Modified positive electrode material, preparation method thereof and secondary battery
By coating the surface of the positive electrode material of a lithium-ion battery with a porous composite material, the problem of lattice collapse was solved, the electrode capacity and cycle performance of the battery were improved, and a lithium-ion battery with high energy density and long life was achieved.
Patent Information
- Application Number
- CN202411321240.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-23
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-09-23
AI Technical Summary
Traditional lithium-ion battery cathode materials suffer from lattice collapse during charging, resulting in slow lithium-ion transport, reduced electrode capacity, shortened lifespan, low electronic conductivity, and poor cycle performance.
A polymer PDP is generated by reacting diketone and diamine. The mixture is then treated with boric acid at high temperature to form a porous composite material, which is then coated on the surface of the cathode material to form a porous composite material modified cathode material.
It improves the rate performance, cycle stability, and structural stability of the cathode material, thereby enhancing the electrode capacity and lifespan of lithium-ion batteries.
Smart Images

Figure CN118877957A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of positive electrode materials for lithium ion batteries, and in particular relates to the modification of positive electrode materials. Background Art
[0002] Lithium-ion batteries are widely used in digital products, new energy electric vehicles, and electrical energy storage. With the accelerated development of electrification in the energy and transportation sectors, traditional cathode materials can no longer meet people's demand for high-energy density batteries, and it is necessary to develop new composite cathode materials with higher energy density and longer cycle life. When traditional cathode materials are charged to a high level, the phase transition causes the lattice to collapse, hindering the rapid transmission of lithium ions inside the electrode, resulting in a decrease in electrode capacity and a shortened battery life.
[0003] The positive electrode material is one of the key components of lithium-ion batteries, which directly affects the comprehensive performance of lithium-ion batteries, such as capacity and cycle life. At present, most multilayered metal oxides have low electronic conductivity, low actual specific capacity of the positive electrode, poor cycle performance, and unsatisfactory capacity retention. It is relatively difficult to achieve high capacity reversibility. Therefore, it is necessary to modify it to break this trade-off by reducing structural degradation and volume change without affecting high capacity. The most common effective modification methods include coating, doping, etc. Summary of the invention
[0004] The present application provides a modified positive electrode material and a preparation method thereof, and a secondary battery.
[0005] To achieve the above objectives, this application proposes the following technical solutions: In a first aspect, a method for preparing a modified positive electrode material is provided, comprising: S1, dissolving a diketone and a diamine in an organic solvent, reacting them under the action of a catalyst, and obtaining a polymer PDP containing both an ester group and an amino group; S2, mixing the polymer PDP with boric acid, and heat-treating the mixture at 700-900° C. under a protective atmosphere to obtain a product, and filtering, washing and drying the product to obtain a porous composite material; S3. The positive electrode material and the porous composite material are subjected to wet ball milling, followed by solid-liquid separation and drying to obtain a modified positive electrode material.
[0006] Furthermore, the diketone is one or more of 2,5-dimethoxyacyl-1,4-cyclohexanedione, 2,5-diethylester-1,4-cyclohexanedione, and 2,5-bis(1-methylethylester)-1,4-cyclohexanedione.
[0007] Furthermore, the diamine is one or more of p-phenylenediamine, 2,6-diaminonaphthalene, and 2,6-diaminoanthracene.
[0008] Furthermore, the catalyst is one or more of p-toluenesulfonamide, triethylamine p-toluenesulfonate, and tetrabutylammonium p-toluenesulfonate.
[0009] Furthermore, the organic solvent is one or more of alcohol and chlorobenzene solvents.
[0010] Furthermore, the molar ratio of the diketone to the diamine is 1:1 to 1:1.2.
[0011] Furthermore, the amount of the catalyst used is 1.5 mol% to 2.0 mol% of the diketone.
[0012] Furthermore, in step S1, the reaction temperature is 100-140° C.; and the reaction time is 40-72 hours.
[0013] Furthermore, in step S2, the weight ratio of the polymer PDP to boric acid is 1:1 to 1:1.2.
[0014] Furthermore, in step S2, the insulation treatment time is 2 to 5 hours.
[0015] Furthermore, in step S2, the protective atmosphere is a nitrogen atmosphere or an inert gas atmosphere.
[0016] Furthermore, in step S2, the mixing is ball milling mixing.
[0017] Furthermore, in step S3, the porous composite material is 2-10 wt.% of the mass of the modified positive electrode material.
[0018] Furthermore, the positive electrode material is one or more of a lithium-ion battery layered positive electrode material, a sodium-ion battery layered positive electrode material, spinel lithium manganese oxide, lithium iron phosphate, sodium iron phosphate, and lithium cobalt oxide.
[0019] Furthermore, the chemical formula of the lithium-ion battery layered positive electrode material is LiNi x Co y Mn z O2, where 0.7≤x≤0.8, 0≤y≤0.1, 0.1≤z≤0.3 and x+y+z=1.
[0020] Furthermore, the chemical formula of the sodium ion battery layered cathode material is NaNi x Co y Mn z O2, where 0.7≤x≤0.8, 0≤y≤0.1, 0.1≤z≤0.3 and x+y+z=1.
