of the present invention is not limited to the following embodiments.
[0015] Embodiment 1: (1) 1.44 g Cu(CH3COO)2•H2O was dissolved in 160 mL deionized water to prepare solution A; then 1.4544 g cysteine was added to 640 mL deionized water, and after it was completely dissolved, 10 mL of a pre-prepared NaOH solution with a concentration of 2 mol / L was added, and after mixing evenly, the pH of the solution was adjusted to 10.58 to obtain solution B, and then solution A was added to solution B, and the mixture was placed in a constant temperature water bath at 30°C and magnetically stirred for 30 minutes. After the reaction was completed, the obtained mixed solution was centrifuged at 8000 rpm for 5 minutes to separate the solid product from the solution, and the upper clear liquid was discarded to obtain the lower precipitate, and the precipitate was centrifuged and washed several times with deionized water, and then vacuum dried at 60°C for 12 hours to obtain Cys-Cu-30min precursor; (2) 100 mg of Cys-Cu-30min precursor was placed in porcelain boat A, and 500 mg of selenium powder was placed in porcelain boat B. Then, porcelain boat B was placed in the upstream of a double-temperature zone tubular furnace, and porcelain boat A was placed in the downstream of the double-temperature zone tubular furnace. The mixture was heated to 450 °C at a heating rate of 2 °C / min in a nitrogen atmosphere, and kept at a constant temperature for 3 hours. After the constant temperature was reached, the mixture was naturally cooled to room temperature to obtain a selenium-induced defective copper-based sulfur / selenide material, which was recorded as Cu 1.96 S / CuSe-30min.
[0016] Embodiment 2: (1) 1.44 g Cu(CH3COO)2•H2O was dissolved in 160 mL deionized water to prepare solution A, and then 1.4544 g cysteine was added to 640 mL deionized water. After it was completely dissolved, 10 mL of a pre-prepared NaOH solution with a concentration of 2 mol / L was added. After mixing evenly, the pH of the solution was adjusted to 10.58 to obtain solution B. Solution A was then added to solution B, and the mixture was placed in a constant temperature water bath at 30°C and magnetically stirred for 24 hours. After the reaction was completed, the obtained mixed solution was centrifuged at 8000 rpm for 5 minutes to separate the solid product from the solution, and the upper clear liquid was discarded to obtain the lower precipitate. The precipitate was centrifuged and washed several times with deionized water, and then vacuum dried at 60°C for 12 hours to obtain the Cys-Cu-24h precursor. (2) 100 mg of Cys-Cu-24h precursor was placed in porcelain boat A, and 500 mg of selenium powder was placed in porcelain boat B. Then, porcelain boat B was placed in the upstream of a dual-temperature zone tubular furnace, and porcelain boat A was placed in the downstream of the dual-temperature zone tubular furnace. The mixture was heated to 450 °C at a heating rate of 2 °C / min in a nitrogen atmosphere, and kept at a constant temperature for 3 hours. After the constant temperature was reached, the mixture was naturally cooled to room temperature to obtain a selenium-induced defective copper-based sulfur / selenide material, which was recorded as Cu 1.96 S / CuSe-24h.
[0017] Embodiment 3: (1) 0.64 g Cu(CH3COO)2•H2O was dissolved in 160 mL deionized water to prepare solution A, and then 0.7744 g cysteine was added to 640 mL deionized water. After the cysteine was completely dissolved, 5 mL of a pre-prepared NaOH solution with a concentration of 4 mol / L was added. After mixing evenly, the pH of the solution was adjusted to 12 to obtain solution B. Solution A was then added to solution B, and the mixture was placed in a constant temperature 20°C water bath with magnetic stirring for 12 minutes. After the reaction was completed, the obtained mixed solution was centrifuged at 5000 rpm for 3 minutes to separate the solid product from the solution, and the upper clear liquid was discarded to obtain the lower precipitate. The precipitate was centrifuged and washed several times with deionized water, and then vacuum dried at 50°C for 12 hours to obtain the Cys-Cu-12min precursor. (2) 300 mg of Cys-Cu-12min precursor was placed in porcelain boat A, and 300 mg of selenium powder was placed in porcelain boat B. Then, porcelain boat B was placed in the upstream of a dual-temperature zone tubular furnace, and porcelain boat A was placed in the downstream of the dual-temperature zone tubular furnace. The mixture was heated to 300 °C at a heating rate of 3 °C / min in a nitrogen atmosphere, and kept at this temperature for 1 hour. After the constant temperature was reached, the mixture was naturally cooled to room temperature to obtain a selenium-induced defective copper-based sulfur / selenide material, which was recorded as Cu 1.96 S / CuSe-12min.
