Doping modified sodium-ion battery precursor as well as preparation method and application thereof
By using a combination of nickel-ferromanganese core and nickel-copper-niobium-manganese coating in the positive electrode material of sodium ion battery, the problems of structural instability and sodium ion deintercalation are solved, and the cycle stability and electrochemical performance of the battery are improved.
Patent Information
- Application Number
- CN202410911948.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-01
AI Technical Summary
The structural instability of the positive electrode material of sodium ion battery and the problem of sodium ion deintercalation lead to poor cycle stability and rate performance, limiting the application of sodium ion batteries.
The doped modified sodium ion battery precursor, including nickel-ferromanganese core and nickel-copper-niobium-manganese coating, is used to construct a uniform element distribution state through co-precipitation method, stabilize the crystal structure, and improve the capacity and stability of the material.
It significantly improves the cycle stability, rate performance and capacity of sodium ion batteries, improves sodium storage performance and electron ion diffusion kinetics, and enhances the overall performance of the battery.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a doped and modified sodium ion battery precursor, a preparation method and an application thereof. Background Art
[0002] Lithium-ion batteries have taken over the rechargeable battery market. In contrast, sodium resources are widely distributed and low-cost, and sodium-ion batteries have excellent high and low temperature performance and safety and stability, becoming a research and development hotspot in the current energy storage and low-speed electric vehicle fields. However, the large ionic radius and slow kinetic rate of sodium ions themselves limit the embedding and deintercalation of sodium ions in the positive electrode material, greatly reducing the performance of the positive electrode material. Therefore, how to prepare high-performance sodium-ion battery positive electrode materials has become a key issue for the successful application of sodium-ion battery positive electrode materials and needs to be solved urgently.
[0003] At present, layered oxide sodium ion battery positive electrode materials are considered to be the most promising positive electrode materials, and their preparation methods mainly adopt high-temperature solid phase methods, such as a sodium ion battery layered manganese-based positive electrode material and its preparation method disclosed in CN108923042B, the method is: sodium salt, manganese carbonate and metal oxide are mixed and pressed into sheets, and then calcined at 400℃-1100℃ to obtain a sodium ion battery layered manganese-based positive electrode material. This traditional process can obtain a sodium ion battery layered manganese-based material with excellent cycle life, but the solid phase method cannot make the particles evenly distributed, resulting in agglomeration and impurities. During the charge and discharge process, the internal structure of the crystal is prone to collapse and cracking, which seriously affects the cycle stability of the battery. The use of a coprecipitation method to prepare a layered oxide sodium ion positive electrode material precursor will effectively avoid problems such as particle agglomeration and cracking, thereby preparing a positive electrode material with excellent electrochemical properties, such as a sodium ion precursor material and a preparation method and use thereof disclosed in CN116282228A, wherein the method comprises adding a nickel-iron-manganese mixed salt solution, a precipitant solution and a complexing agent to a base liquid in parallel, performing a coprecipitation reaction, and obtaining a core; then replacing the nickel-iron-manganese mixed salt solution with a nickel-copper-manganese mixed salt solution and continuing the coprecipitation reaction to obtain a sodium ion precursor material.
[0004] However, there are still some problems with layered oxide sodium ion cathode materials. The sodium ion itself has a larger radius, so it requires higher energy to move, and it is very easy to have phase change and structural dislocation during the deintercalation process, which leads to structural instability and reduces the capacity and stability of the battery during the cycle. Therefore, how to obtain a sodium ion oxide cathode material with a stable structure to improve the electrochemical performance has become a top priority for sodium ion batteries. Summary of the invention
[0005] In view of the above problems existing in the prior art, the object of the present invention is to provide a doped and modified sodium-ion battery precursor, a preparation method thereof and an application thereof.
[0006] To achieve the above object, the present invention adopts the following technical solutions:
[0007] In a first aspect, the present invention provides a doped and modified sodium-ion battery precursor, and the doped and modified sodium-ion battery precursor includes a nickel-iron-manganese core and a nickel-copper-niobium-manganese coating layer coated on the surface of the nickel-iron-manganese core.
[0008] In the present invention, the chemical composition of the nickel-iron-manganese core is a hydroxide of nickel, iron and manganese.
[0009] In the present invention, the chemical composition of the nickel-copper-niobium-manganese coating layer is a hydroxide of nickel, copper, niobium and manganese.
[0010] The present invention uses a high-capacity nickel-iron-manganese core and coats it with a nickel-copper-niobium-manganese coating layer. On the one hand, it can provide high capacity for the cathode material of the sodium-ion battery. On the other hand, due to the doping of niobium and copper in the outer layer, a high-entropy effect is formed, which stabilizes the lattice structure and is beneficial to the deintercalation of sodium ions, thereby achieving excellent sodium storage performance. A more stable crystal structure is obtained through the migration of sodium ions, and the crystal structure is optimized to enhance the diffusion kinetics of electrons and ions. The doped and modified sodium-ion battery precursor of the present invention can solve the problems of unstable structure of the oxide cathode material of the sodium-ion battery and sodium ion deintercalation, and improve the cycle stability, rate performance and capacity of the battery.
