Coating modified lithium-rich manganese-based precursor and preparation method and application thereof
By using P2-type sodium ion positive electrode material on the lithium-rich manganese-based precursor for coating and using spray pyrolysis method, the problem of intimate bonding between the coating layer and the bulk material is solved, and efficient lithium ion transmission channels are achieved. Lithium embedded site improves the initial Coulomb efficiency and cycling performance of lithium-ion batteries.
Patent Information
- Application Number
- CN202410911945.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-01
AI Technical Summary
In the prior art, lithium-rich manganese-based positive electrode material has problems such as coating peeling, particle cracking and grain boundary lithium ion aggregation during the charge and discharge cycle, resulting in the initial Coulomb efficiency being less than 85%, and the high initial Coulomb efficiency cannot be taken into account. Rate performance and excellent cycle performance.
The lithium-rich manganese-based precursor is coated with P2 sodium ion positive electrode material NaxMO2. The coated modified lithium-rich manganese-based precursor is prepared by spray pyrolysis method to build a tight and stable interface to create efficient lithium-ion transmission. Channels and more lithium embedded sites.
The Coulomb efficiency of more than 100% and excellent cycle stability are achieved, and the initial Coulomb efficiency, rate performance and cycle performance of lithium-rich manganese-based cathode materials are improved.
Smart Images

Figure BDA0004933884190000121
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of batteries, and relates to a coated and modified lithium-rich manganese-based precursor, and a preparation method and application thereof. Background Art
[0002] At present, lithium-ion batteries have been widely used in the fields of electronic products and electric vehicles. People have put forward higher requirements on the performance of lithium-ion batteries, such as higher initial coulombic efficiency, higher reversible discharge capacity and good cycle performance.
[0003] The surface lattice of lithium-rich manganese-based materials consumes lithium ions by reacting with the electrolyte during the anion redox process, resulting in the formation of a positive electrode electrolyte interface (CEI). In addition, due to the reduction of oxygen coordination, transition metal ions will migrate to adjacent lithium ion sites, hindering the reinsertion of lithium ions, causing a phase transition from a layered structure to a spinel structure, resulting in capacity loss. In order to improve the initial coulombic efficiency and reversible discharge capacity, researchers usually use metal oxides, fluorides and phosphides as coating layers to coat lithium-rich manganese-based positive electrode materials to protect the oxygen network structure on the surface of the lithium-rich manganese-based positive electrode, thereby alleviating side reactions between the electrode and the electrolyte.
[0004] CN103441252B discloses a method for preparing a lithium-rich manganese-based positive electrode material for a lithium-ion battery coated with a nano-oxide, comprising: (1) preparing a lithium-rich manganese-based positive electrode material [Li 1+(1-2x) / 3 Mn (2-x) / 3 M x ]O2; (2) weighing the nano metal oxide and the prepared lithium-rich manganese-based positive electrode material [Li 1+(1-2x) / 3 Mn (2-x) / 3 M x ]O2, and mix the two evenly; (3) after drying the above mixture, heat it to 400℃~1000℃ at a rate of 0.1~10℃ / min, keep the temperature constant for 2h~20h, then cool it to room temperature at a rate of 0.1℃ / min~10℃ / min, grind it, and obtain nano metal oxide coated lithium-rich manganese-based positive electrode material.
[0005] CN116741963A discloses a method for preparing a lithium-rich manganese-based positive electrode material coated with a metal fluoride, which is specifically implemented in the following steps: step 1, preparing a lithium-rich manganese-based positive electrode material; step 2, adding a certain amount of nickel source and fluorine source to anhydrous ethanol, heating and stirring until dissolved, slowly adding the lithium-rich manganese-based positive electrode material obtained in step 1, continuing heating and stirring, and placing in a drying oven to dry; step 3, grinding the material obtained in step 2 and spreading it flat in a corundum boat, annealing in a protective gas atmosphere, and then obtaining a lithium-rich manganese-based positive electrode material coated with a metal fluoride.
