Copper alloy and preparation method and application thereof
By setting abutment block and copper sheet on the plunger-connecting rod of the hydraulic motor, the wear of the hydraulic pressure on the inner wall of the cylinder bore is reduced, and the hydraulic motor is solved by the silica and carbon aerogel reinforcement materials in the copper alloy. The problem of short service life achieves higher mechanical properties and wear resistance.
Patent Information
- Application Number
- CN202410900415.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-11-01
Smart Images

Figure BDA0004930322340000051 
Figure BDA0004930322340000061 
Figure BDA0004930322340000062
Abstract
Description
Technical Field
[0001] The present application relates to the field of metal materials, and in particular to a copper alloy and a preparation method and application thereof. Background Art
[0002] The hydraulic motor is an actuator in the hydraulic system, which converts the liquid pressure energy provided by the hydraulic pump into the mechanical energy (torque and speed) of its output shaft.
[0003] Existing crankshaft-connecting rod hydraulic motors usually include a housing, an oil pan, an oil distribution pan, a plunger-connecting rod assembly and a crankshaft, wherein an odd number of cylinder holes is provided in the housing, and an odd number of plunger-connecting rod assemblies are also provided, the number of which matches the number of cylinder holes. The plungers in each plunger-connecting rod assembly are slidably arranged in each cylinder hole, and each plunger is provided with a ball socket. Each plunger cooperates with the ball head of the corresponding connecting rod through the ball socket to realize a ball joint connection between the two. The cylindrical surface at the bottom of each connecting rod contacts the eccentric wheel of the crankshaft. After assembly, multiple plunger-connecting rod assemblies are evenly distributed radially on the circumference of the crankshaft. The crankshaft is supported in the housing and the cover by bearings. One end of the crankshaft is connected to the oil distribution pan by a key, and the other end is used to connect the load.
[0004] In normal use, when the pressure oil enters the plunger cylinder from the oil pan through the oil distribution plate and the housing, the hydraulic pressure generated by the pressure oil acts on the top of the plunger. The hydraulic pressure points to the center of the eccentric wheel (that is, the center of the housing) along the center line of the connecting rod. The hydraulic pressure generates torque on the rotation center of the crankshaft, causing the crankshaft to rotate around the rotation center of the crankshaft, thereby achieving the purpose of converting hydraulic energy into mechanical energy and outputting speed and torque for the working machine. At the same time, the plunger will be subjected to the reaction force of the connecting rod. The combined force of the reaction force and the hydraulic pressure points vertically to the inner wall of the cylinder hole, that is, the lateral force. The lateral force is very harmful to the inner wall of the cylinder hole, which can easily cause the inner wall of the cylinder hole to wear too quickly and shorten the service life of the hydraulic cylinder. Summary of the invention
[0005] In order to solve the problem of hydraulic motor's service life being reduced due to excessive wear of the inner wall of the cylinder bore, the present application provides an application of copper alloy, which further avoids direct contact between the crankshaft and the abutment block by setting an abutment block on the plunger-connecting rod, and then opening an oil outlet hole and setting a copper sheet on the abutment block. This design can reduce the damage of lateral force to the inner wall of the cylinder bore, thereby improving the service life of the hydraulic motor.
[0006] In a first aspect, the present application provides an application of a copper alloy, using the following technical solution: An application of a copper alloy includes the following applications: The plunger-connecting rod is provided with an abutment block at the end of the connecting rod, a groove is provided on the side of the abutment block away from the connecting rod, an oil outlet hole is provided at the bottom of the groove, and a copper sheet is provided on the side of the abutment block away from the connecting rod, and the copper sheet is arranged along the circumference of the groove.
[0007] Through the above technical solution, when the crankshaft works on the plunger-connecting rod, high-pressure oil flows out from the oil outlet hole and gradually fills the groove in the entire abutment block, thereby forming a buffer layer composed of high-pressure oil between the crankshaft and the abutment block; in addition, the setting of the copper sheet further avoids direct contact between the crankshaft and the abutment block. Such a design can reduce the damage of lateral force to the inner wall of the cylinder hole, thereby increasing the service life of the hydraulic motor.
