High-temperature-resistant polyethylene wax for heat stabilizer and preparation method of high-temperature-resistant polyethylene wax
By extruding polyethylene, lead stearate, thiourea dioxide and sodium hypophosphite to granulate, the thermal cracking temperature is reduced and the polyethylene wax is modified by combining with each other, the polyethylene wax is solved. The high-temperature resistance performance of polyethylene wax produced by the cracking method is insufficient. The problem is that the thermal stability and product quality of polyvinyl chloride are improved, and energy consumption is reduced.
Patent Information
- Application Number
- CN202411211935.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The polyethylene waxes produced by the existing cracking method are relatively average in high temperature resistance, resulting in a relatively average improvement in the thermal stability of polyvinyl chloride and a higher energy consumption during thermal cracking.
By extruding polyethylene, lead stearate, thiourea dioxide and sodium hypophosphite to granulate, the thermal cracking temperature is reduced, and the polyethylene wax is modified by combining lead stearate, thiourea dioxide and sodium hypophosphite to improve the Its high temperature resistance and controls temperature and residence time in the extrusion equipment. A twin-screw extruder is used to improve shear force and high temperature coordination and improve cracking efficiency.
It significantly improves the high temperature resistance of polyethylene wax, so that it effectively inhibits deHCl under the high temperature processing conditions of polyvinyl chloride, extends the life of polyvinyl chloride products, reduces the temperature required for polyethylene thermal cracking production, and has a higher Economic value.
Abstract
Description
Technical Field
[0001] The invention relates to the field of polyethylene wax, in particular to a high temperature resistant polyethylene wax used as a heat stabilizer. Background Art
[0002] Heat stabilizers are commonly used additives in plastic processing, especially in the production of polyvinyl chloride.
[0003] Polyvinyl chloride is easy to lose HCl during thermal processing. Once polyvinyl chloride loses a large amount of HCl, the polyvinyl chloride products will change color and their strength will drop significantly, seriously affecting the quality of the polyvinyl chloride products.
[0004] Polyethylene wax is a commonly used heat stabilizer. By adding polyethylene wax, the phenomenon of HCl removal can be reduced during the processing of polyvinyl chloride, thereby improving the thermal stability of polyvinyl chloride, extending the life of polyvinyl chloride products, and improving the performance of polyvinyl chloride products.
[0005] However, the processing temperature of polyvinyl chloride is relatively high. Therefore, polyethylene wax needs to have good high temperature resistance to play a better role as a heat stabilizer. The existing methods for preparing polyethylene wax include polymerization method, cracking method, etc. Among them, the high temperature resistance of polyethylene wax obtained by polymerization method is significantly higher than that of cracking method. However, the cracking method can obtain polyethylene wax by directly heating and cracking polyethylene, which is simple to operate and has a wider application. However, the high temperature resistance of polyethylene wax obtained by the cracking method is relatively general, resulting in the fact that the polyethylene wax obtained by the cracking method is generally effective in improving the thermal stability of polyvinyl chloride when used as a heat stabilizer for polyvinyl chloride. Therefore, there is still room for improvement. Summary of the invention
[0006] In order to improve the high temperature resistance of polyethylene wax prepared by a cracking method, the present application provides a high temperature resistant polyethylene wax for use as a heat stabilizer and a preparation method thereof.
[0007] In a first aspect, the present application provides a method for preparing a high temperature resistant polyethylene wax for use as a heat stabilizer, using the following technical solution: A method for preparing a high temperature resistant polyethylene wax for use as a heat stabilizer comprises the following steps: Step 1), polyethylene, lead stearate, thiourea dioxide and sodium hypophosphite are uniformly mixed, extruded and granulated to obtain a masterbatch; Step 2), extruding and granulating the masterbatch through an extruder to obtain a high temperature resistant polyethylene wax for a heat stabilizer, wherein the temperature of the masterbatch in the extrusion equipment is controlled at 270-280°C, and the residence time of the masterbatch in the extrusion equipment is 35-45 minutes.
