High-lubricity diesel oil anti-wear agent and preparation method thereof

Through the combination of modified organic and inorganic lubricants, the lubricating performance and stability of diesel antiwear agents at high temperatures are solved, efficient lubrication and high temperature stability are achieved, and diesel combustion efficiency and environmental friendliness are improved.

CN118879378AActive Publication Date: 2024-11-01YIXING XINGUANG BAOYI CHEM CO LTD

Patent Information

Application Number
CN202411223171.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-01
Estimated Expiration
2044-09-03

AI Technical Summary

Technical Problem

The lubricating performance and high-temperature stability of existing diesel antiwear agents lead to a decrease in combustion performance and an increase in wear under high temperature environments.

Method used

Using a combination of modified organic lubricants and modified inorganic lubricants, through esterification reaction and surface modification technology, diesel antiwear agents with high lubricity and high temperature resistance are prepared, including modified phosphate esters, cross-linked fatty amines and α-MnO2@CTS combines anticorrosion agents, antioxidants and viscosity index improvers to form a stable lubricating film.

Benefits of technology

It significantly improves the lubricating performance and high temperature stability of diesel antiwear agents, reduces wear and incomplete combustion, and improves combustion efficiency and environmental friendliness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879378A_ABST
    Figure CN118879378A_ABST
Patent Text Reader

Abstract

The invention discloses a high-lubricity diesel oil anti-wear agent and a preparation method thereof, and belongs to the technical field of anti-wear agent processing. The high-lubricity diesel oil anti-wear agent and the preparation method thereof are used for solving the technical problem that the lubricating property and the high-temperature stability of a diesel oil anti-wear agent in the prior art need to be further improved. Comprising the following raw material components in parts by weight: 80-100 parts of a modified organic lubricant, 5-10 parts of a modified inorganic lubricant, 1-5 parts of a corrosion inhibitor, 1-5 parts of an antioxidant and 1-5 parts of a viscosity index improver. The preparation method comprises the following steps: polymerizing prepared modified phosphate to synthesize cross-linked fatty amine, amidating the cross-linked fatty amine to obtain amidated fatty amine, esterifying to obtain a modified organic lubricant, and combining the modified organic lubricant with the prepared modified inorganic lubricant and auxiliary materials, thereby enhancing the lubricating property and high-temperature resistance of the anti-wear agent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of diesel antiwear agent processing, and in particular to a high-lubricity diesel antiwear agent and a preparation method thereof. Background Art

[0002] Diesel anti-wear agents are additives used in diesel engine lubricants. Their main function is to reduce friction and wear between metal surfaces, thereby extending the service life of the engine and improving performance stability. The main function of diesel anti-wear agents is to form a protective film during the operation of the engine, reduce the friction coefficient of the metal surface, and thus reduce wear and heat loss. They can also improve the strength and stability of the oil film to ensure effective protection of the engine under various operating conditions. Diesel anti-wear agents play an important role in modern diesel engine technology. By reducing friction and wear, they improve the reliability, efficiency and service life of the engine, which is crucial to the safety and economy of the operation of automobiles, ships and industrial equipment.

[0003] Prior art CN102277212A discloses a diesel antiwear agent, comprising a mixture of the following components: (A) tall oil fatty acid; (B) oleic acid amide; (C) cyclohexane acid imidazoline; characterized in that the weight ratio of component A, component B and component C is A:B:C is 100:5-100:5-50. The invention obtains a diesel antiwear agent by simple physical mixing means, which is easy to implement and convenient to use, but ignores that tall oil fatty acid, oleic acid amide and cyclohexane acid imidazoline will have a negative impact on the combustion of diesel, and under high temperature environment, tall oil fatty acid, oleic acid amide and cyclohexane acid imidazoline produce smoke and residues due to high temperature decomposition, resulting in extremely unstable lubrication performance of the three, resulting in a significant decrease in the performance of the antiwear agent. In summary, the lubrication performance and high temperature stability of diesel antiwear agents in the prior art need to be further improved.

[0004] In view of the technical defects in this aspect, a solution is now proposed. Summary of the invention

[0005] The object of the present invention is to provide a high-lubricity diesel antiwear agent and a preparation method thereof, so as to solve the technical problem that the lubrication performance and high-temperature stability of diesel antiwear agents in the prior art need to be further improved.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A highly lubricating diesel antiwear agent comprises the following raw material components in parts by weight: 80-100 parts of a modified organic lubricant, 5-10 parts of a modified inorganic lubricant, 1-5 parts of an anticorrosive agent, 1-5 parts of an antioxidant and 1-5 parts of a viscosity index improver;

[0008] The preparation method of the modified organic lubricant is as follows: 3-5 parts of N-hydroxysuccinimide, 1-2 parts of N,N-dicyclohexylcarbodiimide, 0.3-0.5 parts of triethylamine and 30-40 parts of N,N-dimethylformamide are weighed by weight and added into a reaction kettle, and after reacting at room temperature for 0.5-1h, 20-30 parts of amidated fatty amine are added into the reaction kettle, the temperature of the reaction kettle is increased to 40-50°C, the reaction is kept warm for 2-4h, and the modified organic lubricant is obtained by post-treatment.

