Binder, electrode and battery
By using polyion liquid, hydroxyl functional groups and carboxy functional groups binders in lithium-ion batteries, a dynamic crosslinking network is formed, which solves the problem of insufficient ionic conductivity of the battery in the prior art, and achieves better cycling performance and conductance Rate.
Patent Information
- Application Number
- CN202411282329.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing lithium-ion battery binders cannot improve ionic conductivity while ensuring battery cycling performance.
Adhesives with polyionic liquids, hydroxyl functional groups and carboxy functional groups are used to form adhesives with dynamic cross-linking networks through specific mass ratios and structural designs, enhancing electric field response and bonding force, and improving the ion transport performance of the electrodes. .
It significantly improves the ionic conductivity and cycling performance of the battery, and improves the stability and capacity retention of the battery.
Smart Images

Figure CN118879244A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a binder, in particular to a binder, an electrode and a battery, belonging to the secondary field. Background Art
[0002] With the continuous breakthroughs in technology, the energy density of lithium-ion batteries has increased, the cost has decreased, and the life has been extended. These advantages have promoted the widespread application of lithium-ion batteries in consumer electronics, electric vehicles, energy storage systems and other fields.
[0003] In lithium-ion batteries, binders are an important component of electrode materials and have an important impact on the performance of lithium-ion batteries. Patent application document CN117757425A discloses a lithium-ion battery negative electrode binder and its preparation method and application, which introduces small molecule tannic acid (TA) and selects small molecule phthalic acid (Phthalic acid) with two carboxyl groups to form a new structure of lithium-ion battery negative electrode binder through reaction with carboxymethyl cellulose (CMC). Patent application document CN117050679A discloses a silicon negative electrode binder with a chemical / ionic / hydrogen bond triple cross-linked network and a preparation method. The β-CD, CA, ALG, active material Si and copper current collector react to form a hydrogen bond cross-linking network through the hydroxyl groups of β-CD and the hydroxyl groups on the Si surface, an in-situ esterification reaction occurs between β-CD, CA, ALG and the Si surface to form a chemical cross-linking network, and the carboxyl groups generated by the hydrolysis of the cross-linked ester groups react with the carboxyl groups of CA and CuO formed by partial oxidation on the copper current collector to form a carboxylate copper complex and diffuse to the electrode to form an ion cross-linking network, thereby forming a triple cross-linking binder with a three-dimensional network structure.
[0004] However, existing binders cannot improve ionic conductivity while ensuring battery cycle performance. Summary of the invention
[0005] The present invention provides a binder, which can improve the ion conductivity while ensuring the cycle performance of the battery after being used in the battery.
[0006] The present invention also provides an electrode, which comprises the above binder, and thus can improve the cycle performance and ion conductivity of the battery after being used in the battery.
[0007] The present invention also provides a battery, which comprises the electrode and thus has excellent cycle performance and ion conductivity.
[0008] In one aspect, the present invention provides a binder, comprising a polyionic liquid, a hydroxyl functional group, and a carboxyl functional group, wherein the mass ratio of the polyionic liquid, the hydroxyl functional group, and the carboxyl functional group is 1:0.01-0.5:0.01-0.5; the polyionic liquid is a polymer having a repeating unit represented by formula (1), Formula (1), wherein R is a C1-C10 alkoxy group; R' - Selected from PF6 - TFSI - 、FSI - 、BF4 - DFOB - One or more of .
[0009] The binder as described above includes a second polymer, and the second polymer includes the hydroxyl functional group and the carboxyl functional group.
[0010] The binder as described above, the binder comprises a first side chain and a second side chain, the first side chain comprises the hydroxyl functional group, and the second side chain comprises the carboxyl functional group; The first side chain and the second side chain are grafted onto the polyionic liquid.
[0011] The binder as described above, wherein the binder comprises a third side chain, and the third side chain comprises the hydroxyl functional group and the carboxyl functional group; The third side chain is grafted onto the polyionic liquid.
[0012] The binder as described above, wherein the hydroxyl functional group is derived from a hydroxyl monomer, and the carboxyl functional group is derived from a carboxyl monomer; The carboxyl monomer includes at least one of acrylic acid, maleic anhydride, crotonic acid, linoleic acid, polylactic dicarboxylic acid, tannic acid, citric acid, and stearic acid; The hydroxy monomer includes at least one of polyvinyl alcohol, dopamine, methacryloyl dopamine, trimethylol methacrylamide, phenyl glycidyl ether acrylate, 2-hydroxy-3-phenoxypropyl acrylate, polyethylene glycol monomethacrylate, and hydroxyethyl methacrylate.
[0013] In the binder as described above, the mass average molecular weight of the polyionic liquid is 10w-400w.
[0014] The binder as described above, wherein the mass average molecular weight of the binder is 20w-500w; And / or, the PDI of the binder is 0.5-5.
