Manufacturing method of novel heavy-duty anti-corrosion material

By doping sulfonic acid cup aromatics on polyfluoroaniline nanowires and introducing rare earth ions into the phosphated acrylate composite emulsion, a high-conductive conductive network and passivation film are formed, the problem of corrosion of metal materials is solved and the metal is significantly improved Anti-corrosion performance and service life.

CN118879150AInactive Publication Date: 2024-11-01CHANGSHENG XINLIAN ECOLOGICAL IND DEVELOPMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411191797.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Metal materials are prone to corrosion under various environmental conditions, resulting in a decrease in mechanical properties and shortened service life. The existing anti-corrosion technology has limitations, especially electrochemical corrosion is difficult to effectively control.

Method used

Rare earth ions are loaded by phosphating acrylate composite emulsion and doping sulfonic acid cup aromatic hydrocarbons on polyfluoroaniline nanowires to form a highly conductive conductive network and passivation film, combining the plasticity of the phosphate groups and the chelation of the metal surface Cooperation is used to form a coating with high flash corrosion resistance and corrosion resistance.

Benefits of technology

It significantly reduces the corrosion rate of the metal surface, improves the adhesion and corrosion resistance of the coating, enhances the corrosion resistance of the metal, and extends the service life of the metal structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879150A_ABST
    Figure CN118879150A_ABST
Patent Text Reader

Abstract

The invention discloses a manufacturing method of a heavy-duty anti-corrosion new material, and belongs to the technical field of anti-corrosion materials. Calixarene is introduced to the polyfluoroaniline nanowire, so that the hydrophilicity of polyfluoroaniline is reduced, the polyfluoroaniline is promoted to form a high-conductivity conductive network in the coating by utilizing the large specific surface area of the calixarene, a compact oxidation film is favorably formed on the surface of metal, the metal is passivated, and the corrosion rate is effectively reduced; due to the nanowire form of the polyfluoroaniline, the conductivity of the material is reduced, and the risk of galvanic corrosion is reduced; porosity and low adhesiveness of the polyfluoroaniline are improved by doping, so that the polyfluoroaniline can be highly dispersed and activated in the acrylate emulsion, and phosphate groups are introduced into the acrylate composite emulsion, so that flexibility of a film formed by the material is enhanced, adhesive force between a coating and metal is improved, and the service life of the coating is prolonged. A passivation film with high flash corrosion resistance and corrosion resistance is formed through migration of fluorine-containing chain segments and chelation of phosphate ester groups and the metal surface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of anti-corrosion materials, and in particular relates to a method for preparing a new heavy-duty anti-corrosion material. Background Art

[0002] Metal materials are prone to corrosion under various environmental conditions, which will significantly reduce their mechanical properties and service life, posing a challenge to the safety and reliability of engineering projects. Metal corrosion mainly includes two forms: chemical corrosion and electrochemical corrosion, of which electrochemical corrosion is the most common type. The corrosion of metal materials not only causes huge economic losses, but also leads to a large waste of metal resources and energy, and may even cause equipment damage accidents and environmental pollution problems. In order to effectively control metal corrosion, a variety of anti-corrosion technologies have been developed, including cathodic protection, alloying modification, organic coating, etc. Cathodic protection is a method of forming a protective layer on the metal surface through an external current or sacrificial anode, which can significantly improve the corrosion resistance of the metal. Alloying modification improves the corrosion resistance of the material by adding other metals or non-metallic elements. For example, stainless steel improves the corrosion resistance of steel by adding elements such as chromium and nickel.

[0003] As an important metal anti-corrosion technology, organic coating forms a protective film on the metal surface to isolate the metal matrix from the external environment and effectively slow down the corrosion rate. Organic coatings include electrochemical protection, corrosion inhibition by corrosion inhibitors, and protection by protective layers. Among them, epoxy resin coatings, polyurethane coatings, fluororesin coatings, and silicone coatings are several organic anti-corrosion coatings with excellent performance. They improve the shielding performance and corrosion resistance of coatings through different modification methods, such as adding nanoparticles and blending modification. In addition, rare earth elements, due to their unique 4f electronic structure, exhibit excellent optical, electrical, magnetic and catalytic properties and are widely used in energy conversion, catalysis, magnetism, photonics and other fields. The doping of rare earth elements can improve the physical and structural properties of matrix compounds and even discover novel material properties. For example, the unique electronic structure of rare earth elements enables them to form a variety of oxidation states and stable coordination compounds, forming a protective layer on the metal surface, which enhances the corrosion inhibition effect of the coating.