[0008] By adopting the above technical scheme, polyethylene, lead stearate, thiourea dioxide and sodium hypophosphite are first extruded to obtain a masterbatch, so that the thermal cracking temperature of polyethylene is low due to the mutual cooperation of lead stearate, thiourea dioxide and sodium hypophosphite during the thermal cracking process, thereby effectively reducing energy consumption. Moreover, during the thermal cracking process, the addition of lead stearate, thiourea dioxide and sodium hypophosphite has the effect of modifying the polyethylene wax, so that the obtained polyethylene wax has better high temperature resistance. Within the processing temperature range of polyvinyl chloride, the polyethylene wax has high stability, so that it can play a good role as a heat stabilizer, so that the quality of the obtained polyvinyl chloride products is better, which can not only achieve the effect of improving the high temperature resistance of polyethylene wax, but also reduce the temperature required for the thermal cracking of polyethylene to produce polyethylene wax, and has high economic value.
[0009] Preferably, the mass ratio of the lead stearate, thiourea dioxide and sodium hypophosphite is 0.5-0.7:0.9-1.1:0.7-0.9.
[0010] By adopting the above technical scheme and specifically selecting the mass ratio of lead stearate, thiourea dioxide and sodium hypophosphite, the coordination effect of lead stearate, thiourea dioxide and sodium hypophosphite is better, the modification effect on polyethylene wax is better, and the high temperature resistance of the obtained polyethylene wax is stronger.
[0011] Preferably, the mass ratio of the polyethylene, lead stearate, thiourea dioxide and sodium hypophosphite is 100:0.5-0.7:0.9-1.1:0.7-0.9.
[0012] By adopting the above technical scheme and specifically selecting the mass ratio of polyethylene, lead stearate, thiourea dioxide and sodium hypophosphite, the contents of lead stearate, thiourea dioxide and sodium hypophosphite in polyethylene are just right, the modification effect on the prepared polyethylene wax is better, the high temperature resistance of the polyethylene wax is better, and the quality of the prepared polyvinyl chloride is better.
[0013] Preferably, in step 1), the extrusion temperature is 180-190°C.
[0014] By adopting the above technical solution and specifically selecting the extrusion temperature, polyethylene, lead stearate, thiourea dioxide and sodium hypophosphite are fully mixed, and when the prepared masterbatch is cracked in the next step, the cracking effect is better.
[0015] Preferably, in step 2), the temperature of the masterbatch in the extrusion equipment is controlled at 273-277°C.
[0016] By adopting the above technical solution and specifically selecting the cracking temperature, the molecular weight distribution of the polyethylene wax obtained after cracking is narrower and the quality is better.
[0017] Preferably, in step 2), the residence time of the masterbatch in the extrusion equipment is 38-42 minutes.
[0018] By adopting the above technical solution and specifically selecting the cracking temperature, the performance of the obtained polyethylene wax is more stable and the quality is better.
[0019] Preferably, in step 2), the extruder is a twin-screw extruder.
[0020] By adopting the above technical solution, by using a twin-screw extruder, and utilizing shear force in combination with high temperature, the cracking efficiency is higher and has higher economic value.
[0021] In a second aspect, the present application provides a high temperature resistant polyethylene wax for a heat stabilizer, which adopts the following technical scheme: a high temperature resistant polyethylene wax for a heat stabilizer is prepared by the above-mentioned preparation method of the high temperature resistant polyethylene wax for a heat stabilizer.
[0022] By adopting the above technical scheme, the polyethylene wax has good high temperature resistance. Under the high temperature processing conditions of polyvinyl chloride, it can protect polyvinyl chloride for a longer time and inhibit the dehydrochlorination of polyvinyl chloride, so that the performance and quality of polyvinyl chloride products are better.
[0023] In summary, this application has the following beneficial effects: 1. Since the present application first extrude polyethylene, lead stearate, thiourea dioxide and sodium hypophosphite to obtain a masterbatch, the thermal cracking temperature of polyethylene is lowered by the mutual cooperation of lead stearate, thiourea dioxide and sodium hypophosphite during the thermal cracking process, which effectively reduces energy consumption. In addition, during the thermal cracking process, the addition of lead stearate, thiourea dioxide and sodium hypophosphite has the effect of modifying the polyethylene wax, so that the obtained polyethylene wax has better high temperature resistance. Within the processing temperature range of polyvinyl chloride, the polyethylene wax has high stability, so that it can play the role of a heat stabilizer well, so that the quality of the obtained polyvinyl chloride products is better, which can not only achieve the effect of improving the high temperature resistance of polyethylene wax, but also reduce the temperature required for the thermal cracking of polyethylene to produce polyethylene wax, and has high economic value.