[0015] In the binder as described above, in formula (1), R is selected from at least one of methoxy, ethoxy, propoxy, butoxy, pentyloxy, hexyloxy, heptyloxy, octyloxy, nonyloxy, decyloxy, isopropoxy, tert-butoxy and sec-butoxy.
[0016] In another aspect, the present invention provides an electrode, comprising the binder as described above.
[0017] In another aspect, the present invention provides a battery, comprising the electrode as described above.
[0018] The binder provided by the present invention includes a polyionic liquid with a specific structural formula, a hydroxyl functional group and a carboxyl functional group, wherein the mass ratio between the polyionic liquid and the hydroxyl functional group and the carboxyl functional group is within a specific range, so that the binder has a unique and reversible response to the electric field, and can improve the bonding force of the binder to the main material during battery charging and discharging, while contributing to high cohesive energy, improving the ion transport performance of the electrode, and improving the ion conductivity while allowing the battery to have excellent cycle performance. DETAILED DESCRIPTION
[0019] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0020] In one aspect, the present invention provides a binder, comprising a polyionic liquid, a hydroxyl functional group, and a carboxyl functional group, wherein the mass ratio of the polyionic liquid, the hydroxyl functional group, and the carboxyl functional group is 1:0.01-0.5:0.01-0.5; the polyionic liquid is a polymer having a repeating unit represented by formula (1), Formula (1), wherein R is a C1-C10 alkoxy group; R' - Selected from One or more of .
[0021] In formula (1), R is at least one selected from the group consisting of methoxy, ethoxy, propoxy, butoxy, pentyloxy, hexyloxy, heptyloxy, octyloxy, nonyloxy, decyloxy, isopropoxy, tert-butoxy and sec-butoxy.
[0022] It can be understood that the mass ratio of the polyionic liquid, hydroxyl functional group and carboxyl functional group in the binder can be controlled by controlling the mass relationship of various raw materials in the binder preparation process.
[0023] The binder can be tested using methods commonly used in the art to determine the component types in the binder and the mass ratio of the polyionic liquid, hydroxyl functional groups, and carboxyl functional groups.
[0024] For example, infrared spectroscopy is used to determine the composition, and nuclear magnetic resonance spectroscopy is used to determine the mass ratio.
[0025] When the binder provided by the present invention is used in a battery, it can significantly improve the ionic conductivity and the cycle performance of the battery. The inventor analyzed this and believed that the reason may be that the binder with polyionic liquid as the main component can give the binder a special electric field responsiveness. The excessively high proportion of hydroxyl and carboxyl groups will increase the rigidity of the material and destroy the function of dynamic crosslinking. The excessively low proportion of hydroxyl and carboxyl groups will make it difficult to achieve the effect of dynamic crosslinking: on the one hand, there are a large number of hydrogen bonds and electrostatic interactions in the binder provided by the present invention, which can improve the strength of the material, and the binder contains a polyionic liquid with a specific structure that can respond to the electric field when the battery is working, improve the bonding force of the binder, and improve the cycle stability of the battery. On the other hand, the binder provided by the present invention has a dynamically crosslinked hydrogen bond structure and has self-healing properties. When the local conductive / ion-conducting network generated during electrode charging and discharging is destroyed, the conductive / ion-conducting network can be repaired by simply leaving the electrode to stand, thereby improving the cycle performance. On the other hand, the binder has an alkoxy group that can be complexed with lithium ions, providing a migration channel for the transmission of lithium ions in the electrode, thereby improving the ionic conductivity.
[0026] Furthermore, in a specific embodiment of the present invention, the binder includes a second polymer, and the second polymer includes a hydroxyl functional group and a carboxyl functional group.
[0027] Specifically, the binder includes a polyionic liquid and a second polymer, and the second polymer includes a hydroxyl functional group and a carboxyl functional group.
[0028] Whether the binder includes the second polymer can be detected by infrared spectroscopy.
[0029] The polyionic liquid in the binder and the second polymer form a cross-linked network through hydrogen bonds and electrostatic interactions, which increases the strength of the binder and further improves the cycle performance of the battery.
[0030] Furthermore, the binder of the present invention comprises a first side chain and a second side chain, the first side chain comprises a hydroxyl functional group, and the second side chain comprises a carboxyl functional group; the first side chain and the second side chain are grafted onto the polyionic liquid.
[0031] Specifically, the first side chain and the second side chain exist in the polyionic liquid in a branched form.
[0032] The hydroxyl functional group in the first side chain may be located at the end or other positions of the side chain, and the carboxyl functional group in the second side chain may be located at the end or other positions of the side chain.
[0033] Whether the binder includes the first side chain and the second side chain may be detected by infrared spectroscopy.
[0034] The present invention does not limit the number of hydroxyl functional groups in the first side chain, which may be one or more hydroxyl functional groups; the present invention does not limit the number of carboxyl functional groups in the second side chain, which may be one or more carboxyl functional groups.
