Clay mineral-based nano composite pigment and preparation method thereof
Through solid phase grinding and high temperature treatment of clay minerals and organic dyes, nanocomposite pigments with wide spectrum and good stability are prepared, and the problems of insufficient stability and complex preparation of clay minerals and organic dye composite pigments in the prior art are solved, and the problem of insufficient preparation of clay minerals and organic dye composite pigments is achieved. Industrial application in coatings and other fields.
Patent Information
- Application Number
- CN202410915779.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-01
AI Technical Summary
The existing nanocomposite pigments of clay minerals and organic dyes are insufficient in stability, the preparation method is complex and costly, which limits its industrial application in the fields of coatings, inks, etc.
By solid phase grinding, mixed clay minerals and organic dyes and processing them at high temperature, nanocomposite pigments with wide chromatography range, chemical stability and light stability are prepared. Slopestone and sepiolite are used as substrates to simplify the process and avoid wastewater pollution .
It realizes high chemical and light stability of pigments, simplifies the preparation process, reduces production costs, improves dispersion and rheology, and is suitable for large-scale industrial production.
Smart Images

Figure BDA0004935045730000031 
Figure BDA0004935045730000061 
Figure BDA0004935045730000112
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of nano composite pigments, and specifically relates to a nano composite pigment formed by nano mineral palygorskite, sepiolite and an organic dye, and more particularly to an organic-inorganic nano composite pigment with simple process, few steps, high pigment stability, good dispersibility in a polar system, excellent rheological properties, outstanding economic and environmental benefits and a preparation process thereof. Background Art
[0002] Pigments are a class of solid colorants that are insoluble in water and other solvents. They are an important component of the paint and coating industry and constitute the most basic ingredient in water-based paint and ink formulations. Today, pigments, as a major coloring material, are not only used in paint and ink production, but also widely used in other fields such as plastics, cosmetics, papermaking and pharmaceuticals due to their excellent physical and chemical properties. The coatings industry currently accounts for nearly 60% of global pigment consumption.
[0003] Commonly used inorganic pigments such as iron oxide and zinc oxide have good stability and durability, but they have problems such as narrow color spectrum, low saturation, poor fluidity, easy agglomeration, etc. Organic pigments have good color saturation and fluidity, but their durability is poor and they are easily affected by external factors such as light and heat, causing discoloration and fading.
[0004] Therefore, the research and application of organic-inorganic nanocomposite pigments is one of the hot topics in the current pigment field. This composite pigment has both the weather resistance and light stability of inorganic pigments and the color richness and good dispersibility of organic pigments. Clay minerals (mainly including montmorillonite, kaolinite, halloysite, palygorskite and sepiolite, etc.) are a kind of excellent nanocarriers due to their unique nanostructure and adjustable surface properties. However, the composite research of clay minerals and organic pigments is still in its infancy, and its preparation method and application have not been fully explored and developed.
[0005] Existing research has mainly focused on laboratory scale, and its preparation methods have many limitations. For example, there is selectivity between minerals and organic dyes. Most nanocomposite pigments based on clay minerals and organic dyes are not stable enough and still need to be coated with a protective layer (such as silica, polysiloxane, etc.) to improve their chemical stability. In addition, some processes are complex, costly, and inefficient, which is not conducive to large-scale industrial production and commercial applications.
[0006] Therefore, it is necessary to conduct in-depth research on the interface interaction and selectivity between clay minerals and organic dyes, so as to develop suitable mineral matrices and organic dyes, and further develop simple and efficient preparation methods to achieve large-scale composites of clay minerals and organic pigments, and apply them to coatings, inks, plastics, etc. This can not only solve the limitations of traditional pigments in terms of performance and application, but also bring new opportunities and challenges to the development of the pigment industry. Summary of the invention
[0007] In order to solve the above problems, the present invention provides a nano composite pigment based on clay minerals, which is obtained by mixing clay minerals and organic dyes through solid phase grinding and then subjected to high temperature treatment. The composite pigment has a wide chromatographic range, good chemical stability and light stability, and good dispersion stability and rheological properties in polar systems. In addition, the preparation method of the present invention is simple and easy to operate, easy to control, does not produce a large amount of three wastes, does not need to add a large amount of stabilizers and rheological agents, and is environmentally friendly, thereby completing the present invention.
[0008] The object of the present invention is to provide a nano composite pigment based on clay minerals, which is obtained by mixing clay minerals with organic dyes and then subjecting them to high temperature treatment.