[0008] In a second aspect, the present application provides a copper alloy, which adopts the following technical solution: A copper alloy, used for being arranged on the abutment block, comprises the following components in parts by weight: 90 parts of copper, 4-7 parts of aluminum, 1-2 parts of silicon dioxide, and 1-3 parts of carbon aerogel.
[0009] By adopting the above technical solution, silicon dioxide has good thermal stability and chemical stability, and can form a bridge between copper element and carbon aerogel, reduce the interfacial tension between the two, and improve the compatibility between the two; Carbon aerogel has a high specific surface area and good mechanical properties. In copper alloys, carbon aerogel may help form a more uniform microstructure and enhance the hardness and wear resistance of the alloy. At the same time, as a nanoporous material, the uniform distribution of carbon aerogel in copper alloys can strengthen the matrix of the alloy, prevent the expansion of cracks, and increase the fracture toughness of the alloy. This strengthening effect helps to improve the yield strength and tensile strength of copper alloys. In addition, as a hard and brittle compound, silicon dioxide may play a role in enhancing the hardness of copper alloys. Its high hardness property helps to improve the wear resistance of copper alloys, making them more durable in the face of friction and wear. Silica particles may also act as a reinforcing phase, hindering grain boundary sliding and dislocation movement, thereby enhancing the yield strength and tensile strength of the alloy. The present application significantly improves the hardness, wear resistance, yield strength and tensile strength of the copper alloy by adding silicon dioxide and carbon aerogel to the copper alloy, which can effectively meet the high wear resistance requirements of the crankshaft for the copper sheet.
[0010] Preferably, the mass ratio of silicon dioxide to carbon aerogel is 1:1.2-1.4.
[0011] By adopting the above technical solution, when the content of carbon aerogel is too low, the effect of carbon aerogel on improving the mechanical properties and stability of copper alloy is not obvious; when the content of carbon aerogel is too high, it is difficult for carbon aerogel to be better compatible with copper through silica, but instead reduce the mechanical properties and stability of copper alloy; for this reason, the applicant finally determined after a lot of research and experimental verification that the silica and carbon aerogel of this application are preferably as above.
[0012] Preferably, the mass ratio of silicon dioxide to aluminum is 1:3-5.
[0013] By adopting the above technical solution, the performance of copper alloy can be enhanced by adding an appropriate amount of aluminum, but excessive aluminum may increase the brittleness and reduce the toughness of the alloy, and may induce phase transformation and microstructural inhomogeneity within the alloy, thereby reducing the mechanical properties and stability of the copper alloy.
[0014] In a third aspect, the present application provides a method for preparing a copper alloy, using the following technical solution: A method for preparing a copper alloy, used for preparing the above copper alloy, comprises the following steps: Ingot casting: The formulated amounts of copper, aluminum, silicon dioxide and carbon aerogel are added in sequence for smelting. After all the materials are smelted, they are refined and cast to obtain a primary processed ingot; Primary annealing: annealing the pre-treated ingot to obtain an annealed ingot; Hot rolling treatment: hot rolling the annealed ingot to obtain a hot-rolled plate; Secondary annealing: The hot-rolled sheet is subjected to secondary annealing to obtain a copper alloy.
[0015] By adopting the above technical scheme, by adding the formulated amounts of copper, aluminum, silicon dioxide and carbon aerogel in sequence for smelting, it can be ensured that the content of each element in the alloy reaches the preset value, thereby obtaining a copper alloy with stable performance; after the refining and casting of the primary ingot, and the subsequent annealing and hot rolling treatment, the grain structure of the alloy can be effectively improved, and its mechanical properties and stability can be improved; through hot rolling treatment and secondary annealing, the copper alloy can obtain better processing performance, which is convenient for subsequent cutting, stamping, welding and other process operations.
[0016] Preferably, before the ingredients are mixed for ingot casting, the silicon dioxide and carbon aerogel in the prescribed amounts are mixed in advance to obtain a premix, and then copper, aluminum and the premix are added in sequence for smelting.
