Water-phase synergistic coagulation process production line and production process of graphene oxide modified natural rubber master batch

Through the water-phase synergistic sinking process production line of graphene oxide modified natural rubber, the problems of many natural rubber production lines and low drying efficiency in the existing technology are solved, and high-performance graphene oxide modified natural rubber master glue is realized. Production reduces costs and improves production efficiency and quality stability.

CN118878720APending Publication Date: 2024-11-01ZHONGBEI UNIV +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410970123.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing natural rubber production lines have many processes, low drying efficiency and unstable quality after drying, resulting in long production cycles, large energy consumption and high cost of graphene modified natural rubber, and the inability to realize instant modification of graphene oxide. Production of high performance master glue.

Method used

The production line of water-phase synergistic polymerization process using graphene oxide modified natural rubber, including the modified graphene oxide aqueous dispersion production system and the graphene oxide modified natural rubber master rubber production system, through ultrasonic reactors, flocculation devices, The glue device and segmented drying device realize the modification and automated monitoring and control of graphene oxide, reduce manual operation strength, improve production efficiency and product quality stability.

Benefits of technology

Real-time modification of graphene oxide and the production of high-performance masterbatches have been achieved, which reduces production costs, improves production efficiency and product quality stability, and optimizes the drying process to improve the quality and production efficiency of rubber masterbatches.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118878720A_ABST
    Figure CN118878720A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of rubber production, in particular to a water-phase synergistic coagulation process production line and production process of graphene oxide modified natural rubber masterbatch, and the water-phase synergistic coagulation process production line comprises a modified graphene oxide aqueous dispersion production system and a graphene oxide modified natural rubber masterbatch production system; the modified graphene oxide aqueous dispersion liquid production system comprises a graphene oxide slurry storage tank, a modifier dispersion liquid storage tank and an ultrasonic reaction kettle, and the graphene oxide modified natural rubber master batch production system comprises a latex storage tank, a flocculant storage tank, a mixing kettle, a flocculation device and a gluing device. The latex storage tank and the ultrasonic reaction kettle are respectively communicated with the mixing kettle through pipelines; according to the invention, instant use of modified graphene oxide can be realized, so that high-performance rubber master batch can be obtained after the modified graphene oxide is added into natural latex; in addition, the rotating speed of the motor and the rubber drying temperature can be regulated and controlled, so that the quality of the obtained rubber master batch product has very high consistency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rubber production, and in particular to an aqueous phase synergistic coagulation process production line and a production process for graphene oxide modified natural rubber masterbatch. Background Art

[0002] Natural rubber is a natural polymer compound with cis-1,4-polyisoprene as the main component. It is an elastic solid made from natural latex collected from rubber trees through coagulation, drying and other processing procedures. It is an important industrial raw material and is widely used in tires, conveyor belts, hoses, sealing rings and other fields.

[0003] Graphene is a sp 2 New materials with hybrid connected carbon atoms tightly stacked into a single-layer two-dimensional honeycomb lattice structure have excellent optical, electrical and mechanical properties, and have broad application prospects in the fields of materials, micro-nano processing, energy, biomedicine and drug delivery, and are considered to be a revolutionary material in the future. One of the most representative ones, graphene oxide (GO), is a two-dimensional (2D) material with multiple oxygen-containing functional groups obtained by oxidizing graphite through physical and chemical means.

[0004] Graphene and its derivatives have excellent mechanical strength, electrical conductivity and thermal conductivity, making them widely used in rubber reinforcement modification, so that the prepared rubber products have better mechanical strength, toughness and thermal conductivity. However, the latex co-precipitation method currently used to prepare graphene-modified natural rubber masterbatch has problems such as long production cycle and high energy consumption due to the dehydration and drying process. In addition, it will increase costs, which has become one of the main obstacles restricting the application of graphene-modified natural rubber.