[0018] Embodiment 4: (1) 1.92 g Cu(CH3COO)2•H2O was dissolved in 160 mL deionized water to prepare solution A, and then 1.5488 g cysteine was added to 640 mL deionized water. After the cysteine was completely dissolved, 15 mL of a pre-prepared NaOH solution with a concentration of 1 mol / L was added. After mixing evenly, the pH of the solution was adjusted to 8 to obtain solution B. Solution A was then added to solution B, and the mixture was placed in a constant temperature 40°C water bath with magnetic stirring for 30 hours. After the reaction was completed, the obtained mixed solution was centrifuged at 10,000 rpm for 8 minutes to separate the solid product from the solution, and the upper clear liquid was discarded to obtain the lower precipitate. The precipitate was centrifuged and washed several times with deionized water, and then vacuum dried at 80°C for 12 hours to obtain the Cys-Cu-30h precursor. (2) 85.7 mg of Cys-Cu-30h precursor was placed in porcelain boat A, and 514.3 mg of selenium powder was placed in porcelain boat B. Then, porcelain boat B was placed in the upstream of a double-temperature zone tubular furnace, and porcelain boat A was placed in the downstream of the double-temperature zone tubular furnace. The mixture was heated to 600 °C at a heating rate of 5 °C / min in a nitrogen atmosphere and kept at a constant temperature for 5 hours. After the constant temperature was reached, the mixture was naturally cooled to room temperature to obtain a selenium-induced defective copper-based sulfur / selenide material, which was recorded as Cu 1.96 S / CuSe-30h.
[0019] Comparative Example 1: This comparative example provides a method for preparing a copper-based sulfide composite material that has not been subjected to selenization treatment, comprising the following steps: (1) 1.44 g Cu(CH3COO)2•H2O was dissolved in 160 mL deionized water to prepare solution A. Then 1.4544 g cysteine was added to 640 mL deionized water. After the cysteine was completely dissolved, 10 mL of a pre-prepared 2 mol / L NaOH solution was added. The pH of the solution was adjusted to 10.58. After mixing evenly, the solution was obtained as solution B. Then solution A was added to solution B and placed in a constant temperature 30°C water bath with magnetic stirring for 30 minutes. After the reaction was completed, the obtained mixed solution was centrifuged at 8000 rpm for 5 minutes to separate the solid product from the solution. The upper clear liquid was discarded to obtain the lower precipitate. The precipitate was centrifuged and washed several times with deionized water, and then vacuum dried at 60°C for 12 hours to obtain the Cys-Cu-30min precursor. (2) 100 mg of Cys-Cu-30min precursor was placed in a porcelain boat, which was then placed in a single-zone tubular furnace and heated to 450°C at a heating rate of 2°C / min under a nitrogen atmosphere. The temperature was maintained constant for 3 hours, and the mixture was naturally cooled to room temperature to obtain a copper-based sulfide composite material that had not been selenized, which was recorded as Cu2S-30min-hot.