[0017] By adopting the above technical scheme, by mixing silica and carbon aerogel into a premix in advance, it can be ensured that the two components are more evenly distributed in the copper-aluminum alloy during the subsequent smelting process; this helps to avoid local component segregation, thereby improving the uniformity and overall performance of the alloy; the preparation of the premix may cause a certain degree of pre-reaction or interaction between silica and carbon aerogel, which helps to improve the reaction efficiency in the subsequent smelting process and reduce smelting time and energy consumption.
[0018] Preferably, in the step of primary annealing, the annealing temperature is 750-850° C., and the annealing time is 2.5-3.5 h.
[0019] By adopting the above technical scheme, annealing treatment is carried out within this temperature and time range, which can effectively eliminate the internal stress generated by the copper alloy during the smelting and ingot casting process; the elimination of internal stress helps to prevent the alloy from cracking or deforming during subsequent processing or use, and improves the reliability and stability of the alloy; the appropriate primary annealing temperature and time can promote the grain growth in the copper alloy and make the grain structure more uniform and refined; this uniform grain structure helps to improve the mechanical and physical properties of the alloy, such as strength, hardness and toughness; the selected annealing temperature and time range avoids overburning that may be caused by excessively high temperature or excessively long time; overburning will destroy the grain structure of the alloy and lead to performance degradation; therefore, by precisely controlling the annealing temperature and time, it can be ensured that the alloy is unlikely to overburn during the annealing process.
[0020] Preferably, in the hot rolling step, the annealed ingot retains an oxide layer on the surface.
[0021] By adopting the above technical scheme, the oxide layer can serve as a protective layer to prevent further oxidation inside the ingot during hot rolling; in the high temperature environment of hot rolling, the metal easily reacts with oxygen in the air to form an oxide layer; if there is already an oxide layer on the surface of the ingot, it will act as a barrier to reduce the oxidation of the internal metal; the aluminum oxide in the oxide layer has good thermal and chemical stability, and can form a bridge between the copper element and the carbon aerogel, reducing the interfacial tension between the two and improving the compatibility between the two, thereby helping to optimize the mechanical properties of the copper alloy.
[0022] Preferably, in the hot rolling step, the hot rolling temperature is 750-850°C.
[0023] By adopting the above technical solution, the plasticity of the copper alloy is significantly improved within this temperature range while maintaining a certain strength; this makes the alloy more susceptible to plastic deformation during hot rolling, with better flow properties, which helps to obtain smoother and more uniform plates; although the hot rolling process is carried out at high temperatures, controlling the temperature at 750-850°C can avoid excessive oxidation of the alloy; excessively high temperatures will accelerate the oxidation process and may form an excessively thick oxide layer, which will not only affect the hot rolling effect, but may also affect the performance and quality of the final product; appropriate hot rolling temperatures can ensure that the alloy's organizational structure remains stable during the hot rolling process, avoiding excessively large grains or grain boundary changes; this helps to maintain the alloy's mechanical and physical properties, providing a good foundation for subsequent processing and use.
[0024] Preferably, in the secondary annealing step, the annealing temperature of the secondary annealing is 600-700° C., and the annealing time is 1.5-2.5 h.
[0025] By adopting the above technical solution, after the first annealing, although most of the internal stresses have been eliminated, some residual stresses may still remain in the material; the secondary annealing is carried out at a lower temperature, which can further release these residual stresses and ensure that the alloy has better stability during subsequent processing and use; during the secondary annealing process, the grain structure of the alloy will be further adjusted and optimized to make the structure more uniform; this helps to improve the mechanical and physical properties of the alloy; compared with the first annealing, the secondary annealing uses a lower temperature range, which can effectively avoid the risk of overburning of the alloy; at the same time, the lower temperature and appropriate annealing time can prevent excessive grain growth and maintain the fine grain structure of the alloy, which helps to maintain the good performance of the alloy.
