Lithium supplement additive for battery positive electrode, preparation method of lithium supplement additive and battery

By using a nickel-copper precursor and mixed lithium salt sintering method in the preparation of lithium-ion battery positive electrode lithium supplement additives, a polycrystalline structure is formed, which solves the problems of complex process, high cost and low irreversible capacity in the prior art, and realizes the problem of High-performance and low-cost lithium-ion battery positive lithium supplement additive.

CN118877951APending Publication Date: 2024-11-01HEFEI GUOXUAN HIGH TECH POWER ENERGY

Patent Information

Application Number
CN202410899016.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The preparation process of existing lithium-ion battery positive lithium supplement material is complex, has high cost and low irreversible capacity, which has problems of environmental pollution and resource loss.

Method used

Using alkali liquid and ammonia water as the base liquid, the co-precipitation reaction of the nickel-copper precursor is carried out under the protection of inert gas, and then presintered under the protection of inert gas to prepare the positive electrode lithium supplement additive for lithium-ion batteries. By adjusting the doping amount of copper and sintering conditions, a polycrystalline structure is formed to improve material performance.

Benefits of technology

It significantly improves the irreversible capacity of lithium-ion battery positive electrode lithium supplement additive, reduces the first charging efficiency, simplifies the process flow, reduces costs, and facilitates industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004929957160000071
    Figure BDA0004929957160000071
  • Figure BDA0004929957160000081
    Figure BDA0004929957160000081
  • Figure HDA0004929957170000011
    Figure HDA0004929957170000011
Patent Text Reader

Abstract

The invention discloses a battery positive electrode lithium supplement additive, a preparation method thereof and a battery. The preparation method of the lithium ion battery positive electrode lithium supplement additive comprises the following steps: S1, taking alkali liquor and ammonia water as a base solution, respectively adding a mixed salt solution of nickel salt and copper salt into the base solution under the protection of inert gas, and carrying out a co-precipitation reaction on the alkali liquor and the ammonia water to obtain a nickel-copper precursor; s2, pre-sintering a lithium source in a vacuum environment to obtain a lithium precursor; and S3, under the protection of inert gas, mixing the nickel-copper precursor and the lithium precursor, and sintering to obtain the lithium supplement additive for the positive electrode of the lithium ion battery. The positive electrode lithium supplement additive is low in initial efficiency, high in irreversible capacity and better in material performance, the preparation method is simple and easy to control, the cost is low, and industrial production is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a battery positive electrode lithium supplement additive, a preparation method thereof, and a battery. Background Art

[0002] Lithium-ion batteries are widely used in various electronic products due to their high energy density and long cycle life. At the same time, with the rapid development of electric vehicles, drones and energy storage devices, higher requirements are placed on the capacity and power of batteries. However, during the first charging of lithium-ion batteries, part of the lithium released from the positive electrode will form an irreversible lithium-containing passivation film SEI on the surface of the negative electrode, resulting in the loss of active lithium and reducing the reversible capacity of the battery.

[0003] To address this problem, the most common improvement measure currently is to pre-replenish lithium to the positive or negative electrode of the battery. Compared with negative electrode lithium replenishment, positive electrode lithium replenishment does not require changes to the existing battery production process, and has the characteristics of low cost, simplification, and high safety. Positive electrode lithium replenishment generally involves mixing the lithium replenishment material with the positive electrode material in proportion, and using the mixed positive electrode material to prepare the battery cell. During the first charging process, the lithium replenisher releases excess lithium to make up for the lithium consumed by the formation of the SEI film on the negative electrode surface, thereby completing the lithium replenishment. Therefore, the positive electrode lithium replenisher needs to have the characteristics of low first efficiency and high irreversible capacity, so as to achieve a better lithium replenishment effect.

[0004] The existing methods for preparing positive electrode lithium replenisher materials have the problems of complex process, high cost, and the prepared positive electrode lithium replenisher materials have high initial effect and low irreversible capacity. For example, Chinese patent CN 110218078A discloses a lithium replenisher material Li2NiO2 and its preparation method and application. Its preparation process requires the use of acetone as a solvent and requires multiple sintering. The process is complicated and easily causes environmental pollution. The prepared positive electrode lithium replenisher material has a low irreversible capacity. Another example is the lithium replenisher additive for lithium ion batteries disclosed in Chinese patent CN113571781A, its preparation method and lithium ion battery. The patent first sintered a mixed lithium salt, and then used the mixed lithium salt to sinter and prepare the positive electrode lithium replenisher material, which also caused additional loss of resources, and the prepared positive electrode lithium replenisher material had a low irreversible capacity. Therefore, it is necessary to provide a positive electrode lithium replenisher additive that is simple to prepare, green, has low initial effect and high irreversible capacity. Summary of the invention

[0005] In view of this, the purpose of the present invention is to provide a battery positive electrode lithium supplement additive and a preparation method and a battery. The positive electrode lithium supplement additive has low initial efficiency, high irreversible capacity, better material performance, and the preparation method is simple and easy to control, low cost, and is conducive to industrial production.

