Zirconium oxide-calcium zirconate composite ceramic as well as preparation method and application thereof
By forming a calcium zirconate coating in zirconia ceramics, the high thermodynamic stability and corrosion resistance of calcium zirconate are used to solve the problems of brittleness and low strength of zirconia ceramics, and the excellent performance of zirconia-zirconic acid is prepared. Calcium composite ceramics are suitable for crucibles for high-temperature alloy smelting, achieving performance improvement and cost reduction.
Patent Information
- Application Number
- CN202411121697.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-15
AI Technical Summary
Due to its brittleness, low fracture toughness and low strength, zirconia ceramics are difficult to meet the market demand for crucibles for high-temperature alloy smelting.
The mixed calcination of zirconium oxide and calcium carbonate is used to generate calcium zirconate coated zirconium oxide particles, and sintering is used to prepare zirconium oxide-calcium zirconate composite ceramics, which are used to improve the ceramics by using the high thermodynamic stability and corrosion resistance of calcium zirconate. comprehensive performance.
The thermal shock resistance of zirconia ceramics is significantly improved, the preparation process is simplified, the cost is reduced, and excellent performance is shown in high-temperature alloy smelting.
Smart Images

Figure CN118878321A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of ceramics, and in particular to a zirconium oxide-calcium zirconate composite ceramic and a preparation method and application thereof. Background Art
[0002] High-temperature alloys play a vital role in today's social production. Their unique properties enable them to maintain stable mechanical properties and chemical stability in extreme environments such as high temperature and high pressure. Because of their excellent high-temperature performance, good mechanical properties and thermal corrosion resistance as well as good comprehensive performance, high-temperature alloys play an important role in aerospace, energy, and chemical industries. However, the widespread application of high-temperature alloys is restricted by their high production costs. At present, vacuum induction melting is a typical process for the preparation of high-temperature alloys, and crucibles are important refractory materials in this process and are indispensable. With the development of high-temperature alloys to higher generations, new challenges have been raised for the selection of crucible materials and the improvement of structural stability.
[0003] Zirconia ceramics are the materials with the best comprehensive toughness and strength among known oxide ceramics. Due to their superior thermal stability and good mechanical properties, in recent years, zirconia ceramics have been widely used as refractory materials in industrial production as crucibles for high-temperature alloy smelting, and have been rapidly developed and applied in many aspects. However, zirconia has three crystal forms: monoclinic, tetragonal, and cubic. The transformation from tetragonal to monoclinic is a martensitic phase transformation, which will produce 8% shear strain and 3% to 5% volume change. Therefore, ZrO 2 The inherent brittleness, low fracture toughness and low strength of ceramics limit their application range. In order to improve the 2 In order to improve the comprehensive performance of ceramics and meet market demand, researchers have conducted extensive research from aspects such as material composition design, doping modification, and process improvement.
[0004] Calcium zirconate material is a perovskite crystal structure with high thermodynamic stability, excellent corrosion resistance, strong temperature bearing capacity, and is not prone to polycrystalline transformation. It has potential advantages as a crucible material for high-temperature alloys. Combining the excellent toughness and strength comprehensive properties of zirconia ceramics and the high thermodynamic stability and non-polycrystalline transformation characteristics of calcium zirconate materials, a ZrO 2 -CaZrO 3 Composite ceramics are very promising for making crucibles for high-temperature alloy smelting. Summary of the invention
[0005] The object of the present invention is to provide a zirconium oxide-calcium zirconate composite ceramic and a preparation method and application thereof, so as to solve the problem that zirconium oxide ceramics are difficult to meet market demand due to their brittleness, low fracture toughness and low strength.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The present invention provides a method for preparing a zirconium oxide-calcium zirconate composite ceramic, comprising the following steps:
[0008] 1) mixing zirconium oxide and calcium carbonate and calcining the mixture to obtain zirconium oxide particles coated with calcium zirconate;
[0009] 2) The calcium zirconate-coated zirconium oxide particles are mixed with zirconium oxide, pressed into shape, and then sintered to obtain zirconium oxide-calcium zirconate composite ceramics.
[0010] Preferably, in step 1), the mass ratio of zirconium oxide to calcium carbonate is 100-110:10-12.
[0011] Preferably, the mixing method in step 1) is ball milling;
[0012] The rotation speed of the ball milling mixing is 80-200 r / min, the time of the ball milling mixing is 180-240 min, and the ball-to-material ratio of the ball milling mixing is 1.5-2:1.