[0004] In summary, the corrosion of metal materials is a complex process involving a variety of internal and external factors. By adopting appropriate anti-corrosion technology, the service life of metal structures can be effectively extended to ensure their safety and reliability. At the same time, the introduction of rare earth elements provides new ideas and methods for the development of new heavy-duty anti-corrosion materials. Based on this, it is necessary to propose a method for making a new heavy-duty anti-corrosion material. Summary of the invention

[0005] In view of the above situation, in order to overcome the defects of the prior art, the present invention prepares a new material with heavy anti-corrosion function by loading rare earth ions through phosphating acrylate composite emulsion and doping sulfonic acid calixarene through polyfluoroaniline nanowires.

[0006] In order to achieve the above object, the following technical scheme is adopted: The present invention provides a method for preparing a new heavy-duty anti-corrosion material, comprising the following steps:

[0007] (1) adding ammonium persulfate, sodium bicarbonate and deionized water to a reaction device to obtain an initial reaction solution, adding a nucleating agent dropwise when the reaction solution is heated to 82-85° C., reacting for 0.5-1.5 hours after the addition is complete, and then adding rare earth nitrate hydrate, and then adding a shelling agent dropwise, reacting for 1-2 hours after the addition is complete, filtering out insoluble solids, and obtaining a phosphated acrylate composite emulsion with rare earth ions loaded on the surface;

[0008] (2) adding a 10%-30% aqueous solution of 4-sulfonic acid calixarene to a reaction device, adding fluoroaniline monomer and mixing under nitrogen atmosphere, controlling the temperature of the reaction system to 0-5°C, slowly adding a 20%-50% aqueous solution of ammonium persulfate, reacting at room temperature for 5-12 hours, centrifuging after the reaction, washing the solid with deionized water until the pH of the deionized water is 7.5, and drying at 60°C for 24-48 hours to obtain polyfluoroaniline nanowires doped with sulfonic acid calixarene;

[0009] (3) The polyfluoroaniline nanowires doped with sulfonic acid calixarene and the phosphated acrylate composite emulsion modified with surface-loaded rare earth ions are mixed, and stirred at high speed to obtain the heavy-duty anti-corrosion new material.

[0010] Furthermore, the mass ratio of ammonium persulfate, sodium bicarbonate and deionized water in the initial reaction solution is 0.05-0.1:0.2-0.5:25-50.

[0011] Furthermore, the nucleating agent comprises components in the following mass ratio: methyl methacrylate: butyl acrylate: methacrylic acid: ammonium persulfate: deionized water = 4-6: 8-12: 0.2-0.4: 0.4-1: 0.02-0.05: 12-20.

[0012] Furthermore, the shell-forming agent comprises components in the following mass ratio: methyl methacrylate: butyl acrylate: methacrylic acid: 2-methyl-2-acrylic acid-2-hydroxyethyl ester phosphate: ammonium persulfate: deionized water 7-10: 3-5: 0.2-0.4: 1.5-3: 0.4-0.6: 0.02-0.05: 12-20.

[0013] Furthermore, the mass ratio of the initial reaction solution, the nucleating agent, the rare earth nitrate hydrate and the shelling agent is 12-15:10-15:0.5-2:10-15.

[0014] Furthermore, in the step (2), the mass ratio of 4-sulfonic acid calixarene, fluoroaniline monomer and ammonium persulfate is 1:0.5-3:1-2.5.

[0015] Furthermore, in the step (3), the mass ratio of the polyfluoroaniline nanowires doped with sulfonic acid calixarene to the phosphated acrylate composite emulsion with rare earth ions loaded on the surface is 0.1-1:3-5.

[0016] Furthermore, the fluoroaniline monomer is one of 2-fluoroaniline, 3-fluoroaniline or 4-fluoroaniline.

[0017] Furthermore, the rare earth nitrate hydrate is one of cerium nitrate hydrate, lanthanum nitrate hydrate, praseodymium nitrate hydrate or neodymium nitrate hydrate.

