Conductive binder and preparation method thereof, negative pole piece and sodium ion battery
The conductive adhesive formed by a three-dimensional network structure by aqueous biomass materials and water-soluble organic acids, the volume expansion problem of tin-based negative electrode materials is solved, the electrochemical performance and energy density of sodium ion batteries are improved, the production cost is reduced, and the production cost is reduced. Good environmental performance.
Patent Information
- Application Number
- CN202410861063.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-11-01
AI Technical Summary
The tin-based anode material has huge volume expansion during the de-embedding process, resulting in rapid attenuation of sodium-ion battery capacity. Existing improvement strategies such as reducing the tin particle size or using elastic carbon material coatings have difficulties in preparation and high cost problems.
The conductive adhesive with a three-dimensional network structure is formed by esterification reaction of aqueous biomass materials and water-soluble organic acids, which enhances the adhesion between the tin-based anode material and the anode sheet, alleviates the problem of volume expansion, and reduces production costs.
Effectively improve the electrochemical performance of sodium ion batteries, improve energy density, reduce production costs, and have excellent environmental protection and ion diffusion properties.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of batteries, and in particular to a conductive adhesive and a preparation method thereof, a negative electrode sheet and a sodium ion battery. Background Art
[0002] Energy is the basis for human survival. Among them, electric energy, as an efficient energy carrier, has become a commonly used and indispensable resource in human daily life. Among various energy storage technologies, lithium-ion batteries are the representative. They have the characteristics of high operating voltage, high energy density, good safety, good cycle performance, wide operating temperature, no obvious self-discharge phenomenon and no memory effect. Therefore, lithium-ion batteries have become the preferred energy storage battery. However, the scarcity of lithium resources, the differences in the regional distribution of lithium resources and the high cost have greatly limited the application of lithium-ion batteries in large-scale energy storage.
[0003] Sodium-ion batteries, which have similar energy storage mechanisms to lithium-ion batteries, have attracted widespread attention from researchers. For sodium-ion batteries, the sodium element is evenly distributed in the earth's crust and the raw materials are cheap. However, studies have shown that graphite, the most widely used commercial lithium-ion battery anode material, has almost no sodium storage properties. Therefore, finding suitable sodium-ion battery anode materials is crucial to realizing the application of sodium-ion batteries in large-scale energy storage. In addition, there are relatively few non-carbon sodium-embedded anodes, mainly a few transition metal oxides, most of which have too high sodium embedding potentials to be of practical use. The alloying reaction mechanism usually occurs at lower potentials, so it is conducive to a significant increase in energy density.
[0004] In recent years, tin-based negative electrode materials have become a research hotspot due to their high theoretical capacity, abundant natural resources, high packing density, and stability in the air. However, there is a huge volume expansion during the sodium deintercalation process, which leads to rapid decay of the battery capacity. There are currently two mainstream improvement strategies. One is to reduce the tin particle size to the nanoscale. This solution has problems such as preparation difficulties, easy agglomeration of tin particles, and uneven particle size. The second is to coat / coat with elastic carbon materials, but due to the low melting point of tin (about 231.9°C), this solution is extremely difficult in terms of process. At the same time, the above two solutions will bring problems such as low initial efficiency, low compaction and high production costs.
[0005] At the same time, since the preparation of electrodes requires the addition of conductive agents, excessive electrode volume is occupied, seriously reducing the volume energy density of the electrode; therefore, how to overcome the above-mentioned technical problems and defects has become a key issue that needs to be solved. Summary of the invention
[0006] In view of the problem that tin-based negative electrode materials have huge volume expansion during the process of sodium insertion and deinsertion, which leads to rapid capacity decay of sodium ion batteries, the present invention provides a conductive binder and a preparation method thereof, a negative electrode plate and a sodium ion battery.
[0007] The technical solution adopted by the present invention to solve the above technical problems is as follows:
[0008] A first aspect of the present invention provides a conductive adhesive, comprising: an aqueous biomass material and a water-soluble organic acid, wherein the aqueous biomass material and the water-soluble organic acid are polymerized to form a three-dimensional network structure.
[0009] Optionally, the mass ratio of the aqueous biomass material to the water-soluble organic acid is 1-9:9-1.
[0010] Optionally, the water-based biomass material includes one or more of furfuryl alcohol (FA), coniferyl alcohol, coumarin, xylitol, sinapyl alcohol, guar gum, xanthan gum, carboxylated chitosan and derivatives thereof.
[0011] Optionally, the water-soluble organic acid includes one or more of polyacrylic acid, r-polyglutamic acid, alginic acid, and tannic acid.