[0009] The reaction equation for preparing modified organic lubricant is:

[0010]

[0011] Where:

[0012] The reaction principle formula for preparing the modified organic lubricant is as follows: a special esterification reaction occurs in the reaction process, and the reaction uses the active intermediate N,N-dicyclohexylcarboximide to convert the carboxylic acid into its corresponding ester. In the reaction, N-hydroxysuccinimide and N,N-dicyclohexylcarboximide are first mixed to form an imide salt at room temperature, and then an amidated fatty amine with a carboxyl group is added. At this time, the imide salt will be attacked by hydroxide ions and lose N,N-dicyclohexylcarboximide ions to generate a modified organic lubricant.

[0013] Furthermore, the post-treatment includes: after the reactor is cooled to room temperature, the reaction liquid is added into a rotary evaporator with a water bath temperature of 80-100° C., and the reaction liquid is distilled under reduced pressure until no liquid is extracted to obtain a modified organic lubricant.

[0014] Furthermore, the preparation method of the amidated fatty amine is as follows: 20-30 parts of cross-linked fatty amine, 5-10 parts of pyromellitic anhydride, 75-100 parts of N,N-dimethylformamide and 1-3 parts of triethylamine are weighed and added into a reaction kettle, stirred at room temperature for 2-4 hours, and post-treated to obtain the amidated fatty amine.

[0015] The reaction equation for preparing amidated polyurethane is:

[0016]

[0017] Where:

[0018] The reaction principle for preparing amidated polyurethane is as follows: a cross-linked fatty amine nucleophile with a secondary amino group attacks the carbonyl carbon atom in the pyromellitic dianhydride molecule, wherein the nitrogen atom of the secondary amino group carries a lone pair of electrons, which can form a new covalent bond with the carbonyl carbon atom to form an amidic acid polymer, and finally an amidated fatty amine is prepared.

[0019] Furthermore, the post-treatment includes: after the reactor is cooled to room temperature, the reaction liquid is added into a rotary evaporator with a water bath temperature of 80-100° C., and distilled under reduced pressure until no liquid is extracted to obtain an amidated fatty amine.

[0020] Furthermore, the preparation method of the cross-linked fatty amine is as follows: 5-8 parts of modified phosphate, 3-5 parts of dimethylbiphenyl diisocyanate, 4-6 parts of tetraethylene glycol and 40-50 parts of N,N-dimethylformamide are weighed by weight and added into a reaction kettle, the temperature of the reaction kettle is increased to 70-90° C., the reaction kettle is stirred for 2-4 hours, and the cross-linked fatty amine is obtained by post-treatment.

[0021] The reaction equation for preparing cross-linked fatty amines is:

[0022]

[0023] Where:

[0024] The reaction principle for preparing cross-linked fatty amines is as follows: isocyanate groups (-NCO) react with hydroxyl groups (-OH) to form a polymer linked by carbamates. During this process, the hydroxyl oxygen atom acts as a nucleophilic agent to attack the isocyanate carbon atom to generate carbamates; the isocyanate group reacts with the hydroxyl groups in tetraethylene glycol and modified phosphates to form a long-chain structure, and finally a cross-linked fatty amine is obtained.

[0025] Furthermore, the post-treatment includes: after the reactor is cooled to room temperature, the reaction liquid is added into a rotary evaporator with a water bath temperature of 80-100° C., and distilled under reduced pressure until no liquid is extracted to obtain a cross-linked fatty amine.

[0026] Furthermore, the preparation method of the modified phosphate ester is as follows: 5-8 parts of binaphthol phosphate, 3-5 parts of 3H,8H-2a,8a:3a,7a diepoxyanthracene [2,3-b]epoxide, octahydro-(9CI), 0.5-0.8 parts of triethylamine and 30-40 parts of N,N-dimethylformamide are weighed by weight and added into a reactor, the temperature of the reactor is increased to 60-80°C, the reaction is kept warm for 1-3 hours, and the modified phosphate ester is obtained by post-treatment.

[0027] The reaction equation for preparing modified phosphate ester is:

[0028]

[0029] Where:

[0030] The reaction principle for preparing the modified phosphate ester is as follows: under weak alkaline conditions, the hydroxyl group (-OH) of binaphthol phosphate and the epoxy group of 3H,8H-2a,8a:3a,7a diepoxyanthracene[2,3-b]epoxyene, octahydro-(9CI) undergo a ring-opening reaction, and the binaphthol phosphate and 3H,8H-2a,8a:3a,7a diepoxyanthracene[2,3-b]epoxyene, octahydro-(9CI) are polymerized through ether bonds to prepare the modified phosphate ester.

[0031] Furthermore, the post-treatment includes: after the reactor is cooled to room temperature, the reaction liquid is added into a rotary evaporator with a water bath temperature of 80-100° C., and the reaction liquid is distilled under reduced pressure until no liquid is extracted to obtain a modified phosphate ester.

[0032] Furthermore, the preparation method of the modified inorganic lubricant is: weigh 10-20 parts by weight of α-MnO 2 @CTS, 1-2 parts of bis(2-ethylhexyl) dithiophosphate, 40-50 parts of N,N-dimethylformamide and 0.5-0.8 parts of triethylamine are added into the reaction kettle, the temperature of the reaction kettle is increased to 40-60°C, the reaction is kept warm for 2-4 hours, and the modified inorganic lubricant is obtained by post-treatment.

[0033] The reaction equation for preparing modified inorganic lubricant is:

[0034]

[0035] The reaction principle for preparing the modified inorganic lubricant is: under alkaline conditions, the thiol group and the carboxyl group undergo a substitution reaction to generate a thioester.