[0006] In a first aspect, a method for preparing a lithium supplement additive for a lithium-ion battery cathode provided by the present invention includes the following steps:

[0007] S1. Using an alkali solution and ammonia water as the bottom solution, adding a mixed salt solution of nickel salt and copper salt, alkali solution and ammonia water to the bottom solution respectively under the protection of an inert gas for coprecipitation reaction to obtain a nickel-copper precursor;

[0008] S2. Pre-sintering a lithium source in a vacuum environment to obtain a lithium precursor;

[0009] S3. Mixing the nickel-copper precursor and the lithium precursor under the protection of an inert gas and then sintering to obtain the lithium supplement additive for the lithium-ion battery cathode.

[0010] Based on the above technical solutions, the total residual alkali of the lithium supplement additive for the lithium-ion battery cathode of the present invention is < 3%; maintaining a constant temperature of 25°C, a voltage range of 2.8 - 4.35V, charging at a constant current and constant voltage of 0.2C, testing the charging gram capacity of a CR2016 type button battery, calculating the irreversible capacity, the first charging gram capacity is 420 - 460 mAh / g, the first efficiency is 3% - 28%, and the irreversible capacity is 300 - 446 mAh / g. By introducing copper element into the precursor and adjusting the doping amount of copper, the present invention reduces the NiO impurity phase in Li2NiO2, improves the purity of the Immm phase, enables the material to form a polycrystalline-like structure during the sintering process, while increasing the charging gram capacity of Li2NiO2, significantly reducing its first efficiency, and thus significantly increasing the irreversible capacity of the material; this method significantly improves the performance of the Li2NiO2 material while reducing the cost of the material, reducing the number of sintering times, having a simple process, and being conducive to industrial production.

[0011] In the above method for preparing a lithium supplement additive for a lithium-ion battery cathode, the nickel salt is at least one of nickel acetate, nickel chloride, nickel nitrate, and nickel sulfate, preferably nickel sulfate;

[0012] The copper salt is at least one of copper chloride, copper sulfate, and copper nitrate, preferably copper sulfate;

[0013] The alkali solution is a sodium hydroxide solution.

[0014] In the above method for preparing a lithium supplement additive for a lithium-ion battery cathode, the molar ratio of nickel element in the nickel salt to copper element in the copper salt is (1 - x):x, where 0 < x < 1, x is preferably 0.1 - 0.5, more preferably 0.1 - 0.3, such as a molar ratio of 0.9:0.1, 0.8:0.2, or 0.7:0.3;

[0015] The total molar concentration of the mixed salt solution of the nickel salt and copper salt is 0.5 - 5 mol / L, such as 2 mol / L;

[0016] The molar concentration of the lye is 3 to 10 mol / L, such as 4 mol / L;

[0017] The molar concentration of the ammonia water is 0.5 to 5 mol / L, such as 1 mol / L.

[0018] In the preparation method of the above lithium-ion battery cathode lithium supplement additive, the pH value of the reaction system of the coprecipitation reaction is 10 to 13, such as 11.5;

[0019] The temperature of the coprecipitation reaction is 40 to 70 °C, such as 55 °C;

[0020] The inert gas is one or more of nitrogen, helium, neon, argon, krypton, and xenon. The gas purity > 99.99%, and the flow rate is 6 to 9 L / min, such as 9 L / min.

[0021] After the coprecipitation reaction in step S1, it further includes: performing solid-liquid separation on the reaction system, collecting the solid powder, and performing vacuum drying, such as drying at 120 °C for 12 h.