[0011] The following are the preferred technical solutions of the present invention, but do not limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the technical purpose and beneficial effects of the present invention can be better achieved.
[0012] Preferably, the chemical general formula of the nickel-iron-manganese core is Ni x Fe y Mn z (OH)2, where 0 < x < 0.25, 0 < y < 0.25, 0.5 < z < 1, and x + y + z = 1. Exemplarily, x can be 0.02, 0.05, 0.08, 0.1, 0.15, 0.2 or 0.23, etc.; y can be 0.02, 0.05, 0.08, 0.1, 0.15, 0.2 or 0.23, etc.; z can be 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9 or 0.95, etc.
[0013] Preferably, the particle size D50 of the nickel-iron-manganese core is 3μm-10μm, for example, it can be 3μm, 3.5μm, 4μm, 4.5μm, 5μm, 5.5μm, 6μm, 6.5μm, 7μm, 7.5μm, 8μm, 8.5μm, 9μm, 9.5μm or 10μm, etc.
[0014] Preferably, the coating layer has a thickness of 0.5 μm-2 μm, for example, 0.5 μm, 0.7 μm, 0.8 μm, 1 μm, 1.2 μm, 1.4 μm, 1.6 μm, 1.8 μm or 2 μm.
[0015] Preferably, the chemical formula of the nickel-copper-niobium-manganese coating layer is Ni a Cu b Nb c Mn d (OH)2, wherein 0.6≤a≤0.9, 0<b≤0.4, 0<c≤0.3, 0<d≤0.2, a+b+c+d=1. For example, a can be 0.6, 0.65, 0.7, 0.75, 0.8, 0.85 or 0.9, etc.; b can be 0.05, 0.08, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35 or 0.4, etc.; c can be 0.05, 0.08, 0.1, 0.15, 0.2, 0.25 or 0.3, etc., and d can be 0.05, 0.08, 0.1, 0.15 or 0.2, etc.
[0016] Preferably, based on the mass of the doped and modified sodium ion battery precursor, the doping amount of the niobium element is 500ppm-10000ppm, for example, it can be 500ppm, 1000ppm, 1500ppm, 2000ppm, 2500ppm, 3000ppm, 3500ppm, 4000ppm, 4500ppm, 5000ppm, 5500ppm, 6000ppm, 6500ppm, 7000ppm, 7500ppm, 8000ppm, 8500ppm, 9000ppm, 9500ppm or 10000ppm, etc.
[0017] Preferably, the molar ratio of niobium element to copper element in the coating layer is 1:(1.4-1.9), for example, 1:1.4, 1:1.5, 1:1.6, 1:1.7, 1:1.8 or 1:1.9.
[0018] In a second aspect, the present invention provides a method for preparing a doped and modified sodium ion battery precursor as described in the first aspect, the preparation method comprising the following steps:
[0019] (1) adding a nickel-iron-manganese mixed salt solution, a precipitant solution and a complexing agent to a bottom liquid in parallel to carry out a coprecipitation reaction to obtain a core;
[0020] (2) replacing the nickel-iron-manganese mixed salt solution with a nickel-copper-manganese mixed salt solution, and adding it to the bottom solution containing the inner core in parallel with the niobium source solution, continuing the coprecipitation reaction, growing a coating layer on the inner core, and obtaining a doped and modified sodium ion battery precursor.
[0021] In the method of the present invention, when the coprecipitation reaction is continued in step (2), the complexing agent solution and the complexing agent are still introduced into the reaction system.
[0022] The present invention utilizes a co-precipitation method to construct a nickel-iron-manganese inner core and coats a copper- and niobium-doped nickel-copper-niobium-manganese coating layer on its surface, thereby obtaining a uniform element distribution state, allowing nickel and manganese to form a single-phase structure, stabilizing the crystal structure, and solving the problems of structural instability of the oxide positive electrode material of a sodium ion battery and sodium ion deintercalation, thereby improving the cycle stability, rate performance, and capacity of the battery.
[0023] The method of the present invention avoids the problem that the copper element is directly added to the inner core, which makes it difficult to precipitate homogeneously with the nickel-iron-manganese solution. The copper element acts synergistically with niobium in the coating layer, effectively improving the capacity and stability of the material.
[0024] The doped and modified sodium ion battery precursor prepared by the method of the present invention has a stable structure, good sphericity and morphology, and the positive electrode material prepared by using the precursor has excellent stability and electrochemical performance.
[0025] As a preferred technical scheme for the preparation method of the doped modified sodium ion battery precursor of the present invention, the total molar concentration of metal ions in the nickel-iron-manganese mixed salt solution in step (1) is 1.5 mol / L-3 mol / L, for example, it can be 1.5 mol / L, 1.7 mol / L, 1.8 mol / L, 2 mol / L, 2.2 mol / L, 2.4 mol / L, 2.6 mol / L, 2.8 mol / L or 3 mol / L, etc.