[0036] Furthermore, the post-treatment includes: after the reactor is cooled to room temperature, the filter cake is collected by suction filtration, and the filter cake is placed in a drying oven at a temperature of 80° C. and vacuum dried until the filter cake has a constant weight, thereby obtaining a modified inorganic lubricant.

[0037] Furthermore, α-MnO 2 The preparation method of @CTS is as follows: weigh 20-30 parts by weight of α-MnO 2 , 50-60 parts of carboxysuccinic acid powder and 800-1000 parts of anhydrous ethanol are added to an ultrasonic instrument, and stirred for 8-12 hours at room temperature while ultrasonicating, with an ultrasonic frequency of 20-40KHz and a stirring rate of 120-180rpm, and α-MnO is obtained by post-treatment. 2 @CTS.

[0038] Preparation of α-MnO 2 @CTS principle: using the mechanical action of ultrasound and the help of stirring, α-MnO 2The carboxyl groups in the carboxyl succinic acid react with the active sites on the surface of manganese dioxide to form coordination bonds. The carboxyl succinic acid is then attached to the MnO2 by chemical grafting. 2 The surface of α-MnO 2 @CTS.

[0039] Further, the post-treatment includes: after the reactor is cooled to room temperature, the filter cake is collected by suction filtration, and the filter cake is placed in a drying oven at a temperature of 80°C and vacuum dried until the filter cake has a constant weight, thereby obtaining α-MnO 2 @CTS.

[0040] Furthermore, α-MnO 2 The preparation method is as follows: 10-20 parts of potassium permanganate powder, 2-4 parts of potassium chloride powder, 0.5-0.8 parts of polyvinyl pyrrolidone with a molecular weight of 1200000-1300000 and 40-50 parts of deionized water are weighed by weight, added into a reaction kettle and stirred, after the solid is completely dissolved, the temperature of the reaction kettle is increased to 150-160°C, the reaction is kept warm for 12 hours, and α-MnO is obtained by post-treatment. 2 .

[0041] Further, the stirring rate is 120-160rpm, and the post-treatment includes: after the reactor is cooled to room temperature, the filter cake is collected by suction filtration, the filter cake is washed with deionized water for 3-5 times, and the filter cake is placed in a drying oven at a temperature of 80°C for vacuum drying for 24 hours to obtain a dry product, and the dry product is placed in a tubular furnace, nitrogen is introduced for protection, and the tubular heating furnace is heated to 400±10°C at a rate of 10°C / min, and after keeping warm for 6-8 hours, it is naturally cooled to room temperature to obtain α-MnO 2 .

[0042] Furthermore, the corrosion inhibitor is one or more of ferrous phosphate, benzothiadiazoline diphenol and mercaptodiethylamine, the antioxidant is one or more of di-tert-butyl-p-cresol, dibutylhydroquinone and diphenyl disulfide phosphate, and the viscosity index improver is polyisobutylene.

[0043] A method for preparing a highly lubricating diesel antiwear agent comprises the following steps: adding a modified organic lubricant, a modified inorganic lubricant, an antioxidant and a viscosity index improver into a reaction kettle, mixing them uniformly, and passing the mixture through a 100-mesh sieve to obtain the diesel antiwear agent.

[0044] The present invention has the following beneficial effects:

[0045] 1. In the process of preparing a high lubricity diesel antiwear agent, the present invention first synthesizes a modified organic lubricant, which has a large number of functional groups, and has the function of cleaning diesel combustion products while having lubricating properties. Further, the functional groups therein also make the modified organic lubricant have the function of a partial dispersant, so that the prepared modified inorganic lubricant remains in a dispersed state in diesel, so as to avoid the formation of sediments at key parts of the engine, and promote the discharge of the modified inorganic lubricant. At the same time, because manganese dioxide can be used as a catalyst for the combustion reaction, the combustion performance of diesel is improved, and the pollution to the environment is reduced; further, in the process of preparing a modified inorganic lubricant, the surface of nano metal oxide particles is modified to have certain lubricity and promote the combustion of diesel, reduce the influence of the diesel antiwear agent on the combustion of diesel, make the combustion of diesel more complete, and reduce the pollution to the environment; finally, a high lubricity and high temperature resistant diesel antiwear agent is obtained by mixing and sieving the modified organic lubricant, the modified inorganic lubricant and auxiliary materials.

