Method for improving microstructure of petroleum coke

Through multi-stage ultrasonic extraction technology, the microstructure of petroleum coke is improved, and the problem of low gasification activity of petroleum coke in the existing technology is solved, and efficient and clean utilization of petroleum coke is achieved, which simplifies operation and reduces energy consumption.

CN118879358APending Publication Date: 2024-11-01SHANDONG PETROCHEMICAL INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411166630.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The methods of improving the petroleum coke structure in the prior art to improve its gasification activity have problems of high cost and high energy consumption, especially the cost of adding catalysts is high and difficult to recover, the energy consumption of microwave activation is high, and the lack of mild operating conditions, clean and environmentally friendly. method.

Method used

After grinding and drying the petroleum coke, multi-stage ultrasonic extraction is performed using extractive agents such as cyclohexane, carbon disulfide, acetone and methanol to gradually improve the microstructure of petroleum coke and improve its gasification activity.

Benefits of technology

The gasification activity of petroleum coke is enhanced, and its utilization efficiency is improved. The method is simple and efficient, and the solvent can be reused, making the operation easy to achieve efficient and clean utilization of petroleum coke.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879358A_ABST
    Figure CN118879358A_ABST
Patent Text Reader

Abstract

The invention provides a method for improving the microstructure of petroleum coke, and belongs to the technical field of fracturing fluid. Petroleum coke is ground, sieved and dried; the method comprises the following steps: adding cyclohexane into a petroleum coke powder sample to serve as an extracting agent, then carrying out first-stage ultrasonic extraction until an extracting solution is nearly colorless to obtain first-stage raffinate petroleum coke, adding carbon disulfide to serve as an extracting agent to carry out second-stage ultrasonic extraction to obtain second-stage raffinate petroleum coke, adding acetone to serve as an extracting agent to carry out third-stage ultrasonic extraction to obtain second-stage raffinate petroleum coke; methanol is added to serve as an extraction agent for fourth-stage ultrasonic extraction, fourth-stage raffinate petroleum coke is obtained, and the raffinate petroleum coke is petroleum coke with the microstructure improved. The method for improving the microstructure of the petroleum coke is mild in operation condition, clean and environmentally friendly, the gasification activity of the petroleum coke is enhanced, efficient and clean utilization of the petroleum coke is achieved, the method is simple and efficient, the solvent can be recycled, and operation is convenient.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fracturing fluid, and in particular to a method for improving the microstructure of petroleum coke. Background Art

[0002] Petroleum coke is a byproduct of the delayed coking process in oil refineries. With the increase of crude oil heaviness and deep processing, the output of petroleum coke is increasing. At present, petroleum coke is generally used only in the electrolytic aluminum industry and as fuel, with low utilization efficiency and easy to pollute the environment. Using petroleum coke as a gasification raw material to produce synthesis gas is the best way to utilize petroleum coke. However, due to its dense structure and high carbon content, petroleum coke has low gasification activity and cannot be widely used as a gasification raw material. Therefore, improving the structure of petroleum coke and improving its gasification activity are the key to efficient and clean utilization of petroleum coke. In current research, there are two main methods to modify the structure of petroleum coke and improve its gasification activity. One is to add catalysts and the other is to use microwave activation. However, both methods have some problems. The cost of adding catalysts is too high and difficult to recover, while the energy consumption of microwave activation is relatively high. Therefore, it is crucial to explore a method for modifying the microstructure of petroleum coke with mild operating conditions, clean and environmentally friendly, to enhance the gasification activity of petroleum coke and to efficiently and reasonably utilize resources. Summary of the invention

[0003] The purpose of the present invention is to provide a method for improving the microstructure of petroleum coke under mild operating conditions and in a clean and environmentally friendly manner, so as to enhance the gasification activity of petroleum coke and realize its efficient and clean utilization.