[0026] Preferably, the nickel-iron-manganese mixed salt solution in step (1) comprises nickel salt, iron salt and manganese salt.
[0027] Preferably, the nickel salt and manganese salt are independently selected from at least one of sulfate, nitrate or chloride.
[0028] Preferably, the iron salt includes at least one of ferrous sulfate, ferrous nitrate or ferrous chloride.
[0029] Preferably, the complexing agent in step (1) comprises at least one of ammonia water, sodium fluoride, sodium citrate and sodium lactate.
[0030] Preferably, the feeding rate of the nickel-iron-manganese mixed salt solution in step (1) is in the range of 40 L / h-15 L / h (for example, it can be 40 L / h, 38 L / h, 37 L / h, 35 L / h, 33 L / h, 30 L / h, 28 L / h, 25 L / h, 22 L / h, 20 L / h, 18 L / h, 16 L / h or 15 L / h, etc.), and the feeding rate gradually decreases.
[0031] This preferred technical solution will cause the iron and manganese metal contents to decrease gradually. In the prepared doped and modified sodium ion battery precursor, the manganese and iron contents in the central layer are the highest, which is beneficial to improving the battery cycle stability, stabilizing the internal structure of the precursor, providing a safe and stable transmission channel for sodium ions, and effectively avoiding channel collapse during the sodium ion deintercalation process, lattice defects, etc.
[0032] Preferably, the base liquid in step (1) is prepared in the following manner: add water accounting for 1 / 4-3 / 4 (for example, 1 / 4, 2 / 4 or 3 / 4, etc.) of the volume of the reactor into the reactor, start stirring, introduce protective gas, then add complexing agent solution and precipitant, adjust the pH value of the base liquid and the concentration of the complexing agent, and obtain the base liquid.
[0033] The present invention does not specifically limit the source and type of water, and those skilled in the art may select it according to their needs, for example, it may be pure water.
[0034] The present invention does not specifically limit the type of protective gas, and it can be, for example, high-purity nitrogen.
[0035] Preferably, the pH value of the base solution in step (1) is 8-10.5, for example, it can be 8, 8.2, 8.5, 8.7, 8.8, 9.0, 9.3, 9.6, 9.7, 9.8, 10.0, 10.2, 10.3 or 10.5, etc.
[0036] Preferably, the mass concentration of the complexing agent in the base solution of step (1) is 7 g / L-10 g / L, for example, 7 g / L, 8 g / L or 10 g / L.
[0037] Preferably, the temperature of the coprecipitation reaction in step (1) is 50°C-75°C, for example, it can be 50°C, 52°C, 53°C, 55°C, 56°C, 58°C, 60°C, 62°C, 64°C, 65°C, 67°C, 68°C, 70°C, 72°C, 73°C or 75°C, etc.
[0038] Preferably, during the coprecipitation reaction in step (1), the pH value is in the range of 8.5-12, and the pH value can be, for example, 8.5, 8.6, 8.8, 9.0, 9.2, 9.3, 9.5, 9.7, 10.0, 10.2, 10.3, 10.5, 10.7, 10.8, 11.0, 11.2, 11.3, 11.5, 11.7 or 12, etc.
[0039] Preferably, the coprecipitation reaction in step (1) is accompanied by stirring, and the stirring speed is 280rpm-400rpm, for example, it can be 280rpm, 300rpm, 325rpm, 350rpm, 360rpm, 380rpm or 400rpm.
[0040] Preferably, the coprecipitation reaction time in step (1) is 40 h to 150 h, for example, it can be 40 h, 45 h, 50 h, 55 h, 60 h, 70 h, 80 h, 90 h, 100 h, 110 h, 120 h, 130 h, 140 h or 150 h.
[0041] Preferably, the reaction system of the coprecipitation reaction in step (1) also includes a reducing agent to prevent oxidation of divalent iron ions.
[0042] Preferably, the amount of reducing agent added is 500g-1000g for every 500L of base liquid, for example, it can be 500g, 550g, 600g, 650g, 700g, 750g, 800g, 850g, 900g, 950g or 1000g, etc.
[0043] The present invention does not specifically limit the type of the reducing agent, and it may be VC, for example.
[0044] In one embodiment, a reducing agent is added to the base solution, or a reducing agent is added to the nickel-iron-manganese mixed salt solution, so that the reaction system of the coprecipitation reaction in step (1) contains a reducing agent, thereby preventing the oxidation of divalent iron ions.
[0045] Preferably, the reducing agent is an acidic reducing agent.
[0046] As a preferred technical solution of the method for preparing the doped modified sodium ion battery precursor of the present invention, the concentration of the nickel-copper-manganese mixed salt solution in step (2) is 1.2 mol / L-2.5 mol / L, for example, it can be 1.2 mol / L, 1.5 mol / L, 1.6 mol / L, 1.8 mol / L, 2.0 mol / L, 2.2 mol / L, 2.3 mol / L or 2.5 mol / L, etc.