[0046] 2. In the process of preparing a modified organic lubricant, the present invention firstly utilizes the epoxy ring-opening reaction between reactive monomers to prepare a modified phosphate ester with a complex spatial structure. The complex spatial structure helps to form a stronger interaction between molecules, thereby enhancing the adhesion and stability of the lubricant on the contact surface and maintaining the integrity of the lubricating film. In addition, the generated active group hydroxyl provides a basis for subsequent reactions. Further, a cross-linked fatty amine with a large number of ether bonds and phosphoric acid groups is prepared using the modified phosphate ester and polymer monomers, and then reacted with pyromellitic acid dianhydride to generate an amidated fatty amine, wherein the phosphoric acid group can chemically react with the metal surface to form a phosphorus compound or a phosphate film. These films can form a protective lubricating film on the metal surface, reduce the friction coefficient, and reduce the direct contact and wear of the metal surface. The amide group forms a protective film on the metal surface, reduces the friction coefficient, and improves the lubrication effect. At the same time, under high temperature conditions, the large number of benzene ring structures and amide groups in the structure can improve the thermal stability and heat resistance of the lubricant, maintain lubrication. The effect does not decrease with increasing temperature. The presence of amide groups can enhance the extreme pressure performance of the lubricant, improve the working ability of the lubricant under high load and high pressure, and prevent the metal surface from contacting and wearing due to excessive pressure. The three cooperate with each other to significantly improve the lubrication performance of the organic chain segment. At the same time, the phosphoric acid group and a large number of ether bonds can improve the thermal stability and oxidation stability of the lubricant, so that it is still effective under high temperature conditions, thereby maintaining its long-term stability and lubricating effect. Under high pressure, the phosphoric acid group can form metal phosphates and form stronger chemical bonds with the metal surface, thereby enhancing the extreme pressure performance of the lubricant and preventing the metal surface from contacting and damaging under extreme loads. Finally, N-hydroxysuccinimide is used to react with amidated fatty amines under the catalysis of N,N-dicyclohexylcarboximide to introduce sulfide and succinimide at the same time. The succinimide group enables the modified organic lubricant to have a certain cleaning ability and the ability to disperse insoluble substances in diesel, while improving the lubrication performance of the modified organic lubricant, and finally a modified organic lubricant with high lubricity and high temperature resistance is obtained.

[0047] 3. In the process of preparing the modified inorganic lubricant, the present invention first prepares a spherical α-MnO 2 The spherical spatial structure improves its lubrication performance and increases its contact area with the modified material. α-MnO 2 @CTS, α-MnO by carboxysuccinic acid 2 Surface modification enhanced the α-MnO 2The dispersion ability of the nanoparticles was improved, and the active group carboxyl was introduced. The bis(2-ethylhexyl) dithiophosphate was further used to react with the carboxyl groups on its surface to form a thioester. At high temperatures, the sulfur and phosphorus elements in the bis(2-ethylhexyl) dithiophosphate formed a tribochemical reaction film during the friction process. The synergistic effect of the chemical reaction film and the "ball bearing" effect of the nanoparticles effectively reduced the friction and wear of the friction pair surface. At the same time, MnO 2 It can reduce the activation energy of the combustion reaction, allowing the fuel to burn at a lower temperature, thereby improving the combustion efficiency, promoting the combustion of diesel, and reducing the impact of diesel additives on diesel combustion performance, ultimately obtaining a highly lubricating modified inorganic lubricant. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0049] Figure 1 is α-MnO 2 SEM image of . DETAILED DESCRIPTION

[0050] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0051] Example 1

[0052] This embodiment provides a method for preparing a high lubricity diesel antiwear agent, comprising the following steps:

[0053] S1. Preparation of modified organic lubricant

[0054] 47.4 g of binaphthol phosphate, 31.6 g of 3H,8H-2a,8a:3a,7a diepoxyanthracene [2,3-b]epoxide, octahydro-(9CI), 4.6 g of triethylamine and 279.6 g of N,N-dimethylformamide were weighed and added into a reactor. The temperature of the reactor was raised to 60° C. and the reaction was kept warm for 1 hour. After the reactor was cooled to room temperature, the reaction liquid was added into a rotary evaporator with a water bath temperature of 100° C. and distilled under reduced pressure until no liquid was produced, to obtain 79.0 g of modified phosphate;

[0055] 58.2 g of modified phosphate, 26.2 g of dimethylbiphenyl diisocyanate, 19.4 g of tetraethylene glycol and 299.6 g of N,N-dimethylformamide were weighed and added to a reactor. The temperature of the reactor was raised to 70° C. and stirred for 2 h. After the reactor was cooled to room temperature, the reaction solution was added to a rotary evaporator with a water bath temperature of 80° C. and distilled under reduced pressure until no liquid was produced to obtain 102.3 g of cross-linked fatty amine.

[0056] 88.3 g of cross-linked fatty amine, 22.1 g of pyromellitic anhydride, 335.3 g of N,N-dimethylformamide and 5.3 g of triethylamine were weighed and added to a reactor, and stirred at room temperature for 2 h. After the reactor was cooled to room temperature, the reaction solution was added to a rotary evaporator with a water bath temperature of 80° C., and distilled under reduced pressure until no liquid was produced, to obtain 108.4 g of amidated fatty amine;

[0057] 16.3 g of N-hydroxysuccinimide, 6.7 g of N,N-dicyclohexylcarbocyanine, 1.6 g of triethylamine and 168.3 g of N,N-dimethylformamide were weighed and added to a reactor. After reacting at room temperature for 0.5 h, 101.3 g of amidated fatty amine was added to the reactor. The temperature of the reactor was raised to 40°C and kept warm for 2 h. After the reactor was cooled to room temperature, the reaction liquid was added to a rotary evaporator with a water bath temperature of 80°C, and distilled under reduced pressure until no liquid was produced to obtain 113.2 g of a modified organic lubricant.