[0009] The organic dye is selected from one or more of the dyes having the structure shown in formula (1) or formula (2):
[0010]
[0011] Wherein, R1-R8 are each independently selected from H, alkyl, halide or sulfonate; R1'-R8' are each independently selected from H, alkyl, halide or sulfonate.
[0012] The clay mineral is selected from palygorskite and / or sepiolite, preferably palygorskite or sepiolite.
[0013] The present invention also aims to provide a method for preparing the nanocomposite pigment based on clay minerals, wherein the method comprises mixing clay minerals with organic dyes and subjecting the mixture to high temperature treatment to obtain the nanocomposite pigment based on clay minerals.
[0014] The mass ratio of the clay mineral to the organic dye is 100:(0.5-20), preferably 100:(1.0-10.0), and more preferably 100:(1.5-5).
[0015] The high temperature treatment temperature is 60-500°C, preferably 100-300°C, and more preferably 150-200°C.
[0016] The present invention has the following beneficial effects:
[0017] (1) The present invention prepares nanocomposite pigments by mixing organic dyes with sepiolite and palygorskite clay minerals and heating them. The preparation process is simple and has few steps. The pigment preparation process does not generate wastewater and is pollution-free, which complies with green industrial production.
[0018] (2) The nanocomposite pigment prepared by the present invention has a wide chromatographic range, and pigments of various hues can be obtained by selecting or designing the functional groups (substituents) of the organic dye.
[0019] (3) The nanocomposite pigment prepared by the present invention has outstanding chemical stability and light stability. Even after being treated with concentrated nitric acid or exposed to simulated light for 100 years, the color of the pigment remains stable, which effectively improves the durability of the pigment in the application scenario.
[0020] (4) Traditional coatings usually need to add a large amount of clay minerals (such as kaolinite, montmorillonite, palygorskite and sepiolite, etc.) as dispersion stability and rheological agents, whose main function is to prevent the pigment from settling and stratifying after a long period of static standing and to improve the construction efficiency and effect. The present invention uses nano clay minerals palygorskite and sepiolite with outstanding rheological properties as the matrix of the pigment, so that the pigment has the multiple functions of colorant, dispersant and rheological agent at the same time, effectively solving the dispersibility and rheological problems of the pigment in water or other polar media. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The nanocomposite pigments obtained in Examples 1 to 4 and the photographs thereof after being respectively irradiated with light and chemically treated;
[0022] Figure 2 The pigment (mixture of mineral and dye) obtained in Comparative Example 1 and its photographs after light exposure and chemical treatment respectively;
[0023] Figure 3 The composite pigment obtained in Comparative Examples 2 to 3 and the photographs thereof after being respectively treated with light and chemically;
[0024] Figure 4 The color difference values of the pigments obtained in Examples 1 to 2 and Comparative Examples 1-1, 1-2, 2-1, 2-2, and 2-3 after light irradiation and chemical treatment, respectively;
[0025] Figure 5 The color difference values of the pigments obtained in Examples 3 to 4 and Comparative Examples 1-3, 1-4, 3-1, 3-2, and 3-3 after light irradiation and chemical treatment, respectively;
[0026] Figure 6 The colloid rate of the nanocomposite pigments obtained in Examples 1 to 4 and the pigments obtained in Comparative Examples 2 and 3 in water;
[0027] Figure 7The viscosity (500s) of the nanocomposite pigments obtained in Examples 1 to 4 and the pigment aqueous dispersions (6%) obtained in Comparative Examples 2 and 3 is -1 );
[0028] Figure 8 Thixotropic ring areas of the nanocomposite pigments obtained in Examples 1 to 4 and the pigment aqueous dispersions (5%) obtained in Comparative Examples 2 and 3;
[0029] Fig. 9 Micropore size distribution diagram of palygorskite, Example 1, Comparative Example 1-1, Example 3 and Comparative Example 1-3;
[0030] Fig.10 Micropore size distribution diagram of sepiolite, Example 2, Comparative Examples 1-2, Example 4 and Comparative Examples 1-4;
[0031] Fig.11 Comparison of infrared spectra of Example 1, Example 2 and indigo;
[0032] Fig.12 Comparison of infrared spectra of Example 3, Example 4 and thioindigo;
[0033] Fig.13 Comparison of infrared spectra of Comparative Example 2 and indigo;
[0034] Fig.14 Comparative Example 3 and infrared spectra of thioindigo;
[0035] Fig.15 Schematic diagram of nanocomposite pigments formed by indigo and thioindigo-based organic dyes and palygorskite or sepiolite. DETAILED DESCRIPTION
[0036] The following detailed description of the present invention will make the features and advantages of the present invention more clear and explicit.