[0047] Preferably, the feeding rate of the nickel-copper-manganese mixed salt solution in step (2) is in the range of 8 L / h-50 L / h (for example, it can be 8 L / h, 10 L / h, 13 L / h, 16 L / h, 18 L / h, 20 L / h, 25 L / h, 28 L / h, 30 L / h, 33 L / h, 36 L / h, 38 L / h, 40 L / h, 42 L / h, 45 L / h, 47 L / h or 50 L / h, etc.), and the feeding rate gradually increases.
[0048] In this preferred technical solution, the concentrations of nickel and copper metals increase in a gradient, and the outer layer of the prepared doped and modified sodium ion battery precursor has a precursor structure with relatively high nickel and copper content, which effectively improves the specific capacity and rate performance of the battery.
[0049] Preferably, the niobium source in the niobium source solution in step (2) comprises at least one of niobium oxalate, niobium chloride or niobate.
[0050] Preferably, the concentration of the niobium source solution in step (2) is 0.5 mol / L-4 mol / L, for example, 0.5 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L, 3 mol / L, 3.5 mol / L or 4 mol / L.
[0051] Preferably, the feeding rate of the niobium source solution in step (2) is 1 L / h-4 L / h, for example, 1 L / h, 1.3 L / h, 1.5 L / h, 1.7 L / h, 2 L / h, 2.5 L / h, 3 L / h, 3.5 L / h or 4 L / h.
[0052] Preferably, during the coprecipitation reaction in step (2), the pH value is in the range of 9.5-10, and the pH value may be, for example, 9.5, 9.6, 9.7, 9.8, 9.9 or 10.
[0053] Preferably, the coprecipitation reaction in step (2) is accompanied by stirring, and the stirring speed is 100rpm-250rpm, for example, it can be 100rpm, 120rpm, 130rpm, 140rpm, 160rpm, 180rpm, 200rpm, 210rpm, 220rpm, 230rpm, 240rpm or 250rpm, etc.
[0054] Preferably, the coprecipitation reaction time in step (2) is 25 h-40 h, for example, it can be 25 h, 26 h, 27 h, 28 h, 30 h, 32 h, 33 h, 35 h, 36 h, 38 h, 39 h or 40 h.
[0055] As a preferred technical solution of the method for preparing the doped and modified sodium ion battery precursor of the present invention, in the method for preparing the doped and modified sodium ion battery precursor, a dispersant is also included in the entire reaction process.
[0056] Preferably, the dispersant includes at least one of sodium lauryl sulfate, coconut oil diethanolamide, methyl high hydrogen silicone oil emulsion and hydroxy silicone oil emulsion.
[0057] Preferably, the dispersant is made into a dispersant solution and added to the reaction system of the coprecipitation reaction at a certain rate, and the certain rate is 1.4L / h-4.5L / h, for example, it can be 1.4L / h, 1.6L / h, 1.8L / h, 2L / h, 2.2L / h, 2.3L / h, 2.5L / h, 2.7L / h, 2.8L / h, 3L / h, 3.2L / h, 3.4L / h, 3.6L / h, 3.8L / h, 4L / h, 4.3L / h or 4.5L / h, etc.
[0058] Preferably, the mass concentration of the dispersant solution is 4%-8%, for example, it can be 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5% or 8%.
[0059] Under the action of the dispersant, the uniform distribution of the elements in the precursor can be improved, avoiding the problems of separate phase formation and agglomeration of the elements, thereby better improving the structural stability and electrochemical performance of the positive electrode material prepared using the precursor.
[0060] In a third aspect, the present invention provides a sodium ion battery oxide positive electrode material, wherein the sodium ion battery oxide positive electrode material is prepared using the doped and modified sodium ion battery precursor as described in the first aspect, and the sodium ion battery oxide positive electrode material comprises a nickel-iron-manganese oxide core and a nickel-copper-niobium-manganese oxide outer layer.
[0061] In a fourth aspect, the present invention provides a method for preparing the sodium ion battery oxide positive electrode material as described in the third aspect, the preparation method comprising the following steps:
[0062] The doped and modified sodium ion battery precursor is mixed with a sodium source and then sintered to obtain a sodium ion battery oxide positive electrode material.
[0063] Preferably, the sintering temperature is 750°C-900°C, for example, it may be 750°C, 760°C, 770°C, 780°C, 800°C, 815°C, 830°C, 840°C, 850°C, 860°C, 880°C or 900°C.
[0064] Preferably, the sintering time is 10h-40h, for example, it can be 10h, 12h, 13h, 14h, 15h, 17h, 18h, 20h, 22h, 25h, 26h, 27h, 28h, 30h, 32h, 33h, 35h, 36h, 38h, 39h or 40h.
[0065] In a fifth aspect, the present invention provides a sodium ion battery, comprising the sodium ion battery oxide positive electrode material described in the third aspect.