[0006] CN104319390A discloses a lithium-rich manganese-based material, the general formula of which is: xLi2MnO3·(1-x)Li(Ni 0.6 Mn 0.2 Co 0.2 )O2, wherein 0.9≤x≤1.5, the mixed metal oxide is a mixture of two metal oxides, wherein the molar number of one metal oxide is 5% to 20% of the molar number of the other metal oxide, and the mixed metal oxide is selected from two oxides of Mg, Ti, V, Mn or Al. The preparation method of the lithium-rich manganese-based material comprises the following steps: Step 1: According to the lithium-rich manganese-based solid solution positive electrode material xLi2MnO3·(1-x)Li(Ni 0.6 Mn 0.2 Co 0.2 )O2 components are mixed in a solvent according to a stoichiometric ratio of lithium source, manganese source, nickel source and cobalt source raw materials, and stirred and wet-milled to obtain a slurry, wherein 0.9≤x≤1.5); step 2: after the slurry in step 1 is mixed evenly by stirring and ball-milling, a sand mill is used for ultra-fine grinding to make the slurry mixed evenly, and the particle size D50 in the slurry is made to be below 500nm to form a suspension; step 3: after the suspension in step 2 is deironed, spray granulation is performed to obtain a lithium-rich manganese-based precursor; step 4: the lithium-rich manganese-based precursor in step 3 is The mixture is kept at 250°C to 400°C for 2h to 4h, and then sintered at 850°C to 950°C for 8h to 14h to obtain a preliminary lithium-rich manganese-based material; Step 5: Pour the preliminary lithium-rich manganese-based material sintered in step 4 into a reactor, add a solvent and a mixed metal oxide coating agent, stir for 1h to 3h, transfer the slurry to a double cone dryer to remove the solvent, and finally subject the powder to a secondary sintering at 400°C to 500°C for 3h to 6h to finally obtain a lithium-rich manganese-based material modified by a mixed metal oxide coating.
[0007] However, since the protective layer coated by conventional liquid phase or solid phase methods is not tightly bonded to the base material, in the actual charge and discharge cycle, the coating layer may experience adverse phenomena such as peeling, particle cracking, and grain boundary lithium ion aggregation, resulting in the initial coulombic efficiency of most modified materials still being lower than 85%, and it is impossible to take into account high initial coulombic efficiency, rate performance and excellent cycle performance.
[0008] Therefore, it is necessary to provide an improvement strategy for lithium-rich manganese-based positive electrode materials so that they have high initial coulombic efficiency, rate performance and excellent cycle performance. Summary of the invention
[0009] In view of the above problems existing in the prior art, the purpose of the present invention is to provide a coated and modified lithium-rich manganese-based precursor and a preparation method and application thereof.
[0010] To achieve the above object, the present invention adopts the following technical solutions:
[0011] In a first aspect, the present invention provides a coated and modified lithium-rich manganese-based precursor. The coated and modified lithium-rich manganese-based precursor includes a lithium-rich manganese-based precursor core and a coating layer coated on the surface of the lithium-rich manganese-based precursor core. The coating layer includes Na x MO2, where 0 < x < 1 and M is a metal different from Na.
[0012] The present invention uses the P2-type sodium ion cathode material Na x MO2 to coat the lithium-rich manganese-based precursor. There are Na + vacancies in this material, and the stable ion diffusion path is composed of continuous prismatic sites with lower diffusion energy barriers. Therefore, the lithium-rich manganese-based precursor coated with it has higher rate performance; in addition, due to the existence of Na + vacancies, during the initial discharge process, additional lithium ions can be reinserted into the Na x MO2 structure. Therefore, the P2-type Na x MO2 usually exhibits a Coulomb efficiency higher than 100%. Coating and modifying the lithium-rich manganese-based precursor with P2-type NaxMO2, these vacancies can serve as spare sites to offset the loss of lithium ions during the first charge and discharge process, thereby improving the cycle stability of the lithium-rich manganese-based material. Therefore, the lithium-rich manganese-based cathode material made of the coated and modified lithium-rich manganese-based precursor of the present invention has high initial Coulomb efficiency, rate performance, and excellent cycle performance.
[0013] The following are the preferred technical solutions of the present invention, but do not limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.
[0014] Preferably, M is selected from at least one of Mn, Zn, Co, Fe, Cu, and Zn.
[0015] Preferably, the lithium-rich manganese-based precursor core is a nickel-manganese precursor.
[0016] Preferably, the particle size D50 of the lithium-rich manganese-based precursor core is 2 μm to 10 μm, and can be, for example, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm, 7.5 μm, 8 μm, 8.5 μm, 9 μm, or 10 μm, etc.