[0021] Furthermore, in step S3, the solvent used in the wet ball milling is one or more of pure water, n-hexane, methanol, acetone, DMF and NMP.
[0022] Furthermore, in step S3, the wet ball milling time is 2 to 5 hours.
[0023] In a second aspect, a modified positive electrode material is provided, which is prepared by the aforementioned preparation method.
[0024] In a third aspect, a secondary battery is provided, comprising the aforementioned modified positive electrode material.
[0025] Compared with the prior art, one or more of the above technical solutions can achieve at least one of the following beneficial effects: A polymer PDP is obtained by reacting a diketone with a diamine, and then the polymer PDP is mixed with boric acid and subjected to high-temperature insulation treatment to obtain a porous composite material, and the porous composite material is coated on the surface of a positive electrode material to obtain a modified positive electrode material. The rate performance, cycle stability and structural stability of the modified positive electrode material coated with the porous composite material are significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0027] Figure 1 This is the infrared spectrum of polymer A prepared in step (1) of Example 1.
[0028] Figure 2 This is the SEM image of the composite material prepared in step (1) of Example 1.
[0029] Figure 3 This is the XPS graph of the composite material prepared in step (1) of Example 1.
[0030] Figure 4 This is a SEM image of the positive electrode material precursor prepared in step (5) of Example 1.
[0031] Figure 5 This is the SEM image of the positive electrode material prepared in step (6) of Example 1.
[0032] Figure 6 This is a cyclic voltammetry test curve of a battery assembled with the modified positive electrode material prepared in Example 2. DETAILED DESCRIPTION
[0033] The present invention provides a method for preparing a modified positive electrode material, comprising: S1, dissolving a diketone and a diamine in an organic solvent, reacting them under the action of a catalyst, and obtaining a polymer PDP containing both an ester group and an amino group; S2, mixing the polymer PDP with boric acid, and heat-treating the mixture at 700-900° C. in a protective atmosphere to obtain a product, and filtering, washing and drying the product to obtain a porous composite material; S3. The positive electrode material and the porous composite material are subjected to wet ball milling, followed by solid-liquid separation and drying to obtain a modified positive electrode material.
[0034] In some preferred embodiments, the diketone is one or more of 2,5-dimethoxyacyl-1,4-cyclohexanedione, 2,5-diethyl ester-1,4-cyclohexanedione, and 2,5-bis(1-methylethyl ester)-1,4-cyclohexanedione. It is worth noting that although the diketone used in the exemplary embodiment is 2,5-dimethoxyacyl-1,4-cyclohexanedione, 2,5-diethyl ester-1,4-cyclohexanedione and 2,5-bis(1-methylethyl ester)-1,4-cyclohexanedione can also be used as substitutes thereof to play a similar role.
[0035] In some preferred embodiments, the diamine is one or more of p-phenylenediamine, 2,6-diaminonaphthalene, and 2,6-diaminoanthracene. It is worth noting that although the diamine used in the exemplary embodiment is p-phenylenediamine, 2,6-diaminonaphthalene and 2,6-diaminoanthracene can also be used as its substitutes to play a similar role.
[0036] In some preferred embodiments, the catalyst is one or more of p-toluenesulfonamide, triethylamine p-toluenesulfonate, and tetrabutyl p-toluenesulfonate. It is worth noting that, although the catalyst used in the exemplary embodiment is p-toluenesulfonamide, ethylamine p-toluenesulfonate and tetrabutyl p-toluenesulfonate can also be used as polymerization catalysts for diamines and diketones.
[0037] In some preferred embodiments, the organic solvent is one or more of alcohols and chlorobenzene solvents, more preferably a mixed solvent of n-butanol and o-dichlorobenzene; more preferably, the volume ratio of n-butanol to o-dichlorobenzene is 1:1.05 to 1:2.
[0038] In some preferred embodiments, the molar ratio of the diketone to the diamine is 1:1 to 1:1.2, for example, 1:1, 1:1.02, 1:1.05, 1:1.08, 1:1.1, 1:1.12, 1:1.15, 1:1.18, 1:1.2, etc.
[0039] In some preferred embodiments, the amount of the catalyst used is 1.5 mol% to 2.0 mol% of the diketone, for example, 1.5 mol%, 1.6 mol%, 1.7 mol%, 1.8 mol%, 1.9 mol%, 2.0 mol%, etc.
[0040] In some preferred embodiments, the amount of the organic solvent used can be routinely determined according to the solubility of the raw materials, and its function is to dissolve the raw materials.
[0041] In some preferred embodiments, in step S1, the reaction temperature is 100-140°C, for example, 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, etc.; the reaction time is 40-72h, for example, 40h, 45h, 50h, 55h, 60h, 65h, 70h, 72h, etc.
[0042] In some preferred embodiments, in step S2, the weight ratio of the polymer PDP to boric acid is 1:1-1:1.2, for example, 1:1, 1:1.02, 1:1.05, 1:1.08, 1:1.1, 1:1.12, 1:1.15, 1:1.18, 1:1.2, etc.