[0024] 2. In the present application, it is preferred to specifically select the mass ratio of lead stearate, thiourea dioxide and sodium hypophosphite so that the coordination effect of lead stearate, thiourea dioxide and sodium hypophosphite is better, the modification effect on polyethylene wax is better, and the high temperature resistance of the obtained polyethylene wax is stronger.
[0025] 3. In the present application, it is preferred to specifically select the mass ratio of polyethylene, lead stearate, thiourea dioxide and sodium hypophosphite so that the content of lead stearate, thiourea dioxide and sodium hypophosphite in polyethylene is just right, which has a better modification effect on the obtained polyethylene wax, better high temperature resistance of the polyethylene wax and better quality of the obtained polyvinyl chloride. DETAILED DESCRIPTION
[0026] The present application is further described in detail below with reference to the embodiments.
[0027] Example 1 A method for preparing a high temperature resistant polyethylene wax for use as a heat stabilizer comprises the following steps: Step 1), 100kg polyethylene, 0.5kg lead stearate, 0.9kg thiourea dioxide, and 0.7kg sodium hypophosphite are put into a stirred tank at a speed of 120r / min, stirred for 5min, and mixed evenly to obtain a premix, and the premix is put into a twin-screw extruder for extrusion granulation. The processing temperatures in zones I-XI of the twin-screw extruder are sequentially set to: 180°C, 180°C, 180°C, 180°C, 185°C, 185°C, 185°C, 190°C, 190°C, 190°C, the main screw speed is 400rpm, the water tank temperature is 25°C during the cooling process, and underwater granulation is performed to obtain a masterbatch.
[0028] Step 2), the masterbatch is put into a twin-screw extruder for extrusion, and underwater granulation is performed to obtain a high temperature resistant polyethylene wax for a heat stabilizer. The temperature of the masterbatch in the twin-screw extruder is controlled at 270°C throughout the process, and the residence time of the masterbatch in the extrusion equipment is 45 minutes.
[0029] The polyethylene is high-density polyethylene purchased from PetroChina with the brand name DMDA-8008.
[0030] Lead stearate was purchased from Hubei Xinghengye Technology Co., Ltd., CAS No.: 1072-35-1.
[0031] Thiourea dioxide was purchased from Hubei Xinghengye Technology Co., Ltd., CAS number: 1758-73-2.
[0032] Sodium hypophosphite was purchased from Hubei Xinghengye Technology Co., Ltd., CAS No.: 7681-53-0.
[0033] Example 2 A method for preparing a high temperature resistant polyethylene wax for use as a heat stabilizer comprises the following steps: Step 1), 100kg polyethylene, 0.55kg lead stearate, 0.95kg thiourea dioxide, and 0.75kg sodium hypophosphite are put into a stirred tank at a speed of 120r / min, stirred for 5min, and mixed evenly to obtain a premix, and the premix is put into a twin-screw extruder for extrusion granulation. The processing temperatures in zones I-XI of the twin-screw extruder are sequentially set to: 178°C, 178°C, 178°C, 178°C, 183°C, 183°C, 183°C, 183°C, 188°C, 188°C, 188°C, the main screw speed is 400rpm, the water tank temperature is 25°C during the cooling process, and underwater granulation is performed to obtain a masterbatch.
[0034] Step 2), the masterbatch is put into a twin-screw extruder for extrusion, and underwater granulation is performed to obtain a high temperature resistant polyethylene wax for a heat stabilizer. The temperature of the masterbatch in the twin-screw extruder is controlled at 273°C throughout the process, and the residence time of the masterbatch in the extrusion equipment is 42 minutes.
[0035] The polyethylene is high-density polyethylene purchased from PetroChina with the brand name DMDA-8008.
[0036] Lead stearate was purchased from Hubei Xinghengye Technology Co., Ltd., CAS No.: 1072-35-1.
[0037] Thiourea dioxide was purchased from Hubei Xinghengye Technology Co., Ltd., CAS number: 1758-73-2.
[0038] Sodium hypophosphite was purchased from Hubei Xinghengye Technology Co., Ltd., CAS No.: 7681-53-0.