[0058] S2. Preparation of modified inorganic lubricant

[0059] Weigh 6.4g potassium permanganate powder, 0.9g potassium chloride powder, 0.28g polyvinyl pyrrolidone with a molecular weight of 1213512.3 and 17.6g deionized water into the reactor and stir. After the solid is completely dissolved, the temperature of the reactor is raised to 150°C and the reaction is kept warm for 12h. After the reactor is cooled to room temperature, the filter cake is collected by suction filtration. After the filter cake is washed 3 times with deionized water, the filter cake is placed in a drying oven at a temperature of 80°C and vacuum dried for 24h to obtain a dry product. The dry product is placed in a tubular furnace and nitrogen is introduced for protection. The tubular heating furnace is raised to 390°C at a rate of 10°C / min, kept warm for 6h, and then naturally cooled to room temperature to obtain 5.6g α-MnO 2 ;

[0060] Weigh 4.2g α-MnO 2 , 9.7g carboxysuccinic acid powder and 140.4g anhydrous ethanol were added to an ultrasonic instrument, and stirred for 8h at room temperature while ultrasonicating. The ultrasonic frequency was 20KHz and the stirring rate was 120rpm. After the reactor was cooled to room temperature, the filter cake was collected by suction filtration and placed in a drying oven at a temperature of 80°C for vacuum drying until the filter cake had a constant weight, to obtain 12.8g α-MnO 2@CTS;

[0061] Weigh 10.2g α-MnO 2 @CTS, 1.8g bis(2-ethylhexyl) dithiophosphate, 42.3g N,N-dimethylformamide and 0.6g triethylamine were added to the reactor, the temperature of the reactor was raised to 40°C, and the reaction was kept warm for 2 hours. After the reactor was cooled to room temperature, the filter cake was collected by filtration, and the filter cake was placed in a drying oven at 80°C and vacuum dried until the filter cake had a constant weight, to obtain 11.3g of modified inorganic lubricant.

[0062] S3. Preparation of diesel antiwear agent

[0063] 94.0 g of modified organic lubricant, 6.0 g of modified inorganic lubricant, 2.0 g of benzothiadiazoline diphenol, 2.0 g of di-tert-butyl-p-cresol and 2.0 g of polyisobutylene were weighed and added into a reaction kettle, mixed evenly, and passed through a 100-mesh sieve to obtain 105.3 g of diesel antiwear agent.

[0064] Example 2

[0065] This embodiment provides a method for preparing a high lubricity diesel antiwear agent, comprising the following steps:

[0066] S1. Preparation of modified organic lubricant

[0067] 48.6 g of binaphthol phosphate, 27.4 g of 3H,8H-2a,8a:3a,7a diepoxyanthracene [2,3-b]epoxyene, octahydro-(9CI), 5.4 g of triethylamine and 273.6 g of N,N-dimethylformamide were weighed and added to a reactor. The temperature of the reactor was raised to 80° C. and the reaction was kept warm for 3 hours. After the reactor was cooled to room temperature, the reaction liquid was added to a rotary evaporator with a water bath temperature of 100° C. and distilled under reduced pressure until no liquid was produced, to obtain 71.2 g of modified phosphate;

[0068] 58.2 g of modified phosphate, 26.4 g of dimethylbiphenyl diisocyanate, 19.4 g of tetraethylene glycol and 258.9 g of N,N-dimethylformamide were weighed and added to a reactor. The temperature of the reactor was raised to 90° C. and stirred for 4 hours. After the reactor was cooled to room temperature, the reaction solution was added to a rotary evaporator with a water bath temperature of 100° C. and distilled under reduced pressure until no liquid was produced to obtain 101.3 g of cross-linked fatty amine.

[0069] 79.1 g of cross-linked fatty amine, 17.4 g of pyromellitic anhydride, 270.0 g of N,N-dimethylformamide and 7.1 g of triethylamine were weighed and added to a reactor, and stirred at room temperature for 4 h. After the reactor was cooled to room temperature, the reaction solution was added to a rotary evaporator with a water bath temperature of 100° C., and distilled under reduced pressure until no liquid was produced, to obtain 93.5 g of amidated fatty amine;

[0070] 19.5 g of N-hydroxysuccinimide, 5.7 g of N,N-dicyclohexylcarboximide, 1.4 g of triethylamine and 125.3 g of N,N-dimethylformamide were weighed and added to a reactor. After reacting at room temperature for 1 hour, 89.1 g of amidated fatty amine was added to the reactor. The temperature of the reactor was raised to 50°C and kept warm for 4 hours. After the reactor was cooled to room temperature, the reaction solution was added to a rotary evaporator with a water bath temperature of 100°C, and distilled under reduced pressure until no liquid was produced to obtain 102.3 g of modified organic lubricant.

[0071] S2. Preparation of modified inorganic lubricant

[0072] 8.4 g potassium permanganate powder, 1.5 g potassium chloride powder, 0.4 g polyvinyl pyrrolidone with a molecular weight of 1284325.5 and 28.8 g deionized water were weighed and added to the reactor and stirred. After the solid was completely dissolved, the temperature of the reactor was raised to 160 ° C. and the reaction was kept warm for 12 hours. After the reactor was cooled to room temperature, the filter cake was collected by suction filtration. After the filter cake was washed with deionized water 5 times, the filter cake was placed in a drying oven at a temperature of 80 ° C. and vacuum dried for 24 hours to obtain a dry product. The dry product was placed in a tubular furnace and nitrogen was introduced for protection. The tubular heating furnace was raised to 410 ° C at a rate of 10 ° C / min, and after being kept warm for 8 hours, it was naturally cooled to room temperature to obtain 6.0 g α-MnO 2 ;

[0073] Weigh 4.8g α-MnO 2 , 11.2g carboxysuccinic acid powder and 179.2g anhydrous ethanol were added to an ultrasonic instrument, and stirred for 12h at room temperature while ultrasonicating. The ultrasonic frequency was 40KHz and the stirring rate was 180rpm. After the reactor was cooled to room temperature, the filter cake was collected by suction filtration and placed in a drying oven at a temperature of 80°C and vacuum dried until the filter cake had a constant weight, to obtain 14.4g α-MnO 2 @CTS;

[0074] Weigh 12.6g α-MnO 2 @CTS, 1.8g bis(2-ethylhexyl) dithiophosphate, 43.2g N,N-dimethylformamide and 0.6g triethylamine were added to the reactor, the temperature of the reactor was raised to 60°C, and the reaction was kept warm for 4 hours. After the reactor was cooled to room temperature, the filter cake was collected by filtration, and the filter cake was placed in a drying oven at 80°C and vacuum dried until the filter cake had a constant weight, to obtain 12.4g of modified inorganic lubricant.