[0043] In some preferred embodiments, in step S2, the insulation treatment time is 2 to 5 hours, for example, 2 hours, 3 hours, 4 hours, 5 hours, etc.
[0044] In step S2, the protective atmosphere may be a conventional protective atmosphere in the art, for example, a nitrogen atmosphere or an inert gas atmosphere (for example, an inert gas atmosphere such as argon or helium).
[0045] In step S2, the mixing may be carried out by any existing method that can achieve uniform mixing of the two substances. In some embodiments, the mixing may be ball milling or grinding mixing.
[0046] In some preferred embodiments, in step S3, the porous composite material is 2-10wt.% of the mass of the modified positive electrode material, for example, 2wt.%, 3wt.%, 4wt.%, 5wt.%, 6wt.%, 7wt.%, 8wt.%, 9wt.%, 10wt.%, etc.
[0047] Although the modified substrate of the modified positive electrode material in each embodiment is a lithium-ion battery layered positive electrode material, the modification scheme is also applicable to other positive electrode materials. It is worth noting that the modified substrate of the modified material can be a conventional positive electrode material of a lithium-ion battery or a sodium-ion battery in the art; for example, the positive electrode material is a sodium-ion battery layered positive electrode material, a lithium-ion battery layered positive electrode material, spinel lithium manganese oxide, lithium iron phosphate, sodium iron phosphate, lithium cobalt oxide, or one or more of these positive electrode materials can be subjected to conventional doping modification in the art. The chemical formula of the sodium-ion battery layered positive electrode material can be NaNi x Co y Mn z O2, wherein 0.7≤x≤0.8, 0≤y≤0.1, 0.1≤z≤0.3, and x+y+z=1. The chemical formula of the lithium ion battery layered positive electrode material can be LiNi x Co y Mn z O2, where 0.7≤x≤0.8, 0≤y≤0.1, 0.1≤z≤0.3, and x+y+z=1.
[0048] It is worth noting that in the above-mentioned preparation method, the positive electrode material can be prepared by conventional preparation methods in the art, for example, it can be prepared by solid phase sintering method, solvent gel method, spray drying method and the like; when the positive electrode material is a sodium ion battery layered positive electrode material or a lithium ion battery layered positive electrode material, a co-precipitation method can also be used to prepare a hydroxide or carbonate precursor, and then mixed with a sodium source or a lithium source for sintering.
[0049] In some embodiments, the modified substrate of the modified cathode material is a layered cathode material for a lithium-ion battery, which is prepared by a conventional coprecipitation method using a spherical or quasi-spherical hydroxide precursor Ni x Co y Mn z(OH)2, wherein 0.7≤x≤0.8, 0≤y≤0.1, 0.1≤z≤0.3, and x+y+z=1, and the median particle size D50 of the precursor material is 3~4μm. The precursor material is then mixed with a lithium source and sintered to obtain a sodium ion battery layered positive electrode material. The lithium source can be a conventional lithium source for preparing lithium ion battery layered positive electrode materials in the art, such as one or more of lithium hydroxide monohydrate, lithium acetate, lithium carbonate, and lithium sulfate. The amount of lithium source can also be a commonly used amount for preparing lithium ion battery layered positive electrode materials in the art. Specifically, the molar ratio of lithium in the precursor and the lithium source can be 1:1.02~1.05. The sintering mechanism can also adopt conventional sintering methods and process parameters in the art. The sintering temperature can be 650~950℃, the heating rate is 5~10℃ / min, and the calcination time is 10~24h; the sintering atmosphere can adopt a conventional sintering atmosphere in the art, such as an oxygen atmosphere, an air atmosphere, etc.
[0050] In some embodiments, in step S3, the solvent used for the wet ball milling can be one or more of pure water, n-hexane, methanol, acetone, DMF and NMP.
[0051] In some implementation modes, in step S3, the wet ball milling time is 2-5 hours, and the ball mill speed is 300-400 rpm.
[0052] The present invention also provides a modified positive electrode material, which is prepared by the above-mentioned preparation method. The modified positive electrode material includes a positive electrode material matrix and a coating material located at least partially on the surface of the positive electrode material matrix, and the coating material is a composite material of porous carbon compound and boric acid.
[0053] The present invention also provides a secondary battery, which may be a lithium ion battery or a sodium ion battery, comprising the aforementioned modified positive electrode material.
[0054] In order to facilitate the understanding of the present invention, the present invention will be described in more comprehensive and detailed manner below in conjunction with the accompanying drawings and preferred embodiments of the specification, but the protection scope of the present invention is not limited to the following specific embodiments.