[0039] Example 3 A method for preparing a high temperature resistant polyethylene wax for use as a heat stabilizer comprises the following steps: Step 1), 100kg polyethylene, 0.6kg lead stearate, 1kg thiourea dioxide, and 0.8kg sodium hypophosphite are put into a stirring tank, the speed is 120r / min, stirring for 5min, mixing evenly, and obtaining a premix, and the premix is put into a twin-screw extruder for extrusion granulation. The processing temperatures in zones I-XI of the twin-screw extruder are sequentially set to: 175°C, 175°C, 175°C, 175°C, 180°C, 180°C, 180°C, 185°C, 185°C, 185°C, 185°C, the main screw speed is 400rpm, the water tank temperature is 25°C during the cooling process, and underwater granulation is performed to obtain a masterbatch.
[0040] Step 2), the masterbatch is put into a twin-screw extruder for extrusion, and underwater granulation is performed to obtain a high temperature resistant polyethylene wax for a heat stabilizer. The temperature of the masterbatch in the twin-screw extruder is controlled at 275°C throughout the process, and the residence time of the masterbatch in the extrusion equipment is 40 minutes.
[0041] The polyethylene is high-density polyethylene purchased from PetroChina with the brand name DMDA-8008.
[0042] Lead stearate was purchased from Hubei Xinghengye Technology Co., Ltd., CAS No.: 1072-35-1.
[0043] Thiourea dioxide was purchased from Hubei Xinghengye Technology Co., Ltd., CAS number: 1758-73-2.
[0044] Sodium hypophosphite was purchased from Hubei Xinghengye Technology Co., Ltd., CAS No.: 7681-53-0.
[0045] Example 4 A method for preparing a high temperature resistant polyethylene wax for use as a heat stabilizer comprises the following steps: Step 1), 100kg polyethylene, 0.65kg lead stearate, 1.05kg thiourea dioxide, and 0.85kg sodium hypophosphite are put into a stirring tank, the speed is 120r / min, stirring for 5min, mixing evenly, and obtaining a premix, and the premix is put into a twin-screw extruder, extruded and granulated, and the processing temperatures in zones I-XI of the twin-screw extruder are sequentially set to: 172°C, 172°C, 172°C, 172°C, 177°C, 177°C, 177°C, 177°C, 182°C, 182°C, 182°C, the main screw speed is 400rpm, the water tank temperature is 25°C during the cooling process, and underwater granulation is performed to obtain a masterbatch.
[0046] Step 2), the masterbatch is put into a twin-screw extruder for extrusion, and underwater granulation is performed to obtain a high temperature resistant polyethylene wax for a heat stabilizer. The temperature of the masterbatch in the twin-screw extruder is controlled at 277° C. throughout the process, and the residence time of the masterbatch in the extrusion equipment is 38 minutes.
[0047] The polyethylene is high-density polyethylene purchased from PetroChina with the brand name DMDA-8008.
[0048] Lead stearate was purchased from Hubei Xinghengye Technology Co., Ltd., CAS No.: 1072-35-1.
[0049] Thiourea dioxide was purchased from Hubei Xinghengye Technology Co., Ltd., CAS number: 1758-73-2.
[0050] Sodium hypophosphite was purchased from Hubei Xinghengye Technology Co., Ltd., CAS No.: 7681-53-0.
[0051] Example 5 A method for preparing a high temperature resistant polyethylene wax for use as a heat stabilizer comprises the following steps: Step 1), 100kg polyethylene, 0.7kg lead stearate, 1.1kg thiourea dioxide, and 0.9kg sodium hypophosphite are put into a stirring tank at a speed of 120r / min, stirred for 5min, and mixed evenly to obtain a premix, and the premix is put into a twin-screw extruder for extrusion granulation. The processing temperatures in zones I-XI of the twin-screw extruder are sequentially set to: 170°C, 170°C, 170°C, 170°C, 175°C, 175°C, 175°C, 175°C, 180°C, 180°C, 180°C, the main screw speed is 400rpm, the water tank temperature is 25°C during the cooling process, and underwater granulation is performed to obtain a masterbatch.
[0052] Step 2), the masterbatch is put into a twin-screw extruder for extrusion, and underwater granulation is performed to obtain a high temperature resistant polyethylene wax for a heat stabilizer. The temperature of the masterbatch in the twin-screw extruder is controlled at 280°C throughout the process, and the residence time of the masterbatch in the extrusion equipment is 35 minutes.