[0004] The technical solution of the present invention is achieved in this way: The present invention provides a method for improving the microstructure of petroleum coke, comprising the following steps: (1) Grinding, sieving and drying petroleum coke; (2) Cyclohexane is added to the petroleum coke powder sample as an extractant, and then a first-stage ultrasonic extraction is performed. The extract is then transferred to a buffer tank by vacuum filtration. Fresh extractant is added to the extracted petroleum coke to perform a second extraction. The extraction operation is repeated until the extract is nearly colorless to obtain a first-stage raffinate petroleum coke. (3) adding carbon disulfide as an extractant to the first-stage raffinate petroleum coke in step (2) to perform a second-stage ultrasonic extraction to obtain a second-stage raffinate petroleum coke; (4) adding acetone as an extractant to the secondary raffinate petroleum coke in step (3) to perform a third-stage ultrasonic extraction to obtain a third-stage raffinate petroleum coke; (5) Methanol is added as an extractant to the third-stage raffinate petroleum coke in step (4) to perform a fourth-stage ultrasonic extraction to obtain a fourth-stage raffinate petroleum coke, wherein the raffinate petroleum coke is a petroleum coke with an improved microstructure.

[0005] As a further improvement of the present invention, the mesh size of the sieve in step (1) is 150-200 meshes, the drying temperature is 95-105° C., and the drying time is 36-56 hours.

[0006] As a further improvement of the present invention, in step (2), the power of the first-stage ultrasonic extraction is 1000-2000 W, the temperature is 35-45° C., and the time is 0.5-1.5 h.

[0007] As a further improvement of the present invention, the solid-to-liquid ratio of the petroleum coke powder sample and the extractant in step (2) is 1:5-10 g / mL.

[0008] As a further improvement of the present invention, the solid-to-liquid ratio of the primary raffinate petroleum coke to the extractant in step (3) is 1:5-10 g / mL.

[0009] As a further improvement of the present invention, in step (3), the power of the second-stage ultrasonic extraction is 1000-2000 W, the temperature is 35-45° C., and the time is 0.5-1.5 h.

[0010] As a further improvement of the present invention, the solid-to-liquid ratio of the secondary raffinate petroleum coke and acetone in step (4) is 1:5-10 g / mL.

[0011] As a further improvement of the present invention, the power of the third stage ultrasonic extraction in step (4) is 1000-2000W, the temperature is 35-45°C, and the time is 0.5-1.5h.

[0012] As a further improvement of the present invention, the solid-to-liquid ratio of the tertiary raffinate petroleum coke and methanol in step (5) is 1:5-10 g / mL.

[0013] As a further improvement of the present invention, the power of the fourth stage ultrasonic extraction in step (5) is 1000-2000W, the temperature is 35-45°C, and the time is 0.5-1.5h.

[0014] The present invention has the following beneficial effects: the present invention provides a method for improving the microstructure of petroleum coke with mild operating conditions, clean and environmentally friendly, thereby enhancing the gasification activity of petroleum coke and realizing its efficient and clean utilization. The method is simple and efficient, the solvent can be reused, and the operation is convenient. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0016] Figure 1 The pore size distribution of petroleum coke under different extractants in Example 1, Series 1: P1; Series 2: P2; Series 3: P3; Series 4: P4; Series 5: petroleum coke. DETAILED DESCRIPTION

[0017] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0018] Example 1 This embodiment provides a method for improving the microstructure of petroleum coke, comprising the following steps: (1) Grind the petroleum coke, sieve it with a 200-mesh sieve, and then put the sieved petroleum coke powder into a drying oven and adjust the temperature to 100 o C, drying time 48 hours to ensure that the petroleum coke powder is fully dried; (2) Add 50 mL of cyclohexane as an extractant to 10 g of petroleum coke powder sample, and then perform 1000 W ultrasonic extraction for 0.5 h at a temperature of 35 °C. The extract is then transferred to a buffer tank by vacuum filtration. Fresh extractant is added to the extracted petroleum coke for a second extraction. The extraction operation is repeated until the extract is nearly colorless to obtain a first-grade raffinate petroleum coke, which is recorded as P1. (3) Add 50 mL of carbon disulfide as an extractant to 10 g of the first-stage raffinate petroleum coke in step (2) and perform ultrasonic extraction at 1000 W for 0.5 h at a temperature of 35 ° C to obtain a second-stage raffinate petroleum coke, recorded as P2; (4) Add 50 mL of acetone as an extractant to 10 g of the secondary raffinate petroleum coke in step (3) and perform ultrasonic extraction at 1000 W for 0.5 h at a temperature of 35 ° C to obtain a tertiary raffinate petroleum coke, which is recorded as P3; (5) Add 50 mL of methanol as an extractant to 10 g of the third-grade raffinate petroleum coke in step (4) and perform ultrasonic extraction at 1000 W for 0.5 h at a temperature of 35 ° C to obtain a fourth-grade raffinate petroleum coke, recorded as P4; (6) A physical adsorption instrument was used to measure the adsorption-desorption isotherms of petroleum coke and residual petroleum coke by CO2 adsorption. Density functional theory (DFT) was used to obtain the specific surface area, pore volume and pore size distribution of the micropores of petroleum coke.

