Rare earth grafted polymer precursor, preparation method and application of rare earth grafted polymer precursor in railway anti-freezing and water-retaining aspects

Through rare earth graft polymer precursor and modified composite amphiphilic polymer, combining rare earth hexaboride and hydroxyethyl cellulose, the problem of anti-icing materials in the prior art is difficult to prevent ice and de-icing at the same time in cold environments. , achieving efficient ice melting and environmentally friendly coating performance.

CN118878744APending Publication Date: 2024-11-01TIANJIN BAOGANG RES INST OF RARE EARTHS CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410948392.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Existing anti-icing materials are difficult to achieve both anti-icing and de-icing effects in cold environments, and are prone to coating peeling and environmental pollution.

Method used

Using rare earth grafted polymer precursor and modified composite amphiphilic polymer, the reaction of rare earth hexaboride and dicarboxylic double bond compound is combined with hydroxyethyl cellulose to form a photothermal property and salt-retaining ability. Materials, grafting inorganic nanoparticles by ionic bonds, enhance the weather resistance and stability of the polymer.

Benefits of technology

It achieves an effective anti-ice melting effect in cold environments, extends the service life of the coating, reduces the impact of acidity corrosion, and has excellent heat-absorbing ice melting performance in environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118878744A_ABST
    Figure CN118878744A_ABST
Patent Text Reader

Abstract

The invention provides a rare earth grafted polymer precursor, a preparation method and application of the rare earth grafted polymer precursor in railway antifreezing and water retention, and the preparation method of the polymer precursor comprises the following steps: adding rare earth hexaboride and a dicarboxyl double bond compound into ethanol, and reacting for 18-24 hours at 75-85 DEG C under the catalysis of concentrated sulfuric acid to obtain the rare earth grafted polymer precursor. And purifying to obtain the rare earth grafted polymer precursor C4H7O5ReB6. The rare earth inorganic nanoparticles and the inorganic material are added into the polymer, so that the polymer has better weather resistance, acid and alkali resistance, wear resistance and stability. Therefore, the coating prepared by the method is beneficial to realizing the anti-icing and ice-melting effects in a cold environment, and the influence of corrosion of the coating due to acidity in water vapor is also reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of railway ice melting and deicing, and in particular relates to a rare earth grafted polymer precursor, a preparation method and application thereof in railway antifreeze and water conservation. Background Art

[0002] Most of the existing anti-icing technologies use hydrophobic groups or thermosensitive polymers for anti-icing. For example, "Preparation of Amphiphilic Block Copolymers and Their Application in Anti-fog and Ice Suppression" reports different types of block polymers, which achieve anti-icing by realizing the structural transformation of polymer hydrogels in response to temperature stimulation. Currently, there are few reports on materials with both anti-icing and de-icing effects. However, materials with only anti-icing or easy de-icing properties are not conducive to large-scale use in cold environments and under conditions of rapid icing. Summary of the invention

[0003] In view of this, the present invention aims to overcome the defects in the prior art and proposes a rare earth grafted polymer precursor, a preparation method and its application in railway antifreeze and water conservation.

[0004] To achieve the above object, the technical solution of the present invention is achieved as follows:

[0005] In a first aspect, the present invention provides a rare earth grafted polymer precursor, the preparation method of which comprises the following steps:

[0006] Rare earth hexaboride and dicarboxyl double bond compound are added to ethanol and reacted at 75-85°C for 18-24 hours under the catalysis of concentrated sulfuric acid. After purification, rare earth grafted polymer precursor C is obtained. 4 H 7 O 5 R 6 .

[0007] Preferably, the mass ratio of the rare earth hexaboride to the dicarboxyl double bond compound is (200-210):(85-150).

[0008] Preferably, the rare earth hexaboride is one of lanthanum hexaboride, cerium hexaboride, and samarium hexaboride, or a mixture of two or more thereof.

[0009] Preferably, the dicarboxyl double bond compound is 2-carboxyacrylic acid and / or 2-carboxybutenoic acid.

[0010] Preferably, the amount of concentrated sulfuric acid used is 0.3-1.0 times the total amount of rare earth hexaboride and dicarboxyl double bond compound.