[0017] Preferably, the mass of the coating layer accounts for 2% to 20% of the mass of the lithium-rich manganese-based precursor core, for example, it can be 2%, 3%, 4%, 6%, 8%, 10%, 12%, 13%, 14%, 15%, 16%, 18% or 20%, etc.
[0018] In a second aspect, the present invention provides a method for preparing a coated and modified lithium-rich manganese-based precursor as described in the first aspect, the preparation method comprising the following steps:
[0019] (1) mixing M salt, sodium salt, lithium-rich manganese-based precursor and solvent to prepare a coating solution;
[0020] (2) The coating solution is sprayed and pyrolyzed to obtain a coated and modified lithium-rich manganese-based precursor.
[0021] The present invention utilizes a spray pyrolysis method to coat and modify a lithium-rich manganese-based precursor, the preparation conditions are relatively simple, the interface structure stability between the coating layer and the base material is good, the elements in the product components are evenly distributed, and the stoichiometric ratio is accurate.
[0022] The present invention prepares a coated and modified lithium-rich manganese-based precursor by spray pyrolysis in the precursor stage, realizes uniform and seamless filling and coating of the surface layer, thereby constructing a tighter and more stable interface, creating a more efficient lithium ion transmission channel and more sites, and can realize in-situ composite of the coating layer and the primary particles of the lithium-rich manganese-based precursor core under the premise of ensuring the integrity of the secondary sphere, overcoming the problem that the gaps between the primary particles cannot be filled in the ordinary liquid phase method or solid phase method, thereby effectively improving the electrochemical performance of the lithium-rich manganese-based positive electrode material prepared by using the precursor.
[0023] Preferably, the M salt in step (1) comprises at least one of chloride, nitrate and sulfate.
[0024] By way of example but not limitation, M is the Ni element, and the nickel salt includes at least one of nickel chloride, nickel nitrate and nickel sulfate; or, M is the Mn element, and the manganese salt includes at least one of manganese chloride, manganese nitrate and manganese sulfate.
[0025] Preferably, the total mass of the M salt and the sodium salt is 1% to 8% of the mass of the lithium-rich manganese-based precursor, for example, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5% or 8%, etc.
[0026] Preferably, the mixing method in step (1) is: dissolving the M salt and the sodium salt in a solvent to obtain a first solution, and mixing the first solution with a lithium-rich manganese-based precursor to obtain a coating solution;
[0027] Preferably, the concentration of the first solution is 0.2 g / L to 2 g / L, for example, it can be 0.2 g / L, 0.4 g / L, 0.5 g / L, 0.7 g / L, 0.8 g / L, 1 g / L, 1.2 g / L, 1.3 g / L, 1.4 g / L, 1.5 g / L, 1.6 g / L, 1.7 g / L, 1.8 g / L or 2 g / L, etc.
[0028] Preferably, the temperature of the spray pyrolysis in step (2) is 600°C to 900°C, for example, it can be 600°C, 650°C, 700°C, 750°C, 800°C, 850°C or 900°C.
[0029] Preferably, the time of the spray pyrolysis in step (2) is 1 s to 30 s, for example, it can be 1 s, 3 s, 5 s, 6 s, 8 s, 10 s, 12 s, 15 s, 17 s, 18 s, 20 s, 22 s, 24 s, 26 s, 28 s or 30 s.
[0030] Preferably, the method for preparing the lithium-rich manganese-based precursor in step (1) comprises:
[0031] (a) mixing a nickel source, a manganese source and a solvent to prepare a mixed salt solution;
[0032] (b) Under a protective gas atmosphere, the mixed salt solution, the alkaline solution and the complexing agent solution are added into a reaction kettle to carry out a coprecipitation reaction to obtain a lithium-rich manganese-based precursor.
[0033] The present invention does not limit the other types of protection, which may be at least one of an inert gas or nitrogen.
[0034] Preferably, the concentration of the mixed salt solution in step (a) is 1 mol / L to 5 mol / L, for example, it can be 1 mol / L, 1.2 mol / L, 1.5 mol / L, 1.8 mol / L, 2 mol / L, 2.3 mol / L, 2.6 mol / L, 2.8 mol / L, 3 mol / L, 3.2 mol / L, 3.4 mol / L, 3.6 mol / L, 3.8 mol / L, 4 mol / L, 4.3 mol / L, 4.5 mol / L, 4.7 mol / L or 5 mol / L, etc.
[0035] Preferably, the temperature of the coprecipitation reaction in step (b) is 40°C to 80°C, for example, 40°C, 42°C, 45°C, 47°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C or 80°C, etc.
