Molybdenum disulfide and carbon composite material and preparation method thereof

Through the sandwich structure composite of molybdenum disulfide and carbon prepared by the template method and hydrothermal method in lithium-ion batteries, the structure of traditional molybdenum disulfide electrode materials is easily collapsed and electronic conduction during charging and discharging. The problem of low rate achieves efficient electrochemical lithium storage performance and good cycle stability.

CN118877941APending Publication Date: 2024-11-01BOZHOU SHANGDA ENG TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410838277.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The negative electrode material of traditional lithium-ion batteries, molybdenum disulfide, has a low electronic conductivity and easy structure to collapse during charging and discharge, resulting in poor electrochemical lithium storage performance and unable to meet the growing demand for energy storage.

Method used

The sandwich structure composite material C@MoS2@C of molybdenum disulfide and carbon is prepared by template method and hydrothermal method. MoS2 is encapsulated through the carbon layer to provide efficient electron transfer channels, prevent MoS2 nanosheets from agglomeration, protect them from electrolyte contact, and inhibit them. Polysulfide production.

Benefits of technology

It significantly improves the electrochemical lithium storage performance, enhances structural stability, maintains electrochemical activity, and achieves high initial discharge capacity and good cycling stability, especially in high current density, which shows excellent rate performance and conductivity. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118877941A_ABST
    Figure CN118877941A_ABST
Patent Text Reader

Abstract

The invention provides a molybdenum disulfide and carbon composite material and a preparation method thereof, and a carbon / molybdenum disulfide / carbon interlayer composite material, namely a C (at) MoS2 (at) C composite material, is prepared by a template method and a hydrothermal method. Experimental results show that the structural stability of the C-coated MoS2-coated C composite material is remarkably enhanced, and the volume change in the charging and discharging process is effectively buffered. The material not only has high initial discharge capacity (1690 mAhg <-1 >) and excellent cycling stability (the capacity retention rate after 50 times of cycling is about 74%), but also shows excellent rate capability, can maintain high-level specific capacity under different current densities, and has good cycling stability, especially under high current density. In addition, the carbon layer of the C-coated MoS2-coated C is highly graphitized, so that the C-coated MoS2-coated C is endowed with good conductivity, meanwhile, aggregation of MoS2 nanosheets is inhibited, and the electrochemical performance is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of nano new materials and electrochemical energy, and particularly to a composite material of molybdenum disulfide and carbon with a sandwich structure and a preparation method thereof. Background Art

[0002] With the acceleration of global industrialization, traditional energy sources such as oil, coal, natural gas and other fossil fuels are facing the dilemma of increasing depletion. At the same time, the demand for energy in modern industry continues to grow, which prompts people to constantly seek and develop new, clean and sustainable energy sources. The development and utilization of new energy sources such as solar energy, wind energy, and nuclear energy have received widespread attention around the world. However, these new energy sources are intermittent and unstable, so efficient energy storage devices are needed to balance the fluctuations between energy supply and demand.

[0003] As an efficient and environmentally friendly energy storage device, lithium-ion batteries (LIBs) have been widely used in consumer electronic products. Their advantages include wide application range, high stability, and no memory effect. However, with the development of high-power electrical appliances such as electric vehicles, higher requirements are placed on the energy density, cycle life and other performance of energy storage systems. Traditional lithium-ion batteries have a low theoretical specific capacity (370 mAh g -1 ) limitations can no longer meet the growing demand for energy storage.

[0004] Negative electrode materials are an important component of lithium-ion batteries, and their performance has a decisive influence on the overall energy storage performance of the battery. Therefore, the development of new high-performance negative electrode materials has become a hot topic in current research. Two-dimensional layered transition metal sulfides, molybdenum disulfide (MoS2), has gained widespread attention in the selection of negative electrode materials for lithium-ion batteries due to its controllable structure and strong lithium storage capacity. However, pure MoS2 electrode materials face some challenges in practical applications, such as low electronic conductivity and irreversible collapse of the two-dimensional layered structure during charging and discharging, which leads to poor electrochemical lithium storage performance, fast energy decay, and poor rate performance. Summary of the invention