[0012] A second aspect of the present invention provides a method for preparing a conductive adhesive, comprising the following steps:
[0013] The water-soluble organic acid and the water-based biomass material are dissolved in water and mixed to obtain a conductive adhesive.
[0014] Optionally, based on the weight of the conductive binder being 100%, the total weight of the water-based biomass material and the water-soluble organic acid accounts for 2%-20% of the conductive binder.
[0015] Optionally, the polymerization temperature of the water-based biomass material and the water-soluble organic acid is 65° C. to 90° C., and the polymerization time of the water-based biomass material and the water-soluble organic acid is 8-18 hours.
[0016] A third aspect of the present invention provides a negative electrode plate, comprising a negative electrode active material layer, wherein the negative electrode active material layer comprises a negative electrode active material and the conductive binder as described above, wherein the negative electrode active material comprises a tin-based active material.
[0017] Optionally, taking the weight of the negative electrode active material layer as 100%, the weight of the negative electrode active material accounts for 80%-95% of the negative electrode active material layer; the weight of the conductive binder accounts for 5%-20% of the negative electrode active material layer.
[0018] A fourth aspect of the present invention provides a sodium ion battery, comprising the negative electrode plate, the positive electrode plate, the electrolyte and the separator as described above, wherein the separator is located between the positive electrode plate and the negative electrode plate.
[0019] According to the conductive binder provided by the present invention, a binder with a three-dimensional network structure is formed by using an aqueous biomass material and a water-soluble organic acid through an esterification reaction. The binder is rich in oxygen functional groups and can form hydrogen bonds with electrode particles to improve the bonding force between the tin-based negative electrode material and the negative electrode sheet. At the same time, the volume expansion problem of the tin-based negative electrode material during the cycle can be effectively alleviated, the electrochemical performance of the sodium ion battery can be greatly improved, and the production cost and processing process can be reduced to improve the production efficiency; moreover, the aqueous biomass material is a low-cost aqueous biomass material, which will not pollute the environment while reducing the cost, and has excellent environmental protection performance; at the same time, the conductive binder of the present application has a carbon-carbon resonance system and an oxygen heteroatom structure, and therefore has good ion diffusion performance and electronic conduction characteristics, and can achieve the purpose of improving the energy density of the sodium ion battery by reducing the amount of the conductive agent, reducing the electrode porosity, improving compaction, and increasing the proportion of active substances. DETAILED DESCRIPTION
[0020] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention clearer, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0021] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods; the materials and reagents used are reagents and materials that can be obtained from commercial channels unless otherwise specified.
[0022] A first aspect of the present invention provides a conductive adhesive, comprising: an aqueous biomass material and a water-soluble organic acid, wherein the aqueous biomass material and the water-soluble organic acid are polymerized to form a three-dimensional network structure.
[0023] Specifically, the present invention uses water-based biomass materials and water-soluble organic acids to form a three-dimensional network structure binder with excellent electron / ion conductivity through esterification reaction, which has the following advantages:
[0024] Compared with the method of reducing the tin particle size to nanoscale or coating / encapsulating the tin particle material with an elastic carbon material, the present application uses an aqueous biomass material and a water-soluble organic acid to form a three-dimensional network structure through an esterification reaction. This can effectively alleviate the volume expansion problem of the tin-based negative electrode material during the cycle process, greatly improve the electrochemical performance of the sodium ion battery, and reduce the production cost and processing process, thereby improving production efficiency.
[0025] Secondly, compared with expensive PVDF (polyvinylidene fluoride) and the toxic solvent NMP (N-methylpyrrolidone) used in the use of PVDF, water-based biomass materials are low-cost water-based biomass materials. While reducing costs, they will not pollute the environment and have excellent environmental performance. At the same time, the adhesion of PVDF is van der Waals force, and the binder formed by the polymerization of water-based biomass materials and water-soluble organic acids is rich in oxygen functional groups, and has a better bonding effect by forming hydrogen bonds with electrode particles.
[0026] Thirdly, compared with single-structure aqueous binders [such as CMC (carboxymethyl cellulose), PAA (polyacrylic acid), SA (sodium alginate), etc.] which are easily ineffective during repeated sodium ion extraction and insertion, aqueous biomass materials and water-soluble organic acids form a three-dimensional structure through esterification reaction, which can provide strong mechanical adhesion and a huge volume expansion buffer zone for the electrode; it can improve the adhesion between tin-based negative electrode materials and negative electrode sheets, and at the same time can effectively alleviate the volume expansion problem of tin-based negative electrode materials during the cycle process.