[0011] The rare earth hexaboride is an inorganic rare earth nanoparticle with photothermal properties. After the powder is prepared, the hydroxyl groups on the surface enable it to be grafted onto the polymer chain through ionic bonds, and it is not easy to fall off from the coating, thereby achieving a better photothermal deicing effect.

[0012] The dicarboxyl double bond compound is one of the reactants for connecting rare earth hexaboride to form a novel rare earth grafted polymer precursor. This molecular structure has a double bond that can continue to polymerize and avoids excessive molecular chain length to form an irregular polymer structure.

[0013] The concentrated sulfuric acid acts as a catalyst and a water absorbent in the esterification reaction. It can promote the esterification reaction, increase the reaction rate, and remove the water produced in the esterification reaction by absorbing water, thereby promoting the reaction to produce esters.

[0014] The reaction route of the above polymer precursor is as follows:

[0015]

[0016] In a third aspect, the present invention provides a rare earth grafted modified composite amphiphilic polymer obtained by using the above rare earth grafted polymer precursor, wherein the rare earth grafted modified composite amphiphilic polymer has the structural formula: (C 11 H 13 O 9 R 6 ) n The method for preparing the rare earth grafted modified composite amphiphilic polymer specifically comprises the following steps:

[0017] (1) Dissolving hydroxyethyl cellulose and 2,4-pentadienoic acid in a solvent, and reacting them at 75-85° C. for 18-24 hours under the catalysis of concentrated sulfuric acid, thereby obtaining a hydroxyethyl cellulose modified polymer monomer;

[0018] (2) dissolving a polymer precursor and a polymer monomer modified with hydroxyethyl cellulose in a deionized water solution, heating the mixture to 60-70° C., adding persulfate as a catalyst, and refluxing the mixture overnight to obtain a water-soluble polymer;

[0019] (3) dissolving a water-soluble polymer and acrylic acid in a solvent, activating for 15-30 minutes, and then adding concentrated sulfuric acid to catalyze the reaction for 12-15 hours, thereby obtaining a rare earth graft-modified composite amphiphilic polymer.

[0020] Preferably, in step (1), the mass ratio of hydroxyethyl cellulose to 2,4-pentadienoic acid is (46-47):(73-74).

[0021] Preferably, in step (2), the mass ratio of the polymer precursor to the hydroxyethyl cellulose modified polymer monomer is (169-272): (213-355).

[0022] Preferably, in step (3), the mass ratio of the water-soluble polymer to the acrylic acid is (50-51): (50-51).

[0023] Preferably, the persulfate in step (3) is one of sodium persulfate, potassium persulfate and ammonium persulfate.

[0024] Preferably, the solvent is ethanol, which is the reaction solvent for the three esterification reactions during the reaction process.

[0025] The reaction route of the above polymer is as follows:

[0026]

[0027]

[0028] The rare earth grafted modified composite amphiphilic polymer of the present invention has both anti-icing and easy deicing capabilities. In terms of deicing, the present invention uses a vinyl compound to end-cap one end of the hydrophilic polymer, giving the polymer a hydrophilic property at one end and a hydrophobic property at the other end. The hydrophilic end will have a strong bond with the metal surface of the railway, which helps to increase the service life of the coating and will not tear off the coating as the ice layer falls off. In terms of deicing, the present invention adds rare earth hexaboride. Unlike blending, the present invention uses ionic bonds to graft inorganic materials into the polymer, which allows the compounds with light and heat absorption properties to be better combined in the polymer system. In addition, in the polymer system, the present invention also adds hydroxyethyl cellulose, which not only has a good thickening power, but also has salt resistance and water retention capabilities. When the coating ages and falls off after being used for too long, this unique salt resistance and water retention will not only not cause harm to the land, but also can achieve environmental protection to a certain extent.

[0029] In a fourth aspect, the present invention also provides a rare earth grafted modified composite amphiphilic polymer prepared by the above preparation method.

[0030] In a fifth aspect, the present invention also provides the use of the rare earth grafted modified composite amphiphilic polymer in the preparation of an antifreeze and water-retaining agent.