[0066] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0067] Compared with the prior art, the present invention has the following beneficial effects:
[0068] (1) The present invention adopts a high-capacity nickel-iron-manganese core and coats it with a nickel-copper-niobium-manganese coating layer. On the one hand, it can provide high capacity for the positive electrode material of the sodium ion battery. On the other hand, due to the doping of niobium and copper in the outer layer, a high entropy effect is formed, which stabilizes the lattice structure and is conducive to the deintercalation of sodium ions, thereby achieving excellent sodium storage performance, and obtaining a more stable crystal structure through the migration of sodium ions, optimizing the crystal structure and enhancing the diffusion kinetics of electrons and ions. The doped and modified sodium ion battery precursor of the present invention can solve the problems of structural instability and sodium ion deintercalation of the oxide positive electrode material of the sodium ion battery, and improve the cycle stability, rate performance and capacity of the battery.
[0069] (2) The doped and modified sodium ion battery precursor provided by the present invention is used to prepare the positive electrode material and assemble it into a battery. Under a discharge voltage of 2-4V, the battery has an initial discharge capacity of 164.3mAh / g or more at 0.1C / 0.1C, a rate performance of 97.9% or more at 1C / 0.1C, and a capacity retention rate of 95.4% or more after 100 cycles at 0.5C / 1C. DETAILED DESCRIPTION
[0070] The technical solution of the present invention is further illustrated below through specific implementation methods.
[0071] Example 1
[0072] This embodiment provides a doped modified sodium ion battery precursor, including a nickel iron manganese core (chemical formula Ni 0.25 Fe 0.25 Mn 0.5 (OH)2) and a nickel-copper-niobium-manganese coating layer (chemical formula: Ni 0.7 Cu0.1 Nb 0.1 Mn 0.1 (OH)2), the particle size D50 of the core is 5 μm, the thickness of the coating layer is 0.8 μm, and the doping amount of niobium element in the precursor is 5000 ppm.
[0073] This embodiment also provides a method for preparing the above-mentioned doped and modified sodium ion battery precursor, comprising the following steps:
[0074] (1) Add pure water accounting for 3 / 4 of the volume of the reactor into the reactor, start stirring, introduce high-purity nitrogen, add sodium hydroxide solution (mass concentration 15 g / L) and ammonia water (mass concentration 8 g / L), adjust the pH value of the bottom liquid to 10, and the ammonia water concentration to 8.5 g / L, to obtain 500 L of bottom liquid;
[0075] A nickel-iron-manganese mixed salt solution containing a reducing agent (wherein each metal element is derived from sulfate, the total molar concentration of metal ions is 2 mol / L, the reducing agent is VC, and the amount of the reducing agent added is 750 g), a sodium hydroxide solution (mass concentration 15 g / L) and an ammonia solution (mass concentration 20 g / L) are added to the bottom liquid in parallel, and the feeding rate of the nickel-iron-manganese mixed salt solution is in the range of 30 L / h-15 L / h, and the feeding rate is gradually reduced; a coprecipitation reaction is carried out at a temperature of 65° C. and a rotation speed of 400 rpm, the pH value of the reaction process is maintained at 9, and the reaction is stopped when D50 reaches 5 μm to obtain a core Ni 0.25 Fe 0.25 Mn 0.5 (OH)2;
[0076] (2) The nickel-iron-manganese mixed salt solution was replaced with a nickel-copper-manganese mixed salt solution (wherein each metal element was derived from sulfate, and the total molar concentration of metal ions was 2 mol / L, and niobium oxalate solution (concentration was 2 mol / L, and the feed rate was 1.4 L / h) was added at the same time, and other raw materials remained unchanged, and the solution was added to the inner core bottom liquid to continue the coprecipitation reaction. The feed rate of the nickel-copper-manganese mixed salt solution was in the range of 15 L / h-30 L / h, and the feed rate was gradually increased. When D50 was 5.8 μm, the machine was stopped, and the material in the kettle was centrifuged, washed, dried, and sieved to obtain a doped and modified sodium ion battery precursor. The whole reaction process used a hydroxy silicone oil emulsion dispersant (model: AD9004), and the dispersant was made into a dispersant solution with a mass concentration of 7% and added to the reaction system at a feed rate of 3 L / h.
[0077] This embodiment also provides a sodium ion battery oxide positive electrode material, and the preparation method thereof comprises the following steps:
[0078] The above precursor was mixed with sodium carbonate and sintered at 800° C. for 30 hours to obtain a sodium ion battery oxide positive electrode material.
[0079] Example 2
[0080] This embodiment provides a doped modified sodium ion battery precursor, including a nickel iron manganese core (chemical formula Ni 0.25 Fe 0.25 Mn 0.5 (OH)2) and a nickel-copper-niobium-manganese coating layer (chemical formula: Ni 0.6 Cu 0.2 Nb 0.1 Mn 0.1 (OH)2), the particle size D50 of the core is 10 μm, the thickness of the coating layer is 2 μm, and the doping amount of niobium element in the precursor is 1000 ppm.