[0022] In the preparation method of the above lithium-ion battery cathode lithium supplement additive, the vacuum degree in the vacuum environment < 100 Pa, such as 90 Pa;

[0023] The conditions for the pre-sintering are as follows: heating to 400 to 1100 °C at a rate of 1 to 10 °C / min, and holding for 10 to 600 min. For example, heating to 750 °C at a heating rate of 10 °C / min and holding for 240 min;

[0024] After the pre-sintering in step S2, it further includes: crushing the pre-sintered product, such as using a high-speed mixing crusher for crushing;

[0025] The lithium source is composed of a first lithium source, a second lithium source, and a third lithium source. The first lithium source is at least one of lithium hydroxide and lithium hydride. The second lithium source is at least one of lithium oxide and lithium peroxide. The third lithium source is at least one of lithium carbonate, lithium oxalate, lithium acetate, and lithium citrate; Preferably, the chemical formula of the lithium precursor is mLiOH·nLi2O·pLi2CO3·wH2O), where m, n, and p are mass fractions, 0 < m < 0.5, 0.5 ≤ n < 1.0, 0 < p < 0.5, m + n + p = 1, and w represents the water of crystallization content, 0 ≤ w ≤ 1;

[0026] The molar ratio of the metal element in the nickel-copper precursor to the lithium element in the lithium source precursor is 1:(1.8 to 2.4), such as 1:1.92.

[0027] In the preparation method of the above-mentioned lithium-ion battery cathode lithium supplement additive, the sintering conditions are as follows: heating to 600-900°C at a rate of 2-5°C / min, and holding for 8-15h. For example, heating to 720°C at a rate of 2°C / min and holding for 12h;

[0028] The sintered product is crushed and sieved. The mesh number of the sieve used for sieving is 300-400 meshes, and the particle size D50 is 5.0-9.0um;

[0029] The lithium-ion battery cathode lithium supplement additive is a polycrystalline-like material.

[0030] In the second aspect, the present invention provides a lithium-ion battery cathode lithium supplement additive obtained by the preparation method described in any one of the above, and the lithium supplement additive includes Li2Ni (1-x) Cu x O2, where 0 < x < 1, hereinafter simply referred to as LNCO.

[0031] In the third aspect, the present invention provides a lithium-ion battery cathode material, which includes a high-nickel cathode material and the above-mentioned lithium-ion battery cathode lithium supplement additive.

[0032] In the above-mentioned lithium-ion battery cathode material, the high-nickel cathode material is LiNi x’ Co y M (1-x’-y) O2, where 0.65 ≤ x ’ <1, 0 < y ≤ 0.2, (x ’ +y) < 1, and M is one or more of Al, Mn, Mg, such as Li(Ni 0.88 Co 0.095 Mn 0.025 )O2;

[0033] The mass of the lithium-ion battery cathode lithium supplement additive is 0.5% - 5% of the lithium-ion battery cathode material, such as 2%.

[0034] In the fourth aspect, the present invention provides a lithium-ion battery, which includes a positive electrode plate, a negative electrode plate, a separator, and an electrolyte. The positive electrode plate includes a current collector and the above-mentioned lithium-ion battery cathode material provided on the current collector.

[0035] The present invention has the following beneficial effects:

[0036] Compared with the prior art, the present invention uses a nickel-copper precursor as the nickel source, including mixing, sintering, and crushing. The total residual alkali of the obtained LNCO is < 3%, the first charge specific capacity is 420 - 460 mAh / g, the first efficiency is 3% - 28%, and the irreversible capacity is 300 - 446 mAh / g. The material performance is better, and the preparation method is simple and easy to control, with low cost, which is beneficial to industrial production. Description of the Drawings

[0037] Figure 1 These are SEM images of the lithium-ion battery positive electrode lithium replenishing additive LNCO prepared in Example 2 and the lithium-ion battery positive electrode lithium replenishing additive Li2NiO2 prepared in Comparative Example 1.

[0038] Figure 2 XRD diagrams of the lithium-ion battery positive electrode lithium replenishing additive LNCO prepared in Example 2 and the lithium-ion battery positive electrode lithium replenishing additive Li2NiO2 prepared in Comparative Example 1.

[0039] Figure 3 This is a charge and discharge curve diagram of the lithium-ion battery positive electrode lithium supplement additive LNCO prepared in Example 2. DETAILED DESCRIPTION

[0040] The present invention is further described in detail below in conjunction with specific embodiments, and the examples provided are only for illustrating the present invention, rather than for limiting the scope of the present invention. The examples provided below can be used as a guide for further improvements by those of ordinary skill in the art, and do not constitute a limitation of the present invention in any way.

[0041] The methods used in the following examples, unless otherwise specified, are all conventional methods, carried out according to the techniques or conditions described in the literature in the art or according to the product instructions. The materials, reagents, etc. used in the following examples, unless otherwise specified, can all be obtained from commercial sources.