[0019] Example 2 This embodiment provides a method for improving the microstructure of petroleum coke, comprising the following steps: (1) Grind the petroleum coke, sieve it with a 200-mesh sieve, and then put the sieved petroleum coke powder into a drying oven and adjust the temperature to 100 o C, drying time 48 hours to ensure that the petroleum coke powder is fully dried; (2) Add 100 mL of cyclohexane as an extractant to 10 g of petroleum coke powder sample, and then perform 2000 W ultrasonic extraction for 1.5 h at a temperature of 45 °C. The extract is then transferred to a buffer tank by vacuum filtration. Fresh extractant is added to the extracted petroleum coke for a second extraction. The extraction operation is repeated until the extract is nearly colorless to obtain a first-grade raffinate petroleum coke, recorded as P1. (3) Add 100 mL of carbon disulfide as an extractant to 10 g of the first-stage raffinate petroleum coke in step (2) and perform ultrasonic extraction at 2000 W for 1.5 h at a temperature of 45 ° C to obtain a second-stage raffinate petroleum coke, recorded as P2; (4) Add 100 mL of acetone as an extractant to 10 g of the secondary raffinate petroleum coke in step (3) and perform ultrasonic extraction at 2000 W for 1.5 h at a temperature of 45 ° C to obtain a tertiary raffinate petroleum coke, which is recorded as P3; (5) Add 100 mL of methanol as an extractant to 10 g of the third-grade raffinate petroleum coke in step (4) and perform ultrasonic extraction at 2000 W for 1.5 h at a temperature of 45 ° C to obtain a fourth-grade raffinate petroleum coke, which is recorded as P4; (6) A physical adsorption instrument was used to measure the adsorption-desorption isotherms of petroleum coke and residual petroleum coke by CO2 adsorption. Density functional theory (DFT) was used to obtain the specific surface area, pore volume and pore size distribution of the micropores of petroleum coke.

[0020] Example 3 This embodiment provides a method for improving the microstructure of petroleum coke, comprising the following steps: (1) Grind the petroleum coke, sieve it with a 200-mesh sieve, and then put the sieved petroleum coke powder into a drying oven and adjust the temperature to 100 o C, drying time 48 hours to ensure that the petroleum coke powder is fully dried; (2) Add 70 mL of cyclohexane as an extractant to 10 g of petroleum coke powder sample, and then perform 1500 W ultrasonic extraction for 1 h at a temperature of 40 °C. The extract is then transferred to a buffer tank by vacuum filtration. Fresh extractant is added to the extracted petroleum coke for a second extraction. The extraction operation is repeated until the extract is nearly colorless to obtain a first-grade raffinate petroleum coke, which is recorded as P1. (3) Add 70 mL of carbon disulfide as an extractant to 10 g of the first-stage raffinate petroleum coke in step (2) and perform ultrasonic extraction at 1500 W for 1 h at a temperature of 40° C. to obtain a second-stage raffinate petroleum coke, denoted as P2; (4) Add 70 mL of acetone as an extractant to 10 g of the secondary raffinate petroleum coke in step (3) and perform ultrasonic extraction at 1500 W for 1 h at a temperature of 40° C. to obtain the tertiary raffinate petroleum coke, which is recorded as P3; (5) Add 70 mL of methanol as an extractant to 10 g of the third-grade raffinate petroleum coke in step (4) and perform ultrasonic extraction at 1500 W for 1 h at a temperature of 40° C. to obtain a fourth-grade raffinate petroleum coke, which is recorded as P4; (6) A physical adsorption instrument was used to measure the adsorption-desorption isotherms of petroleum coke and residual petroleum coke by CO2 adsorption. Density functional theory (DFT) was used to obtain the specific surface area, pore volume and pore size distribution of the micropores of petroleum coke.