[0031] In a sixth aspect, the present invention also provides the use of the rare earth grafted modified composite amphiphilic polymer in the preparation of railway antifreeze and water-retaining products.

[0032] Compared with the prior art, the present invention has the following advantages:

[0033] (1) The polymer material of the present invention firstly adds rare earth inorganic nanoparticles. The addition of inorganic materials makes the polymer have better weather resistance, acid and alkali resistance, wear resistance and stability. This makes the coating made by using the polymer of the present invention conducive to achieving ice-proof and ice-melting effects in cold environments, and also reduces the influence of acidity in water vapor corroding the coating. More importantly, the rare earth inorganic nanoparticles used in the present invention have excellent light absorption performance, especially in the near-infrared region, which can quickly absorb the energy in light energy in a short time and convert it into heat, thereby melting ice.

[0034] (2) The present invention constructs a novel rare earth grafted polymer precursor, which utilizes a simple substitution reaction to ionically bond a rare earth boride with a carboxyl-modified double-bond olefin to synthesize a polymer precursor. The structures of the rare earth grafted polymer precursor and the rare earth grafted amphiphilic polymer of the present invention are characterized by one-dimensional nuclear magnetic resonance hydrogen spectrum, confirming the successful preparation of the novel compound. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 A one-dimensional nuclear magnetic spectrum of the rare earth grafted polymer precursor of the present invention;

[0036] Figure 2 is a carbon spectrum of the rare earth grafted polymer precursor of the present invention;

[0037] Figure 3 It is a one-dimensional nuclear magnetic spectrum of the rare earth grafted modified composite amphiphilic polymer of the present invention;

[0038] Figure 4 The carbon spectrum of the rare earth grafted modified composite amphiphilic polymer of the present invention;

[0039] Figure 5 Ice melting rate curves of rare earth grafted modified composite amphiphilic polymers prepared in Examples 1-5 of the present invention and polymers prepared in Comparative Examples 1-5;

[0040] Figure 6 The stability test data of Example 1 and Comparative Examples 1-5 are shown in FIG. DETAILED DESCRIPTION

[0041] Unless otherwise defined, the technical terms used in the following examples have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. The test reagents used in the following examples, unless otherwise specified, are all conventional biochemical reagents; the experimental methods, unless otherwise specified, are all conventional methods.

[0042] The present invention will be described in detail below with reference to the embodiments.

[0043] Example 1

[0044] A method for preparing a rare earth grafted modified composite amphiphilic polymer comprises the following steps:

[0045] 1) Lanthanum hexaboride (20.38 g) and 2-carboxylic acid (8.78 g) were added to ethanol (75 mL) and reacted at 80 ° C for 24 hours under the catalysis of concentrated sulfuric acid (7 mL). After purification, a rare earth grafted polymer precursor was obtained, and its one-dimensional nuclear magnetic hydrogen spectrum was as follows: Figure 1 As shown, the carbon spectrum is Figure 2 shown.

[0046] 2) Hydroxyethyl cellulose (4.65 g) and 2,4-pentadienoic acid (7.35 g) were dissolved in ethanol (50 mL), and reacted at 80° C. for 24 hours under the catalysis of concentrated sulfuric acid (6 mL) to obtain a hydroxyethyl cellulose modified polymer monomer.

[0047] 3) The rare earth grafted polymer precursor (8.48 g) and the hydroxyethyl cellulose modified polymer monomer (10.65 g) were dissolved in a deionized water solution (18 mL), and sodium persulfate (0.12 g) was added after heating to 70° C. and refluxed overnight to obtain a water-soluble polymer.

[0048] 4) The water-soluble polymer and acrylic acid (5.04 g) were dissolved in ethanol (200 mL), activated for 30 minutes, and then concentrated sulfuric acid (5.74 mL) was added to catalyze the reaction for 12 hours to obtain a rare earth grafted modified composite amphiphilic polymer, whose one-dimensional nuclear magnetic hydrogen spectrum is as follows: Figure 3 As shown, the carbon spectrum is Figure 4 shown.