[0005] In addition, most of the existing natural rubber masterbatch production lines are "standard rubber" production lines and "full latex" production lines. There are the following problems: First, it is impossible to achieve immediate modification of graphene oxide and then use it immediately in the production line, which leads to reduced activity of modified graphene oxide, and thus it is impossible to obtain high-performance masterbatch; in addition, there are many processes, so there are many personnel configurations. Second, the production lines basically use a drying temperature of 60°C for hot air drying, which is a compromise solution that comprehensively considers the drying efficiency and the quality of the rubber after drying, but there are problems such as low drying efficiency and unstable quality of the masterbatch after drying. Summary of the invention

[0006] In order to solve the problems of multiple processes in the current natural rubber production line and unstable quality of the rubber after drying, the present invention proposes an aqueous phase synergistic coagulation process production line and production process for graphene oxide modified natural rubber masterbatch, which can realize full-process monitoring and automatic control of the natural rubber masterbatch production line, reduce the intensity of manual operation, improve production efficiency and product quality stability, thereby stably producing high-performance graphene modified natural rubber masterbatch.

[0007] The present invention is realized by the following technical scheme: a water phase synergistic coagulation process production line of graphene oxide modified natural rubber masterbatch, including a modified graphene oxide water dispersion production system and a graphene oxide modified natural rubber masterbatch production system;

[0008] The modified graphene oxide aqueous dispersion production system comprises a graphene oxide slurry storage tank, a modifier dispersion storage tank and an ultrasonic reactor, wherein the graphene oxide slurry storage tank and the modifier dispersion storage tank are respectively connected to the ultrasonic reactor through pipelines, and metering pumps are respectively arranged in series on the pipelines between the graphene oxide slurry storage tank, the modifier dispersion storage tank and the ultrasonic reactor;

[0009] The graphene oxide modified natural rubber masterbatch production system comprises a latex storage tank, a flocculant storage tank, a mixing kettle, a flocculation device and a gluing device; the latex storage tank and the ultrasonic reactor are respectively connected to the mixing kettle through pipelines; and metering pumps are respectively arranged in series on the pipelines connecting the latex storage tank, the ultrasonic reactor and the mixing kettle;

[0010] The flocculation device comprises a flocculation tank, and the flocculant storage tank is connected to the flocculation tank through a pipeline; a metering pump is arranged in series on the pipeline connecting the flocculant storage tank and the flocculation tank; the gluing device comprises a gluing platform and a transmission roller rotatably arranged on the gluing platform, and at least one creping machine is arranged at the discharge end of the transmission roller in sequence, and each creping machine is provided with a transmission belt at the discharge end; the discharge end of the last transmission belt is located at the upper part of the feed end of the pelletizer; the discharge end of the pelletizer is connected to the feed end of the cleaning water tank; a feeding pump is arranged at the discharge end of the cleaning water tank, and the discharge end of the feeding pump is connected to the drying device through a pipeline;

[0011] The drying device comprises a conveyor belt, which is located below the discharge end of the feeding pump; two drying bins are arranged side by side in sequence on the conveyor belt along the material conveying direction, and the conveyor belt can convey materials in the drying bins through a driving mechanism, and the drying bins are provided with heat-insulating door curtains, and centrifugal fans and air supply fans are correspondingly arranged on the tops; a heating device is correspondingly arranged at the air inlet of the air supply fan, and the air outlet of the air supply fan is respectively connected to the air inlet of the drying bin, and the air inlet of the centrifugal fan is respectively connected to the air outlet of the drying bin; a drying device is arranged at the front end of the air inlet pipeline of at least one drying bin near the heating device, and the drying device is filled with a drying medium;

[0012] The conveyor belt can convey the material to the material platform.

[0013] As a further improvement of the technical solution of the production line of the present invention, the flocculation device also includes a supporting base, the flocculation tank is located above the supporting base, and the bottom of the discharge end of the flocculation tank is rotatably connected to one side of the upper surface of the supporting base, and a lifting cylinder is arranged inside the other side of the supporting base, and the telescopic end of the lifting cylinder passes through the supporting base and contacts and supports the bottom of the feed end of the flocculation tank.

[0014] As a further improvement of the technical solution of the production line of the present invention, a baling machine is also included.