[0081] This embodiment also provides a method for preparing the above-mentioned doped and modified sodium ion battery precursor, comprising the following steps:
[0082] (1) Add pure water accounting for 3 / 4 of the volume of the reactor into the reactor, start stirring, introduce high-purity nitrogen, add sodium hydroxide solution (mass concentration 15 g / L) and ammonia water (mass concentration 10 g / L), adjust the pH value of the bottom liquid to 10.5, and the ammonia water concentration to 9 g / L, to obtain 500 L of bottom liquid;
[0083] A nickel-iron-manganese mixed salt solution containing a reducing agent (wherein each metal element is derived from sulfate, the total molar concentration of metal ions is 2 mol / L, the reducing agent is VC, and the amount of the reducing agent added is 600 g), a sodium hydroxide solution (mass concentration 15 g / L) and an ammonia solution (mass concentration 20 g / L) are added to the bottom solution in parallel, the feeding rate of the nickel-iron-manganese mixed salt solution is within the range of 40 L / h-20 L / h, and the feeding rate is gradually reduced, and a coprecipitation reaction is carried out at a temperature of 50° C. and a rotation speed of 280 rpm. The pH value of the reaction process is maintained at 11, and the reaction is stopped when D50 reaches 10 μm to obtain a core Ni 0.33 Fe 0.33 Mn 0.33 (OH)2;
[0084] (2) The nickel-iron-manganese mixed salt solution was replaced with a nickel-copper-manganese mixed salt solution (wherein each metal element was derived from sulfate, and the total molar concentration of metal ions was 2 mol / L, and niobium oxalate solution (concentration was 4 mol / L, and the feed rate was 1 L / h) was added at the same time, and other raw materials remained unchanged, and the solution was added into the inner core bottom liquid to continue the coprecipitation reaction. The feed rate of the nickel-copper-manganese mixed salt solution was in the range of 8 L / h-20 L / h, and the feed rate was gradually increased. When D50 was 12 μm, the machine was stopped, and the material in the kettle was centrifuged, washed, dried, and sieved to obtain a doped and modified sodium ion battery precursor. Hydroxyl silicone oil emulsion dispersant was used in the whole reaction process, and the feed rate was 1.0 mol / L.
[0085] This embodiment also provides a sodium ion battery oxide positive electrode material, and the preparation method thereof comprises the following steps:
[0086] The above precursors were mixed with sodium hydroxide and sintered at 900° C. for 10 h to obtain a sodium ion battery oxide positive electrode material.
[0087] Example 3
[0088] This embodiment provides a doped modified sodium ion battery precursor, including a nickel iron manganese core (chemical formula Ni 0.3 Fe 0.2 Mn 0.5 (OH)2) and a nickel-copper-niobium-manganese coating layer (chemical formula: Ni 0.8 Cu 0.1 Nb 0.05 Mn 0.05 (OH)2), the particle size D50 of the core is 8μm, the thickness of the coating layer is 1μm, and the doping amount of niobium element in the precursor is 7000ppm.
[0089] This embodiment also provides a method for preparing the above-mentioned doped and modified sodium ion battery precursor, comprising the following steps:
[0090] (1) Add pure water accounting for 2 / 4 of the volume of the reactor into the reactor, start stirring, introduce high-purity nitrogen, add sodium hydroxide solution (mass concentration 10 g / L) and ammonia water (mass concentration 7 g / L), adjust the pH value of the bottom liquid to 9, and the ammonia water concentration to 7 g / L, to obtain 500 L of bottom liquid;
[0091] A nickel-iron-manganese mixed salt solution containing a reducing agent (wherein each metal element is derived from sulfate, the total molar concentration of metal ions is 3 mol / L, the reducing agent is VC, and the amount of the reducing agent added is 900 g), a sodium hydroxide solution (mass concentration 10 g / L) and an ammonia solution (mass concentration 15 g / L) are added to the bottom liquid in parallel, and the feeding rate of the nickel-iron-manganese mixed salt solution is in the range of 35 L / h-15 L / h, and the feeding rate is gradually reduced; a coprecipitation reaction is carried out at a temperature of 75° C. and a rotation speed of 300 rpm, and the pH value of the reaction process is maintained at 9.8. The reaction is stopped when D50 reaches 8 μm to obtain a core Ni 0.3 Fe 0.2 Mn 0.5 (OH)2;
[0092] (2) The nickel-iron-manganese mixed salt solution was replaced with a nickel-copper-manganese mixed salt solution (wherein each metal element was derived from sulfate, and the total molar concentration of metal ions was 3 mol / L, and niobium oxalate solution (concentration was 1 mol / L, and the feed rate was 3 L / h) was added at the same time, and other raw materials remained unchanged, and the solution was added to the inner core bottom liquid to continue the coprecipitation reaction. The feed rate of the nickel-copper-manganese mixed salt solution was in the range of 20 L / h-40 L / h, and the feed rate was gradually increased. When D50 was 9.5 μm, the machine was stopped, and the material in the kettle was centrifuged, washed, dried, and sieved to obtain a doped and modified sodium ion battery precursor. Hydroxyl silicone oil emulsion dispersant was used in the whole reaction process, and the feed rate was 1.2 mol / L.