[0035] The present invention also does not limit the number of the first side chains and the second side chains in the polyionic liquid, and the number of the first side chains and the second side chains may be the same or different.
[0036] When the binder includes the first side chain and the second side chain, hydrogen bonds can be provided to improve the bonding force of the binder, thereby improving the cycle performance. Moreover, the dynamic hydrogen bond structure formed between the first side chain and the second side chain can repair the conductive network by standing still when the conductive / ion-conductive network of the battery is damaged, thereby further improving the cycle performance.
[0037] Furthermore, in another specific embodiment of the present invention, the binder includes a third side chain, and the third side chain includes a hydroxyl functional group and a carboxyl functional group; and the third side chain is grafted onto the polyionic liquid.
[0038] In detail, the third side chain includes both a hydroxyl functional group and a carboxyl functional group.
[0039] It is also possible to detect whether the binder includes a third side chain by infrared spectroscopy.
[0040] The present invention does not limit the number of hydroxyl functional groups and carboxyl functional groups in the third side chain, and the number of hydroxyl functional groups and carboxyl functional groups may be the same or different.
[0041] The present invention does not limit the number of third side chains, and a suitable number of third side chains can be selected according to actual needs.
[0042] When the binder includes a polyionic liquid grafted with a third side chain, the battery has better cycle performance and ionic conductivity. The reason may be that the binder is endowed with electric field response characteristics, adapting to the volume change of the negative electrode during charging and discharging, and preventing the negative electrode material from pulverizing or peeling off from the current collector.
[0043] By controlling different polymerization conditions, the binder can independently include the second polymer or the polyionic liquid having the first side chain, the second side chain, or the polyionic liquid having the third side chain. It can also include the second polymer, the polyionic liquid having the first side chain, the second side chain, and the polyionic liquid having the third side chain at the same time.
[0044] It can be understood that when the hydroxyl functional group in the binder is derived from a hydroxyl monomer, the carboxyl functional group is derived from a carboxyl monomer. Preferably, in the present invention, the carboxyl monomer includes at least one of acrylic acid, maleic anhydride, crotonic acid, linoleic acid, polylactic dicarboxylic acid, tannic acid, citric acid, and stearic acid; the hydroxyl monomer includes at least one of polyvinyl alcohol, dopamine, methacryloyl dopamine, trimethylol methacrylamide, phenyl glycidyl ether acrylic acid, 2-hydroxy-3-phenoxypropyl acrylate, polyethylene glycol monomethacrylate, and hydroxyethyl methacrylate.
[0045] Furthermore, the mass average molecular weight of the polyionic liquid is 10w-400w. Specifically, the mass average molecular weight of the polyionic liquid includes but is not limited to 10w, 100w, 200w, 300w, 400w or a range between any two thereof.
[0046] Further, in a specific embodiment of the present invention, the mass average molecular weight of the binder is 20w-500w; and / or the PDI of the binder is 0.5-5.
[0047] The mass average molecular weight of the binder can be tested by common detection methods in the art, such as gel permeation chromatography, mass spectrometry, spectral analysis, and the like.
[0048] Specifically, the mass average molecular weight of the binder includes, but is not limited to, 20w, 100w, 200w, 300w, 400w, 500w, or a range between any two of them.
[0049] The mass average molecular weight in different ranges affects the strength, fluidity and durability of the binder. When the mass average molecular weight of the binder is within the above range, the binder can be applied to various application scenarios while ensuring that the binder can function, thereby improving the ionic conductivity and the cycle performance of the battery.
[0050] The PDI of the binder refers to the polymer distribution index, which refers to the ratio of the weight average molecular weight to the mass average molecular weight. Specifically, the PDI of the binder includes but is not limited to 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5 or a range between any two thereof.
[0051] When the PDI of the binder is within the above range, the binder has a narrow molecular weight distribution and good uniformity, and the binder has higher bonding strength and better mechanical properties.
[0052] Furthermore, in a specific embodiment of the present invention, the mass ratio of the polyionic liquid, the hydroxyl functional group, and the carboxyl functional group is 1: 0.08-0.33: 0.02-0.27.
[0053] When the mass ratio of the polyionic liquid, the hydroxyl functional group, and the carboxyl functional group is within the above range, the performance of the binder can be further improved, and the ionic conductivity and the cycle performance of the battery can be improved.
[0054] The present invention does not limit the preparation method of the binder. In a specific embodiment, the preparation method of the binder includes the following steps: 1) exchanging ions between a quaternary ammonium polymer including a repeating unit as shown in Formula 2 and a lithium salt monomer to obtain a polyionic liquid; 2) mixing the polyionic liquid with a mixed raw material including a carboxyl monomer and a hydroxyl monomer to obtain a binder; (Formula 2), wherein R is a C1-C10 alkoxy group.