[0049] Example 2

[0050] A method for preparing a rare earth grafted modified composite amphiphilic polymer comprises the following steps:

[0051] 1) Lanthanum hexaboride (20.38 g) and 2-carboxylic acid (11.7 g) were added to ethanol (80 mL) in proportion, and reacted at 80° C. for 24 hours under the catalysis of concentrated sulfuric acid (8 mL). After purification, a rare earth grafted polymer precursor was obtained.

[0052] 2) Hydroxyethyl cellulose (4.65 g) and 2,4-pentadienoic acid (7.35 g) were dissolved in ethanol (50 mL), and reacted at 80° C. for 24 hours under the catalysis of concentrated sulfuric acid (6 mL) to obtain a hydroxyethyl cellulose modified polymer monomer.

[0053] 3) The rare earth grafted polymer precursor (11.03 g) and the hydroxyethyl cellulose modified polymer monomer (14.2 g) were dissolved in a deionized water solution (18 mL), and sodium persulfate (0.12 g) was added after heating to 70° C. and refluxed overnight to obtain a water-soluble polymer.

[0054] 4) The water-soluble polymer and acrylic acid (5.04 g) were dissolved in ethanol (190 mL), activated for 30 minutes, and then concentrated sulfuric acid (5.87 mL) was added to catalyze the reaction for 12 hours to obtain a rare earth grafted modified composite amphiphilic polymer.

[0055] Example 3

[0056] A method for preparing a rare earth grafted modified composite amphiphilic polymer comprises the following steps:

[0057] 1) Lanthanum hexaboride (20.38 g) and 2-carboxylic acid (14.63 g) were added to ethanol (85 mL) in proportion, and reacted at 80° C. for 24 hours under the catalysis of concentrated sulfuric acid (10 mL). After purification, a rare earth grafted polymer precursor was obtained.

[0058] 2) Hydroxyethyl cellulose (4.65 g) and 2,4-pentadienoic acid (7.35 g) were dissolved in ethanol (50 mL), and reacted at 80° C. for 24 hours under the catalysis of concentrated sulfuric acid (6 mL) to obtain a polymer monomer.

[0059] 3) The rare earth grafted polymer precursor (13.575 g) and the hydroxyethyl cellulose modified polymer monomer (17.75 g) were dissolved in a deionized water solution (18 mL), and sodium persulfate (0.12 g) was added after heating to 70° C. and refluxed overnight to obtain a water-soluble polymer.

[0060] 4) The water-soluble polymer and acrylic acid (5.04 g) were dissolved in ethanol (183 mL), activated for 30 minutes, and then concentrated sulfuric acid (5.21 mL) was added to catalyze the reaction for 12 hours to obtain a rare earth grafted modified composite amphiphilic polymer.

[0061] Example 4

[0062] A method for preparing a rare earth grafted modified composite amphiphilic polymer comprises the following steps:

[0063] 1) Cerium hexaboride (20.00 g) and 2-carboxybutenoic acid (8.50 g) were added to ethanol (75 mL), and reacted at 80° C. for 24 hours under the catalysis of concentrated sulfuric acid (28 mL). After purification, a rare earth grafted polymer precursor was obtained.

[0064] 2) Hydroxyethyl cellulose (4.60 g) and 2,4-pentadienoic acid (7.40 g) were dissolved in ethanol (50 mL), and reacted at 80° C. for 24 hours under the catalysis of concentrated sulfuric acid (6 mL) to obtain a hydroxyethyl cellulose modified polymer monomer.

[0065] 3) The rare earth grafted polymer precursor (35.50 g) and the hydroxyethyl cellulose modified polymer monomer (16.90 g) were dissolved in a deionized water solution (36 mL), and potassium persulfate (0.12 g) was added after heating to 70° C. and refluxed overnight to obtain a water-soluble polymer.

[0066] 4) The water-soluble polymer (5.00 g) and acrylic acid (5.10 g) were dissolved in ethanol (200 mL), activated for 30 minutes, and then concentrated sulfuric acid (5.74 mL) was added to catalyze the reaction for 12 hours to obtain a rare earth grafted modified composite amphiphilic polymer.