[0042] Example 1: Preparation of positive electrode lithium supplement additive

[0043] Nickel sulfate and copper sulfate are mixed according to the molar ratio of metal elements of 0.9:0.1 to prepare a mixed salt solution with a total concentration of 2 mol / L; an appropriate amount of NaOH solution and ammonia water are added to the reactor as the base liquid, wherein the concentration of NaOH solution is 4 mol / L and the concentration of ammonia water is 1 mol / L. The mixed salt solution, 4 mol / L NaOH solution and 1 mol / L ammonia water are continuously added in parallel by a flow pump to cause a chemical reaction. The pH value of the system is adjusted to 11.5 by adjusting the flow rate of NaOH solution and ammonia water, and the system is heated to a constant temperature of 55°C. N2 is used as a protective atmosphere throughout the process, and the purity of nitrogen is >99.99% and the flow rate is 9L / min. After the feeding is completed, the material is aged for 12 hours, and the material is taken out from the discharge port, filtered, and the solid is repeatedly washed and dried in a vacuum oven at 120°C for 12 hours.

[0044] Lithium hydroxide, lithium oxide and lithium carbonate are mixed in a ratio of 8:1:1, and the temperature is raised to 750°C at a rate of 10°C / min in a vacuum environment with a vacuum degree of 90 Pa. The mixture is kept warm for 240 min, cooled to room temperature while maintaining vacuum, taken out and crushed using a high-speed mixing crusher to obtain a mixed lithium salt. The composition of the mixed lithium salt is refined and quantitatively analyzed after XRD testing.

[0045] Finally, the dried precursor was weighed and the mass of the required lithium source was calculated. The precursor and the mixed lithium salt were fully mixed in a N2 atmosphere according to a metal element molar ratio of 1:1.92, transferred to a tubular furnace for sintering, heated to 720°C at 2°C / min, kept warm for 12 hours, and cooled naturally. After the material was crushed with a stone mortar mill, it was sieved once with a 300-mesh sieve to obtain LNCO, a lithium-ion battery positive electrode lithium supplement additive.

[0046] Example 2: Preparation of positive electrode lithium supplement additive

[0047] Nickel sulfate and copper sulfate are mixed according to the molar ratio of metal elements of 0.8:0.2 to prepare a mixed salt solution with a total concentration of 2 mol / L; an appropriate amount of NaOH solution and ammonia water are added to the reactor as the base liquid, wherein the concentration of NaOH solution is 4 mol / L and the concentration of ammonia water is 1 mol / L. The mixed salt solution, 4 mol / L NaOH solution and 1 mol / L ammonia water are continuously added in parallel by a flow pump to cause a chemical reaction. The pH value of the system is adjusted to 11.5 by adjusting the flow rate of NaOH solution and ammonia water, and heated to a constant temperature of 55°C. N2 is used as a protective atmosphere throughout the process, and the purity of nitrogen is >99.99% and the flow rate is 9L / min. After the feeding is completed, the material is aged for 12 hours, and the material is taken out from the discharge port, filtered, and the solid is repeatedly washed and dried in a vacuum oven at 120°C for 12 hours.

[0048] Finally, the dried precursor was weighed and the mass of the required lithium source was calculated. The precursor and the mixed lithium salt prepared in Example 1 were fully mixed in a N2 atmosphere at a metal element molar ratio of 1:1.92, transferred to a tubular furnace for sintering, heated to 720°C at 2°C / min, kept warm for 12 hours, and cooled naturally. After the material was crushed with a stone mortar mill, it was sieved once with a 300-mesh sieve to obtain LNCO, a lithium-ion battery positive electrode lithium supplement additive.

[0049] Example 3: Preparation of positive electrode lithium supplement additive

[0050] Nickel sulfate and copper sulfate are mixed according to the molar ratio of metal elements of 0.7:0.3 to prepare a mixed salt solution with a total concentration of 2 mol / L; an appropriate amount of NaOH solution and ammonia water are added to the reactor as the base liquid, wherein the concentration of NaOH solution is 4 mol / L and the concentration of ammonia water is 1 mol / L. The mixed salt solution, 4 mol / L NaOH solution and 1 mol / L ammonia water are continuously added in parallel by a flow pump to cause a chemical reaction. The pH value of the system is adjusted to 11.5 by adjusting the flow rate of NaOH solution and ammonia water, and heated to a constant temperature of 55°C. N2 is used as a protective atmosphere throughout the process, and the purity of nitrogen is >99.99% and the flow rate is 9L / min. After the feeding is completed, the material is aged for 12 hours, and the material is taken out from the discharge port, filtered, and the solid is repeatedly washed and dried in a vacuum oven at 120°C for 12 hours.