[0055] Example 1 The method for preparing the modified positive electrode material comprises the following steps: (1) Take 2,5-dimethoxy-1,4-cyclohexanedione (7.0 g) and p-phenylenediamine (3.5 g) and dissolve them completely in o-dichlorobenzene (10 mL) and n-butanol (10 mL), transfer them to a polymerization tube, then add the catalyst p-toluenesulfonamide (100 mg), ultrasonicate for 3-5 min, transfer to 120 ° C and react for two days. After the reaction is completed, filter and wash to remove impurities, leaving the solid, and dry to obtain the product polymer. The infrared image of the polymer is as follows: Figure 1 As shown in the infrared spectrum, at 3370cm-1 The strong characteristic peak at 1260 cm-1 is attributed to the amino group of the diamine monomer. -1 The characteristic peak at 1630 cm-1 is attributed to the CN group in the diamine monomer; the diketone -1 It has the characteristic absorption peak of carbonyl; after the two monomers are polymerized, 3320cm -1 The characteristic peaks near 1240 cm-1 are attributed to the imino group. -1 and 1200cm -1 The characteristic peak at is attributed to the COC group of the polymer, indicating that the polymer was successfully synthesized. The polymer was prepared by polymerization of diamine monomer and diketone. The polymer was named PDP polymer according to the English name of the raw materials. Subsequently, the PDP polymer and boric acid (weight ratio 1:1.05) were ground and mixed evenly and then placed in a porcelain boat. Under a nitrogen atmosphere, the mixture was transferred to a tube furnace, heated to 800°C at a heating rate of 5°C / min, and reacted at a constant temperature for 3 hours. Boric acid played the role of an activator, dopant and cross-linker in this process. The activator enabled the material to obtain a larger specific surface area, providing a channel for subsequent ion transport; the dopant provided the material with a source of boron; the cross-linker was that during the reaction, due to the action of intermolecular hydrogen bonds, the oxygen in the carbonyl group formed an intermolecular hydrogen bond with the hydroxyl group in the boric acid, and the other oxygen in the ester group formed an N...O bond with the N in the imino group, and the B and N elements were locked in the carbon chain skeleton; after the reaction, the product was filtered out and washed with deionized water 5 times, and the filter cake layer was dried and dehydrated in a vacuum oven at 120°C for 12 hours to obtain a composite material, and its SEM image is shown as follows Figure 2 As shown, from Figure 2 It can be seen that the composite material is a porous material; the XPS full spectrum of the obtained porous composite material is as follows Figure 3 The percentage of B- / N-substances in the porous composite material is shown in Table 1.
[0056] Table 1 Combination Figure 3 From Table 1, it can be seen that the full scan spectrum shows four obvious peaks, B 1s at 190.5 eV, C 1s at 286.1 eV, N 1s at 399.8 eV and O 1s at 531.0 eV, which indicates that the material is mainly composed of four elements B, C, N, and O, confirming that the B element is successfully embedded in the carbon chain skeleton. The source of the B element is boric acid. During the reaction, due to the action of intermolecular hydrogen bonds, the B and N elements are locked in the carbon chain skeleton.
[0057] (2) adding sulfates of nickel, cobalt and manganese into pure water at a molar ratio of 70:10:20 to prepare a ternary metal salt solution with a concentration of 120 g / L; (3) Take 350 mL of 6 mol / L sodium hydroxide solution and 4.2 L of 4 mol / L ammonia solution, mix them into 60 L of pure water as the reaction base liquid, stir them thoroughly and put them into a 100 L reactor, heat and raise the temperature of the reactor to stabilize at 60 °C; (4) At a stirring rate of 800-1000 r / min, the ternary metal salt solution was pumped into the reactor at a flow rate of 1-3 L / h, and a 6 mol / L sodium hydroxide solution and a 4 mol / L ammonia solution were simultaneously introduced, and the pH value and ammonia concentration of the reaction system in the reactor were adjusted in real time within the range of 11.0-12.0 and 5-6 g / L, respectively; the reaction time was maintained between 110-120 h, and the reaction was stopped when the median particle size D50 of the precipitated particles reached 3.5-4 μm; (5) The precipitate was separated and rinsed with hot pure water at 60°C for 5-6 hours. After centrifugal drying, it was transferred to a 130°C oven and dried for 12-15 hours. Subsequently, it was sieved with a 300-mesh vibrating screen to obtain a nickel-cobalt-manganese ternary precursor, whose chemical formula is (Ni 0.70 Co 0.10 Mn 0.20 )(OH)2, its SEM picture is as follows Figure 4 As shown; (6) The nickel-cobalt-manganese ternary precursor and lithium hydroxide monohydrate were fully mixed in a molar ratio of 1:1.05, heated to 850°C in a muffle furnace at a heating rate of 10°C / min, and calcined for 18 hours in a constant temperature pure oxygen atmosphere. After naturally cooling to room temperature, the mixture was crushed and sieved to obtain a layered oxide positive electrode material with a chemical formula of Li[(Ni 0.70 Co 0.10 Mn 0.20 )]O2, its SEM picture is as follows Figure 5 shown.
[0058] (7) Take the nickel-cobalt-manganese positive electrode material (98 g) and the porous composite material (2 g) prepared in step (1), place them in a ball mill, add 3-5 mL of DMF, and wet ball mill them. After ball milling for 3 hours, filter and vacuum dry the filter cake layer to obtain a porous composite material coated modified positive electrode material, wherein the porous composite material accounts for 2 wt.% of the coated modified positive electrode material.