[0067] Example 5

[0068] A method for preparing a rare earth grafted modified composite amphiphilic polymer comprises the following steps:

[0069] 1) Samarium hexaboride (21.00 g) and 2-carboxybutenoic acid (15.00 g) were added to ethanol (75 mL), and reacted at 80° C. for 24 hours under the catalysis of concentrated sulfuric acid (30 mL). After purification, a rare earth grafted polymer precursor was obtained.

[0070] 2) Hydroxyethyl cellulose (4.70 g) and 2,4-pentadienoic acid (7.30 g) were dissolved in ethanol (50 mL), and reacted at 80° C. for 24 hours under the catalysis of concentrated sulfuric acid (6 mL) to obtain a hydroxyethyl cellulose-modified polymer monomer.

[0071] 3) The rare earth grafted polymer precursor (21.30 g) and the hydroxyethyl cellulose modified polymer monomer (27.20 g) were dissolved in a deionized water solution (36 mL), and the temperature was raised to 70° C. and ammonium persulfate (0.12 g) was added to catalytically reflux overnight to obtain a water-soluble polymer.

[0072] 4) The water-soluble polymer (5.10 g) and acrylic acid (5.00 g) were dissolved in ethanol (200 mL), activated for 30 minutes, and then concentrated sulfuric acid (5.74 mL) was added to catalyze the reaction for 12 hours to obtain a rare earth grafted modified composite amphiphilic polymer.

[0073] Comparative Example 1

[0074] The preparation method of an amphiphilic block copolymer with an anti-icing function comprises the following steps: using a RAFT agent BDAAT (0.002 mol), a monomer DMAA (0.08 mol), an initiator ACVA (0.0004 mmol), 1,3,5-trioxane as an internal standard (0.001 mol), and 1,4-dioxane as a solvent. The ratio of the RAFT agent to the initiator is selected to be 5 / 1, a vacuum is drawn four times using a laboratory-made pumping device, and nitrogen is filled after each vacuum drawing. In a reaction bottle with a magnetic device, a reaction is carried out at 70° C. for 3 hours to synthesize a section of PDMAA2X-CTA as a macromolecular initiator. The product is precipitated in n-hexane and purified by dissolution-precipitation three times. After vacuum drying at 40° C., a yellow solid composed of PDMAA2X-CTA is obtained, and the degree of polymerization of PDMAA2X-CTA is calculated by nuclear magnetic resonance. Then design the experiment, add macromolecular RAFT agent and initiator, monomer DAAM (0.18 mol), target DP = 90, 1,4-dioxane (make the monomer account for 20% of the mass of the solvent, recorded as 20wt%) into a glass bottle equipped with a magnet, and place a high-speed magnetic stirrer below. Pump four times and fill with nitrogen in the same way, and then stir the reaction at 70℃ for 4 hours. Precipitate the copolymer with n-hexane in small amounts and multiple times, and then vacuum dry the product at 40℃.

[0075] Comparative Example 2

[0076] The polymer of this comparative example is different from that of Example 1 in that no hexaboride is added during the preparation of the polymer precursor.

[0077] Comparative Example 3

[0078] The polymer of this comparative example is different from that of Example 1 in that the hexaboride is europium hexaboride.

[0079] Comparative Example 4

[0080] The polymer of this comparative example is different from that of Example 1 in that the dosage of lanthanum hexaboride is 19 g, and the dosage of 2-carboxyacrylic acid is 18 g.

[0081] Comparative Example 5

[0082] The polymer of this comparative example is different from that of Example 1 in that the dosage of lanthanum hexaboride is 22 g, and the dosage of 2-carboxyacrylic acid is 8.5 g.

[0083] The materials described in Examples 1-5 and Comparative Examples 1-5 can be subsequently made into coatings by thermal spraying. The materials are heated to 80°C, then placed in a Meiji V-3 air spray gun and sprayed onto the device surface, and dried at room temperature for about three hours to obtain an anti-icing and ice-melting coating.