[0027] Furthermore, in the prior art, in the preparation process of the electrode, it is often necessary to add a conductive agent and a binder, which cannot provide sodium storage capacity for the sodium ion battery, and will also occupy the limited volume in the electrode, especially the low compaction, high porosity conductive agent, which will seriously reduce the volume energy density of the electrode. The conductive binder of the present application uses water-based biomass materials and water-soluble organic acids, which are formed by esterification to have a three-dimensional structure, a carbon-carbon resonance system and an oxygen heteroatom structure, and therefore have good ion diffusion performance and electronic conduction characteristics. The purpose of increasing the energy density of the sodium ion battery can be achieved by reducing the amount of the conductive agent, reducing the electrode porosity, improving compaction, and increasing the proportion of active substances.
[0028] In one embodiment, the mass ratio of the aqueous biomass material to the water-soluble organic acid is 1-9:9-1.
[0029] In a preferred embodiment, the mass ratio of the aqueous biomass material to the water-soluble organic acid is 3-7:7-3; specifically, the mass ratio of the aqueous biomass material to the water-soluble organic acid is any ratio of 1:9, 2:8, 3:7, 4:6, 5:5, 6:4, 7:3, 8:2, 9:1 or a range value consisting of any two ratios.
[0030] In one embodiment, the water-based biomass material includes one or more of furfuryl alcohol (FA), coniferyl alcohol, coumarin, xylitol, sinapyl alcohol, guar gum, xanthan gum, carboxylated chitosan and derivatives thereof.
[0031] Specifically, furfuryl alcohol (FA), coniferyl alcohol, coumarin, xylitol, sinapyl alcohol, guar gum, xanthan gum, carboxylated chitosan and their derivatives are all low-cost water-based biomass materials, which can reduce costs without polluting the environment and have excellent environmental performance.
[0032] In one embodiment, the water-soluble organic acid includes one or more of polyacrylic acid, r-polyglutamic acid, alginic acid, and tannic acid.
[0033] Specifically, the present invention forms a conductive binder with a three-dimensional structure through an esterification reaction between an aqueous biomass material and a water-soluble organic acid. Compared with aqueous binders with a single structure (such as CMC, PAA, SA, etc.) that are easily invalidated during repeated insertion and extraction of sodium ions, the conductive binder of the present invention can provide strong mechanical adhesion and a huge volume expansion buffer zone for the electrode; it can improve the adhesion between the tin-based negative electrode material and the negative electrode sheet, and at the same time can effectively alleviate the volume expansion problem of the tin-based negative electrode material during the cycle process.
[0034] In one embodiment, the second aspect of the present invention provides a method for preparing a conductive adhesive, comprising the following steps:
[0035] The water-soluble organic acid and the water-based biomass material are dissolved in water and mixed to obtain a conductive adhesive.
[0036] In another embodiment, the preparation method of the conductive adhesive of the present invention comprises the following steps: dissolving one or more of furfuryl r-polyglutamic acid, alginic acid, and tannic acid and one or more of polyacrylic acid, r-polyglutamic acid, alginic acid, and tannic acid in water in a certain proportion, and mixing to obtain a conductive adhesive.
[0037] In a preferred embodiment, the method for preparing the conductive adhesive of the present invention comprises the following steps: dissolving furfuryl alcohol and polyacrylic acid in water in a certain proportion, and mixing to obtain the conductive adhesive.
[0038] In one embodiment, based on the weight of the conductive binder being 100%, the total weight of the water-based biomass material and the water-soluble organic acid accounts for 2%-20% of the conductive binder.
[0039] In a preferred embodiment, the total weight of the water-based biomass material and the polyacrylic acid accounts for 8%-12% of the conductive adhesive; specifically, the total weight of the water-based biomass material and the polyacrylic acid accounts for any point value among 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, or 20%, or a range value consisting of any two point values.
[0040] In one embodiment, the polymerization temperature of the water-based biomass material and the water-soluble organic acid is 65° C. to 90° C., and the polymerization time of the water-based biomass material and the water-soluble organic acid is 8-18 hours.
[0041] In a preferred embodiment, the polymerization temperature of the aqueous biomass material and the water-soluble organic acid is 75°C to 85°C; specifically, the polymerization temperature of the aqueous biomass material and the water-soluble organic acid is 65°C, 66°C, 67°C, 68°C, 69°C, 70°C, 71°C, 72°C, 73°C, 74°C, 75°C, 76°C, 77°C, 78°C, 79°C, 80°C, 81°C, 82°C, 83°C, 84°C, 85°C, 86°C, 87°C, 88°C, 89°C or 90°C, any one temperature value or a range value consisting of any two temperature values.