[0026] In summary, this application has the following beneficial effects: 1. Since the present application further avoids direct contact between the crankshaft and the abutment block by arranging an abutment block on the plunger-connecting rod, and then opening an oil outlet hole and arranging a copper sheet on the abutment block, such a design can reduce the damage of the lateral force to the inner wall of the cylinder hole, thereby improving the service life of the hydraulic motor; 2. This application significantly improves the hardness, wear resistance, yield strength and tensile strength of the copper alloy by adding silicon dioxide and carbon aerogel to the copper alloy, which can effectively meet the high wear resistance requirements of the crankshaft for the copper sheet; 3. This application can effectively improve the grain structure of the copper alloy, improve its mechanical properties and stability through the initial refining and casting of the ingot, and subsequent annealing and hot rolling treatment. Through hot rolling treatment and secondary annealing, the copper alloy can obtain better processing performance, which is convenient for subsequent cutting, stamping, welding and other process operations. DETAILED DESCRIPTION
[0027] The raw materials in this application include the following parts: Copper: a commercial product with CAS No. 7440-50-8 was used; Aluminum: a commercially available product with CAS No. 7429-90-5 was used; Silicon dioxide: a commercially available product with CAS number 7631-86-9; Carbon aerogel: commercially available products; The present application is further described in detail below with reference to examples and comparative examples.
[0028] Example 1 A process for preparing a copper alloy comprises the following steps: Ingot making: 900 g copper, 60 g aluminum, 15 g silicon dioxide and 20 g carbon aerogel are added in sequence and smelted at 1250° C., and then refined and cast at 1300° C. to obtain an ingot; Primary annealing: annealing the primary treated ingot at a temperature of 800° C. for 3 h to obtain an annealed ingot; Hot rolling treatment: removing the oxide layer on the surface of the annealed ingot, and then performing hot rolling treatment, in the hot rolling treatment step, the hot rolling temperature of the hot rolling treatment is 800° C., to obtain a hot-rolled plate; Secondary annealing: The hot-rolled plate is subjected to secondary annealing, the annealing temperature of the secondary annealing is 650°C, the annealing time is 2h, and the copper alloy is obtained.
[0029] Example 2-3 Example 2-3 Based on the preparation method of Example 1, the formula amount of each component of the copper alloy is adjusted, and the specific adjustment is shown in Table 1.
[0030] Comparative Examples 1-3 Comparative Example 1 is based on the preparation method of Example 1, without adding carbon aerogel, and the specific adjustments are shown in Table 1.
[0031] Comparative Example 2 is based on the preparation method of Example 1, without adding silicon dioxide, and the specific adjustments are shown in Table 1.
[0032] Comparative Example 3 Comparative Example 3 is based on the preparation method of Example 1, without adding carbon aerogel and silicon dioxide, and the specific adjustments are shown in Table 1.
[0033] Table 1 Formula amount and performance test table of each component of Examples 1-3 and Comparative Examples 1-3 Performance testing The copper alloys of Examples 1-3 and Comparative Examples 1-3 were subjected to the following performance tests, and the test results are shown in Table 1: 1. Wear resistance According to GB / T 35083.1-2018 standard, the wear amount of copper alloy was measured at 300°C, rotation speed 2400r / min, contact load 1N, and friction time 60min. The lower the wear amount, the greater the wear resistance.
[0034] 2. Hardness The copper alloy is tested for hardness using a Rockwell hardness tester with a test load of 150kg. The higher the hardness value, the better.
[0035] 3. Yield strength and tensile strength According to GB / T228.1-2010, the tensile speed is 2mm / min, and the yield strength and tensile strength of the copper alloy are tested. The higher the yield strength and tensile strength values, the better.
[0036] Referring to Table 1, by comparing Examples 1-3 and Comparative Examples 1-3, it can be seen that compared with Comparative Examples 1-3, the hardness, yield strength and tensile strength of Examples 1-3 are much higher than those of Comparative Examples 1-3, and the wear amount of the copper alloy is less than that of Comparative Examples 1-3, indicating that the addition of carbon aerogel to the copper alloy can improve the wear resistance, hardness, yield strength and tensile strength of the copper alloy, and the addition of silicon dioxide to the copper alloy while adding carbon aerogel can greatly improve the wear resistance, hardness, yield strength and tensile strength of the copper alloy; compared with Examples 1-3, Example 1 has the best performance, so Example 1 is preferred over Examples 1-3.