[0051] Finally, the dried precursor was weighed and the mass of the required lithium source was calculated. The precursor and the mixed lithium salt prepared in Example 1 were fully mixed in a N2 atmosphere at a metal element molar ratio of 1:1.92, transferred to a tubular furnace for sintering, heated to 720°C at 2°C / min, kept warm for 12 hours, and cooled naturally. After the material was crushed with a stone mortar mill, it was sieved once with a 300-mesh sieve to obtain LNCO, a lithium-ion battery positive electrode lithium supplement additive.

[0052] Example 4: Preparation of positive electrode lithium supplement additive

[0053] Nickel sulfate and copper sulfate are mixed according to the metal element molar ratio of 0.6:0.4 to prepare a mixed salt solution with a total concentration of 2 mol / L; an appropriate amount of NaOH solution and ammonia water are added to the reactor as the base liquid, wherein the concentration of NaOH solution is 4 mol / L and the concentration of ammonia water is 1 mol / L. The mixed salt solution, 4 mol / L NaOH solution and 1 mol / L ammonia water are continuously added in parallel by a flow pump to cause a chemical reaction. The pH value of the system is adjusted to 11.5 by adjusting the flow rate of NaOH solution and ammonia water, and heated to a constant temperature of 55°C. N2 is used as a protective atmosphere throughout the process, and the purity of nitrogen is >99.99% and the flow rate is 9L / min. After the feeding is completed, the material is aged for 12 hours, and the material is taken out from the discharge port, filtered, and the solid is repeatedly washed and dried in a vacuum oven at 120°C for 12 hours.

[0054] Finally, the dried precursor was weighed and the mass of the required lithium source was calculated. The precursor and the mixed lithium salt prepared in Example 1 were fully mixed in a N2 atmosphere at a metal element molar ratio of 1:1.92, transferred to a tubular furnace for sintering, heated to 720°C at 2°C / min, kept warm for 12 hours, and cooled naturally. After the material was crushed with a stone mortar mill, it was sieved once with a 300-mesh sieve to obtain LNCO, a lithium-ion battery positive electrode lithium supplement additive.

[0055] Example 5: Preparation of positive electrode lithium supplement additive

[0056] Nickel sulfate and copper sulfate are mixed at a metal element molar ratio of 0.5:0.5 to prepare a mixed salt solution with a total concentration of 2 mol / L; an appropriate amount of NaOH solution and ammonia water are added to the reactor as the base liquid, wherein the concentration of the NaOH solution is 4 mol / L and the concentration of the ammonia water is 1 mol / L. The mixed salt solution, 4 mol / L NaOH solution and 1 mol / L ammonia water are continuously added in parallel by a flow pump to cause a chemical reaction. The pH value of the system is adjusted to 11.5 by adjusting the flow rate of the NaOH solution and the ammonia water, and the system is heated to a constant temperature of 55°C. N2 is used as a protective atmosphere throughout the process, and the nitrogen purity is >99.99% and the flow rate is 9L / min. After the feeding is completed, the material is aged for 12 hours, and the material is taken out from the discharge port, filtered, and the solid is repeatedly washed and dried in a vacuum oven at 120°C for 12 hours.

[0057] Finally, the dried precursor was weighed and the mass of the required lithium source was calculated. The precursor and the mixed lithium salt prepared in Example 1 were fully mixed in a N2 atmosphere at a metal element molar ratio of 1:1.92, transferred to a tubular furnace for sintering, heated to 720°C at 2°C / min, kept warm for 12 hours, and cooled naturally. After the material was crushed with a stone mortar mill, it was sieved once with a 300-mesh sieve to obtain LNCO, a lithium-ion battery positive electrode lithium supplement additive.

[0058] Comparative Example 1

[0059] Under N2 atmosphere, nickelous oxide and the mixed lithium salt prepared in Example 1 were fully mixed at a metal element molar ratio of 1:1.92, transferred into a tubular furnace for sintering, heated to 720°C at 2°C / min, kept warm for 12 hours, and cooled naturally. The material was crushed with a stone mortar mill and sieved once with a 300-mesh screen to obtain Li2NiO2, a lithium-ion battery positive electrode lithium supplement additive.