[0042] In a preferred embodiment, the polymerization time of the aqueous biomass material and the water-soluble organic acid is 10-14h; specifically, the polymerization time of the aqueous biomass material and the water-soluble organic acid is any time value among 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h, 16h, 17h or 18h, or a range value consisting of any two time values.
[0043] A third aspect of the present invention provides a negative electrode plate, comprising a negative electrode active material layer, wherein the negative electrode active material layer comprises a negative electrode active material and the conductive binder as described above, wherein the negative electrode active material comprises a tin-based active material.
[0044] Specifically, the tin-based active material includes metallic tin, tin / carbon composite materials, tin alloys, tin-based oxides, tin-based sulfides, tin-based phosphides, and the like.
[0045] Specifically, the negative electrode plate further includes a negative electrode current collector, the negative electrode current collector includes a metal, and the metal includes at least one of aluminum, copper, molybdenum, titanium, niobium, and iron.
[0046] The negative electrode current collector may also be a composite current collector, which may include a polymer material substrate and a metal layer formed on at least one surface of the polymer material substrate, and the material forming the metal layer includes at least one of aluminum, copper, molybdenum, titanium, niobium, and iron.
[0047] As an example, the material forming the polymer material substrate includes at least one of polyamide, polyterephthalate, polyimide, polyethylene, polypropylene, polystyrene, polyvinyl chloride, aramid, polyphenylene dicarboxylate, acrylonitrile-butadiene-styrene copolymer, polybutylene terephthalate, polyparaphenylene terephthalamide, polypropylene, polyoxymethylene, epoxy resin, phenolic resin, polytetrafluoroethylene, polyvinylidene fluoride, silicone rubber, polycarbonate, cellulose and its derivatives, starch and its derivatives, protein and its derivatives, polyvinyl alcohol and its crosslinked products, and polyethylene glycol and its crosslinked products.
[0048] Specifically, the preparation method of the negative electrode sheet is as follows: the negative electrode active material and the conductive binder are mixed in a certain proportion, and the negative electrode slurry is prepared after ball milling at 400 rpm for 3 hours. The negative electrode slurry is evenly coated on the negative electrode collector, and then air-dried at 150°C for 2 hours and vacuum-dried at 60°C for 12 hours. Subsequently, the negative electrode sheet of 59*79 mm is obtained after rolling and slitting.
[0049] In one embodiment, taking the weight of the negative electrode active material layer as 100%, the weight of the negative electrode active material accounts for 80%-95% of the negative electrode active material layer; the weight of the conductive binder accounts for 5%-20% of the negative electrode active material layer.
[0050] In a preferred embodiment, the weight of the negative electrode active material accounts for 85%-90% of the negative electrode active material layer; specifically, the weight of the negative electrode active material accounts for any point value among 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94% or 95%, or a range value consisting of any two point values.
[0051] In a preferred embodiment, the weight of the conductive binder accounts for 10%-15% of the negative electrode active material layer; specifically, the weight of the conductive binder accounts for any point value among 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19% or 20% of the negative electrode active material layer, or a range value consisting of any two point values.
[0052] A fourth aspect of the present invention provides a sodium ion battery, comprising the negative electrode plate, the positive electrode plate, the electrolyte and the separator as described above, wherein the separator is located between the positive electrode plate and the negative electrode plate.
[0053] Specifically, the positive electrode sheet includes a positive electrode active material layer, and the positive electrode active material layer includes a positive electrode active material, a positive electrode conductive agent and a positive electrode binder;
[0054] In some embodiments, the positive electrode active material is at least one of a sodium transition metal oxide, a sodium polyanion compound, and a sodium Prussian blue analogue;
[0055] Among them, sodium transition metal oxides NaCoO2, NaFeO2, NaNiO2, NaNiFeMnO2, NaCuFeMnO2, NaNi 0.5 Mn 0.5 O2; the sodium polyanion compound can be any one of Na3V2(PO4)3, NaFePO4, Na2Fe2(SO4)3, and Na2Fe2P2O7; the sodium Prussian blue analogue can be any one of NaFeFe(CN)6, Na2CoFe(CN)6, and Na2NiFe(CN)6. Preferably, the sodium-based positive electrode active material is a transition metal oxide of sodium. More preferably, the sodium-based positive electrode active material is selected from sodium nickel iron manganese oxide NaNiFeMnO2.