[0005] In order to solve the deficiencies of the prior art and improve the electrochemical energy conversion rate of negative electrode materials for lithium-ion batteries, the present invention provides a composite material of molybdenum disulfide (MoS2) and carbon and a preparation method thereof. Starting from structural design, the present invention designs a sandwich structure of MoS2 and carbon, and prepares a carbon / molybdenum disulfide / carbon sandwich composite material (C@MoS2@C) by template method and hydrothermal method. This sandwich structure provides an efficient channel for lithium ion and electron transfer, prevents the agglomeration of MoS2 nanosheets during the charge and discharge process, and protects MoS2 from direct contact with the electrolyte, inhibits the generation of polysulfide and its shuttle effect, and at the same time combines the high surface area brought by the template to further improve the electrochemical lithium storage performance.

[0006] One aspect of the present invention is to provide a method for preparing a composite material of molybdenum disulfide and carbon, the steps comprising:

[0007] Provided is a fibrous silica sphere, namely KCC-1 nanosphere;

[0008] The KCC-1 nanospheres are mixed and reacted with dopamine to obtain a first intermediate product;

[0009] The first intermediate product is mixed with Mx(MoS4)y and reacted to obtain a second intermediate product;

[0010] The second intermediate product is mixed with dopamine and reacted to obtain a third intermediate product;

[0011] The third intermediate product is calcined and soaked in alkali solution to obtain a composite material of molybdenum disulfide and carbon, namely C@MoS2@C;

[0012] Wherein, M is a cation, and x and y are positive integers.

[0013] In a preferred embodiment, the method for preparing the KCC-1 nanospheres comprises the following steps:

[0014] Urea, cetylpyridinium bromide and ethyl orthosilicate are mixed and reacted to obtain an intermediate product of KCC-1 nanospheres;

[0015] The intermediate product of KCC-1 nanospheres is calcined to obtain fibrous silica spheres, namely KCC-1 nanospheres.

[0016] In a preferred embodiment, the initial reaction concentration of urea is 2-15 g / L, preferably 3-12 g / L, and more preferably 8-10 g / L.

[0017] In a preferred embodiment, the initial reaction concentration of cetylpyridinium bromide is 2-20 g / L, preferably 3-18 g / L, and more preferably 8-17 g / L.

[0018] In a preferred embodiment, the urea and cetylpyridinium bromide are firstly ultrasonically treated in water and mixed uniformly.

[0019] In a preferred embodiment, the ethyl orthosilicate is added dropwise in the form of a solution into a mixed solution of urea and cetylpyridinium bromide.

[0020] Preferably, the solvent of the tetraethyl orthosilicate solution is a mixed solvent of cyclohexane and pentanol.

[0021] In a preferred embodiment, the reaction temperature of urea, cetylpyridinium bromide and tetraethyl orthosilicate is 50-150°C, preferably 60-120°C, more preferably 70-100°C.

[0022] In a preferred embodiment, the reaction time of urea, cetylpyridinium bromide and tetraethyl orthosilicate is 2-48 h, preferably 4-36 h, and more preferably 12-24 h.

[0023] In a preferred embodiment, the reaction product of urea, cetylpyridinium bromide and tetraethyl orthosilicate is further washed and dried to obtain an intermediate product of KCC-1 nanospheres.

[0024] Preferably, the cleaning solvent of the reaction product of urea, cetylpyridinium bromide and tetraethyl orthosilicate is water and / or ethanol and / or acetone.

[0025] Preferably, the drying temperature of the reaction product of urea, cetylpyridinium bromide and tetraethyl orthosilicate is 30-100°C, preferably 40-80°C, more preferably 50-60°C.

[0026] Preferably, the drying time of the reaction product of urea, cetylpyridinium bromide and ethyl orthosilicate is 5-48 h, preferably 8-24 h, more preferably 12-15 h.

[0027] In a preferred embodiment, the intermediate product of KCC-1 nanospheres is calcined in a muffle furnace.