[0036] Preferably, during the coprecipitation reaction in step (b), the pH value is 8 to 12, for example, 8, 8.2, 8.5, 8.8, 9, 9.5, 10, 10.5, 11, 11.5 or 12.
[0037] In a third aspect, the present invention provides a lithium-rich manganese-based positive electrode material, wherein the lithium-rich manganese-based positive electrode material is prepared by using the coated and modified lithium-rich manganese-based precursor described in the first aspect.
[0038] In a fourth aspect, the present invention provides a method for preparing the lithium-rich manganese-based positive electrode material as described in the third aspect, the preparation method comprising the following steps:
[0039] The coated and modified lithium-rich manganese-based precursor is mixed with a lithium source and then calcined to obtain the lithium-rich manganese-based positive electrode material.
[0040] In a fifth aspect, the present invention provides a lithium-ion battery, wherein the lithium-ion battery comprises the lithium-rich manganese-based positive electrode material described in the fourth aspect.
[0041] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0042] Compared with the prior art, the present invention has the following beneficial effects:
[0043] (1) The present invention adopts P2 type sodium ion positive electrode material Na x MO2 is used to coat the lithium-rich manganese-based precursor. The material contains Na + Vacancies, in which the stable ion diffusion path is composed of continuous prismatic sites with low diffusion energy barriers, so the lithium-rich manganese-based precursor coated with it has higher rate performance; in addition, due to the Na + The presence of vacancies allows additional lithium ions to be reinserted into the Na x In the MO2 structure, therefore, the P2 type Na x MO2 usually exhibits a Coulombic efficiency greater than 100%. x MO2 coated modified lithium-rich manganese-based precursor, these vacancies as spare sites can offset the loss of lithium ions during the first charge and discharge process, thereby improving the cycle stability of the lithium-rich manganese-based material. Therefore, the lithium-rich manganese-based positive electrode material made by the coated modified lithium-rich manganese-based precursor of the present invention has high initial coulombic efficiency, rate performance and excellent cycle performance.
[0044] (2) The present invention utilizes a spray pyrolysis method to coat and modify the lithium-rich manganese-based precursor. The preparation conditions are relatively simple, and the interface structure between the coating layer and the base material is stable. The elements in the product components are evenly distributed and the stoichiometric ratio is accurate.
[0045] (3) The present invention prepares the coated and modified lithium-rich manganese-based precursor by spray pyrolysis in the precursor stage, which realizes uniform and seamless filling and coating of the surface layer, thereby constructing a tighter and more stable interface, creating a more efficient lithium ion transmission channel and more sites, and can realize in-situ composite of the coating layer and the primary particles of the lithium-rich manganese-based precursor core under the premise of ensuring the integrity of the secondary sphere, overcoming the problem that the gaps between the primary particles cannot be filled in the ordinary liquid phase method or solid phase method, thereby effectively improving the electrochemical performance of the lithium-rich manganese-based positive electrode material prepared by using the precursor. DETAILED DESCRIPTION
[0046] The technical solution of the present invention is further illustrated below through specific implementation methods.
[0047] In the preparation method of the embodiment of the present invention, step 4 is Ni 0.6 Mn 0.4 (OH)2 is used as an example to prepare the lithium-rich manganese-based precursor, but it is not limited to the substances of this chemical formula and does not constitute a limitation of the present invention. Other lithium-rich manganese-based precursors commonly used in the art are also suitable for the present invention.
[0048] Example 1
[0049] This embodiment provides a coated modified lithium-rich manganese-based precursor, comprising a lithium-rich manganese-based precursor core (particle size D50 is 8 μm) and a coating layer coated on the surface of the lithium-rich manganese-based precursor core, wherein the coating layer includes Na 0.66 MnO2, the mass of the coating layer accounts for 10% of the mass of the lithium-rich manganese-based precursor core.