[0015] As a further improvement of the technical solution of the production line of the present invention, the power range of the ultrasonic reactor is 1-10KW, and the temperature range is 25-120°C.

[0016] The present invention also provides a production process of a water-phase synergistic coagulation process of graphene oxide modified natural rubber masterbatch, which adopts the production line as described above and comprises the following steps:

[0017] S1. The natural rubber latex in the latex storage tank is pumped into a mixing kettle through a metering pump, and then deionized water is added and mixed to obtain a certain concentration of natural rubber latex;

[0018] S2. sequentially adding the graphene oxide slurry in the graphene oxide slurry storage tank and the modifier dispersion in the modifier dispersion storage tank to the ultrasonic reactor through a metering pump, reacting at a certain temperature for a certain time to obtain a modified graphene oxide aqueous dispersion;

[0019] S3. adding the modified graphene oxide aqueous dispersion in the ultrasonic reactor obtained in step S2 to the natural rubber latex in the mixing kettle obtained in step S1, and stirring and mixing them sufficiently to obtain a uniform graphene oxide modified natural rubber mixed emulsion; sequentially adding the graphene oxide modified natural rubber mixed emulsion and the flocculant in the flocculant storage tank to the flocculation tank, mixing them uniformly and flocculating the latex to obtain a flocculated graphene oxide modified natural rubber block;

[0020] S4. The graphene oxide modified natural rubber floccules obtained in step S3 are dragged through each creping machine and the transmission belt in sequence by the gluing device for continuous creping. The rotation speed of the creping machine is controlled according to the glue output speed, so that the rubber sheet passes through the last transmission belt evenly and is conveyed to the granulator for granulation without clogging; S5. The rubber particles obtained in step S4 are washed and deacidified in a washing water tank, and then pumped to the conveyor belt by a feeding pump; the hot air generated by the heating device is conveyed to the drying bin through the air supply fan, and the centrifugal fan discharges the hot and humid air in the drying bin respectively; the rubber particles on the conveyor belt are sequentially passed through the drying bin for drying treatment, so that the material is quickly dried by high temperature in the first drying bin for most of the water, and then the low-temperature dry air is quickly absorbed by the remaining water in the last drying bin, so that the production efficiency and quality stability of the modified natural rubber masterbatch are improved at the same time;

[0021] S6. Quantitatively weigh the dried rubber particles obtained in step S5, and then pack them using a packing machine to obtain a high-performance graphene oxide-modified natural rubber masterbatch product.

[0022] As a further improvement of the technical solution of the production process of the present invention, in step S1, the concentration of the obtained natural rubber latex is such that it can be stably transported by a metering pump.

[0023] As a further improvement of the production process technical solution of the present invention, in step S2, the concentration of the graphene oxide slurry is such that it can be stably delivered by a metering pump, and the concentration of the modifier dispersion is such that it can be stably delivered by a metering pump.

[0024] As a further improvement of the production process technical solution of the present invention, in step S5, the temperature range of the first drying chamber is 60°C-95°C, and the temperature range of the second drying chamber is 25°C-60°C.

[0025] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0026] 1) The aqueous phase synergistic coagulation process production line of high-performance graphene oxide modified natural rubber masterbatch of the present invention can realize the modification treatment of graphene oxide and the subsequent immediate use, so that after adding it to natural latex, a high-performance masterbatch can be obtained; in addition, the motor speed and baking temperature can be adjusted according to the real-time information of each device, so that the quality of the obtained masterbatch product has high stability. Therefore, it has the characteristics of low cost, high efficiency, high stability and intelligence.

[0027] 2) The staged drying process of the present invention uses high-temperature hot air in the front stage to quickly dry most of the moisture in the rubber; and uses low-temperature dry air in the back stage to quickly absorb the remaining moisture in the rubber, which can improve the production efficiency of the modified natural rubber masterbatch and ensure the quality stability.

[0028] 3) The automated coordination among the various devices in the production line of the present invention reduces the number of manpower and the operation intensity; in addition, the process is simple, the drying time is shortened, and the temperature at the drying end is low, which can effectively improve the production efficiency and product quality of the graphene oxide modified natural rubber masterbatch. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.