[0060] Figure 1 The following are SEM images of the lithium-ion battery positive electrode lithium supplement additives prepared in Example 2 and Comparative Example 1. Figure 1 It can be seen that the lithium-ion battery positive electrode lithium supplement additive LNCO prepared in Example 2 has a polycrystalline morphology and a particle size D50 of 5-9 um, while the Li2NiO2 prepared by the traditional method has a large single crystal morphology.

[0061] Figure 2 The XRD diagrams of the lithium-ion battery positive electrode lithium supplement additives prepared in Example 2 and Comparative Example 1 are shown in FIG. Figure 2 It can be seen that the NiO impurities in the lithium-ion battery positive electrode lithium supplement additive LNCO prepared in Example 2 are effectively eliminated, which is beneficial to improving the gram capacity and stability of the material.

[0062] Comparative Example 2

[0063] Under N2 atmosphere, nickelous oxide, CuO and the mixed lithium salt prepared in Example 1 were fully mixed according to the metal element molar ratio of 0.9:0.1:1.92, transferred into a tube furnace for sintering, heated to 720°C at 2°C / min, kept warm for 12 hours, and cooled naturally. The material was crushed with a stone mortar mill and sieved once with a 300-mesh screen to obtain LNCO, a lithium-ion battery positive electrode lithium supplement additive.

[0064] Comparative Example 3

[0065] Under N2 atmosphere, nickelous oxide, CuO and the mixed lithium salt prepared in Example 1 were fully mixed according to the metal element molar ratio of 0.8:0.2:1.92, transferred into a tube furnace for sintering, heated to 720°C at 2°C / min, kept warm for 12 hours, and cooled naturally. The material was crushed with a stone mortar mill and sieved once with a 300-mesh screen to obtain LNCO, a lithium-ion battery positive electrode lithium supplement additive.

[0066] Comparative Example 4

[0067] Under N2 atmosphere, nickelous oxide, CuO and the mixed lithium salt prepared in Example 1 were fully mixed according to the metal element molar ratio of 0.7:0.3:1.92, transferred into a tube furnace for sintering, heated to 720°C at 2°C / min, kept warm for 12 hours, and cooled naturally. The material was crushed with a stone mortar mill and sieved once with a 300-mesh screen to obtain LNCO, a lithium-ion battery positive electrode lithium supplement additive.

[0068] Comparative Example 5

[0069] The lithium supplement additive for the positive electrode of a lithium-ion battery was prepared according to the steps in Example 2, except that lithium hydroxide, lithium oxide and lithium carbonate were mixed in a ratio of 8:1:1, and the steps of pre-sintering and crushing under a vacuum environment were omitted.

[0070] Example 6

[0071] The lithium-ion battery positive electrode lithium supplement additives prepared in the embodiments of the present invention and the comparative examples were used as positive electrodes to assemble CR2016 button batteries.

[0072] Li2NiO2 / LNCO, carbon black SuperP, and polyvinylidene fluoride (Solvey5130) were mixed in a mass ratio of 95:5:5, and N-methylpyrrolidone was used as a solvent to prepare a slurry with a mass fraction of 5%. The slurry was evenly coated on the surface of an aluminum foil and rolled to obtain a positive electrode sheet. Then, a lithium sheet was used as a negative electrode sheet, 1 mol / L lithium hexafluorophosphate ethylene carbonate (EC) and dimethyl carbonate (DMC) solution (the mass ratio of EC to DMC was 1:1) was used as an electrolyte, and cell gard2300 was used as a separator. The cells were assembled in a glove box to obtain a lithium-ion half-cell.

[0073] The electrochemical performance of the lithium-ion half-cell was tested using an electrochemical tester, with the test voltage range being 2.8 to 4.35 V and the test temperature being 25° C. The test results are shown in Table 1.

[0074] The charge and discharge curve of the lithium-ion battery positive electrode lithium supplement additive prepared in Example 2 is shown in Figure 3 .

[0075] Table 1 Data comparison between the embodiment and the comparative example

[0076]

[0077] From Table 1 and Figure 3 It can be seen that the lithium-ion battery positive electrode lithium supplement additive LNCO prepared according to the method of Example 2 has a lower first efficiency and a higher irreversible capacity. It can be seen from the comparison results of Examples 1-3 and Comparative Examples 2-4 in Table 1 that, compared with the direct use of nickelous oxide, CuO and mixed lithium salts in the comparative example and then sintered, the lithium supplement additive prepared by sintering the prepared nickel-copper precursor and mixed lithium salt in the present invention has a higher irreversible capacity and a lower first efficiency. Among them, the residual alkali content of the lithium supplement agent in Comparative Example 5 is very high, resulting in gelation when the positive electrode is slurried, and the test cannot be carried out normally. It can be seen from Examples 4-5 that when the copper content in the nickel-copper precursor is too high, the charging capacity of the positive electrode lithium supplement agent prepared therefrom will show a downward trend. And in the electrochemical performance test, it was found that the electrochemical performance test results of LNCO prepared by CuO doping were less consistent, which is related to the uneven CuO doping.