[0028] In a preferred embodiment, the calcination temperature of the intermediate product of the KCC-1 nanospheres is 300-800°C, preferably 400-650°C, and more preferably 500-550°C.

[0029] In a preferred embodiment, the calcination time of the intermediate product of KCC-1 nanospheres is 2-12 h, preferably 3-10 h, and more preferably 5-6 h.

[0030] In a preferred embodiment, the KCC-1 nanospheres and dopamine are mixed and reacted in a tris (hydroxymethyl)aminomethane buffer solution (Tris).

[0031] In a preferred embodiment, the first intermediate product is dried before being mixed and reacted with Mx(MoS4)y.

[0032] Preferably, the drying temperature of the first intermediate product is 30-100°C, preferably 40-80°C, more preferably 50-60°C.

[0033] Preferably, the drying time of the first intermediate product is 5-48 h, preferably 8-24 h, more preferably 12-15 h.

[0034] In a preferred embodiment, M of Mx(MoS4)y is a metal cation or an ammonium ion.

[0035] Preferably, the Mx(MoS4)y includes one or more of (NH4)2MoS4, Na2MoS4, and K2MoS4.

[0036] In a preferred embodiment, the first intermediate product is mixed and reacted with Mx(MoS4)y in DMF (N,N-dimethylformamide), DMAC (dimethylacetamide), N-methylacetamide, DMP (dimethylpropionamide), DEF (diethylformamide), or DEAC (diethylacetamide).

[0037] In a preferred embodiment, the first intermediate product undergoes a hydrothermal reaction with Mx(MoS4)y in a reactor.

[0038] In a preferred embodiment, the reaction temperature of the first intermediate product and Mx(MoS4)y is 100-250°C, preferably 150-220°C, and more preferably 180-200°C.

[0039] In a preferred embodiment, the reaction time of the first intermediate product and Mx(MoS4)y is 5-48h, preferably 8-24h, and more preferably 12-18h.

[0040] In a preferred embodiment, the second intermediate product is washed and dried before being mixed and reacted with dopamine.

[0041] Preferably, the cleaning solvent for the second intermediate product is water and / or ethanol and / or acetone.

[0042] Preferably, the drying temperature of the second intermediate product is 30-100°C, preferably 40-80°C, more preferably 50-60°C.

[0043] Preferably, the drying time of the second intermediate product is 5-48 h, preferably 8-24 h, more preferably 12-15 h.

[0044] In a preferred embodiment, the second intermediate product is mixed with dopamine in a tris(hydroxymethyl)aminomethane buffer solution and reacted

[0045] In a preferred embodiment, the third intermediate product is calcined in a tube furnace.

[0046] In a preferred embodiment, the third intermediate product is calcined under a protective gas atmosphere.

[0047] Preferably, the protective gas includes one or more combinations of nitrogen, argon and helium.

[0048] Preferably, the calcination temperature of the third intermediate product is 300-900°C, preferably 400-850°C, more preferably 500-800°C.

[0049] Preferably, the calcination time of the third intermediate product is 2-18 h, preferably 3-16 h, and more preferably 5-10 h.

[0050] In a preferred embodiment, the alkali solution includes one or more combinations of sodium hydroxide solution, sodium bicarbonate solution, and ammonia water.

[0051] Preferably, the concentration of the alkali solution is 1-10 mol / L, preferably 1.5-8 mol / L, more preferably 1.8-2 mol / L.

[0052] In a preferred embodiment, the third intermediate product is calcined, soaked in alkali solution, washed and dried.

[0053] In a preferred embodiment, the cleaning solvent for the third intermediate product after calcination and alkali solution soaking is water and / or ethanol and / or acetone.

[0054] In a preferred embodiment, the drying temperature of the third intermediate product after calcination and alkali solution soaking is 30-100°C, preferably 40-80°C, and more preferably 50-60°C.

[0055] In a preferred embodiment, the drying time of the third intermediate product after calcination and alkali solution soaking is 5-48 hours, preferably 8-24 hours, and more preferably 12-15 hours.