[0059] Example 2 The method for preparing the modified positive electrode material comprises the following steps: (1) Take 2,5-dimethoxy-1,4-cyclohexanedione (7.0 g) and p-phenylenediamine (3.5 g) and dissolve them completely in o-dichlorobenzene (10 mL) and n-butanol (10 mL), transfer them to a polymerization sleeve, then add the catalyst p-toluenesulfonamide (100 mg), ultrasonicate for 3-5 min, and transfer them to 120 ° C for two days. After the reaction is completed, filter and wash to remove impurities, leaving the solid, and dry to obtain the product PDP polymer. Subsequently, grind and mix the PDP polymer and boric acid (weight ratio 1:1.05) evenly, put them into a porcelain boat, transfer them to a tube furnace under a nitrogen atmosphere, heat them to 800 ° C at a heating rate of 5 ° C / min, and react them at a constant temperature for 3 h; after the reaction is completed, filter out the product and wash it with deionized water 5 times, and dry the filter cake layer in a vacuum oven at 120 ° C for 12 h to obtain a porous composite material mainly containing B, N, C, and O.
[0060] (2) adding nickel, cobalt and manganese sulfates into pure water at a molar ratio of 75:10:15 to prepare a ternary metal salt solution with a concentration of 120 g / L; (3) Take 350 mL of 6 mol / L sodium hydroxide solution and 4.2 L of 4 mol / L ammonia solution, mix them into 60 L of pure water as the reaction base liquid, stir them thoroughly and put them into a 100 L reactor, heat and raise the temperature of the reactor to stabilize at 60 °C; (4) At a stirring rate of 800-1000 r / min, the ternary metal salt solution was pumped into the reactor at a flow rate of 1-3 L / h, and a 6 mol / L sodium hydroxide solution and a 4 mol / L ammonia solution were simultaneously introduced, and the pH value and ammonia concentration of the reaction system in the reactor were adjusted in real time within the range of 11.0-12.0 and 5-6 g / L, respectively; the reaction time was maintained between 110-120 h, and the reaction was stopped when the median particle size D50 of the precipitated particles reached 3.5-4 μm; (5) The precipitate was separated and rinsed with hot pure water at 60°C for 5-6 hours. After centrifugal drying, it was transferred to a 130°C oven and dried for 12-15 hours. Subsequently, it was sieved with a 300-mesh vibrating screen to obtain a nickel-cobalt-manganese ternary precursor, whose chemical formula is: (Ni 0.75 Co 0.10 Mn 0.15 )(OH)2; (6) The nickel-cobalt-manganese ternary precursor and lithium hydroxide monohydrate were fully mixed in a molar ratio of 1:1.05, heated to 850°C in a muffle furnace at a heating rate of 10°C / min, and calcined for 18 hours in a constant temperature pure oxygen atmosphere. After naturally cooling to room temperature, the mixture was crushed and sieved to obtain a layered oxide positive electrode material with a chemical formula of Li[(Ni 0.75 Co 0.10 Mn 0.15 )]O2.
[0061] (7) Take nickel-cobalt-manganese positive electrode material (95 g) and porous composite material (5 g) and place them in a ball mill, add 3-5 mL DMF, and perform wet ball milling. After ball milling for 3 h, the filter cake layer is vacuum dried after suction to obtain a porous composite material coated modified positive electrode material, wherein the porous composite material accounts for 5 wt.% of the coated modified positive electrode material.
[0062] Example 3 The method for preparing the modified positive electrode material comprises the following steps: (1) Take 2,5-dimethoxy-1,4-cyclohexanedione (7.0 g) and p-phenylenediamine (3.5 g) and dissolve them completely in o-dichlorobenzene (10 mL) and n-butanol (10 mL), transfer them to a polymerization sleeve, then add the catalyst p-toluenesulfonamide (100 mg), ultrasonicate for 3-5 min, and transfer them to 120 ° C for two days. After the reaction is completed, filter and wash to remove impurities, leaving the solid, and dry to obtain the product PDP polymer. Subsequently, grind and mix the PDP polymer and boric acid (weight ratio 1:1.05) evenly, put them into a porcelain boat, transfer them to a tube furnace under a nitrogen atmosphere, heat them to 800 ° C at a heating rate of 5 ° C / min, and react them at a constant temperature for 3 h; after the reaction is completed, filter out the product and wash it with deionized water 5 times, and dry the filter cake layer in a vacuum oven at 120 ° C for 12 h to obtain a porous composite material mainly containing B, C, N, and O.