[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0031] Figure 1 The figure is a schematic diagram of a production line of graphene-modified natural rubber masterbatch of the present invention.

[0032] In the figure: 101: graphene oxide slurry storage tank; 102: modifier dispersion storage tank; 103: ultrasonic reactor; 201: latex storage tank; 202: flocculant storage tank; 203: mixing kettle; 204: gluing platform; 205: crepe machine; 206: flocculation tank; 207: transmission roller; 208: transmission belt; 209: shredder; 210: cleaning pool; 211: feeding pump; 212: conveyor belt; 213: drying bin; 214: centrifugal fan; 215: air supply fan; 216: heating device; 217: baler; 218: drying device; 219: support base; 220: lifting cylinder; 221: material table. DETAILED DESCRIPTION

[0033] In order to more clearly understand the above-mentioned objectives, features and advantages of the present invention, the scheme of the present invention will be further described below. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

[0034] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein; it is obvious that the embodiments in the specification are only part of the embodiments of the present invention, rather than all of the embodiments.

[0035] Example

[0036] like Figure 1 As shown, the present invention provides a specific embodiment of a water-phase synergistic coagulation process production line for graphene oxide modified natural rubber masterbatch, including a modified graphene oxide aqueous dispersion production system and a graphene oxide modified natural rubber masterbatch production system;

[0037] The modified graphene oxide aqueous dispersion production system comprises a graphene oxide slurry storage tank 101, a modifier dispersion storage tank 102 and an ultrasonic reactor 103, wherein the graphene oxide slurry storage tank 101 and the modifier dispersion storage tank 102 are respectively connected to the ultrasonic reactor 103 through pipelines, and metering pumps are respectively arranged in series on the pipelines between the graphene oxide slurry storage tank 101, the modifier dispersion storage tank 102 and the ultrasonic reactor 103;

[0038] The concentration of the graphene oxide slurry is such that it can be stably delivered using a metering pump, and the concentration of the modifier dispersion is such that it can be stably delivered by a metering pump; the power range of the ultrasonic reactor 103 is 8KW, and the temperature range is 70°C.

[0039] The graphene oxide modified natural rubber masterbatch production system comprises a latex storage tank 201, a flocculant storage tank 202, a mixing kettle 203, a flocculation device and a gluing device; the latex storage tank 201 and the ultrasonic reactor 103 are respectively connected to the mixing kettle 203 through pipelines; metering pumps are respectively arranged in series on the pipelines connecting the latex storage tank 201, the ultrasonic reactor 103 and the mixing kettle 203;

[0040] The flocculation device includes a flocculation tank 206, and the flocculant storage tank 202 is connected to the flocculation tank 206 through a pipeline; a metering pump is arranged in series on the pipeline connecting the flocculant storage tank 202 and the flocculation tank 206; the gluing device includes a gluing platform 204 and a transmission roller 207 rotatably arranged on the gluing platform 204, and three crepe machines 205 are arranged in sequence at the discharge end of the transmission roller 207, and each crepe machine 205 is equipped with a transmission belt 208 at the discharge end; the discharge end of the last transmission belt 208 is located at the upper part of the feed end of the pelletizer 209; the discharge end of the pelletizer 209 is connected to the feed end of the cleaning water tank 210; the discharge end of the cleaning water tank 210 is provided with a feeding pump 211, and the discharge end of the feeding pump 211 is connected to the drying device through a pipeline;