[0013] Preferably, the calcination temperature in step 1) is 1400-1600° C., and the calcination time is 180-240 min.
[0014] Preferably, the temperature raising procedure of the calcination in step 1) is to raise the temperature to 1000° C. at a rate of 8 to 10° C. / min and then raise the temperature to the calcination temperature at a rate of 3 to 5° C. / min.
[0015] Preferably, in step 2), the mass ratio of the calcium zirconate-coated zirconium oxide particles to zirconium oxide is 0.5-1.5:1.
[0016] Preferably, the pressing molding in step 2) includes sequentially performing dry pressing preforming and cold isostatic pressing preforming;
[0017] The dry pressing preforming pressure is 50-80 MPa, and the holding time of the dry pressing preforming is 1-3 min;
[0018] The pressure of the cold isostatic pressing preforming is 150-300 MPa, and the holding time of the cold isostatic pressing preforming is 60-90 seconds.
[0019] Preferably, the sintering temperature in step 2) is 1400-1600° C., and the sintering time is 3-4 hours.
[0020] The invention provides a zirconium oxide-calcium zirconate composite ceramic prepared by the above preparation method.
[0021] The present invention also provides an application of the zirconium oxide-calcium zirconate composite ceramic in high-temperature alloy smelting.
[0022] The present invention has at least the following beneficial effects:
[0023] The present invention uses heating to react zirconium oxide and calcium carbonate to generate calcium zirconate, and the generated calcium zirconate is evenly coated on zirconium oxide particles. The obtained calcium zirconate-coated zirconium oxide particles have excellent performance, and comprehensively utilize the characteristics of calcium zirconate materials such as high thermodynamic stability, excellent corrosion resistance, strong temperature bearing capacity, and not prone to polycrystalline transformation, which can greatly improve the thermal shock resistance of zirconium oxide ceramics. In addition, the preparation process is simple to operate, the preparation cycle is short, and the cost is low. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 is the XRD pattern of the calcium zirconate-coated zirconium oxide particles prepared in Example 1;
[0025] Figure 2 This is a SEM image of the calcium zirconate-coated zirconium oxide particles prepared in Example 1;
[0026] Figure 3 This is a SEM image of the calcium zirconate-coated zirconium oxide particles prepared in Example 2;
[0027] Figure 4 This is the SEM image of the calcium zirconate-coated zirconium oxide particles prepared in Example 2. DETAILED DESCRIPTION
[0028] The present invention provides a method for preparing a zirconium oxide-calcium zirconate composite ceramic, comprising the following steps:
[0029] 1) mixing zirconium oxide and calcium carbonate and calcining the mixture to obtain zirconium oxide particles coated with calcium zirconate;
[0030] 2) The calcium zirconate-coated zirconium oxide particles are mixed with zirconium oxide, pressed into shape, and then sintered to obtain zirconium oxide-calcium zirconate composite ceramics.
[0031] In the present invention, the mass ratio of zirconium oxide to calcium carbonate in step 1) is 100-110:10-12, preferably 102-108:10.5-11.5, more preferably 104-106:11, and more preferably 105:11.
[0032] In the present invention, the mixing method in step 1) is ball milling mixing.
[0033] In the present invention, the rotation speed of the ball milling mixing is 80-200 r / min, preferably 100-180 r / min, more preferably 120-160 r / min, and more preferably 140-150 r / min; the ball milling mixing time is 180-240 min, preferably 190-230 min, and more preferably 200-220 min; the ball-to-material ratio of the ball milling mixing is 1.5-2:1, preferably 1.6-1.9:1, and more preferably 1.7-1.8:1.
[0034] In the present invention, ethanol needs to be added as a co-solvent during the ball milling mixing process.
[0035] In the present invention, after the ball milling is completed, the powder is subjected to rotary evaporation and sieving in sequence; the rotary evaporation temperature is 60° C., the rotary evaporation time is 20 min; and the sieving is through a 60-mesh sieve.
[0036] In the present invention, the calcination temperature in step 1) is 1400-1600°C, preferably 1500-1600°C, more preferably 1550-1600°C, and more preferably 1600°C; the calcination time is 180-240 min, preferably 190-230 min, and more preferably 200-220 min.
[0037] In the present invention, the temperature rising program of calcination in step 1) is to heat up to 1000°C at a rate of 8-10°C / min and then heat up to the calcination temperature at a rate of 3-5°C / min, preferably to heat up to 1000°C at a rate of 8-9°C / min and then heat up to the calcination temperature at a rate of 3-4°C / min.