[0020] Comparative Example 2: This comparative example provides a method for preparing a copper-based sulfide composite material that has not been subjected to selenization treatment, comprising the following steps: (1) 1.44 g Cu(CH3COO)2•H2O was dissolved in 160 mL deionized water to prepare solution A, and then 1.4544 g cysteine was added to 640 mL deionized water. After it was completely dissolved, 10 mL of pre-prepared NaOH solution with a concentration of 2 mol / L was added, and the pH of the solution was adjusted to 10.58. After mixing evenly, it was solution B. Then solution A was added to solution B, and the mixture was placed in a constant temperature water bath at 30°C and magnetically stirred for 24 hours. After the reaction was completed, the obtained mixed solution was centrifuged at 8000 rpm for 5 minutes to separate the solid product from the solution, and the upper clear liquid was discarded to obtain the lower precipitate. The precipitate was centrifuged and washed several times with deionized water, and then vacuum dried at 60°C for 12 hours to obtain Cys-Cu-24h precursor; (2) 100 mg of Cys-Cu-24h precursor was placed in a porcelain boat, which was then placed in a single-zone tubular furnace and heated to 450°C at a heating rate of 2°C / min under a nitrogen atmosphere. The temperature was maintained constant for 3 hours, and the mixture was naturally cooled to room temperature to obtain a copper-based sulfide composite material that had not been selenized, which was recorded as Cu2S-24h-hot.
[0021] SEM testing was performed using a ZEISS Gemini SEM 300 scanning electron microscope from Zeiss, Germany. A small amount of powdered sample was coated on a black conductive adhesive and then subjected to gold spraying. SEM can be used to characterize the surface microstructure and particle size of the sample.
[0022] See also Figure 1 , Figure 2 , Figure 3 , the above SEM pictures show that: (1) Figure 1 In Figures (a), (b), and (c), the precursor Cys-Cu-30min prepared in Example 1 exhibits an "ordered interlaced" nanobelt morphology, each component unit has a diameter of about 6-8 μm and is evenly distributed, and a single nanobelt is about 5-10 nm thick. The component unit can refer to Figure (c), which refers to a unit composed of independent interlaced nanobelts; (2) Figure 1 In Figures (d), (e), and (f), the Cys-Cu-24h prepared in Example 2 has a longer stirring reaction time than that in Example 1, and several nanobelt units are combined and superimposed to form a regular cluster morphology; (3) Figure 2 In Figures (a), (b), and (c), after pyrolysis and selenization, the Cu prepared in Example 1 1.96 The S / CuSe-30min composite material still maintains the morphology of the precursor, indicating that further selenization does not change the morphology of the precursor and the precursor has excellent structural stability. This evenly distributed "ordered staggered" nanobelt can avoid disordered stacking between single nanobelts, expose more sodium storage active sites in space, and improve the utilization rate of the material; (4) Similarly, Figure 2 In Figures (d), (e), and (f), after pyrolysis and selenization, the Cu prepared in Example 2 1.96 The nanoribbon structure of the S / CuSe-24h composite shrinks slightly, but the precursor cluster morphology is still maintained; (5) Figure 3 The morphology of the precursor can also be observed in the Cu2S-30min-heat prepared in Comparative Example 1.
[0023] The BET test was performed using the ASAP 2460 surface area and porosity analyzer produced by Micromeritics Instruments, Inc., USA, to analyze the specific surface area of porous materials. Figure 4 BET analysis shows that the specific surface area of the Cys-Cu-30min precursor prepared in Example 1 is 115.53 m 2 / g, and the pore size is mainly concentrated at 15nm. It can be seen that the prepared new metal organic framework compound precursor has a large specific surface area and there are a large number of pores in the material. The large specific surface area of the material can not only increase the wettability between the material and the electrolyte, but also help to expose more sodium storage active sites and enhance the sodium storage capacity of the electrode material. The abundant pores provide a guarantee for the transmission speed of ions and electrons during the sodium storage process, and the fast ion and electron transmission rate can significantly improve the rate performance of the material.
[0024] XRD tests were performed using a D / max-γβ X-ray diffractometer produced by Rigaku Corporation of Japan to analyze the composition and structure of the samples.