[0037] The present invention uses a solid phase mixing method to prepare a nano composite pigment of palygorskite and an organic pigment, or sepiolite and an organic pigment, which is an organic-inorganic composite pigment, and has the advantages of strong hiding power and good stability of inorganic pigments and wide color spectrum, high color saturation, bright colors and strong dyeing ability of organic pigments. In addition, the nano composite pigment based on clay minerals of the present invention has good dispersibility and fluidity in the aqueous solution system. The process is simple and feasible, and the problems of consuming a large amount of water and generating pigment wastewater to pollute the environment in the pigment production process are effectively avoided.
[0038] The invention provides a nano composite pigment based on clay minerals, which is obtained by mixing clay minerals with organic dyes and then subjecting them to high-temperature treatment.
[0039] The organic dye is selected from one or more of the dyes having the structure shown in formula (1) or formula (2):
[0040]
[0041] Wherein, R1 to R8 are each independently selected from H, an alkyl group, a halide group or a sulfonic acid group, preferably selected from H, an alkyl group having a carbon number of C1-C5, a halide group or a sulfonic acid group, and more preferably H; R1' to R8' are each independently selected from H, an alkyl group, a halide group or a sulfonic acid group, preferably selected from H, an alkyl group having a carbon number of C1-C5, a halide group or a sulfonic acid group, and more preferably H. Preferably, the organic dye is indigo and / or thioindigo.
[0042] The clay mineral is selected from palygorskite and / or sepiolite, preferably palygorskite or sepiolite. Palygorskite and sepiolite are typical layered chain clay minerals, and their microscopic morphology is nanofiber-like, with a fiber length of 0.2 to 2 μm, a width of 10 to 30 nm, and a thickness of 5 to 10 nm. Due to their special structure and properties, palygorskite and sepiolite have excellent dispersibility and rheological properties in water or polar solvents, maintaining the stability and ease of construction of the dispersed system. More importantly, the crystal structure of palygorskite and sepiolite is layered chain-like, with a large number of nanochannels (micropores). The channel size of palygorskite is The channel size of sepiolite is Zeolite water and coordinated water groups also exist in these channels and on their edges, which have special interfacial reactivity. Therefore, suitable organic dye molecules can be accommodated in the nanochannels of palygorskite or sepiolite, and may be anchored in them through special interfacial interactions, thus improving the stability of the pigments.
[0043] The content (mass percentage) of palygorskite or sepiolite in the clay mineral raw material is greater than 50%, preferably greater than 80%, and more preferably greater than 90%. The calculation of the mineral content refers to the standard SY / T 5163-2018 "X-ray diffraction analysis method of clay minerals and common non-clay minerals in sedimentary rocks". The whiteness of the clay mineral is greater than 60%, preferably greater than 80%, and more preferably greater than 90%.
[0044] The mass ratio of the clay mineral to the organic dye is 100:(0.5-20), preferably 100:(1.0-10.0), and more preferably 100:(1.5-5).
[0045] The high temperature treatment temperature is 60-500°C, preferably 100-300°C, and more preferably 150-200°C.
[0046] The present invention also provides a method for preparing the nano composite pigment based on clay minerals. The method comprises mixing clay minerals with organic dyes and subjecting the mixture to high temperature treatment to obtain the nano composite pigment based on clay minerals.
[0047] The mass ratio of the clay mineral to the organic dye is 100:(0.5-20), preferably 100:(1.0-10), and more preferably 100:(1.5-5). The maximum loading ratio of the organic dye is restricted by the specific surface area, pore volume and molecular size of the mineral. If the addition ratio of the organic dye is too low, the color saturation of the composite pigment is low and it is difficult to meet the application requirements; if the addition ratio of the organic dye is too high, the excess dye molecules cannot enter the microporous channels of the mineral to react with the mineral, resulting in decreased stability of the pigment and waste of the organic dye.
[0048] The clay mineral and the organic dye solid phase are mixed, and the method includes ball milling, mechanical stirring mixing, air flow mixing, etc., preferably ball milling. When ball milling is adopted, the ball-to-material ratio is (1-100):1, preferably (5-10):1, more preferably (8-10):1. The ball milling speed is 100-1000rpm, preferably 200-500rpm, more preferably 300-400rpm. The ball milling time is 1-60min, preferably 2-30min, more preferably 3-5min. After the ball milling is finished, a clay mineral and an organic dye mixture is obtained. Ball milling makes the organic dye evenly distributed in the clay mineral matrix. Too high ball milling speed and too long ball milling time will not only destroy the material structure, but also increase the process cost, which is not conducive to the preparation of composite pigments. Too low ball milling speed and too short ball milling time are easy to cause the clay mineral and the organic dye to mix unevenly, affecting the reaction effect in the later stage.