[0093] This embodiment also provides a sodium ion battery oxide positive electrode material, and the preparation method thereof comprises the following steps:
[0094] The above precursor was mixed with sodium carbonate and sintered at 750° C. for 40 hours to obtain a sodium ion battery oxide positive electrode material.
[0095] Example 4
[0096] The difference between this embodiment and embodiment 1 is that in step (1) of embodiment 1, the feed rate of the nickel-iron-manganese mixed salt solution is 20 L / h and remains constant.
[0097] Example 5
[0098] The difference between this embodiment and embodiment 1 is that in step (2) of embodiment 1, the feed rate of the nickel-copper-manganese mixed salt solution is 20 L / h and remains constant.
[0099] Example 6
[0100] The difference between this embodiment and embodiment 1 is that no hydroxy silicone oil emulsion dispersant is introduced during the preparation of the precursor.
[0101] Comparative Example 1
[0102] The difference between this comparative example and Example 1 is that niobium oxalate is not added in step (2).
[0103] Preparation of the battery:
[0104] Preparation of the positive electrode: A polyvinylidene fluoride solution with a mass fraction of 7% was prepared with N-methylpyrrolidone as the solvent, and the positive electrode materials provided in Examples 1-6 and Comparative Example 1 were used. The positive electrode materials, polyvinylidene fluoride, and conductive carbon black were mixed evenly in a mass ratio of 95:2:3, and applied on aluminum foil. The coated electrode was placed in a vacuum drying oven at a temperature of 90°C and vacuum dried for 4 hours, and the positive electrode was obtained by roller pressing.
[0105] Battery assembly: Use metallic lithium sheet as counter electrode and 1 mol / L LiPF6 three-component mixed solvent with EC:DMC:EMC=1:1:1 (volume ratio) as electrolyte, and then assemble into 2032 button cells in an argon-filled glove box.
[0106] Performance test: At a discharge voltage of 2V-4V, the battery was tested for its first discharge capacity at 0.1C / 0.1C, rate performance at 1C / 0.1C, and capacity retention after 100 cycles at 0.5C / 1C. The results are shown in Table 1.
[0107] Table 1
[0108]
[0109]
[0110] As shown in Table 1, the battery assembled with the positive electrode material made of the doped and modified sodium ion battery precursor provided by the present invention has good electrochemical properties. The copper and niobium elements work synergistically with each other, which can avoid the problem of copper segregation caused by only copper or excessive copper and uneven element distribution caused by excessive niobium, and the problem of single phase formation, which affects the structural stability, hinders the sodium ion deintercalation, and reduces the electrochemical performance of the battery. The battery prepared by using the precursor of the present invention to prepare the positive electrode material and assemble it can reach a first discharge specific capacity of more than 168.4mAh / g at 0.1C / 0.1C, and the rate performance at 1C / 0.1C can reach more than 98.2%, and the capacity retention rate after 100 cycles of 0.5C / 1C can reach more than 96.7%.
[0111] At the same time, through the comparison between Example 1 and Example 4-5, it can be seen that by comparing Example 1 with Example 4-5, it can be seen that the method of decreasing the flow gradient of the inner core nickel-iron-manganese mixed ternary solution and increasing the flow gradient of the coating layer nickel-copper-manganese mixed ternary solution is adopted to form a ternary precursor with high manganese and iron in the inner layer and high nickel and copper in the outer layer, which stabilizes the internal structure of the precursor and improves the capacity of the battery, which is beneficial to the cycle stability and high capacity of the material.
[0112] By comparing Example 1 with Example 6, it can be seen that the dispersant can make the doping elements evenly distributed, thereby improving the battery stability and capacity.
[0113] By comparing Example 1 with Comparative Example 1, it can be seen that doping with niobium element forms a high entropy effect, stabilizes the lattice structure, and is beneficial to improving the electrochemical performance of the battery.
[0114] The applicant declares that the present invention illustrates the detailed method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed method, that is, it does not mean that the present invention must rely on the above-mentioned detailed method to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A doped and modified sodium ion battery precursor, characterized in that: The doped modified sodium ion battery precursor comprises a nickel-iron-manganese core and a nickel-copper-niobium-manganese coating layer coated on the surface of the nickel-iron-manganese core.
2. The doped and modified sodium ion battery precursor according to claim 1, characterized in that: The general chemical formula of the nickel-iron-manganese core is Ni x Fe y Mn z (OH)2, where 0 <x<0.25,0<y<0.25,0.5<z<1,x+y+z=1; Preferably, the particle size D50 of the nickel-iron-manganese core is 3 μm-10 μm.
3. The doped and modified sodium ion battery precursor according to claim 1 or 2, characterized in that: The thickness of the coating layer is 0.5 μm-2 μm; Preferably, the chemical formula of the nickel-copper-niobium-manganese coating layer is Ni a Cu b Nb c Mn d (OH)2, wherein 0.6≤a≤0.9, 0<b≤0.4, 0<c≤0.3, 0<d≤0.2, a+b+c+d=1; Preferably, based on the mass of the doped and modified sodium ion battery precursor, the doping amount of niobium element is 500ppm-10000ppm; Preferably, the molar ratio of niobium element to copper element in the coating layer is 1:(1.4-1.9).