[0038] In the present invention, the mass ratio of the calcium zirconate-coated zirconium oxide particles to zirconium oxide in step 2) is 0.5-1.5:1, preferably 0.7-1.3:1, more preferably 0.8-1.2:1, and more preferably 0.9-1:1.
[0039] In the present invention, the pressing molding in step 2) includes dry pressing preforming and cold isostatic pressing preforming performed sequentially;
[0040] In the present invention, the dry pressing preforming pressure is 50-80 MPa, preferably 55-75 MPa, more preferably 60-70 MPa, and more preferably 65 MPa; the holding time of the dry pressing preforming is 1-3 min, preferably 2-3 min.
[0041] In the present invention, the pressure of the cold isostatic pressing preforming is 150-300 MPa, preferably 170-280 MPa, more preferably 190-250 MPa, and more preferably 210-230 MPa; the holding time of the cold isostatic pressing preforming is 60-90 s, preferably 65-85 s, more preferably 70-80 s, and more preferably 75 s.
[0042] In the present invention, the sintering temperature in step 2) is 1400-1600°C, preferably 1430-1580°C, more preferably 1450-1550°C, and more preferably 1480-1520°C; the sintering time is 120-240min, preferably 150-210min, more preferably 170-200min, and more preferably 180-190min.
[0043] The invention provides a zirconium oxide-calcium zirconate composite ceramic prepared by the above preparation method.
[0044] The present invention also provides an application of the zirconium oxide-calcium zirconate composite ceramic in high-temperature alloy smelting.
[0045] In the present invention, the zirconium oxide-calcium zirconate composite ceramic is preferably used as a crucible in high-temperature alloy smelting.
[0046] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0047] Example 1
[0048] 1) Add 10.8 g zirconium oxide powder and 1.2 g calcium carbonate powder into a wide-mouth bottle and use a ball mill for ball milling. The mass ratio of grinding balls, ethanol and powder is 1.5:1.2:1. The rotation speed is 90 r / min and the mixing time is 240 min. After ball milling, rotary steam is performed at 60°C for 20 min. The powder obtained after rotary steaming is passed through a 60-mesh sieve to obtain a mixed powder.
[0049] 2) Place the mixed powder in a mortar and grind it evenly. Spread the evenly mixed powder in a crucible, then place the crucible in a muffle furnace, set the heating and cooling system, and start heating. The heating and cooling system is set as follows: when the temperature is below 1000°C, maintain the heating rate at 8°C / min. When the temperature rises to 1000°C, adjust the heating rate to 5°C / min, heat to 1600°C, and keep it for 180 minutes. After the insulation is completed, when the temperature is above 1000°C, maintain the cooling rate at 5°C / min. When the temperature drops to 1000°C, adjust the cooling rate to cool with the furnace. Record the temperature changes during the sintering process. Turn off the heating after cooling to room temperature. Grind and sieve the obtained particles in turn to prepare dispersed calcium zirconate-coated zirconium oxide particles.
[0050] 3) 5 g of the obtained calcium zirconate-coated zirconium oxide particles were ball-milled with 5 g of ordinary zirconium oxide powder (ball-to-material ratio of 1.5:1, rotation speed of 90 r / min, ball milling time of 240 min), and then dry-pressed preformed (70 MPa, holding pressure of 90 s), and then the dry-pressed preformed body was cold isostatically preformed (200 MPa, holding pressure of 90 s) to obtain a green body; the green body was conventionally sintered (1500 ° C, 180 min) to prepare ZrO 2 -CaZrO 3 Composite ceramics.
[0051] The calcium zirconate-coated zirconium oxide particles prepared in this example were subjected to an X-ray diffraction experiment. The XRD pattern is shown in FIG. Figure 1 As shown, from Figure 1 It can be seen that CaZrO is generated in the powder 3 , the powder is CaZrO 3 with ZrO 2 mixture. Figure 2 This is a scanning electron microscope image of the calcium zirconate-coated zirconium oxide particles prepared in this example. Figure 2 It can be seen that the generated CaZrO 3 Uniformly coated on ZrO 2 Particle surface.