[0049] The high temperature treatment temperature is 60-500°C, preferably 100-300°C, more preferably 150-200°C, such as 150-200°C. The high temperature treatment time is 5min-72h, preferably 0.5-24h, more preferably 2-8h. After the high temperature treatment, a nanocomposite pigment based on clay minerals is obtained. The purpose of heat treatment is to break through the energy barrier of mineral-dye interface reaction, promote the diffusion of organic dye molecules into the microporous channels of clay minerals, and further form hydrogen bonds with the coordinated water molecules on both sides of the channels. If the temperature is too low, the diffusion and reaction energy barriers of organic dye molecules cannot be broken through, and the mineral-dye interface reaction does not occur or the reaction is insufficient; if the temperature is too high, the organic dye will be thermally decomposed to remove the coordinated water in the clay mineral structure, thereby affecting the mineral-dye interface reaction process. Similarly, an appropriate heat treatment time is conducive to the interaction between organic dyes and clay minerals. Too short a time will lead to insufficient reaction. After the interaction reaches equilibrium, too long a time will increase the process cost.
[0050] The nano composite pigment based on palygorskite and sepiolite prepared in the present invention has high color saturation, bright color, good chemical stability and light stability, and greatly improved dispersibility and rheological properties in polar systems. On the other hand, the preparation method of the nano composite pigment based on palygorskite and sepiolite of the present invention is simple, efficient, easy to implement and control, achieves product uniformity, and can achieve large-scale production. In the process, no solvent is needed to achieve green production.
[0051] Patent CN111303655A discloses a method for preparing natural pigments by hybridizing natural pigments of Chinese herbal medicines with palygorskite. Its purpose is to solve the problem of complex use of pigments extracted from various plants for plant dyeing and complicated processes. The solution adsorption method is adopted, and the natural plant dye is dispersed in an alcohol-water solution. The palygorskite is subjected to wet purification and activation treatment. In addition, high-temperature baking, microwave-assisted heating, nitrogen and water vapor are also involved. The process is complicated and a large amount of waste liquid is generated. In addition, the stability of plant pigments and composite pigments has not been evaluated.
[0052] Compared with the above patents, the present invention adopts solid phase mixing and heat treatment to prepare mineral-dye nanocomposite pigments. It is confirmed by experimental studies that the interfacial reaction between minerals and organic dyes is highly selective, and only the two clay minerals and two types of dye molecules involved in the present invention can interact with each other, thereby improving the stability of the pigment. Through chemical stability and light stability tests, it is confirmed that the pigment involved in the present invention has outstanding stability. In addition, through X-ray diffraction, infrared spectroscopy and pore analysis, it is found that the stabilization mechanism of the composite pigment is: the organic dye molecules diffuse into the microporous channels of the mineral under heat treatment conditions, and form hydrogen bonds with the coordinated water at the edge of the channel. In short, the raw materials used in the present invention are easy to obtain, the process is simple and environmentally friendly, the interfacial reaction mechanism involved is molecular diffusion and hydrogen bond formation, and the stability, dispersibility and rheology of the product are outstanding.
[0053] Example
[0054] The present invention is further described below by specific examples, but these examples are merely exemplary and do not constitute any limitation to the scope of protection of the present invention.
[0055] Example 1
[0056] Take 10 g of palygorskite and 0.2 g of indigo, add them into the ball mill of Fritsch pulveristte 6 ball mill, with a ball-to-material ratio of 10:1, and ball mill for 3 minutes at a speed of 350 rpm to ensure that the indigo and palygorskite raw materials are evenly mixed to obtain a palygorskite-indigo mixture.
[0057] The above mixture was placed in an oven and heated at 150° C. for 4 h to obtain nanocomposite pigment I.
[0058] Example 2
[0059] Take 10 g of sepiolite and 0.2 g of indigo, add them into the ball mill of Fritsch pulveristte 6 ball mill, with a ball-to-material ratio of 10:1, and ball mill for 5 minutes at a speed of 350 rpm to ensure that the indigo and sepiolite raw materials are evenly mixed to obtain a sepiolite-indigo mixture.
[0060] The above mixture was placed in an oven and heated at 200° C. for 1 h to obtain nanocomposite pigment II.