[0018] Furthermore, the rotation speed of the high-speed stirring is 3000-5000 rpm, and the time is 10-20 min.

[0019] The beneficial effects of the present invention are:

[0020] (1) The present invention not only reduces the hydrophilicity of polyfluoroaniline by introducing calixarene into polyfluoroaniline nanowires, but also utilizes the large specific surface area of ​​calixarene to promote the formation of a highly conductive conductive network of polyfluoroaniline in the coating. This network structure helps to form a dense oxide film on the metal surface, so that the metal is in a passivated state and effectively reduces the corrosion rate. In addition, the nanowire morphology of polyfluoroaniline helps to reduce the conductivity of the material, thereby reducing the risk of galvanic corrosion.

[0021] (2) By doping polyfluoroaniline with sulfonic acid calixarene, its porosity and adhesion are improved, so that it can be highly dispersed and activated in the acrylic emulsion. The phosphate groups introduced into the acrylic composite emulsion by the present invention enhance the flexibility of the film-forming material due to the excellent plasticity of the phosphate, and improve the adhesion between the coating and the metal. The migration of the fluorinated chain segment and the chelation of the phosphate group with the metal surface form a passivation film with high flash corrosion resistance and corrosion resistance.

[0022] (3) The rare earth ions loaded in the phosphated acrylate composite emulsion act as a sustained-release agent and form a stable complex with the metal surface, further improving the corrosion resistance of the material. The unique electronic structure of rare earth elements enables them to form a variety of oxidation states and stable coordination compounds, forming a protective layer on the metal surface, thereby enhancing the corrosion inhibition effect of the coating. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The salt spray resistance test results of various embodiments and comparative examples of a method for preparing a new heavy-duty anti-corrosion material of the present invention are as follows;

[0024] Figure 2 The aging resistance test results of various embodiments and comparative examples of a method for preparing a new heavy-duty anti-corrosion material of the present invention are shown;

[0025] Figure 3 The water resistance test results of various embodiments and comparative examples of a method for preparing a new heavy-duty anti-corrosion material of the present invention are shown;

[0026] Figure 4 The figures are the adhesion test results of various embodiments and comparative examples of a method for making a new heavy-duty anti-corrosion material of the present invention.

[0027] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. They are used to explain the present invention together with the embodiments of the present invention and do not constitute a limitation of the present invention. DETAILED DESCRIPTION

[0028] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0029] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein may be applied to the present invention. The preferred implementation methods and materials described herein are for demonstration purposes only and are not intended to limit the content of this application.

[0030] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are purchased from commercial channels unless otherwise specified.

[0031] Example 1

[0032] A method for producing a new heavy-duty anticorrosion material

[0033] The method comprises the following steps:

[0034] (1) adding ammonium persulfate, sodium bicarbonate and deionized water to a reaction device to obtain an initial reaction solution, adding a nucleating agent dropwise when the reaction solution is heated to 82-85° C., reacting for 0.5 h after the addition is complete, and then adding cerium nitrate hydrate, and then adding a shelling agent dropwise, reacting for 1 h after the addition is complete, filtering out insoluble solids, and obtaining a phosphated acrylate composite emulsion with rare earth ions loaded on the surface;

[0035] (2) adding a 10% aqueous solution of 4-sulfonic acid calixarene to a reaction device, adding 2-fluoroaniline under nitrogen atmosphere, and then controlling the temperature of the reaction system to 0°C, slowly adding a 20% aqueous solution of ammonium persulfate, and reacting at room temperature for 5 hours. After the reaction is completed, centrifugation is performed, and the solid is washed with deionized water until the pH of the deionized water is 7.5, and dried at 60°C for 24 hours to obtain polyfluoroaniline nanowires doped with sulfonic acid calixarene;

[0036] (3) The polyfluoroaniline nanowires doped with sulfonic acid calixarene and the phosphated acrylate composite emulsion modified with surface loaded rare earth ions were mixed, and the mixture was stirred at a high speed of 3000 rpm for 10 minutes to obtain the heavy-duty anti-corrosion new material.

[0037] The mass ratio of ammonium persulfate, sodium bicarbonate and deionized water in the initial reaction solution is 0.05:0.2:25.