[0053] The polyethylene is high-density polyethylene purchased from PetroChina with the brand name DMDA-8008.
[0054] Lead stearate was purchased from Hubei Xinghengye Technology Co., Ltd., CAS No.: 1072-35-1.
[0055] Thiourea dioxide was purchased from Hubei Xinghengye Technology Co., Ltd., CAS number: 1758-73-2.
[0056] Sodium hypophosphite was purchased from Hubei Xinghengye Technology Co., Ltd., CAS No.: 7681-53-0.
[0057] Comparative Example 1 A method for preparing a high temperature resistant polyethylene wax for use as a heat stabilizer comprises the following steps: Step 1), 100kg polyethylene, 0.6kg trimethylolpropane, 1kg thiourea dioxide, and 0.8kg sodium hypophosphite are put into a stirring tank at a speed of 120r / min, stirred for 5min, and mixed evenly to obtain a premix, and the premix is put into a twin-screw extruder for extrusion granulation. The processing temperatures in zones I-XI of the twin-screw extruder are sequentially set to: 175°C, 175°C, 175°C, 175°C, 180°C, 180°C, 180°C, 185°C, 185°C, 185°C, 185°C, the main screw speed is 400rpm, the water tank temperature is 25°C during the cooling process, and underwater granulation is performed to obtain a masterbatch.
[0058] Step 2), the masterbatch is put into a twin-screw extruder for extrusion, and underwater granulation is performed to obtain a high temperature resistant polyethylene wax for a heat stabilizer. The temperature of the masterbatch in the twin-screw extruder is controlled at 275°C throughout the process, and the residence time of the masterbatch in the extrusion equipment is 200 minutes.
[0059] The polyethylene is high-density polyethylene purchased from PetroChina with the brand name DMDA-8008.
[0060] Trimethylolpropane was purchased from Shandong Daoqin Chemical Co., Ltd., CAS No.: 77-99-6.
[0061] Thiourea dioxide was purchased from Hubei Xinghengye Technology Co., Ltd., CAS number: 1758-73-2.
[0062] Sodium hypophosphite was purchased from Hubei Xinghengye Technology Co., Ltd., CAS No.: 7681-53-0.
[0063] Comparative Example 2 A method for preparing a high temperature resistant polyethylene wax for use as a heat stabilizer comprises the following steps: Step 1), 100kg polyethylene, 0.6kg lead stearate, 1kg barium stearate, and 0.8kg sodium hypophosphite are put into a stirring tank at a speed of 120r / min, stirred for 5min, and mixed evenly to obtain a premix, and the premix is put into a twin-screw extruder for extrusion granulation. The processing temperatures in zones I-XI of the twin-screw extruder are sequentially set to: 175°C, 175°C, 175°C, 175°C, 180°C, 180°C, 180°C, 185°C, 185°C, 185°C, the main screw speed is 400rpm, the water tank temperature is 25°C during the cooling process, and underwater granulation is performed to obtain a masterbatch.
[0064] Step 2), the masterbatch is put into a twin-screw extruder for extrusion, and underwater granulation is performed to obtain a high temperature resistant polyethylene wax for a heat stabilizer. The temperature of the masterbatch in the twin-screw extruder is controlled at 275°C throughout the process, and the residence time of the masterbatch in the extrusion equipment is 200 minutes.
[0065] The polyethylene is high-density polyethylene purchased from PetroChina with the brand name DMDA-8008.
[0066] Lead stearate was purchased from Hubei Xinghengye Technology Co., Ltd., CAS No.: 1072-35-1.
[0067] Barium stearate was purchased from Liyang Xinwang Plastic Co., Ltd., CAS No.: 6865-35-6.
[0068] Sodium hypophosphite was purchased from Hubei Xinghengye Technology Co., Ltd., CAS No.: 7681-53-0.