4. A method for preparing a doped and modified sodium ion battery precursor according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: (1) adding a nickel-iron-manganese mixed salt solution, a precipitant solution and a complexing agent to a bottom liquid in parallel to carry out a coprecipitation reaction to obtain a core; (2) replacing the nickel-iron-manganese mixed salt solution with a nickel-copper-manganese mixed salt solution, and adding it to the bottom solution containing the inner core in parallel with the niobium source solution, continuing the coprecipitation reaction, growing a coating layer on the inner core, and obtaining a doped and modified sodium ion battery precursor.
5. The preparation method according to claim 4, characterized in that: The total molar concentration of metal ions in the nickel-iron-manganese mixed salt solution of step (1) is 1.5 mol / L-3 mol / L; Preferably, the nickel-iron-manganese mixed salt solution in step (1) comprises nickel salt, iron salt and manganese salt; Preferably, the nickel salt and manganese salt are independently selected from at least one of sulfate, nitrate or chloride; Preferably, the iron salt comprises at least one of ferrous sulfate, ferrous nitrate or ferrous chloride; Preferably, the complexing agent in step (1) comprises at least one of ammonia water, sodium fluoride, sodium citrate and sodium lactate; Preferably, the feeding rate of the nickel-iron-manganese mixed salt solution in step (1) is in the range of 40 L / h-15 L / h, and the feeding rate is gradually reduced; Preferably, the base liquid in step (1) is prepared in the following manner: add water accounting for 1 / 4-3 / 4 of the volume of the reactor into the reactor, start stirring, introduce protective gas, then add complexing agent solution and precipitant, adjust the pH value of the base liquid and the concentration of the complexing agent, and obtain the base liquid; Preferably, the pH value of the base solution in step (1) is 8-10.5; Preferably, the mass concentration of the complexing agent in the base solution of step (1) is 7 g / L-10 g / L; Preferably, the temperature of the coprecipitation reaction in step (1) is 50°C-75°C; Preferably, during the coprecipitation reaction in step (1), the pH value is in the range of 8.5-12; Preferably, the coprecipitation reaction in step (1) is accompanied by stirring, and the stirring speed is 280 rpm-400 rpm; Preferably, the coprecipitation reaction time in step (1) is 40h-150h; Preferably, the reaction system of the coprecipitation reaction in step (1) further includes a reducing agent; Preferably, the amount of reducing agent added is 500g-1000g per 500L of base liquid; Preferably, the reducing agent is an acidic reducing agent.
6. The preparation method according to claim 4 or 5, characterized in that: The concentration of the nickel-copper-manganese mixed salt solution in step (2) is 1.2 mol / L-2.5 mol / L; Preferably, the feeding rate of the nickel-copper-manganese mixed salt solution in step (2) is in the range of 8 L / h-50 L / h, and the feeding rate gradually increases; Preferably, the niobium source in the niobium source solution in step (2) comprises at least one of niobium oxalate, niobium chloride or niobate; Preferably, the concentration of the niobium source solution in step (2) is 0.5 mol / L-4 mol / L; Preferably, the feeding rate of the niobium source solution in step (2) is 1 L / h-4 L / h; Preferably, during the coprecipitation reaction in step (2), the pH value is in the range of 9.5-10; Preferably, the coprecipitation reaction in step (2) is accompanied by stirring, and the stirring speed is 100 rpm-250 rpm; Preferably, the coprecipitation reaction time in step (2) is 25h-40h.
7. The preparation method according to any one of claims 4 to 6, characterized in that: In the preparation method of the doped and modified sodium ion battery precursor, a dispersant is also included in the entire reaction process; Preferably, the dispersant includes at least one of sodium lauryl sulfate, coconut oil diethanolamide, and hydroxy silicone oil emulsion; Preferably, the dispersant is made into a dispersant solution and added to the reaction system of the coprecipitation reaction at a certain rate, wherein the certain rate is 1.4 L / h-4.5 L / h; Preferably, the mass concentration of the dispersant solution is 4%-8%.
8. A sodium ion battery oxide positive electrode material, characterized in that: The sodium ion battery oxide positive electrode material is prepared using the doped and modified sodium ion battery precursor according to any one of claims 1 to 3, and the sodium ion battery oxide positive electrode material comprises a nickel-iron-manganese oxide core and a nickel-copper-niobium-manganese oxide outer layer.
9. A method for preparing the sodium ion battery oxide positive electrode material as claimed in claim 8, characterized in that: The preparation method comprises the following steps: The doped and modified sodium ion battery precursor is mixed with a sodium source and then sintered to obtain a sodium ion battery oxide positive electrode material; Preferably, the sintering temperature is 750°C-900°C; Preferably, the sintering time is 10h-40h.
10. A sodium ion battery, characterized in that: The sodium ion battery comprises the sodium ion battery oxide positive electrode material according to claim 8.
Citation Information
Cited By
High-voltage sodium ion positive electrode material and preparation method and application thereof
CN119297258A