[0075] S3. Preparation of diesel antiwear agent

[0076] 92.4 g of modified organic lubricant, 7.6 g of modified inorganic lubricant, 2.1 g of benzothiadiazoline diphenol, 2.0 g of di-tert-butyl-p-cresol and 2.1 g of polyisobutylene were weighed and added into a reaction kettle and mixed evenly. The mixture was passed through a 100-mesh sieve to obtain 105.6 g of diesel antiwear agent.

[0077] Example 3

[0078] This embodiment provides a method for preparing a high lubricity diesel antiwear agent, comprising the following steps:

[0079] S1. Preparation of modified organic lubricant

[0080] 56.8 g of binaphthol phosphate, 33.4 g of 3H,8H-2a,8a:3a,7a diepoxyanthracene [2,3-b]epoxyene, octahydro-(9CI), 5.4 g of triethylamine and 315.7 g of N,N-dimethylformamide were weighed and added to a reactor. The temperature of the reactor was raised to 70° C. and the reaction was kept warm for 2 hours. After the reactor was cooled to room temperature, the reaction solution was added to a rotary evaporator with a water bath temperature of 90° C. and distilled under reduced pressure until no liquid was produced, to obtain 86.4 g of modified phosphate;

[0081] 58.2 g of modified phosphate, 26.4 g of dimethylbiphenyl diisocyanate, 19.4 g of tetraethylene glycol and 270.9 g of N,N-dimethylformamide were weighed and added to a reactor. The temperature of the reactor was raised to 80° C. and stirred for 3 hours. After the reactor was cooled to room temperature, the reaction solution was added to a rotary evaporator with a water bath temperature of 90° C. and distilled under reduced pressure until no liquid was produced to obtain 102.3 g of cross-linked fatty amine.

[0082] 75.5 g of cross-linked fatty amine, 23.0 g of pyromellitic anhydride, 255.8 g of N,N-dimethylformamide and 7.9 g of triethylamine were weighed and added to a reactor, and stirred at room temperature for 3 h. After the reactor was cooled to room temperature, the reaction solution was added to a rotary evaporator with a water bath temperature of 90° C., and distilled under reduced pressure until no liquid was produced to obtain 98.4 g of amidated fatty amine;

[0083] 15.5 g of N-hydroxysuccinimide, 4.7 g of N,N-dicyclohexylcarbocyanine, 1.55 g of triethylamine and 135.8 g of N,N-dimethylformamide were weighed and added to a reactor. After reacting at room temperature for 0.75 h, 93.1 g of amidated fatty amine was added to the reactor. The temperature of the reactor was raised to 45°C and kept warm for 3 h. After the reactor was cooled to room temperature, the reaction solution was added to a rotary evaporator with a water bath temperature of 90°C, and distilled under reduced pressure until no liquid was produced to obtain 105.3 g of a modified organic lubricant.

[0084] S2. Preparation of modified inorganic lubricant

[0085] 8.0 g potassium permanganate powder, 1.2 g potassium chloride powder, 0.3 g polyvinyl pyrrolidone with a molecular weight of 1261432.5 and 24.5 g deionized water were weighed and added to the reactor and stirred. After the solid was completely dissolved, the temperature of the reactor was raised to 155 ° C. and the reaction was kept warm for 12 hours. After the reactor was cooled to room temperature, the filter cake was collected by suction filtration. After the filter cake was washed with deionized water 4 times, the filter cake was placed in a drying oven at a temperature of 80 ° C. and vacuum dried for 24 hours to obtain a dry product. The dry product was placed in a tubular furnace and nitrogen was introduced for protection. The tubular heating furnace was raised to 400 ° C at a rate of 10 ° C / min, and after keeping warm for 7 hours, it was naturally cooled to room temperature to obtain 6.4 g α-MnO 2 ;

[0086] Weigh 5.2g α-MnO 2 , 11.4g carboxysuccinic acid powder and 177.5g anhydrous ethanol were added to an ultrasonic instrument, and stirred for 10h at room temperature while ultrasonicating. The ultrasonic frequency was 30KHz and the stirring rate was 150rpm. After the reactor was cooled to room temperature, the filter cake was collected by suction filtration and placed in a drying oven at a temperature of 80°C and vacuum dried until the filter cake had a constant weight, to obtain 15.6g α-MnO 2 @CTS;

[0087] Weigh 13.2g α-MnO 2 @CTS, 1.2g of bis(2-ethylhexyl) dithiophosphate, 43.5g of N,N-dimethylformamide and 0.6g of triethylamine were added to the reactor, the temperature of the reactor was raised to 50°C, and the reaction was kept warm for 3 hours. After the reactor was cooled to room temperature, the filter cake was collected by filtration, and the filter cake was placed in a drying oven at a temperature of 80°C and vacuum dried until the filter cake had a constant weight, to obtain 12.3g of modified inorganic lubricant.