[0055] In detail, in step 1), a quaternary ammonium polymer having a structure as shown in Formula 2 is ion exchanged with a lithium salt monomer, so that lithium ions are exchanged with quaternary ammonium cations having a structure as shown in Formula 2 in the quaternary ammonium polymer, and after removing unreacted lithium salt, residual solvent and other impurities, a polyionic liquid is obtained.
[0056] The lithium salt monomer in the present invention includes but is not limited to at least one of LiPF6, LiTFSI, LiFSI, LiBF4, and LiDFOB.
[0057] Among them, the ion exchange rate can be accelerated by stirring, heating or ultrasound, thereby reducing the time cost in the preparation process.
[0058] It can be understood that in order to achieve charge balance and ensure that all cations in the polymer are effectively replaced during the ion exchange process, the molar ratio of the quaternized polymer to the lithium salt monomer can be controlled to be 1:1.
[0059] The present invention does not limit the preparation method of the quaternary ammonium polymer, and the quaternary ammonium polymer can be prepared by a common preparation method in the art.
[0060] In one specific embodiment, an alkoxy compound containing a halogen substituent is subjected to a quaternization reaction with polyvinyl imidazole, and the halogen group in the alkoxy compound can react with the nitrogen atom in the imidazole group to form a quaternary ammonium salt, and the halogen group serves as a leaving group and is replaced by the imidazole nitrogen atom in the reaction.
[0061] The alkoxy compounds include, but are not limited to, compounds containing at least one of methoxy, ethoxy, propoxy, butoxy, pentyloxy, hexyloxy, heptyloxy, octyloxy, nonyloxy, decyloxy, isopropoxy, tert-butoxy, and sec-butoxy.
[0062] The conversion rate can be improved by controlling the mass ratio of the alkoxy compound and polyvinyl imidazole. In a specific embodiment, the mass ratio of the alkoxy compound to polyvinyl imidazole is (0.2-0.8): 1. As a preferred example, the alkoxy compound can be selected from ethoxyethoxyethyl acrylate.
[0063] In step 2), the polyionic liquid is mixed with a mixed raw material including a carboxyl monomer and a hydroxyl monomer to obtain a binder. The mixed raw material including the carboxyl monomer and the hydroxyl monomer undergoes a polymerization reaction to obtain a second polymer, and the second polymer is mixed with the polyionic liquid to obtain the binder.
[0064] After the mixing reaction in step 2), some carboxyl monomers and hydroxyl monomers that did not participate in the polymerization reaction may remain. To avoid the adverse effects of carboxyl monomers and hydroxyl monomers on the effect of the binder, the binder can be separated by phase conversion method, dialysis method, etc. In a specific embodiment, a dialysis bag with a molecular weight cutoff specification of 20K is selected for dialysis treatment to obtain the binder.
[0065] In order to control the polymerization effect and make the hydroxyl functional group and the carboxyl functional group in the binder within the mass relationship required by the present invention, as known to those skilled in the art, the addition amount can be adjusted based on the selected specific carboxyl monomer, hydroxyl monomer and polyionic liquid, so that the mass ratio of polyionic liquid, hydroxyl functional group and carboxyl functional group in the binder obtained by the final reaction is 1:0.01-0.5:0.01-0.5.
[0066] The preparation method provided by the present invention has a simple and controllable process flow, and the prepared binder has excellent ionic conductivity and can improve the cycle performance of the battery when used in the battery.
[0067] Furthermore, in a specific embodiment provided by the present invention, the mixed raw materials also include an initiator.
[0068] Specifically, an initiator, a hydroxyl monomer, a carboxyl monomer and a polyionic liquid are mixed, and under the action of the initiator, the hydroxyl functional group in the hydroxyl monomer and the carboxyl functional group in the carboxyl monomer are grafted onto the polyionic liquid in various forms.
[0069] In the present invention, the specific type and addition amount of the initiator are commonly used in the art. For example, the ratio of the addition amount of the initiator to the total weight of the hydroxyl monomer, the carboxyl monomer and the polyionic liquid can be 1-5:1000.
[0070] In a specific embodiment, the initiator includes at least one of potassium persulfate, potassium hydrogen persulfate, ammonium persulfate, ammonium hydrogen persulfate, azobisisobutyronitrile, and benzoyl peroxide, the carboxyl monomer is grafted onto the polyionic liquid in the form of a first side chain, and the hydroxyl monomer is grafted onto the polyionic liquid in the form of a second side chain.
[0071] In another specific embodiment, the initiator includes at least one of potassium persulfate, potassium hydrogen persulfate, ammonium persulfate, ammonium hydrogen persulfate, azobisisobutyronitrile, and benzoyl peroxide, and after the carboxyl monomer and the hydroxyl monomer are copolymerized, the polymer including the carboxyl monomer and the hydroxyl monomer is grafted onto the polyionic liquid in the form of a third side chain. In another aspect, the present invention provides an electrode, including the binder as described above or the binder prepared by the preparation method as described above.