[0050] This embodiment also provides a method for preparing the above-mentioned coated modified lithium-rich manganese-based precursor, comprising the following steps:
[0051] Phase 1: Co-precipitation synthesis of lithium-rich manganese-based precursors
[0052] Step 1, fully mixing nickel chloride and manganese chloride in a molar ratio of Ni:Mn of 0.6:0.4 to prepare a mixed salt solution with a concentration of 2 mol / L for standby use;
[0053] Step 2, in an inert gas atmosphere, the mixed salt solution, alkaline solution and ammonia water described in step 1 are respectively added to the reactor through a metering pump, and a coprecipitation reaction is carried out under the conditions of 60° C. and pH=10. When the particle size D50 of the particles in the reactor reaches the required size, the reaction is stopped, and the materials in the reactor are transferred to an aging tank for aging;
[0054] Step 3, washing the aged material with liquid alkali and water twice and then drying to obtain a lithium-rich manganese-based precursor;
[0055] The second stage: spray pyrolysis surface coating of lithium-rich manganese-based precursor
[0056] Step 4, preparing a first solution with a concentration of 1 g / L by mixing manganese acetate and sodium acetate according to a stoichiometric ratio;
[0057] Step 5, according to the solute in the first solution accounting for 5% of the mass ratio of the lithium-rich manganese-based precursor, the first solution and the lithium-rich manganese-based precursor are mixed to obtain a coating solution;
[0058] Step 6, spray pyrolysis the coating solution at 700° C. for 10 seconds to obtain a coated and modified lithium-rich manganese-based precursor.
[0059] Example 2
[0060] This embodiment provides a coated modified lithium-rich manganese-based precursor, comprising a lithium-rich manganese-based precursor core (particle size D50 is 5 μm) and a coating layer coated on the surface of the lithium-rich manganese-based precursor core, wherein the coating layer includes Na 0.66 FeO2, the mass of the coating layer accounts for 5% of the mass of the lithium-rich manganese-based precursor core.
[0061] This embodiment also provides a method for preparing the above-mentioned coated modified lithium-rich manganese-based precursor, comprising the following steps:
[0062] Phase 1: Co-precipitation synthesis of lithium-rich manganese-based precursors
[0063] Step 1, fully mixing nickel chloride and manganese chloride in a molar ratio of Ni:Mn of 0.6:0.4 to prepare a mixed salt solution with a concentration of 4 mol / L for standby use;
[0064] Step 2, in an inert gas atmosphere, the mixed salt solution, alkaline solution and ammonia water described in step 1 are respectively added to the reactor through a metering pump, and a coprecipitation reaction is carried out under the conditions of 80° C. and pH=9. When the particle size D50 of the particles in the reactor reaches the required size, the reaction is stopped, and the materials in the reactor are transferred to an aging tank for aging;
[0065] Step 3, washing the aged material with liquid alkali and water for 3 times and then drying to obtain a lithium-rich manganese-based precursor;
[0066] The second stage: spray pyrolysis surface coating of lithium-rich manganese-based precursor
[0067] Step 4, preparing a first solution with a concentration of 2 g / L by mixing ferrous chloride and sodium acetate according to a stoichiometric ratio;
[0068] Step 5, according to the solute in the first solution accounting for 2% of the mass ratio of the lithium-rich manganese-based precursor, the first solution and the lithium-rich manganese-based precursor are mixed to obtain a coating solution;
[0069] Step 6, spray pyrolysis the coating solution at 800° C. for 7 seconds to obtain a coated and modified lithium-rich manganese-based precursor.
[0070] Example 3
[0071] This embodiment provides a coated modified lithium-rich manganese-based precursor, comprising a lithium-rich manganese-based precursor core (particle size D50 is 10 μm) and a coating layer coated on the surface of the lithium-rich manganese-based precursor core, wherein the coating layer includes Na 0.66 MnO2, the mass of the coating layer accounts for 15% of the mass of the lithium-rich manganese-based precursor core.
[0072] This embodiment also provides a method for preparing the above-mentioned coated modified lithium-rich manganese-based precursor, comprising the following steps:
[0073] Phase 1: Co-precipitation synthesis of lithium-rich manganese-based precursors
[0074] Step 1, fully mixing nickel chloride and zinc chloride in a molar ratio of Ni:Mn of 0.6:0.4 to prepare a mixed salt solution with a concentration of 1 mol / L for standby use;
[0075] Step 2, in an inert gas atmosphere, the mixed salt solution, alkaline solution and ammonia water described in step 1 are respectively added to the reactor through a metering pump, and a coprecipitation reaction is carried out under the conditions of 45° C. and pH=11. When the particle size D50 of the particles in the reactor reaches the required size, the reaction is stopped, and the materials in the reactor are transferred to an aging tank for aging;
[0076] Step 3, washing the aged material with liquid alkali and water for 3 times and then drying to obtain a lithium-rich manganese-based precursor;
[0077] The second stage: spray pyrolysis surface coating of lithium-rich manganese-based precursor
[0078] Step 4, preparing a first solution with a concentration of 0.5 g / L by mixing manganese acetate and sodium acetate according to a stoichiometric ratio;
[0079] Step 5, according to the solute in the first solution accounting for 8% of the mass ratio of the lithium-rich manganese-based precursor, the first solution and the lithium-rich manganese-based precursor are mixed to obtain a coating solution;
[0080] Step 6, spray pyrolysis the coating solution at 600° C. for 30 seconds to obtain a coated and modified lithium-rich manganese-based precursor.