[0088] S3. Preparation of diesel antiwear agent

[0089] Weigh 92.3 g of modified organic lubricant, 7.7 g of modified inorganic lubricant, 2.3 g of benzothiadiazoline diphenol, 2.1 g of di-tert-butyl-p-cresol and 2.0 g of polyisobutylene into a reactor, mix well, and pass through a 100-mesh sieve to obtain 105.5 g of diesel antiwear agent.

[0090] Comparative Example 1

[0091] The difference between this comparative example and Example 3 is that step S1 is eliminated, and in step S3, an equal amount of dithiodiphenol phosphate is used to replace the modified organic lubricant.

[0092] Comparative Example 2

[0093] The difference between this comparative example and Example 3 is that step S2 is eliminated, and in step S3, the use of modified inorganic lubricant is eliminated.

[0094] Comparative Example 3

[0095] The difference between this comparative example and Example 3 is that step S1 and step S2 are eliminated, and in step S3, an equal amount of dithiodiphenol phosphate is used to replace the modified organic lubricant, and the use of the modified inorganic lubricant is eliminated.

[0096] Performance Test:

[0097] The acid value, anti-wear performance and combustion performance of the diesel anti-wear agents prepared in Examples 1-3 and Comparative Examples 1-3 were tested:

[0098] The acid value and anti-wear performance were determined according to the standard NB / SH / T 6074-2023 "Diesel Anti-wear Agent".

[0099] The combustion performance refers to the standard GB 36886-2018 "Exhaust Smoke Limits and Measurement Methods for Non-road Mobile Diesel Machinery" to test the opacity method smoke density and Ringelmann blackness base of the combustion products. The test results are shown in Table 1.

[0100] A high-frequency reciprocating friction tester was used to test the high-temperature wear resistance of the oils in Examples 1-3 and Comparative Examples 1-3. The test conditions were: load 1000 g, frequency 20 Hz, temperature 100°C, test time 60 min, and the wear spot diameter and friction coefficient of the samples were statistically analyzed. An engine crankcase coking simulation test was used to test the cleaning performance of Examples 1-3 and Comparative Examples 1-3. 300 mL of the test sample was added to a coking plate simulator, heated to 150°C, and oil was continuously splashed onto an aluminum plate at a temperature of 310°C. After 6 hours, the amount of coke generated on the aluminum plate was weighed and expressed as the mass of the deposit to simulate the deposit on the piston. The test results are shown in Table 2.

[0101] Table 1-Performance test data of samples

[0102]

[0103] Table 2-Performance simulation test data of the sample

[0104]

[0105] Data Analysis:

[0106] Comparing and analyzing the data in Table 1 and Table 2 above, the acid value (in terms of KOH) of the diesel antiwear agent prepared by the present invention is 0.5 mg·g -1 The average wear spot diameter is 228um, and the opacity smoke density (P Max< 19) is 1.68m -1The Ringelmann blackness base is level 1, the amount of deposits in the focus spot test is 13.6 mg, the wear spot diameter obtained in the high-frequency reciprocating friction test is 235 um, and the friction coefficient is 0.092. All performance test data are better than those of the comparative example, indicating that the diesel antiwear agent prepared by the present invention achieves the expected effect.

[0107] By comparing the data of Example 3, Comparative Example 1 and Comparative Example 3, it can be found that compared with the diesel anti-wear agent prepared by using dithiodiphenol phosphate in Comparative Example 1, the various properties of the diesel anti-wear agent prepared by using the modified organic lubricant in Example 3 are significantly improved. By comparing the anti-wear performance and the data of the high-frequency reciprocating test, it can be found that the lubricating performance of the modified organic lubricant prepared by the present invention is excellent. By providing the data of the comparison of the amount of deposits in the focus spot test, it can be found that the modified organic lubricant prepared by the present invention has an excellent dispersion and discharge effect on the modified inorganic lubricant prepared by the present invention. It only has a very strong promoting effect, which greatly improves the performance of the modified inorganic lubricant; by comparing the data of Example 3, Comparative Example 2 and Comparative Example 3, it can be found that the addition of the prepared modified inorganic lubricant greatly improves the lubrication performance of the diesel anti-wear agent, and by comparing the data of the amount of deposits in the coke test, it can be found that the modified inorganic lubricant promotes the combustion of diesel more fully and the amount of deposits is greatly reduced; by comparing the data of Example 3 and Comparative Example 3, it can be found that the various properties of the diesel anti-wear agent prepared in Example 3 are better than those of Comparative Example 3, which directly uses dithiodiphenol phosphate as a diesel anti-wear agent.

[0108] In summary, the present invention prepares a cross-linked fatty amine by polymerizing the prepared modified phosphate, amidates the cross-linked fatty amine, and further introduces an amide group to obtain a modified organic lubricant. Finally, the modified organic lubricant is obtained by using carboxysuccinic acid and bis(2-ethylhexyl) dithiophosphate to react α-MnO 2 The modified inorganic lubricant obtained by surface modification and auxiliary materials are mixed and sieved to obtain a diesel anti-wear agent with high lubricity and high temperature resistance.