[0061] Example 3
[0062] Take 10 g of palygorskite and 0.3 g of sulfur indigo, add them into the ball mill of Fritsch pulveristte 6 ball mill, with a ball-to-material ratio of 10:1, and ball mill for 5 minutes at a speed of 350 rpm to ensure that the sulfur indigo and palygorskite raw materials are evenly mixed to obtain a palygorskite-sulfur indigo mixture.
[0063] The mixture was placed in an oven and heated at 200° C. for 8 h to obtain nanocomposite pigment III.
[0064] Example 4
[0065] Take 10 g of sepiolite and 0.2 g of thioindigo, add them into the ball mill of Fritsch pulveristte 6 ball mill, with a ball-to-material ratio of 10:1, and ball mill for 5 min at a speed of 350 rpm to ensure that the thioindigo and sepiolite raw materials are evenly mixed to obtain a sepiolite-thioindigo mixture.
[0066] The mixture was placed in an oven and heated at 180° C. for 4 h to obtain nanocomposite pigment IV.
[0067] Comparative Example
[0068] Comparative Example 1
[0069] The same raw material ratio and mixing scheme as in Examples 1 to 4 were adopted, but without heat treatment, to obtain mixtures having the same material ratio as in the examples, i.e., a palygorskite / indigo mixture, a sepiolite / indigo mixture, a palygorskite / sulfur indigo mixture and a sepiolite / sulfur indigo mixture, which were respectively recorded as Comparative Example 1-1, Comparative Example 1-2, Comparative Example 1-3 and Comparative Example 1-4.
[0070] Comparative Example 2
[0071] Take 10g each of montmorillonite, kaolinite and halloysite, take 2g (3 parts) of indigo, add them into the ball mill of Fritsch pulveristte 6 ball mill, with a ball-to-material ratio of 10:1, and ball mill for 3min at a rate of 350rpm to ensure that the indigo is evenly mixed with the montmorillonite, kaolinite and halloysite raw materials, respectively, to obtain montmorillonite-indigo, kaolinite-indigo and halloysite-indigo mixtures.
[0072] The above mixture was placed in an oven and heated at 150° C. for 4 h to obtain montmorillonite-indigo, kaolinite-indigo and halloysite-indigo composite pigments, which were respectively recorded as Comparative Example 2-1, Comparative Example 2-2 and Comparative Example 2-3.
[0073] Comparative Example 3
[0074] Take 10g each of montmorillonite, kaolinite, halloysite and 2g of thioindigo (3 parts), add them into the ball mill of Fritsch pulveristte 6 ball mill with a ball-to-material ratio of 10:1, and ball mill for 3min at a rate of 350rpm to ensure that the thioindigo is evenly mixed with the montmorillonite, kaolinite and halloysite raw materials to obtain montmorillonite-thioindigo, kaolinite-thioindigo and halloysite-thioindigo mixtures.
[0075] The above mixture was placed in an oven and heated at 150° C. for 8 h to obtain montmorillonite-sulfur indigo, kaolinite-sulfur indigo and halloysite-sulfur indigo composite pigments, which were respectively recorded as Comparative Example 3-1, Comparative Example 3-2 and Comparative Example 3-3.
[0076] Experimental example
[0077] Experimental Example 1 CIE Color Parameter Analysis
[0078] The color properties of the pigments were analyzed using the Shanghai Fuxiang Optical FX2000L multifunctional spectrometer, and the light source was HL-2000 (wavelength: 380-2000nm). The color properties of the pigments were analyzed by the reflectance spectrum measured by the instrument and the CIE 1976 color space parameters, where L* represents lightness, a* represents red when it is positive, green when it is negative, yellow when it is positive, and blue when it is negative. In the CIE color parameters, the larger the L* value, the higher the lightness, and the larger the |a*| and |b*| values, the stronger the corresponding hue. Before testing the color of the pigment, the pigment powder was first gently pressed into a tablet using a HF-2 manual tablet press (5mm mold).
[0079] S ab is the color saturation,
[0080] Table 1 CIE color parameters of Examples 1 to 2 and Comparative Examples
[0081]
[0082]
[0083] The color parameters of Examples 1-2 and Comparative Examples are shown in Table 1. As can be seen from Table 1, the L* values of the nanocomposite pigments in Examples 1-2 are 44.5 and 38.9, respectively, and the a* and b* values are negative, indicating that the color of the pigment is a mixture of green and blue (i.e., blue-green), and the saturation reaches 40% and 45%, respectively. The components of Comparative Examples 1-1 and 1-2 are the same as those of Examples 1 and 2, respectively, but have not been subjected to heat treatment, and their |a*| and |b*| are both less than those of the embodiments, and the saturation is not high. In addition, the |a*| of Comparative Examples 1-1 and 1-2 is close to 0, indicating that its color is blue. Comparative Examples 2-1, 2-2 and 2-3 are substantially the same as the organic dyes and process methods used in the embodiments, but the mineral matrices selected are montmorillonite, kaolinite and halloysite, respectively. From the color parameters, it can be seen that montmorillonite, kaolinite and halloysite cannot be used with indigo to prepare a blue-green pigment with a high saturation.