[0063] (2) adding nickel, cobalt and manganese sulfates into pure water at a molar ratio of 80:5:15 to prepare a ternary metal salt solution with a concentration of 120 g / L; (3) Take 350 mL of 6 mol / L sodium hydroxide solution and 4.2 L of 4 mol / L ammonia solution, mix them into 60 L of pure water as the reaction base liquid, stir them thoroughly and put them into a 100 L reactor, heat and raise the temperature of the reactor to stabilize at 60 °C; (4) At a stirring rate of 800-1000 r / min, the ternary metal salt solution was pumped into the reactor at a flow rate of 1-3 L / h, and a 6 mol / L sodium hydroxide solution and a 4 mol / L ammonia solution were simultaneously introduced, and the pH value and ammonia concentration of the reaction system in the reactor were adjusted in real time within the range of 11.0-12.0 and 5-6 g / L, respectively; the reaction time was maintained between 110-120 h, and the reaction was stopped when the median particle size D50 of the precipitated particles reached 3.5-4 μm; (5) The precipitate was separated and rinsed with hot pure water at 60°C for 5-6 hours. After centrifugal drying, it was transferred to a 130°C oven and dried for 12-15 hours. Subsequently, it was sieved with a 300-mesh vibrating screen to obtain a nickel-cobalt-manganese ternary precursor, whose chemical formula is: (Ni 0.80 Co 0.05 Mn 0.15)(OH)2; (6) The nickel-cobalt-manganese ternary precursor and lithium hydroxide monohydrate were fully mixed in a molar ratio of 1:1.05, heated to 850°C in a muffle furnace at a heating rate of 10°C / min, and calcined for 18 hours in a constant temperature pure oxygen atmosphere. After naturally cooling to room temperature, the mixture was crushed and sieved to obtain a layered oxide positive electrode material with a chemical formula of Li[(Ni 0.80 Co 0.05 Mn 0.15 )]O2.
[0064] (7) The nickel-cobalt-manganese positive electrode material (92 g) and the porous composite material (8 g) obtained in step (5) were placed in a ball mill, 3-5 mL of DMF were added, and wet ball milling was performed. After ball milling for 3 h, the filter cake layer was vacuum dried after suction filtration to obtain a porous composite material coated modified positive electrode material, wherein the porous composite material accounts for 8 wt.% of the coated modified positive electrode material.
[0065] Comparative Example 1 The difference between this comparative example and Example 1 is that no coating modification is performed, and the preparation method specifically includes: (1) adding nickel, cobalt and manganese sulfates into pure water at a molar ratio of 70:10:20 to prepare a ternary metal salt solution with a concentration of 120 g / L; (2) Take 350 mL of 6 mol / L sodium hydroxide solution and 4.2 L of 4 mol / L ammonia solution, mix them into 60 L of pure water as the reaction base liquid, stir them thoroughly and put them into a 100 L reactor, heat and raise the temperature of the reactor to stabilize at 60 °C; (3) At a stirring rate of 800-1000 r / min, the ternary metal salt solution was pumped into the reactor at a flow rate of 1-3 L / h, and a 6 mol / L sodium hydroxide solution and a 4 mol / L ammonia solution were simultaneously introduced, and the pH value and ammonia concentration of the reaction system in the reactor were adjusted in real time to be within the range of 11.0-12.0 and 5-6 g / L, respectively; the reaction time was maintained between 110-120 h, and the reaction was stopped when the median particle size D50 of the precipitated particles reached 3.5-4 μm; (4) Separate the precipitate, rinse it with hot pure water at 60°C for 5-6 hours, centrifuge and dry it in a 130°C oven for 12-15 hours, and then sieve it with a 300-mesh vibrating screen to obtain a nickel-cobalt-manganese ternary precursor, whose chemical formula is: (Ni 0.70 Co 0.10 Mn 0.20 )(OH)2; (5) The nickel-cobalt-manganese ternary precursor and lithium hydroxide monohydrate were fully mixed in a molar ratio of 1:1.05, heated to 850°C in a muffle furnace at a heating rate of 10°C / min, and calcined for 18 hours in a constant temperature pure oxygen atmosphere. After naturally cooling to room temperature, the mixture was crushed and sieved to obtain a layered oxide positive electrode material with a chemical formula of Li[(Ni 0.70 Co 0.10 Mn 0.20 )]O2.
[0066] Comparative Example 2 The difference between this comparative example and Example 2 is that no coating modification is performed, and the preparation method specifically includes: (1) adding nickel, cobalt and manganese sulfates into pure water at a molar ratio of 75:10:15 to prepare a ternary metal salt solution with a concentration of 120 g / L; (2) Take 350 mL of 6 mol / L sodium hydroxide solution and 4.2 L of 4 mol / L ammonia solution, mix them into 60 L of pure water as the reaction base liquid, stir them thoroughly and put them into a 100 L reactor, heat and raise the temperature of the reactor to stabilize at 60 °C; (3) At a stirring rate of 800-1000 r / min, the ternary metal salt solution was pumped into the reactor at a flow rate of 1-3 L / h, and a 6 mol / L sodium hydroxide solution and a 4 mol / L ammonia solution were simultaneously introduced, and the pH value and ammonia concentration of the reaction system in the reactor were adjusted in real time to be within the range of 11.0-12.0 and 5-6 g / L, respectively; the reaction time was maintained between 110-120 h, and the reaction was stopped when the median particle size D50 of the precipitated particles reached 3.5-4 μm; (4) Separate the precipitate, rinse it with hot pure water at 60°C for 5-6 hours, centrifuge and dry it in a 130°C oven for 12-15 hours, and then sieve it with a 300-mesh vibrating screen to obtain a nickel-cobalt-manganese ternary precursor, whose chemical formula is: (Ni 0.75 Co 0.10 Mn 0.15 )(OH)2; (5) The nickel-cobalt-manganese ternary precursor and lithium hydroxide monohydrate were fully mixed in a molar ratio of 1:1.05, heated to 850°C in a muffle furnace at a heating rate of 10°C / min, and calcined for 18 hours in a constant temperature pure oxygen atmosphere. After naturally cooling to room temperature, the mixture was crushed and sieved to obtain a layered oxide positive electrode material with a chemical formula of Li[(Ni 0.75 Co 0.10 Mn 0.15 )]O2.