[0056] Another aspect of the present invention is to provide a composite material of molybdenum disulfide and carbon, namely C@MoS2@C, which is obtained based on the preparation method described in the present invention.

[0057] In this application specification, "@" means that a material is encapsulated or coated by another material to protect the core material from the external environment, or to control the release of the core material. In MOFs materials, this encapsulation is used to improve the porosity, stability or other physical and chemical properties of the material. In the context of C@MoS2@C, "@" means C encapsulated MoS2 encapsulated C, and C@MoS2@C is a sandwich structure with MoS2 as the sandwich and C as the core and shell.

[0058] Compared with the prior art, the beneficial technical effects of the present invention are as follows:

[0059] The present invention provides a composite material of molybdenum disulfide and carbon and a preparation method thereof. The present invention prepares a carbon / molybdenum disulfide / carbon sandwich composite material, namely, a C@MoS2@C composite material, by a template method and a hydrothermal method. The experimental results of the present invention show that the C@MoS2@C composite material significantly enhances its structural stability, effectively buffers the volume change during the charge and discharge process, prevents structural damage, and thus maintains electrochemical activity. The material not only has a high initial discharge capacity (1690mAhg -1 ) and excellent cycle stability (capacity retention rate is about 74% after 50 cycles), and also shows excellent rate performance, can maintain a high level of specific capacity at different current densities, and has good cycle stability, especially at high current density. In addition, the carbon layer of C@MoS2@C is highly graphitized, which gives it good conductivity, while inhibiting the aggregation of MoS2 nanosheets, further improving the electrochemical performance. Electrochemical impedance spectroscopy (EIS) tests show that C@MoS2@C has a lower charge transfer impedance, indicating that its electron transfer efficiency is higher, providing a new way to prepare high-performance electrochemical energy storage materials. Therefore, the present invention relies on the unique layered fibrous carbon structure to inhibit the aggregation of MoS2 during the charge and discharge process, enhance the charge transfer, and enable the composite material to obtain a higher specific capacity, better rate performance and good cycle stability than MoS2 NPs (materials without a sandwich structure). BRIEF DESCRIPTION OF THE DRAWINGS

[0060] Figure 1 XRD diffraction spectra of C@MoS2@C and MoS2 NPs obtained by implementing the present invention.

[0061] Figure 2 Raman spectra of C@MoS2@C and MoS2 NPs obtained by implementing the present invention.

[0062] Figure 3 SEM and TEM images of KCC-1 obtained by the implementation of the present invention (a, b); SEM and TEM images of C@MoS2@C (c, d); SEM images of MoS2 NPs at different magnifications (e, f).

[0063] Figure 4 This is the CV curve of C@MoS2@C obtained by implementing the present invention at 0.01-3.0V.

[0064] Figure 5 The C@MoS2@C obtained by the present invention is 0.1Ag -1 The charge and discharge curves below.

[0065] Figure 6 The C@MoS2@C and MoS2 NPs obtained by the present invention are subjected to a current density of 0.1Ag -1 Cycle performance under .

[0066] Figure 7 The rate performance of C@MoS2@C and MoS2 NPs obtained by the implementation of the present invention at different current densities.

[0067] Figure 8 The C@MoS2@C obtained by the present invention has a high current density of 1A. -1 Cyclic stability under .

[0068] Fig. 9 Electrochemical impedance spectra of C@MoS2@C and MoS2 NPs obtained by implementing the present invention.

[0069] Fig.10 Schematic diagram of KCC-1 nanospheres obtained by implementing the present invention. DETAILED DESCRIPTION

[0070] The present invention provides a composite material of molybdenum disulfide and carbon and a preparation method thereof. In order to make the purpose, technical scheme and effect of the present invention clearer and more specific, the present invention is further described in detail with reference to the accompanying drawings and examples. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0071] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged under appropriate circumstances. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0072] Example

[0073] (1) Synthesis of fibrous silica spheres (KCC-1 nanospheres): 0.6 g of urea and 1 g of cetylpyridinium bromide were added to 30 mL of deionized water and dispersed evenly by ultrasonication for 30 min. A solution of 30 mL of cyclohexane, 1.5 mL of amyl alcohol, and 2.7 mL of tetraethyl orthosilicate was then added dropwise. The reaction solution was stirred at room temperature for 1 h and then refluxed at 70°C in an oil bath for 24 h. After the reactants were cooled to room temperature naturally, they were repeatedly washed with water, ethanol, and acetone, and the lower precipitate was removed by centrifugation and dried in an oven at 60°C for 12 h. The dried white powder was transferred to a muffle furnace and calcined at 550°C for 6 h to obtain the target product KCC-1.