[0084] Table 2 CIE color parameters of Examples 3 to 4 and Comparative Examples
[0085]
[0086] The color parameters of Examples 3-4 and Comparative Examples are shown in Table 2. The L* values of the nanocomposite pigments in Examples 3-4 are 37.9 and 41.7, respectively, a* is a positive value, and b* is a negative value, indicating that the color of the pigment is a mixture of red and blue (i.e., purple), and the saturation is 69% and 73%, respectively. The components of Comparative Examples 1-3 and 1-4 are the same as those of Examples 3 and 4, respectively, but Comparative Examples 1-3 and 1-4 are mixtures of minerals and dyes and have not been heated. The blue hue of the nanocomposite pigments in Examples 3 and 4 is heavier, while the red hue of Comparative Examples 1-3 and 1-4 is heavier. In addition, the saturation of Comparative Examples 1-3 and 1-4 is less than that of Examples 3 and 4. Comparative Examples 3-1, 3-2 and 3-3 are composite pigments prepared by using montmorillonite, kaolinite and halloysite as the matrix and sulfur indigo, respectively. The results show that the colors of these pigments are mainly red hues, and the saturation is lower than that of the nanocomposite pigments in Examples 3 and 4.
[0087] Experimental Example 2: Stability Analysis
[0088] The prepared pigment was treated with concentrated nitric acid (HNO3, 68wt%) and dimethyl sulfoxide (DMSO) respectively to test the chemical stability of the pigment. The steps of concentrated nitric acid treatment are: weigh 0.03g of pigment sample, add it to 2mL of concentrated nitric acid, shake for 15min and then quickly centrifuge, continue to add ultrapure water to wash 3 times, dry and grind the sample to obtain the treated pigment. The steps of DMSO treatment are: weigh 0.03g of pigment sample, add it to 5mL of DMSO, shake for 24h and then centrifuge, dry and grind the pigment to obtain the treated pigment. The specific color of the pigment after treatment with concentrated nitric acid or DMSO is as follows: Figure 1 shown.
[0089] The SL21-63.9-WDG LED point light source produced by Dongguan Kangshida Automation Co., Ltd. was used as a white light simulation light source to irradiate the sample. The working distance between the light and the sample was 10 cm, the diameter of the effective irradiation area was 2.5 cm, and the illumination was 100 kLux. The color of the pigment was tested after 600 hours of irradiation, and the corresponding total illumination was 60000 kLux h (600 hours), which is equivalent to 100 years of illumination in an ordinary museum (illuminance is 200 Lux, 10 hours of irradiation per day, 6 days a week, and 50 weeks a year). The color difference of the pigment before and after illumination was compared to analyze its light stability. The color of the pigment after illumination is as follows: Figure 1 shown.
[0090] Test the color parameters of the treated pigment and calculate the color difference before and after treatment. The formula is:
[0091] Where ΔE* is the total color difference, L1* is the lightness of the sample after treatment, a1* and b1* are the color hue values of the sample after treatment; L0* is the lightness of the sample before treatment, a0* and b0* are the color hue values of the sample before treatment.
[0092] from Figure 1 It can be seen that Examples 1 to 4 still retain their colors after being treated with light, nitric acid and DMSO, respectively, while Comparative Examples 2 and 3 severely fade after being treated with light or chemicals (e.g. Figure 2 and 3 The color difference values of Examples 1 to 4 and the comparative example after being treated with light, concentrated nitric acid or DMSO are shown in FIG. Figure 4 and 5 As shown. Figure 4 and 5 It can be seen that after being treated with light, concentrated nitric acid or DMSO, the color difference values of Examples 1 to 4 are all less than 10, while the color difference values of the comparative examples are all greater than 10, and some color difference values are above 40. Therefore, compared with the comparative examples, Examples 1 to 4 have good light stability and chemical stability.