[0109] The above contents are merely examples and explanations of the structure of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the structure of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

[0110] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0111] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A high lubricity diesel antiwear agent, characterized in that: The raw material components include the following parts by weight: 80-100 parts of modified organic lubricant, 5-10 parts of modified inorganic lubricant, 1-5 parts of anticorrosive agent, 1-5 parts of antioxidant and 1-5 parts of viscosity index improver; The preparation method of the modified organic lubricant is as follows: 3-5 parts of N-hydroxysuccinimide, 1-2 parts of N,N'-dicyclohexylcarbodiimide, 0.3-0.5 parts of triethylamine and 30-40 parts of N,N-dimethylformamide are weighed by weight and added into a reaction kettle, reacted at room temperature for 0.5-1h, 20-30 parts of amidated fatty amine are added into the reaction kettle, the temperature of the reaction kettle is increased to 40-50°C, the reaction is kept warm for 2-4h, and the modified organic lubricant is obtained by post-treatment.

2. A high lubricity diesel antiwear agent according to claim 1, characterized in that: The preparation method of the amidated fatty amine is as follows: 20-30 parts of cross-linked fatty amine, 5-10 parts of pyromellitic dianhydride, 75-100 parts of N,N-dimethylformamide and 1-3 parts of triethylamine are weighed and added into a reaction kettle, stirred at room temperature for 2-4 hours, and post-treated to obtain the amidated fatty amine.

3. A high lubricity diesel anti-wear agent according to claim 2, characterized in that: The preparation method of the cross-linked fatty amine is as follows: 5-8 parts of modified phosphate, 3-5 parts of dimethylbiphenyl diisocyanate, 4-6 parts of tetraethylene glycol and 40-50 parts of N,N-dimethylformamide are weighed and added into a reaction kettle, the temperature of the reaction kettle is increased to 70-90° C., the reaction kettle is kept warm and stirred for 2-4 hours, and the cross-linked fatty amine is obtained by post-treatment.

4. A high lubricity diesel anti-wear agent according to claim 3, characterized in that: The preparation method of the modified phosphate ester comprises the following steps: 5-8 parts of binaphthol phosphate ester, 3-5 parts of 3H,8H-2a,8a:3a,7a diepoxyanthracene [2,3-b]epoxide, octahydro-(9CI), 0.5-0.8 parts of triethylamine and 30-40 parts of N,N-dimethylformamide are weighed and added into a reaction kettle, the temperature of the reaction kettle is increased to 60-80°C, the reaction is kept warm for 1-3 hours, and the modified phosphate ester is obtained by post-treatment.

5. A highly lubricating diesel antiwear agent according to claim 1, characterized in that: The preparation method of the modified inorganic lubricant is as follows: 10-20 parts of α-MnO2@CTS, 1-2 parts of bis(2-ethylhexyl) dithiophosphate, 40-50 parts of N,N-dimethylformamide and 0.5-0.8 parts of triethylamine are weighed by weight and added into a reactor, the temperature of the reactor is increased to 40-60°C, the reaction is kept warm for 2-4 hours, and the modified inorganic lubricant is obtained by post-treatment.

6. A highly lubricating diesel antiwear agent according to claim 5, characterized in that: The preparation method of α-MnO2@CTS is as follows: 20-30 parts of α-MnO2, 50-60 parts of carboxysuccinic acid powder and 800-1000 parts of anhydrous ethanol are weighed by weight and added into an ultrasonic instrument, and stirred for 8-12 hours while ultrasonicating at room temperature, the ultrasonic frequency is 20-40KHz, the stirring rate is 120-180rpm, and α-MnO2@CTS is obtained by post-treatment.

7. A high lubricity diesel anti-wear agent according to claim 6, characterized in that: The preparation method of α-MnO2 is as follows: 10-20 parts of potassium permanganate powder, 2-4 parts of potassium chloride powder, 0.5-0.8 parts of polyvinyl pyrrolidone with a molecular weight of 1200000-1300000 and 40-50 parts of deionized water are weighed by weight, added into a reactor and stirred, after the solid is completely dissolved, the temperature of the reactor is increased to 150-160°C, the reaction is kept warm for 8-12 hours, and α-MnO2 is obtained by post-treatment.

8. A highly lubricating diesel antiwear agent according to claim 1, characterized in that: The corrosion inhibitor is one or more of ferrous phosphate, benzothiadiazoline diphenol and mercaptodiethylamine, the antioxidant is one or more of di-tert-butyl-p-cresol, dibutylhydroquinone and diphenyl disulfide phosphate, and the viscosity index improver is polyisobutylene.

9. The method for preparing a highly lubricating diesel antiwear agent according to any one of claims 1 to 8, characterized in that: The method for preparing the high-lubricity diesel antiwear agent comprises the following steps: adding a modified organic lubricant and a modified inorganic lubricant into a reaction kettle, mixing them evenly, and passing the mixture through a 100-mesh sieve to obtain the diesel antiwear agent.

Citation Information

Patent Citations

  • Nanoparticle additives and lubricant formulations containing the nanoparticle additives

    CN101338244A

  • Stabilized blends containing friction modifiers

    CN103649279A

  • Copolymer disperser and fuel contg. it, and lubricant composition contg. it and use thereof

    CN1297026A

  • Lubricant composition for internal combustion engine

    JP2010126607A

  • Lubricating oil compositions and concentrates

    WO1990015124A1

Cited By

  • Environment-friendly additive for replacing phosphorus-chlorine anti-wear agent

    CN121674126A