[0038] The nucleating agent includes components in the following mass ratio: methyl methacrylate: butyl acrylate: methacrylic acid: ammonium persulfate: deionized water = 4:8:0.2:0.4:0.02:12.

[0039] The shell-forming agent comprises components in the following mass ratio: methyl methacrylate: butyl acrylate: methacrylic acid: 2-methyl-2-acrylic acid-2-hydroxyethyl ester phosphate: ammonium persulfate: deionized water 7:3:0.2:1.5:0.4:0.02:12.

[0040] The mass ratio of the initial reaction solution, the nucleating agent, the cerium nitrate hydrate and the shelling agent is 12:10:0.5:10.

[0041] In the step (2), the mass ratio of 4-sulfonic acid calixarene, 2-fluoroaniline and ammonium persulfate is 1:0.5:1.

[0042] The mass ratio of the polyfluoroaniline nanowires doped with sulfonic acid calixarene and the phosphated acrylate composite emulsion with rare earth ions loaded on the surface in step (3) is 0.1:3.

[0043] Example 2

[0044] A method for producing a new heavy-duty anticorrosion material

[0045] The method comprises the following steps:

[0046] (1) adding ammonium persulfate, sodium bicarbonate and deionized water to a reaction device to obtain an initial reaction solution, adding a nucleating agent dropwise when heated to 85° C., reacting for 1.5 hours after the addition is complete, and then adding praseodymium nitrate hydrate, and then adding a shelling agent dropwise, after the addition is complete, reacting for 2 hours, filtering out insoluble solids, and obtaining a phosphated acrylate composite emulsion with rare earth ions loaded on the surface;

[0047] (2) adding a 30% aqueous solution of 4-sulfonic acid calixarene to a reaction device, adding 3-fluoroaniline under nitrogen atmosphere, and mixing, controlling the temperature of the reaction system to 5°C, slowly adding a 50% aqueous solution of ammonium persulfate, reacting at room temperature for 12 hours, centrifuging after the reaction, washing the solid with deionized water until the pH of the deionized water is 7.5, and drying at 60°C for 48 hours to obtain polyfluoroaniline nanowires doped with sulfonic acid calixarene;

[0048] (3) The polyfluoroaniline nanowires doped with sulfonic acid calixarene and the phosphated acrylate composite emulsion modified with surface loading of rare earth ions are mixed, and stirred at a high speed of 5000 rpm for 10-20 minutes to obtain the heavy-duty anti-corrosion new material.

[0049] The mass ratio of ammonium persulfate, sodium bicarbonate and deionized water in the initial reaction solution is 0.1:0.5:50.

[0050] The nucleating agent includes components in the following mass ratio: methyl methacrylate: butyl acrylate: methacrylic acid: ammonium persulfate: deionized water = 6:12:0.4:1:0.05:20.

[0051] The shell-forming agent comprises components in the following mass ratio: methyl methacrylate: butyl acrylate: methacrylic acid: 2-methyl-2-acrylic acid-2-hydroxyethyl ester phosphate: ammonium persulfate: deionized water 10:5:0.4:3:0.6:0.05:20.

[0052] The mass ratio of the initial reaction liquid, the nucleating agent, the praseodymium nitrate hydrate and the shelling agent is 15:15:2:15.

[0053] In the step (2), the mass ratio of 4-sulfonic acid calixarene, 3-fluoroaniline and ammonium persulfate is 1:3:2.5.

[0054] The mass ratio of the polyfluoroaniline nanowires doped with sulfonic acid calixarene and the phosphated acrylate composite emulsion with rare earth ions loaded on the surface in step (3) is 1:5.

[0055] Example 3

[0056] A method for producing a new heavy-duty anticorrosion material

[0057] The method comprises the following steps:

[0058] (1) adding ammonium persulfate, sodium bicarbonate and deionized water to a reaction device to obtain an initial reaction solution, adding a nucleating agent dropwise when heated to 83° C., reacting for 1 h after the addition is complete, and then adding lanthanum nitrate hydrate, and then adding a shelling agent dropwise, after the addition is complete, reacting for 1.5 h, filtering out insoluble solids, and obtaining a phosphated acrylate composite emulsion with rare earth ions loaded on the surface;