[0025] See also Figure 5 , Figure 6 , the XRD pattern shows that: (1) Figure 5 The Cys-Cu-30min precursor and the Cys-Cu-24h precursor prepared in Example 1 and Example 2, respectively, have similar diffraction peaks and peak positions, and are different from the reported possible forms of copper-based oxides, copper-based hydroxides, copper-based sulfides, etc., further confirming the novelty of the prepared precursor structure. In addition, the similar XRD diffraction peaks of the precursors prepared in Example 1 and Example 2 also indicate that the increase in reaction time will change the morphology of the material, but will not change the crystal structure and composition; (2) Figure 6 The three composite materials prepared in Example 1, Example 2 and Comparative Example 1 have different components. In Comparative Example 1, the product obtained by direct pyrolysis of the Cys-Cu-30min precursor is Cu2S, indicating that the product is only copper sulfide in the absence of a selenium source. In Examples 1 and 2, when the Cys-Cu-30min precursor is treated with selenium powder at 450°C, the product is Cu 1.96 S and CuSe, indicating that the introduction of Se can not only form Cu containing copper vacancies 1.96 S, and can also generate CuSe species. 1.96 Compared with Cu2S, S species have abundant copper vacancies. The generation of vacancies can regulate the electronic structure of the substrate material, enhance the conductivity of the material and improve its electrochemical activity. The weak Cu-Se bond in the formed CuSe species is more conducive to the conversion reaction than sulfide, accelerating the diffusion of sodium ions. In addition, the formed Cu 1.96 S and CuSe can spontaneously form a homologous heterojunction. The existence of the heterojunction redistributes the charge at the interface, constructs a built-in electric field, and thus increases the internal conductivity of the material, which is conducive to the rapid transfer of electrons. 1.96 S / CuSe-30min and Cu prepared in Example 21.96 S / CuSe-24h has the same Cu 1.96 S and CuSe components, but Cu 1.96 The XRD curve of S / CuSe-30min shows that Cu 1.96 The peak intensity of S is higher than that of CuSe species, while Cu 1.96 The CuSe peak intensity of S / CuSe-24h is higher, indicating that the product CuSe formed by the precursor with a relatively short stirring reaction time is 1.96 S has better crystallinity, while the product CuSe formed by the precursor obtained with long stirring reaction time has better crystallinity and more exposed crystal faces.
[0026] The composite material Cu prepared in Example 1 1.96 S / CuSe-30min, the composite material Cu prepared in Example 2 1.96 S / CuSe-24h, the composite material Cu2S-30min-hot prepared in Comparative Example 1, and the composite material Cu2S-24h-hot prepared in Comparative Example 2 were all ground into powders and used as negative electrode active materials, respectively. The battery performance of the negative electrode of the sodium ion battery was measured using CR2032 coin-type battery test materials.
[0027] First, the Cu prepared in Example 1 1.96 The working electrode was prepared by mixing S / CuSe-30min powder, polymer binder (carboxymethyl cellulose aqueous solution, mass fraction of 1.5%) and conductive material (Super-P) to obtain a slurry, which was then coated on a copper foil and dried at 80 °C for 12 h. 1.96 The mass fractions of S / CuSe-30min powder, polymer binder, and conductive material were 80wt%, 10wt%, and 1.5wt%, respectively. The battery was assembled in a glove box, using Whatman glass fiber separators and metal sodium sheets as counter electrodes. The electrolyte was diethylene glycol dimethyl ether (DIGLYME) containing NaPF6, where the concentration of NaPF6 was 1M. The voltage window of 0.01-3V (relative to Na) was set on a LANHE (CT2001A, Wuhan, China) battery test system. + / Na) for constant current charge / discharge and rate test. Shanghai Chenhua electrochemical workstation CHI660E was used for battery electrochemical impedance test. The test voltage was open circuit voltage and the frequency was 0.01-10 5 Hz.