[0041] The drying device includes a conveyor belt 212, and the conveyor belt 212 is located below the discharge end of the feeding pump 211; two drying bins 213 are arranged side by side in sequence along the material conveying direction on the conveyor belt 212, and the conveyor belt 212 can convey materials in the drying bins 213 through a driving mechanism, and the drying bins 213 are all provided with heat-insulating door curtains, and centrifugal fans 214 and air supply fans 215 are respectively arranged on the top; a heating device 216 is correspondingly arranged at the air inlet of the air supply fan 215, and the air outlet of the air supply fan 215 is respectively connected to the air inlet of the drying bin 213, and the centrifugal fan The air inlets 214 are respectively connected to the air outlets of the drying chamber 213; a drying device 218 is provided at the front end of the air inlet pipeline of the second drying chamber 213 near the heating device 216, and the drying device 218 is filled with a drying medium; in this embodiment, a high-power heating and ventilation device is used in the first drying chamber 213 to achieve the purpose of quickly drying most of the moisture by high temperature; the second drying chamber 213 uses a high-power dry air ventilation device to achieve the purpose of quickly absorbing the remaining moisture by low-temperature dry air, thereby improving the production efficiency and quality stability of the modified natural rubber masterbatch at the same time;

[0042] The conveyor belt 212 can convey the material to the material platform 221 .

[0043] In this embodiment, in order to facilitate dragging the graphene oxide modified natural rubber masterbatch in the flocculation tank 206 onto the driving roller 207 on the gluing platform 204, the flocculation device further includes a support base 219, the flocculation tank 206 is located above the support base 219, and the bottom of the discharge end of the flocculation tank 206 is rotatably connected to one side of the upper surface of the support base 219, and a lifting cylinder 220 is provided inside the other side of the support base 219, and the telescopic end of the lifting cylinder 220 passes through the support base 219 and contacts and supports the bottom of the feed end of the flocculation tank 206. After the mixed emulsion is flocculated, the lifting cylinder 220 is started, and the telescopic end of the lifting cylinder 220 passes through the support base 219. In the process of the feed end of the flocculation tank 206 being continuously raised, the contact point between the telescopic end of the lifting cylinder 220 and the bottom of the discharge end of the flocculation tank 206 moves from the inside to the outside until the feed end of the flocculation tank 206 is raised to the required height.

[0044] like Figure 1 As shown, a packaging machine 217 is also included.

[0045] The specific production process includes the following steps:

[0046] S1. The natural rubber latex in the latex storage tank 201 is pumped into the mixing kettle 203 by a metering pump, and then deionized water is added and mixed to obtain natural rubber latex;

[0047] S2. The graphene oxide slurry (concentration of 1 wt.%) in the graphene oxide slurry storage tank 101 and the modifier dispersion (concentration of 2 wt.%) in the modifier dispersion storage tank 102 are sequentially added to the ultrasonic reactor 103 through a metering pump, and reacted at a certain temperature for a certain time to obtain a modified graphene oxide aqueous dispersion;

[0048] S3. Add the modified graphene oxide aqueous dispersion in the ultrasonic reactor 103 obtained in step S2 to the natural rubber latex in the mixing reactor 203 obtained in step S1, and stir and mix them thoroughly to obtain a uniform graphene oxide modified natural rubber mixed emulsion; sequentially add the graphene oxide modified natural rubber mixed emulsion and the flocculant in the flocculant storage tank 202 to the flocculation tank 206, mix them evenly and flocculate the latex to obtain a flocculated graphene oxide modified natural rubber block;

[0049] S4. The graphene oxide modified natural rubber floccules obtained in step S3 are dragged through each creping machine 205 and the transmission belt 208 in sequence by a gluing device for continuous creping. The rotation speed of the creping machine 205 is controlled according to the glue output speed, so that the rubber sheet passes through the last transmission belt 208 evenly and is transported to the granulator 209 for granulation without clogging;

[0050] S5. The colloid particles obtained in step S4 are cleaned and deacidified in the cleaning water pool 210, and then pumped to the conveyor belt 212 by the feeding pump 211; the hot air generated by the heating device 216 is respectively transported to the drying bin 213 through the air supply fan 215, and the centrifugal fan 214 discharges the hot and humid air in the drying bin 213; in this embodiment, the temperature sensor provided in the drying bin 213 is used to obtain the corresponding temperature, and the PLC controller adjusts the power of the heating device 216 according to the set drying temperature, and obtains the required drying temperature and drying time through the temperature and humidity of the air outlet of the drying bin 213; in specific implementation, the drying temperature and drying time in the drying bin 213 are shown in the following table; the colloid particles on the conveyor belt 212 are sequentially passed through the drying bin 213 for drying;

[0051] S6. Quantitatively weigh the dried rubber particles obtained in step S5, and then pack them using a packing machine 217 to obtain a high-performance graphene oxide-modified natural rubber masterbatch product.