[0072] Since the electrode includes the binder, the electrode has excellent cycle performance and ion conductivity when used in a battery.
[0073] In a specific embodiment, the electrode of the present invention is a negative electrode. Specifically, the negative electrode sheet includes a negative electrode current collector and a negative electrode active layer formed of a negative electrode active material, a binder, and a conductive agent and disposed on the surface of the negative electrode current collector.
[0074] When preparing the negative electrode, the negative electrode active material, the conductive agent and the binder can be dispersed in an appropriate amount of deionized water, and the mixture is stirred and mixed to form a uniform negative electrode slurry; the negative electrode slurry is evenly coated on the negative electrode current collector, and the negative electrode sheet is obtained after drying, rolling and slitting. In a specific embodiment, the negative electrode active layer includes 70-99wt% of the negative electrode active material, 0.5-15wt% of the conductive agent, and 0.5-15wt% of the binder in terms of mass percentage, and further includes 80-98wt% of the negative electrode active material, 1-10wt% of the conductive agent, and 1-10wt% of the binder.
[0075] Among them, the material of the negative electrode current collector layer can be at least one of copper foil, nickel foam, and copper foam; the conductive agent can be selected from at least one of natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, and graphene.
[0076] In a specific embodiment, the electrode further comprises a silicon-based negative electrode material.
[0077] The silicon-based negative electrode material is used as the negative electrode active material and together with the binder and the conductive agent constitutes the negative electrode active layer.
[0078] The silicon-based negative electrode material in the present invention includes but is not limited to at least one of silicon, silicon oxide, and silicon-carbon negative electrode.
[0079] When the silicon-based negative electrode material and the above-mentioned binder and conductive agent together constitute the negative electrode active layer, the binder provided by the present invention has high cohesion and adhesion, which can effectively limit the volume expansion of the negative electrode and improve the integrity of each component in the electrode material, including the connection between the active material, the conductive agent and the binder, and the connection between the current collector and the binder, thereby improving the electrode capacity and the battery energy density.
[0080] In another aspect, the present invention provides a battery, comprising the electrode as described above.
[0081] It is conceivable that the battery of the present invention includes, in addition to the negative electrode sheet, a positive electrode sheet, an electrolyte and a separator.
[0082] The present invention does not strictly limit the positive electrode active material in the positive electrode sheet, and can be a positive electrode active material commonly used in current batteries, such as at least one composite oxide of lithium and metals of cobalt, manganese, nickel and combinations thereof. Specifically, it can be at least one of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, nickel-cobalt-manganese ternary material, nickel-cobalt-aluminum ternary material, lithium iron phosphate (LFP), lithium nickel manganese oxide, lithium-rich manganese-based material, etc.
[0083] The present invention does not strictly limit the selection of the electrolyte, and may include one or more of the solvents commonly used in the current lithium-ion battery electrolyte, and the electrolyte lithium salts commonly used in the current lithium-ion electrolyte, for example: the solvent may be ethylene carbonate, propylene carbonate, butylene carbonate, fluoroethylene carbonate (FEC), dimethyl carbonate (DMC), diethyl carbonate (DEC), difluoroethylene carbonate (DFEC), dipropyl carbonate, ethyl methyl carbonate (EMC), ethyl acetate, ethyl propionate, propyl acetate, propyl propionate, cyclopentane, γ-butyrolactone, etc.; the lithium salt may be, for example, one or more of lithium hexafluorophosphate (LiPF6), lithium bis(fluorosulfonyl)imide (LiFSI), and lithium bis(trifluoromethylsulfonyl)imide (LiTFSI).
[0084] The present invention does not strictly limit the material selection of the diaphragm, which can be a diaphragm material commonly used in lithium-ion batteries, such as a polypropylene diaphragm (PP), a polyethylene diaphragm (PE), a polypropylene / polyethylene double-layer composite film (PP / PE), a polyimide electrospinning diaphragm (PI), a polypropylene / polyethylene / polypropylene three-layer composite film (PP / PE / PP), a cellulose non-woven fabric diaphragm, or a diaphragm with a ceramic coating.
[0085] When preparing lithium-ion batteries, the positive electrode sheet, separator and negative electrode sheet are wound or stacked to obtain a bare cell, and the bare cell is packaged in a pre-stamped aluminum-plastic film bag. After the packaged battery is dried at 85°C, the electrolyte is injected into the dry battery, and the battery is placed, formed and sealed for the second time to complete the preparation of the lithium-ion battery.
[0086] Since the battery includes the electrode, the battery provided by the present invention has excellent cycle performance and ion conductivity.
[0087] Hereinafter, the adhesive provided by the present invention is described in detail through specific embodiments.