[0056] The positive electrode conductive agent includes one or more of a metal conductive agent, a carbon material, a metal oxide conductive agent, and a composite conductive agent. Specifically, the metal conductive agent can be a metal such as copper powder, nickel powder, silver powder, etc.; the carbon material can be a carbon material such as conductive graphite, conductive carbon black, conductive carbon fiber or graphene; the metal oxide conductive agent can be tin oxide, iron oxide, zinc oxide, etc.; the composite conductive agent can be a composite powder, composite fiber, etc. More specifically, the conductive carbon black can be one or more of acetylene black, 350G, Ketjen black, carbon fiber (VGCF), and carbon nanotubes (CNTs).
[0057] The positive electrode binder includes polyvinylidene fluoride, copolymers of vinylidene fluoride, polytetrafluoroethylene, copolymers of vinylidene fluoride-hexafluoropropylene, copolymers of tetrafluoroethylene-hexafluoropropylene, copolymers of tetrafluoroethylene-perfluoroalkyl vinyl ether, copolymers of ethylene-tetrafluoroethylene, copolymers of vinylidene fluoride-tetrafluoroethylene, copolymers of vinylidene fluoride-trifluoroethylene, copolymers of vinylidene fluoride-trichloroethylene, copolymers of vinylidene fluoride-fluoroethylene, copolymers of vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene, thermoplastic polyimide, thermoplastic resins such as polyethylene and polypropylene; acrylic resin; and one or more of styrene butadiene rubber.
[0058] In one embodiment, taking the weight of the positive electrode active material layer as 100%, the weight of the positive electrode active material accounts for 65%-95% of the positive electrode active material layer; the weight of the positive electrode conductor accounts for 5%-15% of the positive electrode active material layer; the weight of the positive electrode binder accounts for 5%-15% of the positive electrode active material layer.
[0059] In a preferred embodiment, the weight of the positive electrode active material accounts for 75%-85% of the positive electrode active material layer; specifically, the weight of the positive electrode active material accounts for any point value among 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94% or 95%, or a range value composed of any two point values.
[0060] In a preferred embodiment, the weight of the positive electrode conductive agent accounts for 15%-25% of the positive electrode active material layer; specifically, the weight of the positive electrode conductive agent accounts for any point value among 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14% or 15% of the positive electrode active material layer, or a range value consisting of any two point values.
[0061] In a preferred embodiment, the weight of the positive electrode binder accounts for 5%-15% of the positive electrode active material layer; specifically, the weight of the positive electrode binder accounts for any point value among 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14% or 15% of the positive electrode active material layer, or a range value consisting of any two point values.
[0062] Specifically, the preparation method of the positive electrode sheet is: the positive electrode active material, the positive electrode conductive agent and the positive electrode binder are mixed in a certain proportion, and the positive electrode slurry is prepared after ball milling at 400 rpm for 3 hours, and the positive electrode slurry is evenly coated on the positive electrode collector, and vacuum dried at 100°C overnight, and then rolled and cut to obtain a 57*77 mm positive electrode sheet.
[0063] Specifically, it also includes a diaphragm, which can be various diaphragm materials suitable for lithium-ion batteries or sodium-ion batteries in the art, for example, it can be a combination of one or more including but not limited to single-layer PP (polypropylene), single-layer PE (polyethylene), double-layer PP / PE, double-layer PP / PP, three-layer PP / PE / PP, polyvinylidene fluoride, aramid, polyethylene terephthalate, polytetrafluoroethylene, polyacrylonitrile, polyimide, polyamide, polyester and natural fiber.
[0064] In the sodium ion battery provided by the present invention, the electrolyte comprises an electrolyte salt and a solvent.
[0065] In some embodiments, the electrolyte salt can be selected from at least one of sodium hexafluorophosphate, sodium tetrafluoroborate, sodium perchlorate, sodium hexafluoroarsenate, sodium bis(fluorosulfonyl)imide, sodium bis(trifluoromethanesulfonyl)imide, sodium trifluoromethanesulfonate, sodium difluorophosphate, sodium difluorooxalatoborate, sodium dioxalatoborate, sodium difluorodioxalatophosphate, and sodium tetrafluorooxalatophosphate.
[0066] In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane sulfone, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.
[0067] In some embodiments, the electrolyte may further optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and may also include additives that can improve certain properties of the sodium ion battery, such as additives that improve the overcharge performance of the sodium ion battery, additives that improve the high temperature or low temperature performance of the sodium ion battery, etc.