[0078] Example 7

[0079] High nickel cathode material Li(Ni 0.88 Co 0.095 Mn 0.025 )O2 is used as the positive electrode, and the lithium-ion battery positive electrode lithium supplement additive LNCO prepared in Example 2 of the present invention is added to the positive electrode material. The added amount of the lithium supplement additive is 2wt% of the mass of the positive electrode active material to prepare a composite positive electrode active material, and a CR2016 button battery is assembled.

[0080] The composite positive electrode active material, carbon black SuperP, and polyvinylidene fluoride (Solvey5130) were mixed in a mass ratio of 95:5:5, and N-methylpyrrolidone was used as a solvent to prepare a slurry with a mass fraction of 5%. The slurry was evenly coated on the surface of an aluminum foil and rolled to obtain a positive electrode sheet. Then, a lithium sheet was used as a negative electrode sheet, 1 mol / L lithium hexafluorophosphate ethylene carbonate (EC) and dimethyl carbonate (DMC) solution (the mass ratio of EC to DMC was 1:1) was used as an electrolyte, and cell gard2300 was used as a separator. The cells were assembled in a glove box to obtain a lithium-ion half-cell.

[0081] The electrochemical performance of the lithium-ion half-cell was tested using an electrochemical tester, with the test voltage range of 2.8 to 4.35 V and the test temperature of 25° C. The test results are shown in Table 2.

[0082] Comparative Example 6

[0083] High nickel cathode material Li(Ni 0.88 Co 0.095 Mn 0.025 )O2 was used as the positive electrode and a CR2016 button cell was assembled.

[0084] The positive electrode active material, carbon black SuperP, and polyvinylidene fluoride (Solvey5130) were mixed in a mass ratio of 95:5:5, and N-methylpyrrolidone was used as a solvent to prepare a slurry with a mass fraction of 5%, which was evenly coated on the surface of an aluminum foil and rolled to obtain a positive electrode sheet; then, a lithium sheet was used as a negative electrode sheet, 1 mol / L lithium hexafluorophosphate ethylene carbonate (EC) and dimethyl carbonate (DMC) solution (the mass ratio of EC to DMC was 1:1) was used as an electrolyte, and cell gard2300 was used as a separator, and they were assembled in a glove box to obtain a lithium ion half-cell.

[0085] The electrochemical performance of the lithium-ion half-cell was tested using an electrochemical tester, with the test voltage range of 2.8 to 4.35 V and the test temperature of 25° C. The test results are shown in Table 2.

[0086] Table 2 Comparison of data in the examples

[0087]

[0088] As can be seen from Table 2, the lithium-ion battery positive electrode lithium supplement additive LNCO prepared according to the method of Example 2 is applied to a lithium-ion half-cell with a high-nickel ternary as the positive electrode material. Compared with the lithium-ion half-cell to which the positive electrode lithium supplement additive LNCO is not added, the 0.2C charging capacity is significantly improved, while the initial efficiency is significantly reduced.

[0089] The present invention has been described in detail above. For those skilled in the art, without departing from the purpose and scope of the present invention, can implement the present invention in a wider range under equivalent parameters, concentrations and conditions. Although the present invention provides specific embodiments, it should be understood that the present invention can be further improved. In a word, according to the principle of the present invention, the application is intended to include any changes, uses or improvements to the present invention, including departing from the disclosed scope in the application and the changes made with conventional techniques known in the art.

Claims

1. A method for preparing a lithium-ion battery positive electrode lithium supplement additive, characterized in that: It includes the following steps: S1. Using an alkali solution and ammonia water as the bottom solution, under the protection of an inert gas, adding a mixed salt solution of nickel salt and copper salt, an alkali solution, and ammonia water to the bottom solution respectively for coprecipitation reaction to obtain a nickel-copper precursor; S2. Pre-sintering the lithium source in a vacuum environment to obtain a lithium precursor; S3. Under the protection of an inert gas, mixing the nickel-copper precursor and the lithium precursor and then sintering them to obtain the lithium-ion battery cathode lithium supplement additive.