[0088] Example 1 The preparation method of the binder provided in this embodiment comprises the following steps: 1. Vinyl imidazole is polymerized by free radical polymerization to obtain polyvinyl imidazole (mass average molecular weight: 30w), ethoxyethoxyethyl acrylate and polyvinyl imidazole are subjected to quaternization reaction at a mass ratio of 0.3:1 to obtain a quaternized polymer, and then LiTFSI and the quaternized polymer are ion exchanged at a molar ratio of 1:1 to obtain a polyionic liquid.
[0089] 2. Maleic anhydride and methacryloyl dopamine are free radical copolymerized in a mass ratio of 1:1 to obtain poly(maleic anhydride-co-methacryloyl dopamine), polyionic liquid and poly(maleic anhydride-co-methacryloyl dopamine) are blended in a ratio of 1:0.5 to obtain a primary product, and the primary product is dialyzed using a dialysis bag with a molecular weight cutoff specification of 20K to finally obtain a binder.
[0090] The adhesive provided in this embodiment was tested. The adhesive included a polyionic liquid and a second polymer. The mass ratio of the polyionic liquid, hydroxyl functional group, and carboxyl functional group in the adhesive was 1:0.08:0.02. The mass average molecular weight of the adhesive was 50w, and the PDI was 1.5.
[0091] Example 2 The preparation method of the binder provided in this embodiment comprises the following steps: 1. Vinyl imidazole is polymerized by free radical polymerization to obtain polyvinyl imidazole (mass average molecular weight is 300w), ethoxyethoxyethyl acrylate and polyvinyl imidazole are quaternized at a mass ratio of 0.6:1 to obtain a quaternized polymer, and LiTFSI and the quaternized polymer are ion exchanged at a molar ratio of 1:1 to obtain a polyionic liquid.
[0092] 2. Maleic anhydride and methacryloyl dopamine are free radical copolymerized in a mass ratio of 2:1 to obtain poly(maleic anhydride-co-methacryloyl dopamine), polyionic liquid and poly(maleic anhydride-co-methacryloyl dopamine) are blended in a ratio of 1:0.3 to obtain a primary product, and the primary product is dialyzed using a dialysis bag with a molecular weight cutoff specification of 20K to finally obtain a binder.
[0093] The adhesive provided in this embodiment was tested. The adhesive included a polyionic liquid and a second polymer. The mass ratio of the polyionic liquid, hydroxyl functional group, and carboxyl functional group in the adhesive was 1:0.33:0.27. The mass average molecular weight of the adhesive was 400w, and the PDI was 2.
[0094] Example 3 The preparation method of the binder provided in this embodiment comprises the following steps: 1. Vinyl imidazole is polymerized by free radical polymerization to obtain polyvinyl imidazole (mass average molecular weight is 45w), ethoxyethoxyethyl acrylate and polyvinyl imidazole are subjected to quaternization reaction at a mass ratio of 0.6:1 to obtain a quaternized polymer, and then LiTFSI and the quaternized polymer are ion exchanged at a molar ratio of 1:1 to obtain a polyionic liquid.
[0095] 2. The maleic anhydride, methacryloyl dopamine and ionic liquid are reacted in sequence according to a mass ratio of 2:1:10. Maleic anhydride and initiator potassium persulfate are first added to carry out the first step reaction, and then methacryloyl dopamine and initiator potassium persulfate are added to carry out the second step reaction. Finally, polyionic liquid and initiator potassium persulfate are added to carry out the last step reaction to obtain a primary product. The primary product is dialyzed with a dialysis bag with a molecular weight cutoff specification of 20K to finally obtain a binder.
[0096] The adhesive provided in this embodiment was tested. The adhesive included a polyionic liquid grafted with a first side chain and a second side chain. The mass ratio of the polyionic liquid, hydroxyl functional group, and carboxyl functional group in the adhesive was 1:0.08:0.02. The mass average molecular weight of the adhesive was 50w, and the PDI was 1.5.
[0097] Example 4 The preparation method of the binder provided in this embodiment comprises the following steps: 1. Vinyl imidazole is polymerized by free radical polymerization to obtain polyvinyl imidazole (mass average molecular weight is 45w), ethoxyethoxyethyl acrylate and polyvinyl imidazole are subjected to quaternization reaction at a mass ratio of 0.6:1 to obtain a quaternized polymer, and then LiTFSI and the quaternized polymer are ion exchanged at a molar ratio of 1:1 to obtain a polyionic liquid.
[0098] 2. Maleic anhydride and methacryloyl dopamine are mixed in a ratio of 2:1, and an initiator potassium persulfate is added to carry out the first step reaction. Then, polyionic liquid is added and mixed in a mass ratio of maleic anhydride, methacryloyl dopamine and polyionic liquid of 2:1:10, and an initiator potassium persulfate is added to carry out the second step reaction to obtain a primary product. The primary product is dialyzed using a dialysis bag with a molecular weight cutoff specification of 20K to finally obtain a binder.