[0069] Comparative Example 3 A method for preparing a high temperature resistant polyethylene wax for use as a heat stabilizer comprises the following steps: Step 1), 100kg polyethylene, 0.6kg lead stearate, 1kg thiourea dioxide, and 0.8kg dibutyltin dilaurate are put into a stirring tank, the speed is 120r / min, stirring for 5min, mixing evenly, to obtain a premix, the premix is put into a twin-screw extruder, extrusion granulation, the processing temperatures of the twin-screw extruder I-XI zones are sequentially set to: 175°C, 175°C, 175°C, 175°C, 180°C, 180°C, 180°C, 185°C, 185°C, 185°C, the main screw speed is 400rpm, the water tank temperature is 25°C during the cooling process, underwater granulation, to obtain a masterbatch.
[0070] Step 2), the masterbatch is put into a twin-screw extruder for extrusion, and underwater granulation is performed to obtain a high temperature resistant polyethylene wax for a heat stabilizer. The temperature of the masterbatch in the twin-screw extruder is controlled at 275°C throughout the process, and the residence time of the masterbatch in the extrusion equipment is 200 minutes.
[0071] The polyethylene is high-density polyethylene purchased from PetroChina with the brand name DMDA-8008.
[0072] Lead stearate was purchased from Hubei Xinghengye Technology Co., Ltd., CAS No.: 1072-35-1.
[0073] Thiourea dioxide was purchased from Hubei Xinghengye Technology Co., Ltd., CAS number: 1758-73-2.
[0074] Dibutyltin dilaurate was purchased from Shandong Yuanjin New Materials Co., Ltd., CAS No.: 77-58-7.
[0075] Comparative Example 4 A method for preparing a high temperature resistant polyethylene wax for use as a heat stabilizer comprises the following steps: Step 1), 100kg polyethylene, 0.6kg trimethylolpropane, 1kg barium stearate, and 0.8kg dibutyltin dilaurate are put into a stirring tank at a speed of 120r / min, stirred for 5min, and mixed evenly to obtain a premix, and the premix is put into a twin-screw extruder for extrusion granulation. The processing temperatures in zones I-XI of the twin-screw extruder are sequentially set to: 175°C, 175°C, 175°C, 175°C, 180°C, 180°C, 180°C, 185°C, 185°C, 185°C, 185°C, the main screw speed is 400rpm, the water tank temperature is 25°C during the cooling process, and underwater granulation is performed to obtain a masterbatch.
[0076] Step 2), the masterbatch is put into a twin-screw extruder for extrusion, and underwater granulation is performed to obtain a high temperature resistant polyethylene wax for a heat stabilizer. The temperature of the masterbatch in the twin-screw extruder is controlled at 275°C throughout the process, and the residence time of the masterbatch in the extrusion equipment is 200 minutes.
[0077] The polyethylene is high-density polyethylene purchased from PetroChina with the brand name DMDA-8008.
[0078] Trimethylolpropane was purchased from Shandong Daoqin Chemical Co., Ltd., CAS No.: 77-99-6.
[0079] Barium stearate was purchased from Liyang Xinwang Plastic Co., Ltd., CAS No.: 6865-35-6.
[0080] Dibutyltin dilaurate was purchased from Shandong Yuanjin New Materials Co., Ltd., CAS No.: 77-58-7.
[0081] Experiment 1 The end group titration method was used to detect the number average molecular weight Mn of the high temperature resistant polyethylene wax used as a heat stabilizer in each embodiment and comparative example.
[0082] Experiment 2 Prepare polyvinyl chloride test samples, and test the tensile strength of the polyvinyl chloride test samples to which high temperature resistant polyethylene wax used as a heat stabilizer of each embodiment and comparative example was added according to GB / T1040.2-2022 "Determination of Tensile Properties of Plastics Part 2: Test Conditions for Molded and Extruded Plastics", and use Type 1A specimens for testing.
[0083] The preparation method of the polyvinyl chloride test sample is as follows: Step 01), take 100kg of polyvinyl chloride and 4kg of high temperature resistant polyethylene wax used as a heat stabilizer, put them into a stirring tank, rotate at 120r / min, stir for 10min, and obtain a mixture; Step 02), putting the mixture into a twin-screw extruder, extruding it into a mold, cooling it, and demolding it to obtain a polyvinyl chloride sample to be tested.
[0084] In step 02), the processing temperatures of the twin-screw extruder zones I-XI are set to: 175°C, 175°C, 185°C, 185°C, 190°C, 190°C, 190°C, 200°C, 200°C, 200°C, and the main screw speed is 300rpm.