[0074] (2) Synthesis of C@MoS2@C: 80 mg of KCC-1 nanoparticles were put into 100 mL of Tris (10 mM) buffer solution, and after uniform dispersion, 40 mg of dopamine was added and magnetic stirring was performed at room temperature for 24 h. The obtained product was washed and centrifuged, and then dried in an oven at 60 °C for 12 h. After drying, 50 mg of the obtained product and 20 mg of (NH4)2MoS4 were taken and poured into 30 mL of DMF and uniformly dispersed. The mixed solution was transferred to a reactor and hydroheated at 200 °C for 18 h. After naturally cooling to room temperature, the mixture was washed with water and ethanol, centrifuged and vacuum dried at 60°C for 12 hours; 80 mg of the dried product was taken and put into 100 mL (10 mM) Tris buffer solution, and after uniform dispersion, 40 mg of dopamine was added and magnetically stirred at room temperature for 24 hours; the obtained product was washed and centrifuged, and vacuum dried at 60°C for 12 hours; the dried product was placed in a tubular furnace and calcined at 800°C for 10 hours under a nitrogen atmosphere; the calcined product was soaked in 2M NaOH solution for 24 hours; the soaked product was washed, centrifuged and vacuum dried at 60°C for 12 hours to obtain the target product C@MoS2@C.

[0075] (4) Synthesis of MoS2 nanoparticles (MoS2 NPs): Take 20 mg of (NH4)2MoS4 and pour it into 30 mL of DMF to disperse it evenly; transfer the mixed solution to a reactor and hydrothermal it at 200°C for 18 h. After the reactants are naturally cooled to room temperature, they are washed with water and ethanol, centrifuged and vacuum dried at 60°C for 12 h; the dried product is placed in a tube furnace and calcined at 500°C for 2 h under a nitrogen atmosphere to obtain the target product MoS2 NPs.

[0076] The above products were characterized and the results were as follows Figure 1-9 As shown:

[0077] Figure 1The X-ray diffraction spectra of the prepared C@MoS2@C and the comparative sample MoS2 NPs are presented. C@MoS2@C has four relatively obvious diffraction peaks in the range of 10° to 80°, located at 13.4°, 33.1°, 39.3° and 58.6°, which correspond to the (002), (100), (103) and (110) crystal planes of the standard hexagonal phase of MoS2 (JCPDS 37-1492). At the same time, there is also good consistency between the main diffraction peaks of C@MoS2@C and MoS2 NPs. This preliminarily proves the successful synthesis of MoS2 composite materials.

[0078] Figure 2 This is the Raman spectrum of C@MoS2@C and the comparative sample MoS2 NPs. It can be seen from the figure that MoS2 NPs has a Raman spectrum of 360-460 cm -1 There are three different characteristic peaks in the range, located at 378cm -1 、406cm -1 、450cm -1 This is a typical Raman peak of molybdenum sulfide, further proving that the MoS2 composite material was successfully prepared. -1 The two peaks appearing at are the D peak and G peak that characterize carbon-based materials. D and I G The ratio of proves that our carbon-based graphitization degree is high and has excellent conductivity.