[0084] Test Example 1: Ice melting experiment

[0085] The coating samples of Examples 1-5 and Comparative Examples 1-5 were placed on platforms of the same height in a -20°C freezer, and were continuously sprayed with water mist using a spray gun. When the amount of ice on each sample reached 30 g, the samples were taken out and transferred to another dry freezer at -20°C. After freezing for 24 hours, the ice melting experiment was started. During the ice melting experiment, ten samples were placed under the same power light source for irradiation at the same time, and the remaining ice content of the samples was recorded. The ice melting rate curves of the coating samples of Examples 1-5 and Comparative Examples 1-5 were plotted. The results are shown in Figure 3. It can be seen that under the condition of the same initial ice content, the two polymer materials were subjected to a simulation experiment of irradiating with the same light source for 20 minutes. It can be seen that the rare earth grafted modified composite amphiphilic polymer of Example 1 can achieve complete melting of the ice layer in 8 minutes, and the ice melting rate varies with the change of rare earth content, that is, when the content of another monomer remains unchanged, the more rare earth is added, the faster the ice melting rate. However, since no rare earth is added to the polymers of Comparative Examples 1 and Comparative Examples 2, the ice melting rate is very slow. After 20 minutes of illumination, there is still about 4.1g of ice layer that has not melted, and the ice melting rate is about one-third of that of the coating with rare earth added. It can be seen that the rare earth grafted modified composite amphiphilic polymer has a very excellent endothermic ice melting effect.

[0086] Test Example 2 Weather resistance, acid and alkali resistance, wear resistance and stability test

[0087] (1) Weathering test: The test was conducted in a xenon lamp aging test chamber with an irradiation intensity of 1000W / m 2 , the aging of the sample coating was observed after continuous testing for 350 hours, and the following data were obtained:

[0088]

[0089] It can be seen that in Comparative Example 1, aging of the coating began as early as 200 hours due to the absence of rare earth compounds. This is because inorganic materials can improve the chemical and physical stability of organic materials. In Comparative Examples 2-5, there are no rare earth compounds and a three-dimensional network structure cannot be formed, and the strength is greatly reduced. However, the coating described in the present invention did not age within 350 hours because it formed a three-dimensional network and was an inorganic-organic composite material.

[0090] (2) Acid and alkali resistance test: The samples of Examples 1-5 and Comparative Examples 1-5 were placed in 1 mol / L hydrochloric acid and 1 mol / L sodium hydroxide solutions, respectively. After immersion for 24 hours, the surface coating state of the samples was observed. The results are as follows:

[0091] Example 1: The coating surface is smooth in acid solution and alkaline solution, and no corrosion occurs.

[0092] Example 2: The coating surface was smooth in acid solution and alkaline solution, and no corrosion occurred.

[0093] Example 3: The coating surface was smooth in acid solution and alkaline solution, and no corrosion occurred.

[0094] Example 4: The coating surface was smooth in acid solution and alkaline solution, and no corrosion occurred.

[0095] Example 5: The coating surface was smooth in acid solution and alkaline solution, and no corrosion occurred.

[0096] Comparative Example 1: Delamination of the coating occurred in acid solution and alkaline solution.

[0097] Comparative Example 2: The coating turned white and gradually peeled off in the acid solution, but there was no obvious corrosion in the alkaline solution.

[0098] Comparative Example 3: The coating surface was smooth in the acid solution and the alkaline solution, and no obvious corrosion occurred. However, as the immersion time increased, the color of the coating surface became slightly uneven.

[0099] Comparative Example 4: The coating surface was smooth in both the acid solution and the alkaline solution, but fine lines were produced, which was the early stage of delamination and slight corrosion occurred.

[0100] Comparative Example 5: The coating surface was smooth in the alkaline solution without corrosion. There was a slight swelling sensation in the acid solution, but the non-delaminated surface was also relatively smooth.

[0101] The data show that the coating modified with rare earth borides greatly improves the corrosion resistance of the material, while the organic polymer material destroys the three-dimensional structure due to its own strong swelling effect, resulting in coating shedding.