[0085] Polyvinyl chloride was purchased from Sinopec, brand: S-1000.
[0086] The specific test data of Experiment 1-2 are shown in Table 1.
[0087] Table 1 Number average molecular weight Mn Tensile strength(MPa) Example 1 959 15.3 Example 2 953 15.2 Example 3 948 15.6 Example 4 941 15.4 Example 5 935 15.1 Comparative Example 1 998 12.7 Comparative Example 2 1035 12.3 Comparative Example 3 985 13.1 Comparative Example 4 1049 11.9 According to the data comparison between the embodiments and the comparative examples in Table 1, the molecular weights of the embodiments and the comparative examples are similar. Under the premise that the cracking temperatures of the embodiments and the comparative examples are the same, the time required for cracking of the comparative examples is significantly longer than that of the embodiments. It can be seen that the addition of the composite system of lead stearate, thiourea dioxide and sodium hypophosphite in the embodiments can effectively promote the cracking speed of polyethylene at low temperature, thereby achieving higher production efficiency.
[0088] At the same time, the strength of the polyvinyl chloride test sample to which the polyethylene wax of each embodiment is added is significantly higher than that of the polyvinyl chloride test sample to which the polyethylene wax of each comparative example is added. It can be seen that the high temperature resistance of the polyethylene wax can be effectively improved by adding the composite system of lead stearate, thiourea dioxide, and sodium hypophosphite in each embodiment. Even if an experimental temperature higher than the conventional polyvinyl chloride extrusion temperature is used in Experiment 2, the prepared polyvinyl chloride sample still has better physical properties. It can be seen that the polyethylene wax of each embodiment plays a good role in improving the thermal stability of polyvinyl chloride, making it difficult for polyvinyl chloride to remove HCl at high temperature, thereby better maintaining the original physical properties.
[0089] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A method for preparing high temperature resistant polyethylene wax for heat stabilizer, Features: The following steps are involved: Step 1), polyethylene, lead stearate, thiourea dioxide and sodium hypophosphite are uniformly mixed, extruded and granulated to obtain a masterbatch; Step 2), the masterbatch is extruded and granulated through an extruder to obtain a high temperature resistant polyethylene wax used as a heat stabilizer. The temperature of the masterbatch in the extrusion equipment is controlled at 270-280°C, and the residence time of the masterbatch in the extrusion equipment is 35-45 minutes.
2. The method for preparing a high temperature resistant polyethylene wax for a heat stabilizer according to claim 1, Features: The mass ratio of the lead stearate, thiourea dioxide and sodium hypophosphite is 0.5-0.7:0.9-1.1:0.7-0.
9.
3. The method for preparing a high temperature resistant polyethylene wax for a heat stabilizer according to claim 2, Features: The mass ratio of the polyethylene, lead stearate, thiourea dioxide and sodium hypophosphite is 100:0.5-0.7:0.9-1.1:0.7-0.
9.
4. The method for preparing a high temperature resistant polyethylene wax for a heat stabilizer according to claim 1, Features: In the step 1), the extrusion temperature is 180-190°C.
5. The method for preparing a high temperature resistant polyethylene wax for a heat stabilizer according to claim 1, Features: In the step 2), the temperature of the masterbatch in the extrusion equipment is controlled at 273-277°C.
6. The method for preparing a high temperature resistant polyethylene wax for a heat stabilizer according to claim 1, Features: In the step 2), the residence time of the masterbatch in the extrusion equipment is 38-42 minutes.
7. The method for preparing a high temperature resistant polyethylene wax for a heat stabilizer according to claim 1, Features: In the step 2), the extruder is a twin-screw extruder.
8. A high temperature resistant polyethylene wax for use as a heat stabilizer, Features: The wax is prepared by the method for preparing the high temperature resistant polyethylene wax used as a heat stabilizer according to any one of claims 1 to 7.
Citation Information
Patent Citations
Method for preparing polyethylene wax from recycled plastics through low-temperature cracking by screw extruder
CN107286277A
Special wax for heat stabilizer and preparation method of special wax
CN113667202A
Continuously producing waxy low molecular weight polyethylene from solid high molecular weight polyethylene
GB1310260A
Production of thermal decomposition wax
JP1992020509A
Production method of polyethylene-based thermal decomposition wax
JP2024044108A