[0079] Figure 3(a, b) are SEM and TEM images of KCC-1. It can be seen that the synthesized KCC-1 has a uniform size, a fibrous structure, and has more pores with a diameter of about 300nm. Figures (c, d) are SEM and TEM images of C@MoS2@C synthesized using KCC-1 as a hard template. It can be seen that it exhibits a hierarchical fiber structure. Compared with KCC-1, it can be seen that C@MoS2@C exhibits a certain degree of hollow structure after removing the template. The presence of hollow pores will further improve the energy conversion and storage performance of the material. The size of the composite material remains basically unchanged. From the difference in contrast of the TEM image of C@MoS2@C, it can be inferred that the light-colored part is the carbon layer and the earthworm-like dark stripes are MoS2, indicating that PDA and MoS2 nanosheets grow uniformly and stably on the surface of the template KCC-1 during the synthesis process, forming a similar hierarchical fiber structure. At the same time, the hydrothermal and NaOH etching processes did not cause a large degree of damage to the overall morphology. The results preliminarily show that C@MoS2@C nanocomposites were prepared by the template method. At the same time, Figures (e, f) are SEM images of MoS2 NPs synthesized by the same hydrothermal method at different scales. It can be seen that with the same synthesis method, without adding precursors, MoS2 NPs present a microsphere structure with textures, which is quite different from C@MoS2@C.

[0080] Figure 4 The cyclic voltammetry test curve of C@MoS2@C electrode is presented. During the first discharge cycle, a weak peak appears at 1.0V, which can be attributed to Li + Inserted into MoS2 nanosheets to form Li x MoS2, can be expressed as: MoS2+xe - →Li x MoS2. The peak at 0.4 V can be attributed to Li x MoS2 and Li + The conversion reaction occurs to generate Mo and Li2S, which can be expressed as: Li x MoS2+(4-x)Li + +(4-x)e - →Mo+2Li2S, accompanied by the formation of a solid electrolyte membrane (SEI). During the first charge, the very weak anode peak at 1.71V comes from the oxidation reaction between Mo and LiS2, and the reaction formula is: Another prominent peak appearing at 2.3 V is attributed to the delithiation of Li2S, and the reaction equation is: In the subsequent charge-discharge cycles, the reduction peaks at 1.0 V and 0.4 V disappeared, and two new reduction peaks appeared at 0.9 V and 1.8 V.

[0081] Figure 5The sample C@MoS2@C at 0.1Ag -1 The 1st, 2nd and 10th constant current charge-discharge curves under current density. Polarization causes voltage hysteresis in the sample during the charge-discharge process, that is, there is a potential difference between the discharge and charge platforms. The charge-discharge curve of C@MoS2@C shows that during the first cycle of discharge, there are voltage platforms at 1.2-1.0V and 0.5-0.3V, corresponding to the Li + Insertion of MoS2 sheets to form Li x MoS2 and Li x MoS2 and Li + The conversion reaction generates Mo and Li2S. In the subsequent charging process, the voltage platform at 2.2-2.4V corresponds to the delithiation of Li2S and the formation of polysulfides. In addition, the subsequent charge and discharge curves are basically the same, indicating that the electrochemical lithium storage process of C@MoS2@C is highly reversible. At the same time, the discharge and charge processes of C@MoS2@C in the first cycle can provide 1690 and 920 mAhg -1 The specific capacity of C@MoS2@C is 1030mAhg, and the Coulombic efficiency is about 54%. The low initial Coulombic efficiency may be due to the decomposition of the electrolyte and the formation of the SEI film. At the same time, the second discharge of C@MoS2@C can provide 1030mAhg -1 The specific capacity of the battery was 926 mAh g after 10 cycles. -1 ). Compared with MoS2 NPs, the synthesized C@MoS2@C composite material exhibits better electrochemical lithium storage performance.