[0068] Production of sodium-ion batteries: stack the positive electrode sheet, separator and negative electrode sheet in order, so that the separator is between the positive electrode sheet and the negative electrode sheet to play an isolating role, and then use the lamination process to prepare the bare battery cell. The bare battery cell is placed in an aluminum-plastic film for packaging, and the preparation of the sodium-ion battery is completed after vacuum packaging, static, formation, shaping and other processes.
[0069] The sodium ion battery disclosed in the embodiments of the present application can be used in electrical devices that use sodium ion batteries as power sources or various energy storage systems that use sodium ion batteries as energy storage elements. Electrical devices can be, but are not limited to, mobile phones, tablets, laptops, electric toys, electric tools, battery cars, electric cars, ships, spacecraft, and the like. The vehicle can be a fuel vehicle, a gas vehicle, or a new energy vehicle, and the new energy vehicle can be a pure electric vehicle, a hybrid vehicle, or an extended-range vehicle, etc.; the spacecraft includes airplanes, rockets, space shuttles, and spacecraft, etc.; electric toys include fixed or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys, etc.; electric tools include metal cutting electric tools, grinding electric tools, assembly electric tools, and railway electric tools, such as electric drills, electric grinders, electric wrenches, electric screwdrivers, electric hammers, impact drills, concrete vibrators, and electric planers, etc.
[0070] The present invention is further described below by way of examples.
[0071] Embodiment 1:
[0072] (1) Preparation of conductive adhesive:
[0073] Disperse FA and PAA in a weight ratio of 6:4 in water, wherein the total weight of FA-PAA accounts for 10% of the conductive adhesive, and stir at 80° C. for 12 hours;
[0074] (2) Preparation of negative electrode sheet:
[0075] μ-Sn:FA-PAA were mixed in a weight ratio of 8:2, and after ball milling at 400 rpm for 3 hours, the slurry was evenly coated on the copper foil, and then dried at 150°C for 2 hours and vacuum dried at 60°C for 12 hours. Subsequently, the electrode pieces of 59*79 mm were obtained by roller pressing and slitting.
[0076] (3) Preparation of positive electrode sheet:
[0077] The electrode was prepared by mixing Na3V2(PO4)3 / C, SP and PVDF in a weight ratio of 8:1:1. After ball milling at 400 rpm for 3 h, the slurry was evenly coated on aluminum foil and dried under vacuum at 100 °C overnight.
[0078] (4) Production of sodium ion batteries:
[0079] The positive electrode sheet, separator and negative electrode sheet are stacked in order, so that the separator is in the middle of the positive and negative electrodes to play an isolating role, and then the bare battery cell is prepared by the stacking process. The bare battery cell is placed in an aluminum-plastic film for packaging, and the preparation of the sodium ion battery is completed after vacuum packaging, static, formation, shaping and other processes.
[0080] Embodiment 2:
[0081] Example 2 includes most of the steps in Example 1, except that:
[0082] Preparation of the conductive adhesive: FA and PAA in a weight ratio of 1:1 are dispersed in water, the total weight of FA-PAA accounts for 10% of the conductive adhesive, and stirred at 80° C. for 12 hours.
[0083] Embodiment 3:
[0084] Example 3 includes most of the steps in Example 1, except that:
[0085] Preparation of the conductive adhesive: FA and PAA in a weight ratio of 1:9 are dispersed in water, the total weight of FA-PAA accounts for 10% of the conductive adhesive, and stirred at 80° C. for 12 hours.
[0086] Embodiment 4:
[0087] Example 4 includes most of the steps in Example 1, except that:
[0088] Preparation of the conductive adhesive: FA and PAA with a weight ratio of 9:1 are dispersed in water, the total weight of FA-PAA accounts for 10% of the conductive adhesive, and stirred at 80° C. for 12 hours.
[0089] Embodiment 5:
[0090] Example 5 includes most of the steps in Example 1, except that:
[0091] Preparation of the conductive adhesive: FA and PAA in a weight ratio of 6:4 are dispersed in water, the total weight of FA-PAA accounts for 2% of the conductive adhesive, and stirred at 80° C. for 12 hours.
[0092] Embodiment 6:
[0093] Example 6 includes most of the steps in Example 1, except that:
[0094] Preparation of the conductive adhesive: FA and PAA are dispersed in water at a weight ratio of 1:1, with the total weight of FA-PAA accounting for 20% of the conductive adhesive, and stirred at 80° C. for 12 hours.