[0081] Example 4
[0082] The difference between this embodiment and embodiment 1 is that the mass ratio of the solute in the first solution to the lithium-rich manganese-based precursor in step 6 is adjusted so that the mass of the coating layer accounts for 1% of the mass of the core of the lithium-rich manganese-based precursor.
[0083] Example 5
[0084] The difference between this embodiment and embodiment 1 is that the mass ratio of the solute in the first solution to the lithium-rich manganese-based precursor in step 6 is adjusted so that the mass of the coating layer accounts for 22% of the mass of the lithium-rich manganese-based precursor core.
[0085] Comparative Example 1
[0086] The difference between this comparative example and Example 1 is that the second stage of spray pyrolysis surface coating is not performed.
[0087] Comparative Example 2
[0088] The difference between this comparative example and Example 1 is that the first solution is replaced with a 1 g / L aluminum chloride solution.
[0089] Comparative Example 3
[0090] The difference between this comparative example and Example 1 is that the first solution is replaced with a 1 g / L magnesium chloride solution.
[0091] Battery Assembly:
[0092] Prepare the positive electrode and assemble the battery:
[0093] The coated and modified lithium-rich manganese-based precursors of Examples 1-5 and Comparative Examples 1-3 were mixed with lithium hydroxide at a molar ratio of 1:1.03, and sintered at 800° C. for 10 hours to obtain a positive electrode material.
[0094] The positive electrode material, the binder polyvinylidene fluoride and the conductive agent Super P were added to N-methylpyrrolidone at a mass ratio of 97:1.5:1.5 and stirred to form a positive electrode slurry; the positive electrode slurry was then evenly coated on the positive electrode current collector aluminum foil, and the positive electrode sheet was obtained after drying and rolling;
[0095] Graphite, conductive agent acetylene black, thickener CMC and binder SBR are mixed in a mass ratio of 96:1:1.5:1.5, and deionized water is added as a solvent and stirred to obtain a negative electrode slurry; the negative electrode slurry is evenly coated on the negative electrode current collector copper foil, and the negative electrode sheet is obtained after drying, cold pressing and slitting;
[0096] Ethylene carbonate EC, ethyl methyl carbonate EMC, and diethyl carbonate DEC are mixed in a volume ratio of 1:1:1 to obtain a mixed solvent, and then fully dried lithium salt LiPF6 is dissolved in the mixed solvent to prepare an electrolyte with a concentration of 1 mol / L;
[0097] The positive electrode sheet, the separator and the negative electrode sheet are stacked in sequence, then wrapped with an aluminum-plastic film, and injected with an electrolyte after drying. After packaging, standing and forming, a lithium-ion battery is obtained; the separator is a PE porous film with a thickness of 11 μm, an air permeability of 280 s / 100 mL, and a porosity of 40%.
[0098] After the battery is assembled and aged for 12 hours, its performance is tested.
[0099] Performance Testing:
[0100] Initial Coulombic efficiency: The ratio of the first cycle discharge capacity to the charge capacity after 1C / 1C full charge.
[0101] Rate performance: The discharge capacity value obtained by fully charging and discharging at different predetermined rates.
[0102] Cycle performance: The test condition for the cycle capacity retention rate is the ratio of the discharge specific capacity to the initial specific capacity after 200 cycles of 1C / 1C.
[0103] See Table 1 for the results.
[0104] Table 1
[0105]
[0106] As can be seen from Table 1, the positive electrode material made from the coated and modified lithium-rich manganese-based precursor prepared in the embodiment of the present invention and applied to lithium-ion batteries can effectively improve the initial coulombic efficiency, rate performance and cycle performance of the battery.