[0052] Comparative Example 1

[0053] S1-S4 are the same as S1-S4 in the embodiment.

[0054] S5 is the same as S5 in the embodiment, except that the drying temperature in the two drying chambers 213 is kept constant at 60° C., and the drying is performed to a constant weight.

[0055] S6 is the same as S6 in the embodiment.

[0056] Comparative Example 2

[0057] S1 is the same as S1 in the embodiment.

[0058] S2 and S3 are the same as S2 and S3 in the example, except that no modified graphene oxide is added.

[0059] S5 and S6 are the same as S5 and S6 in the embodiment, the only difference is that the drying temperature in the two drying chambers 213 is constant at 60° C., and the drying is performed to a constant weight.

[0060] Comparative Example 3

[0061] S1-S4 are the same as S1-S4 in the embodiment.

[0062] S5 is the same as S5 in the embodiment, except that the drying temperature in the two drying chambers 213 is kept constant at 80° C., and the drying is performed to a constant weight.

[0063] S6 is the same as S6 in the embodiment.

[0064] In order to obtain the mechanical properties of the vulcanized rubber based on the masterbatch produced in Example 1 and Comparative Examples 1 to 3, it is necessary to prepare the vulcanized rubber. The specific process is as follows: the graphene oxide modified natural rubber masterbatch is placed in an internal mixer, and the rubber is discharged after internal mixing at a temperature of 110°C for 16 minutes. During this period, 100phr of graphene oxide modified natural rubber masterbatch, 2phr of accelerator CZ (N-cyclohexyl-2-benzothiazole sulfonamide), 2phr of antioxidant RD (2,2,4-trimethyl-1,2-dihydroquinoline polymer), 2phr of antioxidant 4020 (N-(1,3-dimethylbutyl)-N' -phenyl-1,4-phenylenediamine) 2phr, activator zinc oxide 5phr, plasticizer stearic acid 2phr, reinforcing agent carbon black 35phr; after the discharged rubber material is cooled to room temperature, it is milled on an open mill at 60°C for 10 minutes, during which 2phr of sulfur is added, mixed evenly, and thinly passed until there are no bubbles in the rubber material to obtain a mixed rubber; after the mixed rubber material is placed at room temperature for 24 hours, it is hot-pressed and vulcanized in a mold, the hot-pressing conditions are 150°C*15MPa, and the vulcanization time is Tc 90 (obtained by testing with a rubber processing analyzer), and finally vulcanized graphene-modified natural rubber is obtained.

[0065] The performance tests were performed on the vulcanized natural rubber composite materials based on the masterbatch obtained in Example 1 and Comparative Examples 1 to 3. The tensile performance test standard is GB / T 528-2009, and the tensile rate is 500 mm / min. The tear performance test standard is GB / T 529-2008. Vulcanization time Tc 90 Measured by rubber processing analyzer. Table 1 is the performance test rubber formula table of Example 1 and Comparative Examples 1-3; Table 2 is the comprehensive performance of Example 1 and Comparative Examples 1-3.

[0066] Table 1 Formula table of Example 1 and Comparative Examples 1 to 3

[0067] sample Comparative Example 1 Comparative Example 2 Comparative Example 3 Example 1 Natural rubber (phr) 100 100 100 100 4020(phr) 2 2 2 2 RD(phr) 2 2 2 2 Zinc oxide (phr) 5 5 5 5 Stearic acid (phr) 2 2 2 2 Carbon black (phr) 35 35 35 35 Accelerator CZ(phr) 2 2 2 2 Sulfur (phr) 2 2 2 2

[0068] Table 2 Comprehensive performance of Example 1 and Comparative Examples 1 to 3

[0069]

[0070]

[0071] As shown in Table 2, compared with the graphene oxide modified natural rubber masterbatch and the vulcanized rubber prepared therefrom in Comparative Examples 1 to 3, the high performance graphene oxide modified natural rubber masterbatch of the present invention (Example 1) has a higher Mooney viscosity and plasticity value, which can avoid sticking to the roller in the mixing stage; and the tensile strength, tear strength, hardness, dynamic compression heat generation performance and other comprehensive properties of the vulcanized rubber prepared therefrom are all improved. In addition, the drying time of the same rubber is the shortest, and the production efficiency is significantly improved.