[0067] Comparative Example 3 The difference between this comparative example and Example 3 is that no coating modification is performed, and the preparation method specifically includes: (1) adding nickel, cobalt and manganese sulfates into pure water at a molar ratio of 80:5:15 to prepare a ternary metal salt solution with a concentration of 120 g / L; (2) Take 350 mL of 6 mol / L sodium hydroxide solution and 4.2 L of 4 mol / L ammonia solution, mix them into 60 L of pure water as the reaction base liquid, stir them thoroughly and put them into a 100 L reactor, heat and raise the temperature of the reactor to stabilize at 60 °C; (3) At a stirring rate of 800-1000 r / min, the ternary metal salt solution was pumped into the reactor at a flow rate of 1-3 L / h, and a 6 mol / L sodium hydroxide solution and a 4 mol / L ammonia solution were simultaneously introduced, and the pH value and ammonia concentration of the reaction system in the reactor were adjusted in real time within the range of 11.0-12.0 and 5-6 g / L, respectively; the reaction time was maintained between 110-120 h, and the reaction was stopped when the median particle size D50 of the precipitated particles reached 3.5-4 μm; (4) Separate the precipitate, rinse it with hot pure water at 60°C for 5-6 hours, centrifuge and dry it in a 130°C oven for 12-15 hours, and then sieve it with a 300-mesh vibrating screen to obtain a nickel-cobalt-manganese ternary precursor, whose chemical formula is: (Ni 0.80 Co 0.05 Mn 0.15 )(OH)2; (5) The nickel-cobalt-manganese ternary precursor and lithium hydroxide monohydrate were fully mixed in a molar ratio of 1:1.05, heated to 850°C in a muffle furnace at a heating rate of 10°C / min, and calcined for 18 hours in a constant temperature pure oxygen atmosphere. After naturally cooling to room temperature, the mixture was crushed and sieved to obtain a layered oxide positive electrode material with a chemical formula of Li[(Ni 0.80 Co 0.05 Mn 0.15 )]O2.
[0068] The layered oxide positive electrode materials prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were assembled into button-type lithium-ion batteries. The specific process was as follows: 24 mg of positive electrode material, 3 mg of acetylene black and 3 mg of polyvinylidene chloride (PVDF) were weighed and added to a 25 mL weighing bottle, 10 to 12 drops of N-methyl-2-pyrrolidone (NMP) were dripped in and mixed evenly, and stirred for 3 hours after ultrasonic treatment for 20 minutes to obtain a homogeneous black slurry. Subsequently, the slurry was coated on a copper foil with an automatic coating machine, placed under vacuum conditions at 120 ° C for 8 hours to remove the solvent, and pressed with a tablet press at 16 MPa to obtain a positive electrode sheet. The mass of active material loaded on each single working electrode is about 3.0 mg / cm 2. The positive electrode sheet was used as the positive electrode, the lithium sheet was used as the negative electrode, the electrolyte used EC+DMC (molar ratio of 1:1.2) as the solvent, the LiPF6 concentration in the electrolyte was 1 mol / L, and the microporous polyethylene diaphragm was assembled into a 2032 button cell in an argon atmosphere glove box. The button cell was transferred to a constant temperature box at 25°C and subjected to constant current charge and discharge tests on a blue battery test system with a voltage range of 2.7~4.5V. The electrode was first activated by cycling at 0.1C for two cycles, and then cycled at 0.5C for 200 cycles. The first cycle charge and discharge capacity, discharge capacity at 0.5C rate, and capacity retention rate after 200 cycles at 0.5C are shown in Table 1.
[0069] Table 1: It can be seen from Table 1 that the electrochemical performance of the battery assembled by the composite positive electrode material prepared by coating modification in each embodiment is compared with the positive electrode material prepared by the corresponding comparative example without coating modification. It can be seen that the positive electrode material assembled in each embodiment has a high buckle capacity, the first cycle discharge capacity can be as high as 261mAh / g, and the 200-cycle capacity retention rate at a current density of 0.5C can be as high as 88%. It can be seen that the discharge capacity and cycle performance of the modified positive electrode material are significantly improved. After analysis, this may be due to: 1. The porous composite material forms a core-shell structure with the internal nickel-cobalt-manganese matrix material, and the coating layer of the porous composite material effectively alleviates the volume expansion caused by the charging and discharging process, reduces the side reaction of the electrolyte and the positive electrode material, and makes the electrode material have better stability; 2. Due to the molecular covalent bonding of the porous composite material, a porous conductive network is formed, the electrochemical active area is increased, and the electron transmission and ion migration inside the electrode are promoted. Therefore, the electrode material can have high capacity, good cycle stability and rate performance.