[0052] Example 2
[0053] 1) Add 10.8g zirconium oxide powder and 1.2g calcium carbonate powder into a wide-mouth bottle and use a ball mill for ball milling. The ratio of grinding balls, ethanol and powder is 1.5:1.2:1, the rotation speed is 90r / min, and the mixing time is 240min. After ball milling, rotary steam is performed at 60°C for 20min. The powder obtained after rotary steaming is passed through a 60-mesh sieve to obtain a mixed powder.
[0054] 2) Place the mixed powder in a mortar and grind it evenly. Spread the evenly mixed powder in a crucible, then place the crucible in a muffle furnace, set the heating and cooling system, and start heating. The heating and cooling system is set as follows: when the temperature is below 1000°C, maintain the heating rate at 8°C / min. When the temperature rises to 1000°C, adjust the heating rate to 5°C / min, heat to 1600°C, and keep it for 240 minutes. After the insulation is completed, when the temperature is above 1000°C, maintain the cooling rate at 5°C / min. When the temperature drops to 1000°C, adjust the heating rate to cool with the furnace. Record the temperature changes during the sintering process. Turn off the heating after cooling to room temperature. Grind and sieve the obtained particles in turn to prepare dispersed calcium zirconate-coated zirconium oxide particles.
[0055] 3) 5 g of the obtained calcium zirconate-coated zirconium oxide particles were ball-milled with 5 g of ordinary zirconium oxide powder (ball-to-material ratio of 1.5:1, rotation speed of 90 r / min, ball milling time of 240 min), and then dry-pressed preformed (70 MPa, holding pressure of 1.5 min), and then the dry-pressed preformed body was cold isostatically preformed (200 MPa, holding pressure of 90 s) to obtain a green body; the green body was microwave sintered (1500 ° C, 180 min) to prepare ZrO 2 -CaZrO 3 Composite ceramics.
[0056] Figure 3 and Figure 4 This is a scanning electron microscope image of the calcium zirconate-coated zirconium oxide particles prepared in this example. It can be seen from the figure that ZrO 2 and CaCO 3 The reaction generates calcium zirconate, and the generated CaZrO 3 Uniformly coated on ZrO 2 On particles.
[0057] Example 3
[0058] 1) Add 10g zirconium oxide powder and 1.1g calcium carbonate powder into a wide-mouth bottle and use a ball mill for ball milling. The ratio of grinding balls, ethanol and powder is 1.8:1.5:1, the rotation speed is 120r / min, and the mixing time is 180min. After ball milling, rotary steam is performed at 60°C for 20min. The powder obtained after rotary steaming is passed through a 60-mesh sieve to obtain a mixed powder.
[0059] 2) Place the mixed powder in a mortar and grind it evenly. Spread the evenly mixed powder in a crucible, then place the crucible in a muffle furnace, set the heating and cooling system, and start heating. The heating and cooling system is set as follows: when the temperature is below 1000°C, maintain the heating rate at 10°C / min. When the temperature rises to 1000°C, adjust the heating rate to 5°C / min, heat to 1550°C, and keep it for 200 minutes. After the insulation is completed, when the temperature is above 1000°C, maintain the cooling rate at 5°C / min. When the temperature drops to 1000°C, adjust the heating rate to cool with the furnace. Record the temperature changes during the sintering process. Turn off the heating after cooling to room temperature. Grind and sieve the obtained particles in turn to prepare dispersed calcium zirconate-coated zirconium oxide particles.
[0060] 3) 7.5 g of the obtained calcium zirconate-coated zirconium oxide particles were ball-milled with 5 g of ordinary zirconium oxide powder (ball-to-material ratio of 1.5:1, rotation speed of 90 r / min, ball milling time of 240 min), and then dry-pressed preformed (80 MPa, holding pressure for 2 min), and then the dry-pressed preformed body was cold isostatically preformed (250 MPa, holding pressure for 60 s) to obtain a green body; the green body was microwave sintered (1600 ° C, 4 h) to prepare ZrO 2 -CaZrO 3 Composite ceramics.
[0061] Example 4
[0062] 1) Add 11g zirconium oxide powder and 1g calcium carbonate powder into a wide-mouth bottle and use a ball mill for ball milling. The ratio of grinding balls, ethanol and powder is 1.5:1.2:1, the rotation speed is 150r / min, and the mixing time is 200min. After ball milling, rotary steam is performed at 60°C for 20min. The powder obtained after rotary steaming is passed through a 60-mesh sieve to obtain a mixed powder.