[0028] The Cu prepared in Example 1 1.96 S / CuSe-30min powder was replaced by Cu prepared in Example 2 1.96S / CuSe-24h powder, Cu2S-30min-hot powder prepared in Comparative Example 1, and Cu2S-24h-hot powder prepared in Comparative Example 2, and the rest of the methods for preparing the working electrode and the testing process are the same as those described above.
[0029] Figure 7 The composite material Cu prepared in Example 1 1.96 S / CuSe-30min, the composite material Cu prepared in Example 2 1.96 When the Cu2S-30min-hot composite materials prepared in S / CuSe-24h and Comparative Example 1 were used as negative electrodes of sodium ion batteries, the impedance diagrams before and after 5 cycles at a current density of 1A / g were shown. It can be seen from the figure that Cu2S-30min-hot has a smaller impedance before the cycle, while Cu 1.96 S / CuSe-30min and Cu 1.96 The impedance value of S / CuSe-24h is relatively large, but after 5 cycles, Cu 1.96 The impedance value of S / CuSe-30min is similar to that of Cu 1.96 The decrease in impedance is mainly due to the activation of the material. At the same time, the special nanoribbon structure provides a transmission channel for electron transmission. 1.96 The S component and the formation of heterostructures also help to improve the conductivity of the material.
[0030] Figure 8 It shows that the Cu prepared in Example 1 1.96 When the S / CuSe-30min composite material is used as a negative electrode material for sodium ion batteries and is tested at a current density of 1A / g, the initial discharge capacity can reach 528.43mAh / g, and the discharge capacity is still as high as 513.42mAh / g after 1000 cycles, showing excellent long-cycle performance. 1.96 The first discharge capacity of S / CuSe-24h is 654.69mAh / g, and the discharge capacity after 1000 cycles is 435.49mAh / g. The discharge capacity of Cu2S-30min-hot prepared in Comparative Example 1 is 231.83mAh / g after 499 cycles at a current density of 1A / g, and the discharge capacity of Cu2S-24h-hot prepared in Comparative Example 2 is 75.3mAh / g after 384 cycles at a current density of 1A / g, indicating that the long cycle performance of the composite materials prepared in Examples 1 and 2 is significantly better than that of Comparative Examples 1 and 2.
[0031] Fig. 9 It shows that even after 1000 cycles at a high current density of 5 A / g, the Cu prepared in Example 1 1.96S / CuSe-30min still has a discharge capacity of 207.7 mAh / g. 1.96 The excellent long-cycle stability and high capacity of the S / CuSe-30min composite material originate from the copper vacancies in the material, which can enhance the electrochemical activity of copper-based sulfides, and the built-in electric field constructed by the heterostructure can reduce the diffusion of sodium ions.
[0032] Fig.10 It shows that the composite material Cu prepared in Example 1 1.96 The capacities of S / CuSe-30min as the negative electrode material of sodium ion battery at different current densities of 0.1A / g, 0.2A / g, 0.5A / g, 1A / g, 2A / g, and 5A / g were 542mAh / g, 560.2mAh / g, 551.4mAh / g, 539mAh / g, 524.5mAh / g, and 492.1mAh / g, respectively, indicating that the material has a good capacity retention rate. 1.96 S / CuSe-24h and Cu 1.96 S / CuSe-30min has similar rate performance and is better than Comparative Example 1 and Comparative Example 2.
[0033] Fig.11 It shows that the composite material Cu prepared in Example 1 1.96 After S / CuSe-30min was used as the negative electrode and assembled into a full battery with sodium nickel iron manganese oxide as the positive electrode, the capacity could still be maintained at 196.61 mAh / g after 100 cycles at a current density of 0.5 A / g. The results show that the composite material with rich copper vacancies and homogeneous heterojunction prepared by this method has better long-cycle performance and high-rate characteristics, and is a potential application material for high energy density and high power density sodium ion batteries.