[0037] Embodiment 4-5 Example 4-5 Based on the preparation method of Example 1, the mass ratio of silicon dioxide to carbon aerogel is adjusted, and the specific adjustment is shown in Table 2.
[0038] Comparative Examples 4-5 Comparative Example 4-5 Based on the preparation method of Example 1, the mass ratio of silicon dioxide to carbon aerogel was adjusted, and the specific adjustment is shown in Table 2.
[0039] The copper alloys of Examples 4-5 and Comparative Examples 4-5 were subjected to the above performance tests, and the test results are shown in Table 2.
[0040] Table 2 Mass ratio of silicon dioxide to carbon aerogel and performance test table of Example 1, Examples 4-5 and Comparative Examples 4-5 Referring to Table 2, by comparing Example 1, Examples 4-5 and Comparative Examples 4-5, it can be seen that as the mass ratio of silica to carbon aerogel continues to increase, the hardness, yield strength and tensile strength of the copper alloy show a trend of first increasing and then decreasing, and the wear amount of the copper alloy shows a trend of first decreasing and then increasing. This may be because as the mass ratio of silica to carbon aerogel continues to increase, the carbon aerogel continuously improves the mechanical properties of the copper alloy and improves the wear resistance of the copper alloy; when it exceeds a certain range, it is difficult for the carbon aerogel to better be compatible with aluminum through the silica element, but instead reduces the mechanical properties of the copper alloy and reduces the wear resistance of the copper alloy.
[0041] Embodiment 6-7 In Example 6-7, based on the preparation method of Example 1, the mass ratio of silicon dioxide to aluminum was adjusted, and the specific adjustment is shown in Table 3.
[0042] Comparative Examples 6-7 Comparative Example 6-7 is based on the preparation method of Example 1, and the mass ratio of silicon dioxide to aluminum is adjusted. The specific adjustment is shown in Table 3.
[0043] The copper alloys of Examples 6-7 and Comparative Examples 6-7 were subjected to the above performance tests, and the test results are shown in Table 3.
[0044] Table 3 Mass ratio of silicon dioxide to aluminum and performance test table of Example 1, Examples 6-7 and Comparative Examples 6-7 project Example 1 Example 6 Example 7 Comparative Example 6 Comparative Example 7 Quality Ratio 1:4 1:3 1:5 1:2 1:6 Wear amount / g 0.51 0.93 0.76 1.12 0.99 Hardness / HRC 45.3 41.3 43.8 39.3 42.3 Yield strength / MPa 1062 1035 1052 1020 1038 Tensile strength / MPa 1235 1189 1216 1165 1194 Referring to Table 3, by comparing Example 1, Examples 6-7 and Comparative Examples 6-7, it can be seen that as the mass ratio of silicon dioxide to aluminum continues to increase, the hardness, yield strength and tensile strength of the copper alloy show a trend of first increasing and then decreasing, and the wear amount of the copper alloy shows a trend of first decreasing and then increasing. This may be because as the mass ratio of silicon dioxide to aluminum continues to increase, aluminum continues to improve the mechanical properties of the copper alloy and improves the wear resistance of the copper alloy; when it exceeds a certain range, aluminum may cause the alloy to become more brittle and less tough, and may induce phase change and microstructural inhomogeneity within the alloy, which in turn reduces the mechanical properties of the copper alloy and reduces the wear resistance of the copper alloy.
[0045] Embodiment 8-11 In Example 8-9, based on the preparation method of Example 1, the primary annealing temperature is adjusted, and the specific adjustment is shown in Table 4.
[0046] In Examples 10-11, based on the preparation method of Example 1, the time of the first annealing treatment is adjusted, and the specific adjustment is shown in Table 5.
[0047] Comparative Examples 8-11 In Comparative Examples 8-9, based on the preparation method of Example 1, the primary annealing temperature was adjusted, and the specific adjustment is shown in Table 4.
[0048] In Comparative Examples 10-11, based on the preparation method of Example 1, the time of the first annealing treatment was adjusted, and the specific adjustment is shown in Table 5.
[0049] The copper alloys of Examples 8-11 and Comparative Examples 8-11 were subjected to the above performance tests, and the test results are shown in Tables 4-5, respectively.