[0070] The button cell assembled with the positive electrode material prepared in Example 2 has a cyclic voltammetry curve as shown in Figure 6 As shown. Due to the presence of the porous carbon polymer coating, the electrode activation is slow, so the redox peak of the first cycle CV curve is weak. As the test progresses, Li + It is constantly activated and free in the material crystal framework, and the conductivity of the electrode is further improved, so the redox peak of the second CV curve is enhanced; the redox peak of the third circle is basically consistent with the second circle, indicating that the conductivity of the electrode is stable. The high overlap between the redox peaks of the second and third circles means that the potential value of the material is stable during charging or discharging, indicating that the prepared positive electrode material has good reversibility during charging and discharging, and it can be seen that the material has good electrochemical stability.
[0071] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a modified positive electrode material, characterized in that: include: S1, dissolving a diketone and a diamine in an organic solvent, reacting them under the action of a catalyst, and obtaining a polymer PDP containing both an ester group and an amino group; S2, mixing the polymer PDP with boric acid, and heat-treating the mixture at 700-900° C. under a protective atmosphere to obtain a product, and filtering, washing and drying the product to obtain a porous composite material; S3. The positive electrode material and the porous composite material are subjected to wet ball milling, followed by solid-liquid separation and drying to obtain a modified positive electrode material.
2. The method for preparing the modified positive electrode material according to claim 1, characterized in that: The diketone is one or more of 2,5-dimethoxyacyl-1,4-cyclohexanedione, 2,5-diethylester-1,4-cyclohexanedione, and 2,5-bis(1-methylethylester)-1,4-cyclohexanedione; The diamine is one or more of p-phenylenediamine, 2,6-diaminonaphthalene, and 2,6-diaminoanthracene; The catalyst is one or more of p-toluenesulfonamide, triethylamine p-toluenesulfonate, and tetrabutylammonium p-toluenesulfonate; The organic solvent is one or more of alcohol and chlorobenzene solvents.
3. The method for preparing a modified positive electrode material according to claim 1 or 2, characterized in that: The molar ratio of the diketone to the diamine is 1:1 to 1:1.2; The amount of the catalyst used is 1.5 mol% to 2.0 mol% of the diketone.
4. The method for preparing a modified positive electrode material according to claim 1 or 2, characterized in that: In step S1, the reaction temperature is 100-140° C.; the reaction time is 40-72 hours.
5. The method for preparing a modified positive electrode material according to claim 1 or 2, characterized in that: In step S2, the weight ratio of the polymer PDP to boric acid is 1:1 to 1:1.
2.
6. The method for preparing a modified positive electrode material according to claim 1 or 2, characterized in that: In step S2, the heat preservation treatment time is 2 to 5 hours; In step S2, the protective atmosphere is a nitrogen atmosphere or an inert gas atmosphere; In step S2, the mixing is ball milling mixing.
7. The method for preparing a modified positive electrode material according to claim 1 or 2, characterized in that: In step S3, the porous composite material is 2-10wt.% of the mass of the modified positive electrode material; The positive electrode material is one or more of a lithium ion battery layered positive electrode material, a sodium ion battery layered positive electrode material, spinel lithium manganese oxide, lithium iron phosphate, sodium iron phosphate, and lithium cobalt oxide; The chemical formula of the lithium-ion battery layered positive electrode material is LiNi x Co y Mn z O2, where 0.7≤x≤0.8, 0≤y≤0.1, 0.1≤z≤0.3 and x+y+z=1; The chemical formula of the sodium ion battery layered cathode material is NaNi x Co y Mn z O2, where 0.7≤x≤0.8, 0≤y≤0.1, 0.1≤z≤0.3 and x+y+z=1.
8. The method for preparing a modified positive electrode material according to claim 1 or 2, characterized in that: In step S3, the solvent used for the wet ball milling is one or more of pure water, n-hexane, methanol, acetone, DMF and NMP; In step S3, the wet ball milling time is 2 to 5 hours.
9. A modified positive electrode material, characterized in that: The method is prepared according to any one of claims 1 to 8.
10. A secondary battery, characterized in that: Includes the modified positive electrode material as described in claim 9.
Citation Information
Patent Citations
Method for preparing porous carbon coated nickel-doped lithium cobalt oxide composite anode material
CN104393287A
Nitrogen-boron co-doped carbon quantum dot coated nickel cobalt lithium aluminate battery cathode material and preparation method
CN110098394A
Modified boron-doped lithium-rich manganese-based anode material, and preparation method and application thereof
CN110429268A
Pre-oxidation preparation process of surface modified nickel cobalt lithium manganate ternary positive electrode material
CN114335506A
Coated modified lithium cobalt oxide material and preparation method thereof, positive plate and lithium ion battery
CN114551826A