[0102] (3) Abrasion resistance test: The test is conducted in accordance with the international standard "Paints and varnishes - Determination of abrasion resistance - Rotating rubber wheel method" (GB / T1768-2006) (ISO 7784-2:1997). This standard specifies the test method for determining the abrasion resistance of dry films of paints, varnishes or related products by rubbing with a rubber wheel using the rotating motion of the rubber wheel.

[0103] The experimental results show that the average loss values ​​of the coating mass of Examples 1-5 and Comparative Examples 3-5 are both less than 1 mg, but compared with Examples 1-5, the coating of Comparative Examples 3-5 can be clearly seen to have scratches. As the number of experiments increases, the average mass loss value tends to increase. Comparative Examples 1 and 2 produced average loss values ​​of 23 mg and 72 mg, respectively, after testing for 30 minutes.

[0104] (4) Stability test: The test adopts a cycle method to test whether the melting rate of the six coatings in Example 1 and Comparative Examples 1-5 decreases after five cycles of freezing and melting, so as to judge the stability of the coatings. The results are as follows: Figure 6 The results show that Example 1 and Comparative Examples 3-5 have excellent stability, and there is no obvious change in the ice melting rate in the five-cycle experiment. As the number of cycles increases, the ice melting rate of Comparative Examples 1 and 2 slows down, and even the coating of Comparative Example 2 almost completely falls off in the fourth cycle, indicating poor stability.

[0105] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A rare earth grafted polymer precursor, Features: The preparation method of the polymer precursor comprises the following steps: Rare earth hexaboride and dicarboxyl double bond compound are added to ethanol and reacted at 75-85°C for 18-24 hours under the catalysis of concentrated sulfuric acid. After purification, rare earth grafted polymer precursor C is obtained. 4 H 7 O 5 R 6 .

2. The rare earth grafted polymer precursor according to claim 1, Features: The mass ratio of the rare earth hexaboride to the dicarboxyl double bond compound is (200-210):(85-150).

3. The rare earth grafted polymer precursor according to claim 1, Features: The rare earth hexaboride is one of lanthanum hexaboride, cerium hexaboride and samarium hexaboride, or a mixture of two or more thereof.

4. The rare earth grafted polymer precursor according to claim 1, Features: The dicarboxyl double bond compound is 2-carboxy acrylic acid and / or 2-carboxy crotonic acid.

5. A method for preparing a rare earth grafted modified composite amphiphilic polymer, Features: The steps include: (1) Dissolving hydroxyethyl cellulose and 2,4-pentadienoic acid in a solvent, and reacting them at 75-85° C. for 18-24 hours under the catalysis of concentrated sulfuric acid, thereby obtaining a hydroxyethyl cellulose modified polymer monomer; (2) dissolving the polymer precursor according to any one of claims 1 to 4 and the hydroxyethyl cellulose modified polymer monomer obtained in step (1) in deionized water, heating the water to 60-70° C., adding persulfate as a catalyst, and refluxing the water overnight to obtain a water-soluble polymer; (3) dissolving a water-soluble polymer and acrylic acid in a solvent, activating for 15-30 minutes, and then adding concentrated sulfuric acid to catalyze the reaction for 12-15 hours, thereby obtaining a rare earth graft-modified composite amphiphilic polymer.

6. The method for preparing the rare earth graft modified composite amphiphilic polymer according to claim 5, Features: In the step (1), the mass ratio of hydroxyethyl cellulose to 2,4-pentadienoic acid is (46-47):(73-74).

7. The method for preparing the rare earth graft modified composite amphiphilic polymer according to claim 5, Features: In the step (2), the mass ratio of the polymer precursor to the polymer monomer modified with hydroxyethyl cellulose is (169-272): (213-355).

8. The method for preparing the rare earth graft modified composite amphiphilic polymer according to claim 5, Features: In the step (3), the mass ratio of the water-soluble polymer to the acrylic acid is (50-51): (50-51).

9. The rare earth grafted modified composite amphiphilic polymer prepared by the preparation method according to any one of claims 5 to 8.

10. Use of the rare earth graft modified composite amphiphilic polymer according to claim 9 in the preparation of railway antifreeze and water-retaining products.