[0082] Figure 6 The C@MoS2@C and MoS2 NPs obtained by the present invention are subjected to a current density of 0.1Ag -1 The C@MoS2@C composite material exhibits good electrochemical lithium storage performance and has a high initial discharge capacity of 1690 mA hg -1 After 50 cycles, C@MoS2@C still has 768mA hg -1 The specific capacity of the second cycle (1030mAhg -1 ) compared with the first charge and discharge capacity decay is about 74%. The first charge and discharge capacity decay comes from the decomposition of the electrolyte and the formation of the SEI film during the first charge and discharge process. The coulomb efficiency of the subsequent cycle process is basically maintained above 95%, showing good stability. In comparison, the MoS2 NPs electrode has 831mAhg -1 The initial discharge capacity of the battery dropped sharply after several cycles, and after twenty cycles, it was less than 200 mAhg. -1The specific capacity of the 20th cycle is only 20% compared with the second cycle. We believe that this is because the hierarchical fibrous carbon structure inhibits the aggregation of MoS2 nanosheets during the charge and discharge process, while the carbon skeleton maintains the overall structural stability, showing better charge and discharge cycle stability than MoS2 NPs.

[0083] Figure 7 The rate performance of C@MoS2@C and MoS2 NPs obtained by the present invention at different current densities. -1 At current densities of 2.5, 1.5, 2.5, 3.5, and 4.0 mAh g / cm2, the specific capacities of C@MoS2@C are maintained at 950, 870, 760, 670, 570, and 450 mAh g / cm2, respectively. -1 When the current density returns to 0.1Ag -1 The specific capacity also recovered and remained at 880 mAh g after several cycles. -1 In contrast, the reversible capacity of MoS2 NPs at different current densities is lower than that of C@MoS2@C under the same conditions, and when the current density returns to 0.1Ag -1 The battery capacity cannot be restored well and decays rapidly after several cycles.

[0084] Figure 8 The C@MoS2@C obtained by the present invention has a high current density of 1A. -1 Cyclic stability under 1.2Ag -1 At a current density of 1.5 200 mAh, the capacity showed almost no attenuation after 400 cycles of charge and discharge, showing a capacity of 690 mAh g -1 The reversible capacity of the battery is 2.5W, and the coulombic efficiency during the charge and discharge process is basically maintained above 95%, showing good cycle stability.

[0085] Fig. 9 The electrochemical impedance spectra of C@MoS2@C and MoS2 NPs obtained by the implementation of the present invention. The results show that the electrochemical impedance spectra composed of a semicircle at high frequency and a slant line at low frequency, the semicircle in the high frequency region is controlled by electrochemical kinetics and represents the impedance of charge migration on the electrode surface, the inclined straight line in the low frequency region represents the diffusion kinetics of lithium ions, and the slope reflects the diffusion rate of lithium ions. It can be seen that the semicircle of C@MoS2@C at high frequency is smaller than that of MoS2 NPs, indicating that the C@MoS2@C electrode has a lower charge transfer impedance. Compared with MoS2 NPs, the C@MoS2@C composite material exhibits better conductivity.

[0086] In summary, the embodiments of the present invention provide a composite material of molybdenum disulfide and carbon and a preparation method thereof, and prepare a carbon / molybdenum disulfide / carbon sandwich composite material, namely, a C@MoS2@C composite material, by a template method and a hydrothermal method. Figure 1-9 The experimental results show that the C@MoS2@C composite material significantly enhances its structural stability, effectively buffers the volume change during charge and discharge, prevents structural damage, and thus maintains electrochemical activity. The material not only has a high initial discharge capacity (1690mAhg -1 ) and excellent cycle stability (capacity retention rate is about 74% after 50 cycles), and also shows excellent rate performance, can maintain a high level of specific capacity at different current densities, and has good cycle stability, especially at high current density. In addition, the carbon layer of C@MoS2@C is highly graphitized, which gives it good conductivity, while inhibiting the aggregation of MoS2 nanosheets, further improving the electrochemical performance. Electrochemical impedance spectroscopy (EIS) tests show that C@MoS2@C has a lower charge transfer impedance, indicating that its electron transfer efficiency is higher, providing a new way to prepare high-performance electrochemical energy storage materials. Therefore, the present invention relies on the unique layered fibrous carbon structure to inhibit the aggregation of MoS2 during the charge and discharge process, enhance the charge transfer, and enable the composite material to obtain a higher specific capacity, better rate performance and good cycle stability than MoS2 NPs (materials without a sandwich structure).