2. The method for preparing the lithium-ion battery positive electrode lithium supplement additive according to claim 1, characterized in that: The nickel salt is at least one of nickel acetate, nickel chloride, nickel nitrate, and nickel sulfate; The copper salt is at least one of copper chloride, copper sulfate, and copper nitrate; The alkali solution is a sodium hydroxide solution; 3. The method for preparing the lithium-ion battery positive electrode lithium supplement additive according to claim 1, characterized in that: The molar ratio of nickel element in the nickel salt to copper element in the copper salt is (1 - x):x, where 0 < x < 1; The total molar concentration of the mixed salt solution of nickel salt and copper salt is 0.5 - 5 mol / L; The molar concentration of the alkali solution is 3 - 10 mol / L; The molar concentration of the ammonia water is 0.5 - 5 mol / L; 4. The method for preparing the lithium-ion battery positive electrode lithium supplement additive according to claim 1, characterized in that: The pH value of the reaction system of the coprecipitation reaction is 10 - 13; The temperature of the coprecipitation reaction is 40 - 70 °C; After the coprecipitation reaction in step S1, it further includes: performing solid-liquid separation on the reaction system, collecting the solid powder, and drying it in vacuum.

5. The method for preparing the lithium-ion battery positive electrode lithium supplement additive according to claim 1, characterized in that: The vacuum degree in the vacuum environment < 100 Pa; The conditions for the pre-sintering are as follows: heating to 400 - 1100 °C at a rate of 1 - 10 °C / min and holding for 10 - 600 min; After the pre-sintering in step S2, it further includes: crushing the pre-sintered product; The lithium source consists of a first lithium source, a second lithium source, and a third lithium source. The first lithium source is at least one of lithium hydroxide and lithium hydride, the second lithium source is at least one of lithium oxide and lithium peroxide, and the third lithium source is at least one of lithium carbonate, lithium oxalate, lithium acetate, and lithium citrate; preferably, the chemical formula of the lithium precursor is mLiOH·nLi2O·pLi2CO3·wH2O, where m, n, p are mass fractions, 0 < m < 0.5, 0.5 ≤ n < 1.0, 0 < p < 0.5, m + n + p = 1, and w represents the water content of crystallization, 0 ≤ w ≤ 1; The molar ratio of the metal elements in the nickel-copper precursor to the lithium element in the lithium precursor is 1:(1.8 - 2.4); 6. The method for preparing the lithium-ion battery positive electrode lithium supplement additive according to claim 1, characterized in that: The sintering conditions are as follows: heating to 600 - 900 °C at a rate of 2 - 5 °C / min and holding for 8 - 15 h; Crushing and sieving the sintered product, and the mesh number of the sieve used for sieving is 300 - 400 meshes, and the particle size D50 is 5.0 - 9.0 μm; The lithium-ion battery cathode lithium supplement additive is a polycrystalline-like substance; 7. The lithium-ion battery positive electrode lithium supplement additive obtained by the preparation method according to any one of claims 1 to 6, wherein the lithium supplement additive comprises Li2Ni (1-x) Cu x O2, where 0 <x<1。 8. A positive electrode material for a lithium ion battery, characterized in that: It includes a high-nickel cathode material and the lithium-ion battery cathode lithium supplement additive according to claim 7; 9. The positive electrode material for lithium-ion batteries according to claim 8, characterized in that: The high nickel positive electrode material is LiNi x’ Co y M (1-x’-y) O2, where 0.65≤x ’ <1,0<y≤0.2,(x ’ +y)<1, M is one or more of Al, Mn and Mg; The mass of the lithium-ion battery cathode lithium supplement additive is 0.5% - 5% of the lithium-ion battery cathode material; 10. A lithium ion battery, comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, characterized in that: The positive electrode sheet includes a current collector and the lithium-ion battery cathode material according to claim 8 or 9 provided on the current collector.

Citation Information

Patent Citations

  • Lithium-supplementing material Li2NiO2 as well as preparation method and application thereof

    CN110218078A

  • Lithium supplement additive for positive electrode of lithium ion battery, preparation method of lithium supplement additive and lithium ion battery

    CN113571781A

  • Anode active material for lithium ion secondary battery and its making method

    CN101262057A

  • Positive additive and preparation method and application thereof

    CN111653770A

  • Positive electrode lithium supplementing material and preparation method and application thereof

    CN113140722A

Cited By

  • Composite positive electrode lithium supplement additive and preparation method and application thereof

    CN120089743A

  • Lithium supplement additive, preparation method and battery containing lithium supplement additive

    CN121307032A