[0063] 2) Place the mixed powder in a mortar and grind it evenly. Spread the evenly mixed powder in a crucible, then place the crucible in a muffle furnace, set the heating and cooling system, and start heating. The heating and cooling system is set as follows: when the temperature is below 1000°C, maintain the heating rate at 9°C / min. When the temperature rises to 1000°C, adjust the heating rate to 4°C / min, heat to 1500°C, and keep it for 220 minutes. After the insulation is completed, when the temperature is above 1000°C, maintain the cooling rate at 5°C / min. When the temperature drops to 1000°C, adjust the heating rate to cool with the furnace. Record the temperature changes during the sintering process. Turn off the heating after cooling to room temperature. Grind and sieve the obtained particles in turn to prepare dispersed calcium zirconate-coated zirconium oxide particles.
[0064] 3) 6 g of the obtained calcium zirconate-coated zirconium oxide particles were ball-milled with 5 g of ordinary zirconium oxide powder (ball-to-material ratio of 1.5:1, rotation speed of 90 r / min, ball milling time of 240 min), and then dry pressed (80 MPa, holding pressure for 3 min), and then the dry pressed preformed body was cold isostatically preformed (230 MPa, holding pressure for 90 s) to obtain a green body; the green body was microwave sintered (1600 ° C, 200 min) to prepare ZrO 2 -CaZrO 3 Composite ceramics.
[0065] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing zirconium oxide-calcium zirconate composite ceramics, characterized in that: The following steps are involved: 1) mixing zirconium oxide and calcium carbonate and calcining the mixture to obtain zirconium oxide particles coated with calcium zirconate; 2) The calcium zirconate-coated zirconium oxide particles are mixed with zirconium oxide, pressed into shape, and then sintered to obtain zirconium oxide-calcium zirconate composite ceramics.
2. The method for preparing a zirconium oxide-calcium zirconate composite ceramic according to claim 1, characterized in that: The mass ratio of zirconium oxide to calcium carbonate in step 1) is 100-110:10-12.
3. The method for preparing a zirconium oxide-calcium zirconate composite ceramic according to claim 2, characterized in that: The mixing method in step 1) is ball milling; The rotation speed of the ball milling mixing is 80-200 r / min, the time of the ball milling mixing is 180-240 min, and the ball-to-material ratio of the ball milling mixing is 1.5-2:
1.
4. The method for preparing a zirconium oxide-calcium zirconate composite ceramic according to claim 2 or 3, characterized in that: The calcination temperature in step 1) is 1400-1600° C., and the calcination time is 180-240 min.
5. The method for preparing a zirconium oxide-calcium zirconate composite ceramic according to claim 4, characterized in that: The temperature raising procedure of the calcination in step 1) is to raise the temperature to 1000° C. at a rate of 8 to 10° C. / min and then raise the temperature to the calcination temperature at a rate of 3 to 5° C. / min.
6. The method for preparing a zirconium oxide-calcium zirconate composite ceramic according to claim 5, characterized in that: In step 2), the mass ratio of the calcium zirconate-coated zirconium oxide particles to zirconium oxide is 0.5-1.5:
1.
7. The method for preparing a zirconium oxide-calcium zirconate composite ceramic according to claim 6, characterized in that: The pressing molding in step 2) includes dry pressing preforming and cold isostatic pressing preforming performed sequentially; The dry pressing preforming pressure is 50-80 MPa, and the holding time of the dry pressing preforming is 1-3 min; The pressure of the cold isostatic pressing preforming is 150-300 MPa, and the holding time of the cold isostatic pressing preforming is 60-90 seconds.
8. The method for preparing a zirconium oxide-calcium zirconate composite ceramic according to claim 7, characterized in that: The sintering temperature in step 2) is 1400-1600° C., and the sintering time is 3-4 hours.
9. The zirconium oxide-calcium zirconate composite ceramic prepared by the method for preparing a zirconium oxide-calcium zirconate composite ceramic according to any one of claims 1 to 8.
10. Use of the zirconium oxide-calcium zirconate composite ceramic according to claim 9 in high temperature alloy smelting.
Citation Information
Patent Citations
Production of calcium zirconate
JP1997142929A
Firing setter
JP2012056831A
CaO-ZrO2 COMPOSITION, METHOD OF PRODUCING CaO-ZrO2 COMPOSITION, CaO-ZrO2 CONTAINED REFRACTORY, AND CASTING NOZZLE
JP2021070048A
Material for sintering appliance
TW405132B
Thermal shock-resistant and corrosion-resistant ceramic material based on calcium zirconate and process for the production thereof
WO2013124183A2