[0050] Table 4 Primary annealing temperature and performance test table of Example 1, Examples 8-9 and Comparative Examples 8-9 project Example 1 Example 8 Example 9 Comparative Example 8 Comparative Example 9 One annealing / ℃ 800 750 850 700 900 Wear amount / g 0.51 0.95 0.81 1.13 1.06 Hardness / HRC 45.3 41.1 43.6 39.2 41.8 Yield strength / MPa 1062 1034 1050 1019 1034 Tensile strength / MPa 1235 1187 1213 1164 1188 Table 5: Primary annealing time and performance test table of Example 1, Examples 10-11 and Comparative Examples 10-11 Referring to Table 4-5, by comparing Example 1, Examples 8-11 and Comparative Examples 8-11, it can be seen that as the primary annealing temperature continues to increase, the hardness, yield strength and tensile strength of the copper alloy show a trend of first increasing and then decreasing, and the wear amount of the copper alloy shows a trend of first decreasing and then increasing. This may be because as the primary annealing temperature continues to increase, the internal stress generated by the copper alloy during the smelting and ingot casting process is gradually eliminated, and the grain growth in the copper alloy is gradually promoted, making the grain structure more uniform and refined, thereby improving the wear resistance, hardness, yield strength and tensile strength of the copper alloy; however, when it exceeds a certain range, some overburning may occur in the copper alloy, which will destroy the grain structure of the alloy and reduce the wear resistance of the copper alloy. Abrasiveness, hardness, yield strength and tensile strength; with the continuous increase of the primary annealing time, the hardness, yield strength and tensile strength of the copper alloy show a trend of first increasing and then decreasing, and the wear amount of the copper alloy shows a trend of first decreasing and then increasing. This may be because as the primary annealing time continues to increase, the internal stress generated by the copper alloy during the smelting and ingot casting process is gradually eliminated, and the grain growth in the copper alloy is gradually promoted, making the grain structure more uniform and refined, thereby improving the wear resistance, hardness, yield strength and tensile strength of the copper alloy; but when it exceeds a certain range, some overburning may occur in the copper alloy, which will destroy the grain structure of the alloy and reduce the wear resistance, hardness, yield strength and tensile strength of the copper alloy.
[0051] Examples 12-13 In Examples 12-13, based on the preparation method of Example 1, the hot rolling temperature is adjusted, and the specific adjustments are shown in Table 6.
[0052] Comparative Examples 12-13 In Comparative Examples 12-13, based on the preparation method of Example 1, the hot rolling temperature was adjusted, and the specific adjustments are shown in Table 6.
[0053] The copper alloys of Examples 12-13 and Comparative Examples 12-13 were subjected to the above performance tests, and the test results are shown in Table 6.
[0054] Table 6 Hot rolling temperature and performance test table of Example 1, Examples 12-13 and Comparative Examples 12-13 Referring to Table 6, by comparing Example 1, Examples 12-13 and Comparative Examples 12-13, it can be seen that as the hot rolling temperature continues to increase, the hardness, yield strength and tensile strength of the copper alloy show a trend of first increasing and then decreasing, and the wear amount of the copper alloy shows a trend of first decreasing and then increasing. This may be because as the hot rolling temperature continues to increase, the copper alloy is more susceptible to plastic deformation and has better fluidity. The microstructure of the copper alloy gradually remains stable during the hot rolling process, thereby improving the wear resistance, hardness, yield strength and tensile strength of the copper alloy; however, when it exceeds a certain range, some excessive oxidation may occur in the copper alloy, forming an excessively thick oxide layer. In addition, too high a temperature may make it difficult for the microstructure of the alloy to remain stable during the hot rolling process, resulting in excessive grain or grain boundary changes, thereby reducing the wear resistance, hardness, yield strength and tensile strength of the copper alloy.
[0055] Examples 14-17 In Examples 14-15, based on the preparation method of Example 1, the secondary annealing temperature is adjusted, and the specific adjustment is shown in Table 7.