[0095] Embodiment 7:
[0096] Example 7 includes most of the steps in Example 1, except that:
[0097] Preparation of the conductive adhesive: Disperse coniferyl alcohol and r-polyglutamic acid in a weight ratio of 6:4 in water, wherein the total weight of coniferyl alcohol and r-polyglutamic acid accounts for 10% of the conductive adhesive, and stir at 80° C. for 12 hours.
[0098] Embodiment 8:
[0099] Example 8 includes most of the steps in Example 1, except that:
[0100] Preparation of the conductive adhesive: disperse sinapyl alcohol and alginic acid in a weight ratio of 6:4 in water, wherein the total weight of sinapyl alcohol and alginic acid accounts for 10% of the conductive adhesive, and stir at 80° C. for 12 hours.
[0101] Embodiment 9:
[0102] Example 9 includes most of the steps in Example 1, except that:
[0103] Preparation of the conductive adhesive: guar gum and tannic acid in a weight ratio of 6:4 are dispersed in water, the total weight of the guar gum and tannic acid accounting for 10% of the conductive adhesive, and stirred at 80° C. for 12 hours.
[0104] Embodiment 10:
[0105] Example 10 includes most of the steps in Example 1, except that:
[0106] Preparation of the conductive adhesive: disperse carboxylated chitosan and tannic acid in a weight ratio of 6:4 in water, wherein the total weight of the carboxylated chitosan and tannic acid accounts for 10% of the conductive adhesive, and stir at 80° C. for 12 hours.
[0107] Comparative Example 1:
[0108] Comparative Example 1 includes most of the steps in Example 1, except that:
[0109] Preparation of tin-based negative electrode: μ-Sn: FA-PAA: SP were mixed in a weight ratio of 8:1.5:0.5, and after ball milling at 400 rpm for 3 hours, the slurry was evenly coated on the copper foil, and then dried at 150°C for 2 hours and vacuum dried at 60°C for 12 hours. Subsequently, it was rolled and cut to obtain 59*79 mm pole pieces.
[0110] Comparative Example 2:
[0111] Comparative Example 2 includes most of the steps in Example 1, except that:
[0112] Preparation of tin-based negative electrode: μ-Sn: FA-PAA: SP were mixed in a weight ratio of 8:1.75:0.25. After ball milling at 400 rpm for 3 hours, the slurry was evenly coated on the copper foil, and then dried at 150°C for 2 hours and vacuum dried at 60°C for 12 hours. Subsequently, the electrode pieces of 59*79 mm were obtained by rolling and slitting.
[0113] Comparative Example 3:
[0114] Comparative Example 3 includes most of the steps in Example 1, except that:
[0115] Preparation of tin-based negative electrode: μ-Sn: FA: SP were mixed in a weight ratio of 8:1.5:0.5, and after ball milling at 400 rpm for 3 hours, the slurry was evenly coated on the copper foil, and then dried by air at 150°C for 2 hours and vacuum dried at 60°C for 12 hours. Subsequently, it was rolled and cut to obtain 59*79 mm pole pieces.
[0116] Comparative Example 4:
[0117] Comparative Example 4 includes most of the steps in Example 1, except that:
[0118] Preparation of tin-based negative electrode: μ-Sn: PVDF: SP were mixed in a weight ratio of 8:1.5:0.5, and after ball milling at 400 rpm for 3 hours, the slurry was evenly coated on the copper foil, and then dried by air at 150°C for 2 hours and vacuum dried at 60°C for 12 hours. Subsequently, it was rolled and cut to obtain 59*79 mm pole pieces.
[0119] Comparative Example 5:
[0120] Comparative Example 5 includes most of the steps in Example 1, except that:
[0121] Preparation of tin-based negative electrode: μ-Sn:PAA:SP was mixed in a weight ratio of 8:1.5:0.5, and after ball milling at 400 rpm for 3 hours, the slurry was evenly coated on copper foil, and then dried at 150°C for 2 hours and vacuum dried at 60°C for 12 hours. Subsequently, it was rolled and cut to obtain a 59*79 mm electrode sheet;
[0122] Performance Testing
[0123] The sodium ion batteries prepared in the above examples 1-10 and comparative examples 1-5 were subjected to the following performance tests:
[0124] Capacity retention test
[0125] Test method: At room temperature 25±3℃, charge and discharge each sodium ion battery at a rate of 0.5C, with a voltage range of 3.0V to 4.5V. Cycle for 300 cycles under the above conditions and then stop. Calculate the capacity retention rate of each battery at the 300th week.