[0087] The specific embodiments of the present invention are described in detail above, but they are only examples, and the present invention is not limited to the specific embodiments described above. For those skilled in the art, any equivalent modifications and substitutions made to the present invention are also within the scope of the present invention. Therefore, the equalization changes and modifications made without departing from the spirit and scope of the present invention should be included in the scope of the present invention.

Claims

1. A method for preparing a composite material of molybdenum disulfide and carbon, comprising the steps of: Provided is a fibrous silica sphere, namely KCC-1 nanosphere; The KCC-1 nanospheres are mixed and reacted with dopamine to obtain a first intermediate product; The first intermediate product is mixed with Mx(MoS4)y and reacted to obtain a second intermediate product; The second intermediate product is mixed with dopamine and reacted to obtain a third intermediate product; The third intermediate product is calcined and soaked in alkali solution to obtain a composite material of molybdenum disulfide and carbon, namely C@MoS2@C; Wherein, M is a cation, and x and y are positive integers.

2. The preparation method according to claim 1, characterized in that: The preparation method of the KCC-1 nanospheres comprises the following steps: Urea, cetylpyridinium bromide and ethyl orthosilicate are mixed and reacted to obtain an intermediate product of KCC-1 nanospheres; The intermediate product of KCC-1 nanospheres is calcined to obtain fibrous silica spheres, namely KCC-1 nanospheres.

3. The preparation method according to claim 2, characterized in that: The urea and cetylpyridinium bromide are firstly ultrasonically treated in water and mixed uniformly; and / or The ethyl orthosilicate is added dropwise in the form of a solution into a mixed solution of urea and cetylpyridinium bromide.

4. The preparation method according to claim 2, characterized in that: The reaction temperature of the urea, cetylpyridinium bromide and ethyl orthosilicate is 50-150°C, preferably 60-120°C, and more preferably 70-100°C.

5. The preparation method according to claim 2, characterized in that: The intermediate product of KCC-1 nanospheres is calcined in a muffle furnace; and / or The calcination temperature of the intermediate product of the KCC-1 nanospheres is 300-800°C, preferably 400-650°C, more preferably 500-550°C; and / or The calcination time of the intermediate product of the KCC-1 nanospheres is 2-12 hours, preferably 3-10 hours, and more preferably 5-6 hours.

6. The preparation method according to claim 1, characterized in that: The first intermediate product undergoes a hydrothermal reaction with Mx(MoS4)y in a reactor; and / or The reaction temperature of the first intermediate product and Mx(MoS4)y is 100-250°C, preferably 150-220°C, more preferably 180-200°C; and / or The reaction time of the first intermediate product and Mx(MoS4)y is 5-48h, preferably 8-24h, and more preferably 12-18h.

7. The preparation method according to claim 1, characterized in that: The third intermediate product is calcined in a tube furnace; and / or The third intermediate product is calcined under a protective gas atmosphere; and / or The calcination temperature of the third intermediate product is 300-900° C., preferably 400-850° C., more preferably 500-800° C.; and / or The calcination time of the third intermediate product is 2-18 hours, preferably 3-16 hours, and more preferably 5-10 hours.

8. The preparation method according to claim 1, characterized in that: The alkali solution includes one or more combinations of sodium hydroxide solution, sodium bicarbonate solution, and ammonia solution; and / or The concentration of the alkali solution is 1-10 mol / L, preferably 1.5-8 mol / L, and more preferably 1.8-2 mol / L.

9. The preparation method according to claim 1, characterized in that: The third intermediate product is calcined, soaked in alkali solution, and washed and dried; and / or The third intermediate product after calcination and alkali solution soaking, wherein the washing solvent is water and / or ethanol and / or acetone; and / or The drying temperature of the third intermediate product after calcination and alkali solution soaking is 30-100° C., preferably 40-80° C., more preferably 50-60° C.; The drying time of the third intermediate product after calcination and alkali solution soaking is 5-48 hours, preferably 8-24 hours, and more preferably 12-15 hours.

10. A composite material of molybdenum disulfide and carbon, namely C@MoS2@C, characterized in that: Obtained based on the preparation method according to any one of claims 1 to 9.