[0059] (2) adding a 20% by mass aqueous solution of 4-sulfonic acid calixarene to a reaction device, adding 4-fluoroaniline under nitrogen atmosphere, and mixing, controlling the temperature of the reaction system to 2°C, slowly adding a 30% by mass aqueous solution of ammonium persulfate, reacting at room temperature for 10 hours, centrifuging after the reaction, washing the solid with deionized water until the pH of the deionized water is 7.5, and drying at 60°C for 30 hours to obtain polyfluoroaniline nanowires doped with sulfonic acid calixarene;

[0060] (3) The polyfluoroaniline nanowires doped with sulfonic acid calixarene and the phosphated acrylate composite emulsion modified with surface loading of rare earth ions were mixed, and the mixture was stirred at a high speed of 4000 rpm for 15 minutes to obtain the new heavy-duty anti-corrosion material.

[0061] The mass ratio of ammonium persulfate, sodium bicarbonate and deionized water in the initial reaction solution is 0.07:0.3:35.

[0062] The nucleating agent includes components in the following mass ratio: methyl methacrylate: butyl acrylate: methacrylic acid: ammonium persulfate: deionized water = 5:10:0.3:0.5:0.04:15.

[0063] The shell-forming agent comprises components in the following mass ratio: methyl methacrylate: butyl acrylate: methacrylic acid: 2-methyl-2-acrylic acid-2-hydroxyethyl ester phosphate: ammonium persulfate: deionized water 8:4:0.3:2.5:0.5:0.04:15.

[0064] The mass ratio of the initial reaction solution, the nucleating agent, the lanthanum nitrate hydrate and the shelling agent is 14:12:1.2:12.

[0065] In the step (2), the mass ratio of 4-sulfonic acid calixarene, 4-fluoroaniline and ammonium persulfate is 1:1.2:2.

[0066] The mass ratio of the polyfluoroaniline nanowires doped with sulfonic acid calixarene and the phosphated acrylate composite emulsion with rare earth ions loaded on the surface in step (3) is 4:0.5.

[0067] Comparative Example 1

[0068] The difference between this comparative example and Example 3 is that the phosphated acrylate composite emulsion is not doped with rare earth ions, that is, lanthanum nitrate hydrate is not added during the preparation, and the remaining components, component contents, and preparation process are the same as those in Example 3.

[0069] Comparative Example 2

[0070] The difference between this comparative example and Example 3 is that the polyfluoroaniline nanowires are not doped with sulfonic acid calixarene, that is, no 4-sulfonic acid calixarene aqueous solution is added during preparation, and the remaining components, component contents, and preparation process are the same as those in Example 3.

[0071] Results Analysis

[0072] The salt spray resistance performance of the heavy-duty anticorrosion materials prepared in various embodiments and comparative examples of the present invention was tested with reference to GB / T10125-2012. The results are shown in Figure 1 The salt spray test conditions are: temperature (35±2)℃, concentration of sodium chloride solution (50±5)g / L, 80cm 2 The average sedimentation rate of the horizontal area was (1.5±0.5) mL / h, and the pH value was 6.5-7.2.

[0073] Referring to GB / T1865-2009, the heavy-duty anti-corrosion materials prepared in the embodiments and comparative examples of the present invention were tested for their aging resistance using a MZ-B20 xenon arc lamp weathering aging test chamber. The air temperature in the test chamber was (38±3)°C. The results are shown in Table 1. Figure 2 .

[0074] The water resistance of the heavy anti-corrosion materials prepared in the embodiments and comparative examples of the present invention was tested with reference to GB / T1766-2008. Figure 3 .

[0075] Referring to GB1720-79, the adhesion test of the heavy anti-corrosion materials prepared in each embodiment of the present invention and the comparative example was carried out using a KS-M adhesion tester. The results are shown in Figure 4 The size of the aluminum ingot used for the test was 20 mm, and the test was repeated 3 times at different positions to obtain the average value.

[0076] According to the above test results Figure 1-4 It can be seen that the medium-anticorrosion material prepared by the present invention has excellent salt spray resistance, aging resistance and water resistance, and has strong adhesion. It is proved that the present invention dopes the polyfluoroaniline nanowires with sulfonic acid calixarene and introduces phosphate groups into the acrylate composite emulsion. The material has flexibility after film formation, and has high adhesion between the coating and the metal substrate. The migration of the fluorinated chain segments and the chelation of the phosphate groups with the metal surface significantly improve the salt spray performance, aging resistance and wear resistance of the heavy-duty anticorrosion material, and the adhesion on the metal surface is stronger.