[0072] The above is only a specific implementation of the present invention, which enables those skilled in the art to understand or implement the present invention. Although detailed descriptions are given with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments, and they should all be covered by the protection scope of the claims.

Claims

1. Aqueous phase synergistic coagulation process production line for graphene oxide modified natural rubber masterbatch, characterized in that: Including modified graphene oxide water dispersion production system and graphene oxide modified natural rubber masterbatch production system; The modified graphene oxide aqueous dispersion production system comprises a graphene oxide slurry storage tank (101), a modifier dispersion storage tank (102) and an ultrasonic reactor (103); the graphene oxide slurry storage tank (101) and the modifier dispersion storage tank (102) are respectively connected to the ultrasonic reactor (103) via pipelines; and metering pumps are respectively arranged in series on the pipelines between the graphene oxide slurry storage tank (101), the modifier dispersion storage tank (102) and the ultrasonic reactor (103); The graphene oxide modified natural rubber masterbatch production system comprises a latex storage tank (201), a flocculant storage tank (202), a mixing kettle (203), a flocculation device and a gluing device; the latex storage tank (201) and the ultrasonic reaction kettle (103) are respectively connected to the mixing kettle (203) through pipelines; and metering pumps are respectively arranged in series on the pipelines connecting the latex storage tank (201), the ultrasonic reaction kettle (103) and the mixing kettle (203); The flocculation device comprises a flocculation tank (206), the flocculant storage tank (202) being connected to the flocculation tank (206) via a pipeline; a metering pump is arranged in series on the pipeline connecting the flocculant storage tank (202) and the flocculation tank (206); the gluing device comprises a gluing platform (204) and a driving roller (207) rotatably arranged on the gluing platform (204), and at least one crepe sheet is arranged in sequence at the discharge end of the driving roller (207) The crepe machine (205) is provided with a transmission belt (208) at the discharge end of each crepe machine (205); the discharge end of the last transmission belt (208) is located above the feed end of the shredder (209); the discharge end of the shredder (209) is connected to the feed end of the cleaning pool (210); the discharge end of the cleaning pool (210) is provided with a feed pump (211), and the discharge end of the feed pump (211) is connected to the drying device through a pipeline; The drying device comprises a conveyor belt (212), wherein the conveyor belt (212) is located below the discharge end of the feeding pump (211); two drying bins (213) are arranged in parallel in the material conveying direction on the conveyor belt (212); the conveyor belt (212) is capable of conveying materials in the drying bins (213) through a driving mechanism; the drying bins (213) are each provided with a heat-insulating door curtain, and a centrifugal fan (214) and an air supply fan (215) are respectively arranged on the top; A heating device (216) is provided at the air inlet of the air supply fan (215), the air outlet of the air supply fan (215) is respectively connected to the air inlet of the drying bin (213), and the air inlet of the centrifugal fan (214) is respectively connected to the air outlet of the drying bin (213); a drying device (218) is provided at the front end of the air inlet pipeline of at least one drying bin (213) close to the heating device (216), and the drying device (218) is filled with a drying medium; The conveyor belt (212) can convey the material to the material platform (221).

2. The aqueous phase synergistic coagulation process production line of graphene oxide modified natural rubber masterbatch according to claim 1, characterized in that: The flocculation device further comprises a support base (219), the flocculation tank (206) is located above the support base (219), and the bottom of the discharge end of the flocculation tank (206) is rotatably connected to one side of the upper surface of the support base (219), and a lifting cylinder (220) is provided inside the other side of the support base (219), and the telescopic end of the lifting cylinder (220) passes through the support base (219) and contacts and supports the bottom of the feed end of the flocculation tank (206).