[0126] The test results are shown in Table 1:
[0127] Table 1 Cycle life results of sodium ion batteries of Examples 1-10 and Comparative Examples 1-5
[0128] Battery First effect (%) Capacity retention after 300 weeks (%) Example 1 72.9 61.0 Example 2 71.0 62.2 Example 3 73.2 63.7 Example 4 73.0 62.5 Example 5 72.5 60.5 Example 6 70.8 60.3 Example 7 68.6 60.9 Example 8 66.5 59.8 Example 9 70.2 62.0 Example 10 46.8 48.9 Comparative Example 1 78.9 66.3 Comparative Example 2 75.5 65.8 Comparative Example 3 76.8 63.1 Comparative Example 4 46.8 48.9 Comparative Example 5 50.3 43.6
[0129] As can be seen from Table 1, Examples 1-10 and Comparative Examples 1-2 all exhibit high initial efficiency and good cycle life. At the same time, Examples 1-10 still exhibit good electrochemical performance without adding a conductive agent. This is due to the fact that the water-based biomass material and the water-soluble organic acid binder form a three-dimensional network structure through an esterification reaction, which can effectively alleviate the volume expansion of the tin-based negative electrode material and greatly improve the electrochemical performance of the sodium ion battery, and it has excellent electron / ion conductivity.
[0130] As can be seen from Table 1, compared with Comparative Examples 3-5, when only adding water-based biomass materials and one of the water-soluble organic acid binders or PVDF, Examples 1-10 have the problem of low first efficiency and rapid capacity decay in cycle performance; this is because the water-based biomass materials and the water-soluble organic acid binders are esterified to form a three-dimensional structure, which can provide strong mechanical adhesion and a huge volume expansion buffer zone for the electrode; it can improve the adhesion between the tin-based negative electrode material and the negative electrode sheet, and at the same time can effectively alleviate the volume expansion problem of the tin-based negative electrode material during the cycle. The single-structure water-based binder (such as CMC, PAA, SA, etc.) is easy to fail during the repeated insertion and extraction of sodium ions, and cannot effectively alleviate the volume expansion problem of the tin-based negative electrode material during the cycle.
[0131] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A conductive adhesive, characterized in that: include: Aqueous biomass material and a water-soluble organic acid, wherein the aqueous biomass material and the water-soluble organic acid are polymerized to form a three-dimensional network structure.
2. The conductive adhesive according to claim 1, characterized in that: The mass ratio of the water-based biomass material to the water-soluble organic acid is 1-9:9-1.
3. The conductive adhesive according to claim 1, characterized in that: The water-based biomass material includes one or more of furfuryl alcohol (FA), coniferyl alcohol, coumarin, xylitol, sinapyl alcohol, guar gum, xanthan gum, carboxylated chitosan and derivatives thereof.
4. The conductive adhesive according to claim 1, characterized in that: The water-soluble organic acid includes one or more of polyacrylic acid, r-polyglutamic acid, alginic acid and tannic acid.
5. The method for preparing a conductive adhesive according to claim 1, characterized in that: The following steps are involved: The water-soluble organic acid and the water-based biomass material are dissolved in water and mixed to obtain a conductive adhesive.
6. The method for preparing a conductive adhesive according to claim 5, characterized in that: Taking the weight of the conductive binder as 100%, the total weight of the water-based biomass material and the water-soluble organic acid accounts for 2%-20% of the conductive binder.
7. The method for preparing a conductive adhesive according to claim 5, characterized in that: The polymerization temperature of the water-based biomass material and the water-soluble organic acid is 65° C. to 90° C., and the polymerization time of the water-based biomass material and the water-soluble organic acid is 8 to 18 hours.
8. A negative electrode plate, characterized in that: The invention comprises a negative electrode active material layer, wherein the negative electrode active material layer comprises a negative electrode active material and the conductive adhesive according to any one of claims 1 to 3, wherein the negative electrode active material comprises a tin-based active material.
9. The negative electrode plate according to claim 8, characterized in that: Taking the weight of the negative electrode active material layer as 100%, the weight of the negative electrode active material accounts for 80%-95% of the negative electrode active material layer; the weight of the conductive binder accounts for 5%-20% of the negative electrode active material layer.
10. A sodium ion battery, characterized in that: It comprises the negative electrode sheet, the positive electrode sheet, the electrolyte and the separator as described in any one of claims 8 to 9, wherein the separator is located between the positive electrode sheet and the negative electrode sheet.
Citation Information
Cited By
Modified material for lithium-rich manganese-based positive electrode of lithium ion battery
CN119108550A