[0093] Experimental Example 3: Colloid Rate Analysis
[0094] The nanocomposite pigments prepared in Examples 1 to 4 or Comparative Example 1 were added to ultrapure water at a concentration of 0.06 g / mL. After being fully dispersed, the dispersion was added to a 25 mL stoppered measuring cylinder to the 25 mL mark. After standing for 24 hours, the colloid volume (mL) of the dispersion in the measuring cylinder was read. The calculation formula for the colloid rate is:
[0095]
[0096] The colloid rate results of Examples 1 to 4 in aqueous solution are shown in Figure 6 At the initial stage, the colloid rate of all samples was 100%. After standing for 24 hours, the colloid rates of Examples 1 to 4 were 70%, 100%, 80%, and 100%, respectively, while the colloid rates of the comparative examples were all less than 30%. It can be seen that Examples 1 to 4 have good dispersibility in the aqueous solution system.
[0097] Experimental Example 4 Rheological Analysis
[0098] 6 g of the nanocomposite pigments prepared in Examples 1 to 4 and the comparative example were added to 100 mL of water and dispersed with a high-speed stirrer at a speed of 8000 rpm for 5 min to obtain an aqueous dispersion of the pigment. The prepared dispersion was added to the measuring plate of the ThermoScientific Haake Mars iQ rheometer, using a C60 flat rotor, the temperature was set to 25°C, and after keeping warm for 2 min, the rheological properties of the dispersion were tested. -1 The viscosity of the dispersion was tested continuously for 30 seconds at a shear rate of 1.5, and the average value was taken. Thixotropy was characterized by the thixotropic ring area, that is, within 300 seconds, the shear rate was changed from 0s to -1 Increase to 500s -1 , in 500s -1 After shearing for 30 seconds at a rate of -1 Reduce to 0s -1 , test the thixotropic ring area.
[0099] The viscosity and thixotropic ring area of Examples 1 to 4 and the comparative example are shown in FIG. Figure 7 and 8 As can be seen from the figure, the viscosity of Examples 1 to 4 is above 100 mPa·s, while that of the comparative examples is less than 70 mPa·s. Correspondingly, the thixotropic ring area of Examples 1 to 4 is 460 Pa·s. -1 Above, while the maximum value of the comparative example is 198 Pa·s -1 It can be seen that Examples 1 to 4 have very good viscosity and thixotropy, while the rheological properties of the comparative example are relatively poor.
[0100] Experimental Example 5 Analysis of Micropore Size Distribution
[0101] MicroActive ASAP2020 physical adsorption instrument was used to measure the N2 adsorption and desorption isotherms of the samples, with a degassing temperature of 60°C and an adsorption temperature of 77K. The micropore volume and pore size distribution of the samples were calculated according to the HK model. Example 1, Example 3, Comparative Example 1-1 and Comparative Example 1-3 all used palygorskite as the matrix. The micropore distribution diagram of the obtained pigment and palygorskite ore is shown in Fig. 9 . Among them, the palygorskite ore has obvious micropores between 0.5-0.6nm, corresponding to the nanochannels in the palygorskite crystal structure (0.37×0.64nm). In the samples of Examples 1 and 3, the micropore volume in this area is sharply reduced, while in Comparative Examples 1-1 and 1-3, although the micropore volume in this area is reduced, there is still an obvious micropore distribution. Therefore, in the composite pigment samples of Examples 1 and 3, the dye molecules enter the nanochannels of palygorskite, while in the unheated pigment (i.e., a mixture of palygorskite and dye), the dye molecules are mainly surface-coated (which will block the entrance of some nanochannels and cause the pore volume to decrease). The micropore volume distribution of Example 2, Example 4, Comparative Example 1-2, Comparative Example 1-4 and sepiolite ore is shown in FIG. Fig.10 As can be seen from the figure, sepiolite has a significant distribution of micropores between 0.5-0.6nm, corresponding to the nanochannels (0.37×1.06nm) in the crystal structure of sepiolite. The micropore volume of Example 2 in this region is smaller than that of Comparative Examples 1-2, and the micropore volume of Example 4 in this region is also smaller than that of Comparative Examples 1-4. It can be seen that for sepiolite, heat treatment helps dye molecules enter the nanochannels in its structure.