3. The aqueous phase synergistic coagulation process production line of graphene oxide modified natural rubber masterbatch according to claim 1, characterized in that: Also included is a packaging machine (217).

4. The aqueous phase synergistic coagulation process production line of graphene oxide modified natural rubber masterbatch according to claim 1, characterized in that: The power range of the ultrasonic reactor (103) is 1-10 KW, and the temperature range is 25-120°C.

5. A production process of graphene oxide modified natural rubber masterbatch by aqueous phase synergistic coagulation process, characterized in that: The production line according to any one of claims 1 to 4 is used, comprising the following steps: S1. The natural rubber latex in the latex storage tank (201) is pumped into the mixing kettle (203) through a metering pump, and then deionized water is added and mixed to obtain a natural rubber latex of a certain concentration; S2. sequentially adding the graphene oxide slurry in the graphene oxide slurry storage tank (101) and the modifier dispersion in the modifier dispersion storage tank (102) to the ultrasonic reactor (103) through a metering pump, reacting at a certain temperature for a certain time to obtain a modified graphene oxide aqueous dispersion; S3. adding the modified graphene oxide aqueous dispersion in the ultrasonic reactor (103) obtained in step S2 to the natural rubber latex in the mixing reactor (203) obtained in step S1, and stirring and mixing them thoroughly to obtain a uniform graphene oxide modified natural rubber mixed latex; sequentially adding the graphene oxide modified natural rubber mixed latex and the flocculant in the flocculant storage tank (202) to the flocculation tank (206), mixing them uniformly and flocculating the latex to obtain flocculated graphene oxide modified natural rubber blocks; S4. Using a gluing device, the graphene oxide modified natural rubber flocs obtained in step S3 are dragged through each creping machine (205) and a transmission belt (208) in sequence for continuous creping. According to the glue output speed, the rotation speed of the creping machine (205) is controlled so that the rubber sheet passes through the last transmission belt (208) evenly and is transported to the granulator (209) for granulation without clogging. S5. The rubber particles obtained in step S4 are washed and deacidified in a washing water tank (210), and then pumped to a conveyor belt (212) by a feeding pump (211); the hot air generated by the heating device (216) is respectively transported to a drying bin (213) by air supply fans (215), and the hot and humid air in the drying bin (213) is respectively discharged by a centrifugal fan (214); the rubber particles on the conveyor belt (212) are sequentially passed through the drying bins (213) for drying treatment, so that most of the moisture of the material is quickly dried by high temperature in the first drying bin (213), and then the remaining moisture is quickly absorbed by low temperature dry air in the last drying bin (213), so that the production efficiency and quality stability of the modified natural rubber masterbatch are improved at the same time; S6. The dried rubber particles obtained in step S5 are quantitatively weighed, and then packaged using a packaging machine (217) to obtain a high-performance graphene oxide-modified natural rubber masterbatch product.

6. The production process of a graphene oxide modified natural rubber masterbatch by aqueous phase synergistic coagulation process according to claim 5, characterized in that: In step S1, the concentration of the obtained natural rubber latex is such that it can be stably transported by a metering pump.

7. The production process of a graphene oxide modified natural rubber masterbatch by aqueous phase synergistic coagulation process according to claim 5, characterized in that: In step S2, the concentration of the graphene oxide slurry is such that it can be stably delivered by a metering pump, and the concentration of the modifier dispersion is such that it can be stably delivered by a metering pump.

8. The production process of a graphene oxide modified natural rubber masterbatch by aqueous phase synergistic coagulation process according to claim 5, characterized in that: In step S5, the temperature range of the first drying chamber (213) is 60°C-95°C, and the temperature range of the second drying chamber (213) is 25°C-60°C.

Citation Information

Cited By

  • High-strength, high-toughness and low-heat-generation dual-bonded graphene / natural rubber based on high-molecular-weight cationic polymer and simplified preparation

    CN119684688A

  • Aqueous-phase synergistic coagulation process production line and production process for graphene oxide-modified natural rubber masterbatch

    WO2026016347A1