[0107] At the same time, by comparing Example 1 with Examples 4-5, it can be seen that the coating layer is too thin and cannot provide sufficient lithium insertion sites and buffers, and the lithium-rich manganese-based bulk material cannot maintain a stable structure, resulting in poor rate performance and deteriorated cycle stability; while the coating layer is too thick, the proportion of high-capacity bulk material is reduced, and the material capacity is greatly reduced.
[0108] By comparing Example 1 with Comparative Example 1, it can be seen that the energy barrier for lithium ion diffusion in the lithium-rich manganese-based material without a coating layer is relatively high, and the rate performance is limited; and the unstable manganese is exposed, which also affects the cycle stability.
[0109] By comparing Example 1 with Comparative Examples 2-3, it can be seen that when aluminum oxide or magnesium oxide is used for coating, elements such as aluminum or magnesium cannot produce a synergistic effect with the nickel-manganese body, and may even accelerate the structural transformation, and the aluminum-magnesium coating layer cannot exert sufficient capacity, so it has no improvement effect on the cycle and rate of the material.
[0110] The applicant declares that the present invention illustrates the detailed method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed method, that is, it does not mean that the present invention must rely on the above-mentioned detailed method to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A coated and modified lithium-rich manganese-based precursor, It is characterized in that The coated and modified lithium-rich manganese-based precursor includes a lithium-rich manganese-based precursor core and a coating layer coated on the surface of the lithium-rich manganese-based precursor core, and the coating layer includes Na x MO 2 , where 0 < x < 1, and M is a metal different from Na.
2. The coated modified lithium-rich manganese-based precursor according to claim 1, It is characterized in that M is selected from at least one of Mn, Zn, Co, Fe, Cu and Zn; preferably, the particle size D50 of the core of the lithium-rich manganese-based precursor is 2 μm to 10 μm; Preferably, the mass of the coating layer accounts for 2% to 20% of the mass of the lithium-rich manganese-based precursor core.
3. A method for preparing a coated and modified lithium-rich manganese-based precursor as claimed in claim 1 or 2, It is characterized in that The preparation method comprises the following steps: (1) mixing M salt, sodium salt, lithium-rich manganese-based precursor and solvent to prepare a coating solution; (2) The coating solution is sprayed and pyrolyzed to obtain a coated and modified lithium-rich manganese-based precursor.
4. The preparation method according to claim 3, It is characterized in that The M salt in step (1) includes at least one of chloride, nitrate and sulfate; Preferably, the total mass of the M salt and the sodium salt accounts for 1% to 8% of the mass of the lithium-rich manganese-based precursor; Preferably, the mixing method in step (1) is: dissolving the M salt and the sodium salt in a solvent to obtain a first solution, and mixing the first solution with a lithium-rich manganese-based precursor to obtain a coating solution; Preferably, the concentration of the first solution is 0.2 g / L to 2 g / L.
5. The preparation method according to claim 3 or 4, It is characterized in that The temperature of the spray pyrolysis in step (2) is 600° C. to 900° C.; Preferably, the spray pyrolysis time in step (2) is 1 s to 30 s.
6. The preparation method according to any one of claims 3 to 5, It is characterized in that The method for preparing the lithium-rich manganese-based precursor in step (1) comprises: (a) mixing a nickel source, a manganese source and a solvent to prepare a mixed salt solution; (b) Under a protective gas atmosphere, the mixed salt solution, the alkaline solution and the complexing agent solution are added into a reaction kettle to carry out a coprecipitation reaction to obtain a lithium-rich manganese-based precursor.
7. The preparation method according to claim 6, It is characterized in that The concentration of the mixed salt solution in step (a) is 1 mol / L to 5 mol / L; Preferably, the temperature of the coprecipitation reaction in step (b) is 40°C to 80°C; Preferably, during the coprecipitation reaction in step (b), the pH value is 8-12.
8. A lithium-rich manganese-based positive electrode material, It is characterized in that The lithium-rich manganese-based positive electrode material is prepared by using the coated and modified lithium-rich manganese-based precursor according to claim 1 or 2.
9. A method for preparing the lithium-rich manganese-based positive electrode material as claimed in claim 8, It is characterized in that The preparation method comprises the following steps: The coated and modified lithium-rich manganese-based precursor is mixed with a lithium source and then calcined to obtain the lithium-rich manganese-based positive electrode material.
10. A lithium ion battery, It is characterized in that The lithium-ion battery comprises the lithium-rich manganese-based positive electrode material according to claim 8.