[0021] Test Example 1 The gasification reactivity of petroleum coke is closely related to the pore structure. The present invention uses BET characterization to examine the changes in the pore structure of petroleum coke before and after extraction by using the fourth-stage raffinate petroleum coke P4 obtained in Examples 1-3 of petroleum coke to reveal the modification effect of extraction on the petroleum coke structure. The results are shown in Table 1.

[0022] Table 1 sample <![CDATA[Specific surface area (m 2 / g)]]> <![CDATA[Pore volume (cm 3 / g)]]> Petroleum coke 0.4761 0.5276 Example 1 1.2741 2.0516 Example 2 1.2984 2.0841 Example 3 1.3012 2.0997 From the above table, we can see that the specific surface area of ​​petroleum coke before treatment is about 0.48m 2 / g, and the pore volume is only 0.53cm 3 / g, the specific surface area increased significantly after extraction.

[0023] For petroleum coke, when the pore size is less than 10nm, the number of corresponding pores increases after extraction, especially after methanol extraction, a larger peak appears, indicating that the number of corresponding pores increases the most after the fourth stage of methanol extraction. After the pore size is greater than 10nm, although no larger peak appears, the trend of increasing pores after extraction is maintained. This shows that solvent extraction can improve the pore structure of petroleum coke.

[0024] By analyzing the changes in the pore structure before and after petroleum coke extraction, it is found that after four-stage ultrasonic extraction of cyclohexane, CDS, acetone and methanol, the microstructure improvement effects of petroleum coke such as specific surface area, pore volume and pore size are better. Comprehensive analysis shows that cyclohexane, CDS, acetone and methanol can be used as solvents to effectively improve the structure of petroleum coke, providing a method for improving the microstructure of petroleum coke.

[0025] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for improving the microstructure of petroleum coke, characterized in that: The following steps are involved: (1) Grinding, sieving and drying petroleum coke; (2) Cyclohexane is added to the petroleum coke powder sample as an extractant, and then a first-stage ultrasonic extraction is performed. The extract is then transferred to a buffer tank by vacuum filtration. Fresh extractant is added to the extracted petroleum coke to perform a second extraction. The extraction operation is repeated until the extract is nearly colorless to obtain a first-stage raffinate petroleum coke. (3) adding carbon disulfide as an extractant to the first-stage raffinate petroleum coke in step (2) to perform a second-stage ultrasonic extraction to obtain a second-stage raffinate petroleum coke; (4) adding acetone as an extractant to the secondary raffinate petroleum coke in step (3) to perform a third-stage ultrasonic extraction to obtain a third-stage raffinate petroleum coke; (5) Methanol is added as an extractant to the third-stage raffinate petroleum coke in step (4) to perform a fourth-stage ultrasonic extraction to obtain a fourth-stage raffinate petroleum coke.

2. The method according to claim 1, characterized in that The mesh size of the sieve in step (1) is 150-200 meshes, the drying temperature is 95-105° C., and the drying time is 36-56 hours.

3. The method according to claim 1, characterized in that In step (2), the power of the first-stage ultrasonic extraction is 1000-2000W, the temperature is 35-45°C, and the time is 0.5-1.5h.

4. The method according to claim 1, characterized in that: The solid-to-liquid ratio of the petroleum coke powder sample and the extractant in step (2) is 1:5-10 g / mL.

5. The method according to claim 1, characterized in that The solid-to-liquid ratio of the primary raffinate petroleum coke to the extractant in step (3) is 1:5-10 g / mL.

6. The method according to claim 1, characterized in that In step (3), the power of the second-stage ultrasonic extraction is 1000-2000W, the temperature is 35-45°C, and the time is 0.5-1.5h.

7. The method according to claim 1, characterized in that The solid-to-liquid ratio of the secondary raffinate petroleum coke and acetone in step (4) is 1:5-10 g / mL.

8. The method according to claim 1, characterized in that The power of the third stage ultrasonic extraction in step (4) is 1000-2000W, the temperature is 35-45°C, and the time is 0.5-1.5h.

9. The method according to claim 1, characterized in that: The solid-to-liquid ratio of the tertiary raffinate petroleum coke and methanol in step (5) is 1:5-10 g / mL.

10. The method according to claim 1, characterized in that The power of the fourth stage ultrasonic extraction in step (5) is 1000-2000W, the temperature is 35-45°C, and the time is 0.5-1.5h.