[0102] Experimental Example 6 Fourier Transform Infrared Spectroscopy Analysis
[0103] The sample was analyzed by a Bruker 70v Fourier transform infrared spectrometer. The sample and potassium bromide were weighed at a mass ratio of 1:100, ground and mixed evenly in a mortar, pressed into a transparent sheet using a tablet press and a mold, and then placed in the light path of the infrared spectrometer. The infrared spectrum of the sample was tested in transmission mode. The infrared spectra of Examples 1 and 2 are shown in Fig.11 As can be seen from the figure, the characteristic absorption frequencies of indigo are 1626, 1583, 1483, 1461, 1392, 1317 and 1298 cm -1 Among them, 1626cm -1The absorption at belongs to the stretching vibration of C=O, and the rest are CC skeleton and CH vibration. In Examples 1 and 2, the C=O stretching vibration of indigo is red-shifted, while its skeleton vibration is blue-shifted. The reason is that the intermolecular hydrogen bond of indigo is broken, and its C=O forms a new intermolecular hydrogen bond with the coordinated water in the palygorskite or sepiolite structure. The infrared spectra of Examples 3 and 4 ( Fig.12 ) also has similar changes. The characteristic absorption frequencies of thioindigo are 1651, 1583, 1446 and 1285 cm -1 After sulfur indigo and palygorskite or sepiolite form nanocomposite pigments, the vibration of C=O is red-shifted, while the skeleton vibration is blue-shifted. The reason is that sulfur indigo molecules form hydrogen bonds with the coordinated water in the palygorskite or sepiolite structure. However, the infrared spectra of the pigments in Comparative Examples 2 and 3 ( Fig.13 and 14 ) is basically consistent with the signal of organic dyes, which shows that the pigment in the comparative example is only a mixture of minerals and dyes and no hydrogen bonds are formed.
[0104] In the present invention, the mechanism by which clay mineral palygorskite (or sepiolite) and organic dyes form stable nanocomposite pigments is as follows: Fig.15 As shown, that is, under heat treatment conditions, the organic molecules diffuse in the nanochannels of the mineral and form hydrogen bonds with the coordinated water molecules of the octahedron at the edge of the channel through their C=O, thereby being firmly bound in the mineral structure, and finally forming a nanocomposite pigment with excellent light stability and chemical stability. Based on the excellent dispersibility and rheology of palygorskite and sepiolite, this type of pigment has outstanding dispersibility and rheology in polar solvents.
[0105] The present invention is described in detail above in conjunction with specific embodiments and / or exemplary examples and drawings, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, various equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.
Claims
1. A nano composite pigment based on clay minerals, which is obtained by mixing and grinding clay minerals and organic dyes and then subjecting them to high temperature treatment.
2. The nanocomposite pigment according to claim 1, characterized in that: The organic dye is selected from one or more of the dyes having the structure shown in formula (1) or formula (2): Among them, R1~R8 are each independently selected from H, alkyl, halide or sulfonate, preferably selected from H, alkyl with a carbon number of C1-C5, halide or sulfonate; R1`~R8` are each independently selected from H, alkyl, halide or sulfonate, preferably selected from H, alkyl with a carbon number of C1-C5, halide or sulfonate.
3. The nanocomposite pigment according to claim 2, characterized in that: The organic dye is indigo and / or thioindigo.
4. A method for preparing a nanocomposite pigment based on clay minerals according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: mixing and grinding clay minerals and organic dyes, and then subjecting the mixture to high temperature treatment to obtain nano composite pigments based on clay minerals.
5. The preparation method according to claim 4, characterized in that: The mass ratio of the clay mineral to the organic dye is 100:(0.5-20), preferably 100:(1.0-10), and more preferably 100:(1.5-5).
6. The preparation method according to claim 4, characterized in that: The clay mineral is selected from palygorskite and / or sepiolite.
7. The preparation method according to claim 4, characterized in that: The clay mineral and the organic dye are mixed by a solid phase method, including manual mixing, mechanical stirring mixing, ball milling mixing, and air flow mixing, preferably ball milling mixing and stirring mixing.
8. The preparation method according to claim 7, characterized in that: The grinding is ball milling, and the ball milling time is 3-11 min, preferably 3-8 min, and more preferably 3-5 min.
9. The preparation method according to claim 3, characterized in that: The high temperature treatment temperature is 100-400°C, preferably 100-350°C, more preferably 100-300°C.
10. The preparation method according to claim 3, characterized in that: The high temperature treatment time is 0.5-12 h, preferably 2.5-10 h, and more preferably 4-8 h.
Citation Information
Patent Citations
Method for preparing natural pigment from palygorskite hybridized Chinese herbal medicine natural colorant
CN111303655A
Method for preparing attapulgite supported high weather resistance composite pigment
CN102329524A
Preparation method of chlorophyll / clay mineral hybrid green pigment
CN112175414A
Color compositions
US20040011254A1
Hybrid pigment composition comprising dyes or pigments and fibrous clay
US20110113986A1