[0077] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

[0078] The present invention and its implementation methods are described above, which is not restrictive. The drawings are only one of the implementation methods of the present invention, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it and design methods and embodiments similar to the technical solution without creativity without departing from the purpose of the invention, they should all fall within the protection scope of the present invention.

Claims

1. A method for producing a new heavy-duty anti-corrosion material. Features: The steps include: (1) adding ammonium persulfate, sodium bicarbonate and deionized water to a reaction device to obtain an initial reaction solution, adding a nucleating agent dropwise when the reaction solution is heated to 82-85° C., reacting for 0.5-1.5 hours after the addition is complete, and then adding rare earth nitrate hydrate, and then adding a shelling agent dropwise, reacting for 1-2 hours after the addition is complete, filtering out insoluble solids, and obtaining a phosphated acrylate composite emulsion with rare earth ions loaded on the surface; (2) adding a 10%-30% aqueous solution of 4-sulfonic acid calixarene to a reaction device, adding fluoroaniline monomer and mixing under nitrogen atmosphere, controlling the temperature of the reaction system to 0-5°C, slowly adding a 20%-50% aqueous solution of ammonium persulfate, reacting at room temperature for 5-12 hours, centrifuging after the reaction, washing the solid with deionized water until the pH of the deionized water is 7.5, and drying at 60°C for 24-48 hours to obtain polyfluoroaniline nanowires doped with sulfonic acid calixarene; (3) The polyfluoroaniline nanowires doped with sulfonic acid calixarene and the phosphated acrylate composite emulsion modified with surface-loaded rare earth ions are mixed, and stirred at high speed to obtain the heavy-duty anti-corrosion new material.

2. A method for producing a new heavy-duty anti-corrosion material according to claim 1, Features: The mass ratio of ammonium persulfate, sodium bicarbonate and deionized water in the initial reaction solution is 0.05-0.1:0.2-0.5:25-50.

3. A method for producing a new heavy-duty anti-corrosion material according to claim 2, Features: The nucleating agent comprises components in the following mass ratio: methyl methacrylate: butyl acrylate: methacrylic acid: ammonium persulfate: deionized water = 4-6: 8-12: 0.2-0.4: 0.4-1: 0.02-0.05: 12-20.

4. A method for producing a new heavy-duty anti-corrosion material according to claim 3, Features: The shell forming agent comprises the following components in the following mass ratio: methyl methacrylate: butyl acrylate: methacrylic acid: 2-methyl-2-acrylic acid-2-hydroxyethyl ester phosphate: ammonium persulfate: deionized water 7-10: 3-5: 0.2-0.4: 1.5-3: 0.4-0.6: 0.02-0.05: 12-20.

5. A method for producing a new heavy-duty anticorrosion material according to claim 4, Features: The mass ratio of the initial reaction liquid, the nucleating agent, the rare earth nitrate hydrate and the shelling agent is 12-15:10-15:0.5-2:10-15.

6. A method for producing a new heavy-duty anticorrosion material according to claim 5, Features: In the step (2), the mass ratio of 4-sulfonic acid calixarene, fluoroaniline monomer and ammonium persulfate is 1:0.5-3:1-2.

5.

7. A method for producing a new heavy-duty anticorrosion material according to claim 6, Features: In the step (3), the mass ratio of the polyfluoroaniline nanowires doped with sulfonic acid calixarene to the phosphated acrylate composite emulsion with rare earth ions loaded on the surface is 0.1-1:3-5.

8. A method for producing a new heavy-duty anti-corrosion material according to claim 7, Features: The fluoroaniline monomer is one of 2-fluoroaniline, 3-fluoroaniline or 4-fluoroaniline.

9. A method for producing a new heavy-duty anti-corrosion material according to claim 8, Features: The rare earth nitrate hydrate is one of cerium nitrate hydrate, lanthanum nitrate hydrate, praseodymium nitrate hydrate or neodymium nitrate hydrate.

10. A method for producing a new heavy-duty anti-corrosion material according to claim 9, Features: The high-speed stirring has a rotation speed of 3000-5000 rpm and a time of 10-20 min.