[0056] In Examples 16-17, based on the preparation method of Example 1, the secondary annealing time is adjusted, and the specific adjustment is shown in Table 8.
[0057] Comparative Examples 14-17 In Comparative Examples 14-15, based on the preparation method of Example 1, the secondary annealing temperature was adjusted, and the specific adjustment is shown in Table 7.
[0058] In Comparative Examples 16-17, based on the preparation method of Example 1, the secondary annealing time was adjusted, and the specific adjustments are shown in Table 8.
[0059] The copper alloys of Examples 14-17 and Comparative Examples 14-17 were subjected to the above performance tests, and the test results are shown in Tables 7-8.
[0060] Table 7 Secondary annealing temperature and performance test table of Example 1, Examples 14-15 and Comparative Examples 14-15 project Example 1 Embodiment 14 Embodiment 15 Comparative Example 14 Comparative Example 15 Secondary annealing temperature / ℃ 650 600 700 550 750 Wear amount / g 0.51 0.86 0.67 0.98 0.87 Hardness / HRC 45.3 42.0 44.4 40.6 43.0 Yield strength / MPa 1062 1039 1055 1029 1044 Tensile strength / MPa 1235 1197 1223 1181 1205 Table 8 Secondary annealing time and performance test table of Example 1, Examples 16-17 and Comparative Examples 16-17 project Example 1 Example 16 Embodiment 17 Comparative Example 16 Comparative Example 17 Secondary annealing time / h 2 1.5 2.5 1 3 Wear amount / g 0.51 0.82 0.64 0.96 0.85 Hardness / HRC 45.3 42.4 44.5 40.8 43.1 Yield strength / MPa 1062 1042 1057 1031 1045 Tensile strength / MPa 1235 1201 1225 1183 1206 Referring to Tables 7-8, by comparing Example 1, Examples 14-17 and Comparative Examples 14-17, it can be seen that as the secondary annealing temperature continues to increase, the hardness, yield strength and tensile strength of the copper alloy show a trend of first increasing and then decreasing, and the wear amount of the copper alloy shows a trend of first decreasing and then increasing. This may be because as the secondary annealing temperature continues to increase, the secondary annealing can further release these residual stresses, and the grain structure of the copper alloy will be further adjusted and optimized, making the organization more uniform, thereby improving the wear resistance, hardness, yield strength and tensile strength of the copper alloy; but when it exceeds a certain range, the grains in the copper alloy grow excessively, it is difficult to maintain the fine grain structure of the alloy, and the wear resistance, hardness, yield strength and tensile strength of the copper alloy are reduced; As the secondary annealing time continues to increase, the hardness, yield strength and tensile strength of the copper alloy show a trend of first increasing and then decreasing, and the wear amount of the copper alloy shows a trend of first decreasing and then increasing. This may be because as the secondary annealing time continues to increase, the secondary annealing can further release these residual stresses, and the grain structure of the copper alloy will be further adjusted and optimized, making the structure more uniform, thereby improving the wear resistance, hardness, yield strength and tensile strength of the copper alloy; but when it exceeds a certain range, the grains in the copper alloy grow excessively, it is difficult to maintain the fine-grained structure of the alloy, and the wear resistance, hardness, yield strength and tensile strength of the copper alloy are reduced.
[0061] Examples 18-19 Example 18 Based on the preparation method of Example 1, before the ingredients are cast into ingots, 15g of silica and 20g of carbon aerogel are mixed in advance to obtain a premix, and then 900g of copper, 60g of aluminum and 35g of the premix are added in sequence for smelting.
[0062] Example 19 is based on the preparation method of Example 1. In the hot rolling step, the annealed ingot retains the oxide layer on the surface for hot rolling.
[0063] The copper alloys of Examples 18-19 were subjected to the above performance tests, and the test results are shown in Table 9.