[0099] The adhesive provided in this embodiment was tested. The adhesive included a polyionic liquid grafted with a third side chain. The mass ratio of the polyionic liquid, hydroxyl functional group, and carboxyl functional group in the adhesive was 1:0.08:0.02. The mass average molecular weight of the adhesive was 50w, and the PDI was 1.5.
[0100] Example 5 The preparation method of the binder provided in this embodiment is basically the same as that in embodiment 1, except that: In step 2), the mass ratio of maleic anhydride, methacryloyl dopamine and polyionic liquid is 2:1:15.
[0101] The adhesive provided in this embodiment was tested. The adhesive included a polyionic liquid and a second polymer. The mass ratio of the polyionic liquid, hydroxyl functional group, and carboxyl functional group in the adhesive was 1:0.01:0.01. The mass average molecular weight of the adhesive was 50w, and the PDI was 1.5.
[0102] Example 6 The preparation method of the binder provided in this embodiment is basically the same as that in embodiment 1, except that the reaction conditions of step 1 are adjusted so that the mass average molecular weight of the obtained polyionic liquid is 8w.
[0103] The adhesive provided in this embodiment was tested. The adhesive included a polyionic liquid and a second polymer. The mass ratio of the polyionic liquid, hydroxyl functional group, and carboxyl functional group in the adhesive was 1:0.08:0.02. The mass average molecular weight of the adhesive was 10w, and the PDI was 1.5.
[0104] Example 7 The preparation method of the binder provided in this embodiment is basically the same as that in embodiment 1, except that: The initial product in step 2 is used directly as a binder without dialysis.
[0105] The adhesive provided in this embodiment was tested. The adhesive included a polyionic liquid and a second polymer. The mass ratio of the polyionic liquid, hydroxyl functional group, and carboxyl functional group in the adhesive was 1:0.08:0.02. The mass average molecular weight of the adhesive was 50w, and the PDI was 15.
[0106] Comparative Example 1 The preparation method of the binder provided in this comparative example comprises the following steps: 1. Poly(maleic anhydride-co-methacryl dopamine) was obtained by free radical copolymerization of maleic anhydride and methacryl dopamine in a mass ratio of 2:1, with a mass average molecular weight of 50w; 2. The polyionic liquid in Example 1 and poly(maleic anhydride-co-methacryl dopamine) are blended in a ratio of 8:2 to obtain a primary product; 3. The initial product is dialyzed using a dialysis bag with a molecular weight cutoff specification of 20K to finally obtain the binder.
[0107] The binder provided in this comparative example was tested, and the mass ratio of the polyionic liquid, the hydroxyl functional group, and the carboxyl functional group in the binder was 1:1:1.
[0108] Comparative Example 2 The adhesive provided in this comparative example is PAA adhesive (brand number LA132).
[0109] Comparative Example 3 The adhesive provided in this comparative example is 1788 type PVA adhesive.
[0110] Test Case 1. Ionic conductivity test The ionic conductivity test of the binders provided in all the embodiments and comparative examples comprises the following steps: The binder was cast on a stainless steel electrode (stainless steel disc diameter is φ=1.4 cm) by solution casting and dried at 85°C for 12 h, and then vacuum dried at 60°C for 24 h. The thickness of the binder after drying was tested. The stainless steel electrode cast with the binder was assembled into a blocking electrode with a stainless steel counter electrode of equal area, and the electrolyte (1M LiPF6+EC / DEC (1:1wt%)) was added dropwise to assemble a button cell. After standing for 24 h, an EIS test was performed. The binder ion conductivity was calculated according to Formula I: Formula I, where L is the thickness of the adhesive, R is the bulk impedance, and S is the area of the stainless steel.
[0111] The specific test results are shown in Table 1.
[0112] 2. Cycle performance test After the binders in all the embodiments and comparative examples are made into negative electrode sheets, they are assembled with positive electrode sheets, electrolytes and separators according to the following method to obtain lithium-ion batteries. The method includes: 1) The binder in the embodiment and the comparative example was blended with the silicon negative electrode active material and the conductive agent super P in a mass ratio of 1:97:1 and 2:97:1, respectively, to obtain a blended powder, and the powder was blended with deionized water in a ratio of 1:20 to obtain a slurry, and the slurry was coated on a copper foil with a coating thickness of 300 μm. After drying at 80° C., it was cut into negative electrode sheets of a fixed size.
[0113] 2) Mix the NCM positive electrode active material with conductive carbon black and PVDF in a weight ratio of 96%:2%:2% to obtain a positive electrode slurry by dispersion. Apply the slurry on the aluminum foil current collector and set the positive electrode surface density to 4.12 g / cm 3 Rolling is performed to prepare a positive electrode sheet; 3) Assemble the positive electrode sheet, negative electrode sheet and separator into a lithium-ion battery and inject non-aqueous electrolyte. The electrolyte is 1M LiPF6+EC / DEC (1:1 wt%).