[0034] The above is only an embodiment of the present invention, and does not limit the present invention in any form. The present invention can also have other forms of embodiments according to the above structures and functions, which are not listed one by one. Therefore, any simple modification, equivalent change and modification made by any technician familiar with the profession to the above embodiment according to the technical essence of the present invention without departing from the scope of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.
Claims
1. A method for preparing a selenium-induced defect copper-based sulfur / selenide material, characterized in that: The specific steps include: (1) Dissolve copper acetate in water to prepare solution A; dissolve cysteine in water, and after cysteine is completely dissolved, add NaOH solution to adjust the pH value of the above solution to alkaline, thereby obtaining solution B; Then, solution A is added to solution B, and the mixture is stirred in a constant temperature water bath to react. After the reaction is completed, the obtained mixed solution is centrifuged, and the upper liquid is discarded to obtain a lower precipitate. The precipitate is centrifuged and washed with water for multiple times, and then vacuum dried to obtain a Cys-Cu precursor. (2) Place the Cys-Cu precursor in porcelain boat A and the selenium powder in porcelain boat B. Then place porcelain boats A and B in the downstream and upstream of a dual-temperature zone tubular furnace respectively. Heat the mixture to a certain temperature under an inert atmosphere and keep the temperature constant for a period of time. After the temperature is constant, cool the mixture naturally to room temperature to obtain selenium-induced defective copper-based sulfur / selenide materials.
2. The method for preparing the selenium-induced defective copper-based sulfur / selenide material according to claim 1, characterized in that: In step (1), the molar concentration of copper acetate in solution A is 0.02-0.06 mol / L, and the molar concentration of cysteine in solution B is 0.01-0.02 mol / L.
3. The method for preparing the selenium-induced defective copper-based sulfur / selenide material according to claim 1, characterized in that: In step (1), the water used is deionized water; the concentration of the NaOH solution is 1-4 mol / L, the volume of the added NaOH solution is 5-15 mL, and the pH value of solution B is 8-12.
4. The method for preparing the selenium-induced defective copper-based sulfur / selenide material according to claim 1, characterized in that: In step (1), the temperature of the constant temperature water bath is 20-40° C., and the stirring reaction time is 0.2-30 hours.
5. The method for preparing the selenium-induced defective copper-based sulfur / selenide material according to claim 1, characterized in that: In step (1), the rotation speed of centrifugal separation is 5000-10000 rpm, the time of each centrifugal separation is 3-8 minutes; and the drying temperature is 50-80°C.
6. The method for preparing the selenium-induced defective copper-based sulfur / selenide material according to claim 1, characterized in that: In step (2), the mass ratio of the Cys-Cu precursor to the selenium powder is 1:1 to 1:
6.
7. The method for preparing the selenium-induced defective copper-based sulfur / selenide material according to claim 1, characterized in that: In step (2), the heating rate is 2-5°C / min, the temperature is raised to 300-600°C, the constant temperature time is 1-5 hours, and the inert atmosphere is N2 atmosphere.
8. The selenium-induced defective copper-based sulfur / selenide material obtained by the preparation method according to any one of claims 1 to 7.
9. The selenium-induced defect copper-based sulfur / selenide material according to claim 8, characterized in that: The material contains Cu 1.96 S and CuSe, and Cu 1.96 A homologous heterojunction is formed between S and CuSe.
10. Use of the selenium-induced defect copper-based sulfur / selenide material as claimed in claim 8 as a negative electrode material for sodium ion batteries.
Citation Information
Patent Citations
Component-controllable copper sulfur selenium nanometer sheet as well as preparation method and application thereof
CN103964401A
Chemical method of synthesizing Se-S-Cu (Selenium-Sulphur-Copper) ternary compound through constant temperature in-situ control
CN104876195A
Sodium ion battery taking copper-selenium compound as negative electrode material
CN106920989A
Preparation method of metal sulfide and carbon composite material and application of metal sulfide and carbon composite material in sodium ion battery
CN106992293A
Preparation method of duplex-metal selenide sodium ion battery negative electrode material
CN109768236A