[0064] Table 9 Performance test table of Example 1 and Examples 18-19 project Example 1 Embodiment 18 Embodiment 19 Wear amount / g 0.51 0.46 0.43 Hardness / HRC 45.3 45.8 46.1 Yield strength / MPa 1062 1065 1067 Tensile strength / MPa 1235 1240 1244 Referring to Table 9, by comparing Example 1 with Examples 18-19, it can be seen that the hardness, yield strength and tensile strength of the copper alloy of Example 18 are higher than those of Example 1, and the wear loss is lower than that of Example 1, indicating that mixing silica and carbon aerogel into a premix in advance can ensure that the two components are more evenly distributed in the copper-aluminum alloy during the subsequent smelting process, which helps to avoid local component segregation and can further improve the wear resistance, hardness, yield strength and tensile strength of the copper alloy; The hardness, yield strength and tensile strength of the copper alloy of Example 19 are higher than those of Example 1, and the wear amount is lower than that of Example 1. This may be because alumina has good thermal stability and chemical stability, and can form a bridge between the copper element and the carbon aerogel, reducing the interfacial tension between the two, and improving the compatibility between the two, which can further improve the wear resistance, hardness, yield strength and tensile strength of the copper alloy.
[0065] Application Examples The plunger-connecting rod is provided with an abutment block at the end of the connecting rod, a groove is provided on the side of the abutment block away from the connecting rod, an oil outlet hole is provided at the bottom of the groove, and a copper sheet is provided on the side of the abutment block away from the connecting rod, and the copper sheet is arranged along the circumference of the groove.
[0066] This application further avoids direct contact between the crankshaft and the abutment block by setting an abutment block on the plunger-connecting rod, and then opening an oil outlet hole and setting a copper sheet on the abutment block. This design can reduce the damage of lateral force to the inner wall of the cylinder hole, thereby increasing the service life of the hydraulic motor.
[0067] In addition, the copper alloy of the present application can be used in any field that requires a copper sheet with high wear resistance.
[0068] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. An application of a copper alloy, characterized in that: The invention comprises the following applications: a plunger-connecting rod is provided with an abutment block at the end of the connecting rod, a groove is provided on the side of the abutment block away from the connecting rod, an oil outlet hole is provided at the bottom of the groove, a copper sheet is provided on the side of the abutment block away from the connecting rod, and the copper sheet is arranged along the circumference of the groove.
2. A copper alloy, characterized in that: The method comprises applying to the abutment block as claimed in claim 1, comprising the following components in parts by weight: 90 parts of copper, 4-7 parts of aluminum, 1-2 parts of silicon dioxide, and 1-3 parts of carbon aerogel.
3. The copper alloy according to claim 2, characterized in that: The mass ratio of the silicon dioxide to the carbon aerogel is 1:1.2-1.
4.
4. The copper alloy according to claim 2, characterized in that: The mass ratio of silicon dioxide to aluminum is 1:3-5.
5. The method for preparing the copper alloy according to any one of claims 2 to 4, characterized in that: The following steps are involved: Ingot casting: The formulated amounts of copper, aluminum, silicon dioxide and carbon aerogel are added in sequence for smelting. After all the materials are smelted, they are refined and cast to obtain a primary processed ingot; Primary annealing: annealing the primary treated ingot to obtain an annealed ingot; Hot rolling treatment: hot rolling the annealed ingot to obtain a hot-rolled plate; Secondary annealing: The hot-rolled sheet is subjected to secondary annealing to obtain a copper alloy.
6. The method for preparing the copper alloy according to claim 5, characterized in that: Before the ingredients are prepared for ingot casting, the silicon dioxide and carbon aerogel in the prescribed amounts are mixed in advance to obtain a premix, and then copper, aluminum and the premix are added in sequence for smelting.
7. The method for preparing the copper alloy according to claim 5, characterized in that: In the step of primary annealing, the annealing temperature of the primary annealing is 750-850° C., and the annealing time is 2.5-3.5 hours.
8. The method for preparing the copper alloy according to claim 5, characterized in that: During the hot rolling process, the annealed ingot retains an oxide layer on the surface.
9. The method for preparing the copper alloy according to claim 5, characterized in that: In the step of hot rolling treatment, the hot rolling temperature of the hot rolling treatment is 750-850°C.
10. The method for preparing the copper alloy according to claim 5, characterized in that: In the step of secondary annealing, the annealing temperature of the secondary annealing is 600-700° C., and the annealing time is 1.5-2.5 hours.