[0114] The capacity retention rate of each battery was tested. The specific test method was as follows: at 25°C, the battery was charged to 4.50V at a constant current of 1C, then charged to 4.50V at a constant voltage of 0.05C, and then discharged to 3.0V at a discharge rate of 1C. This charge and discharge cycle was repeated 200 times, and the discharge capacity at the first cycle and the discharge capacity at the 200th cycle were measured. The capacity retention rate Q after 200 cycles was calculated according to the following formula: Capacity retention rate Q = Q 200 / Q1*100%Specific test results are shown in Table 1.
[0115] 3. Peel strength test The binders in the embodiments and comparative examples were used to prepare negative electrode sheets according to the method in the cycle performance test.
[0116] The peel strength of the negative electrode sheet was tested using an electronic tensile testing machine in accordance with the national standard GB / T 2792-2014 “Test method for peel strength of adhesive tape”. The test results are shown in Table 1.
[0117] Table 1
[0118] It can be seen from Table 1 that the electrode sheet prepared by using the adhesive provided by the present invention can improve the peel strength to a certain extent, and the ion conductivity and capacity retention rate are very excellent.
[0119] Among them, by comparing the test results of Examples 1, 6 and 7, it can be seen that when the mass average molecular weight and PDI of the binder are within the preferred range of the present invention, it is very beneficial to further improve the ionic conductivity and capacity retention rate of the electrode.
[0120] By comparing the results of Example 1 and Comparative Example 1, it can be seen that when the mass ratio of the polyionic liquid, the hydroxyl functional group, and the carboxyl functional group in the binder is not within the scope of the present invention, the ionic conductivity and capacity retention rate thereof will be significantly reduced.
[0121] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A binder, characterized in that: The binder comprises a polyionic liquid, a hydroxyl functional group, and a carboxyl functional group. The mass ratio of the polyionic liquid, hydroxyl functional group and carboxyl functional group is 1:0.01-0.5:0.01-0.5; The polyionic liquid is a polymer having a repeating unit represented by formula (1), Formula (1), wherein R is a C1-C10 alkoxy group; R' - Selected from One or more of .
2. The adhesive according to claim 1, characterized in that The binder includes a second polymer, and the second polymer includes the hydroxyl functional group and the carboxyl functional group.
3. The adhesive according to claim 1, characterized in that The binder includes a first side chain and a second side chain, the first side chain includes the hydroxyl functional group, and the second side chain includes the carboxyl functional group; The first side chain and the second side chain are grafted onto the polyionic liquid.
4. The adhesive according to claim 1, characterized in that The binder includes a third side chain, and the third side chain includes the hydroxyl functional group and the carboxyl functional group; The third side chain is grafted onto the polyionic liquid.
5. The adhesive according to any one of claims 2 to 4, characterized in that: The hydroxyl functional group is derived from a hydroxyl monomer, and the carboxyl functional group is derived from a carboxyl monomer; The carboxyl monomer includes at least one of acrylic acid, maleic anhydride, crotonic acid, linoleic acid, polylactic dicarboxylic acid, tannic acid, citric acid, and stearic acid; The hydroxy monomer includes at least one of polyvinyl alcohol, dopamine, methacryloyl dopamine, trimethylol methacrylamide, phenyl glycidyl ether acrylate, 2-hydroxy-3-phenoxypropyl acrylate, polyethylene glycol monomethacrylate, and hydroxyethyl methacrylate.
6. The adhesive according to claim 1, characterized in that The mass average molecular weight of the polyionic liquid is 10w-400w.
7. The adhesive according to any one of claims 1 to 4, characterized in that The mass average molecular weight of the binder is 20w-500w; And / or, the PDI of the binder is 0.5-5.
8. The adhesive according to claim 1, characterized in that In formula (1), R is at least one selected from the group consisting of methoxy, ethoxy, propoxy, butoxy, pentyloxy, hexyloxy, heptyloxy, octyloxy, nonyloxy, decyloxy, isopropoxy, tert-butoxy and sec-butoxy.
9. An electrode, characterized in that: The invention comprises the adhesive according to any one of claims 1 to 8.
10. A battery, characterized in that: Comprising the electrode according to claim 9.
Citation Information
Patent Citations
Polyionic liquid adhesive and preparation method thereof
CN110699020A
Polyionic liquid conductive adhesive and preparation method thereof
CN117229734A
Binder, positive electrode plate and battery
US20230327121A1
Cited By
Solid-state battery pole piece and preparation method thereof
CN120895596A
Solid-state battery electrode sheet and method of making same
CN120895596B
Polymer composite binder for lithium secondary battery electrode mixture and lithium secondary battery including same