High-thermal-conductivity and high-strength Al-Si-Mg-Cu-Sb-Fe alloy and preparation method thereof

Through high and low temperature cycle aging treatment and the addition of Ag and Ho elements, the Al-Si-Mg-Cu-Sb-Fe alloys are solved, and the casting performance with high thermal conductivity and high strength is achieved. In the manufacture of heat dissipation and structural parts.

CN118880128APending Publication Date: 2024-11-01中力鸿(惠州)新材料科技有限公司
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410970929.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

There is a contradiction between the improvement of thermal conductivity and mechanical properties of existing aluminum alloys, resulting in the problems of low thermal conductivity, insufficient strength and elongation.

Method used

The Al-Si-Mg-Cu-Sb-Fe alloy, which is treated with high and low temperature cycle aging, forms a nano-sized reinforced phase by adding transition elements Ag and rare earth element Ho, optimizes the microstructure of the alloy and improves thermal conductivity and mechanical properties.

Benefits of technology

Significantly improves the thermal conductivity and mechanical properties of the alloy, the tensile strength, yield strength and thermal conductivity reach ≥190W/(m·K) and ≥250MPa, with an elongation of ≥20%. It is suitable for heat dissipation parts and structural parts, and improves high temperatures. Service performance and efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880128A_ABST
    Figure CN118880128A_ABST
Patent Text Reader

Abstract

The invention discloses a high-thermal-conductivity and high-strength Al-Si-Mg-Cu-Sb-Fe alloy, which is prepared from the following components in percentage by mass: 4.0 to 6.0 percent of Si, 0.9 to 1.1 percent of Mg, 0.5 to 0.6 percent of Cu, 0.05 to 0.3 percent of Sb, 0.2 to 0.3 percent of Fe, 0.05 to 0.1 percent of Ag, 0.05 to 0.1 percent of Ho and the balance of Al. The cast Al-Si-Mg-Cu-Sb-Fe alloy containing the transition element Ag and the rare earth Ho is provided for solving the problems that an existing aluminum alloy is low in heat conductivity, contradictory in strength and heat conductivity and the like, and the cast Al-Si-Mg-Cu-Sb-Fe alloy is high in strength and excellent in heat conductivity and can be used for various shells, structural parts and heat dissipation parts. The problems of serious heating, insufficient high-temperature service performance, low use efficiency and the like caused by insufficient heat dissipation of electronic communication equipment are effectively avoided, and meanwhile, the mechanical property and the heat-conducting property of the alloy are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of aluminum alloy development, and specifically relates to a high thermal conductivity and high strength Al-Si-Mg-Cu-Sb-Fe alloy and a preparation method thereof. Background Art

[0002] With the development of the new energy vehicle industry and the 5G communication industry, computing power has been unprecedentedly improved, which requires heat dissipation components to have better thermal conductivity. At the same time, in order to reduce the volume of the heat dissipation components themselves, higher mechanical properties are required for the materials. During the manufacturing process of heat dissipation components, due to their complex and special shapes, casting processes are generally used, so the materials are required to have good casting properties.

[0003] The thermal conductivity of aluminum is 237W / (m·K), second only to silver, copper, and gold. Although the thermal conductivity of pure aluminum is relatively high at room temperature, its mechanical properties and casting properties are relatively poor, making it unsuitable for direct use in product manufacturing. Adding alloying elements can improve the mechanical properties and casting properties of aluminum alloys. Si is widely distributed in nature, and this element can greatly improve the mechanical properties and casting properties of aluminum alloys. Therefore, Al-Si alloys are the most commonly used cast aluminum alloys. Cast Al-Si alloys are ideal materials for manufacturing heat dissipation structures on new energy vehicle batteries and 5G communication equipment.

[0004] Alloying elements are the most basic factors affecting the thermal conductivity of metals. The biggest role of Si in aluminum-silicon alloys is to increase fluidity and reduce solidification shrinkage. However, if Si is not modified, the primary Si crystals usually appear in coarse blocks, and the eutectic silicon appears in coarse needles. The lattice distortion caused by silicon in the solid solution state and the splitting of the matrix by eutectic silicon lead to a decrease in thermal conductivity. Mg can increase the yield strength of the alloy, but Mg is more likely to dissolve in the Al matrix, increasing the degree of lattice distortion of the alloy and reducing the thermal conductivity of the alloy. At the same time, the coarse primary Mg2Si crystals generated will also increase the scattering of electrons. Cu can significantly improve the fluidity, strength and hardness of the alloy and improve the mechanical properties of the alloy, but Cu is easily dissolved in the Al matrix, causing lattice distortion of the alloy, and Cu can refine the grains and increase grain boundaries, both of which increase the probability of electrons being scattered and reduce the thermal conductivity of the alloy. Adding a certain amount of Fe can reduce the tendency of castings to stick to the mold. In addition, since the Fe element has less effect on the thermal conductivity of pure aluminum than the Si element, adding an appropriate amount of Fe to the Al-Si alloy to form an Al-Fe-Si phase can appropriately reduce the solid solubility of Si in Al, thereby reducing the adverse effect of Si on the thermal conductivity of the aluminum alloy.

[0005] CN117888007A discloses a high-strength, high-electrical and high-thermal-conductivity aluminum alloy, the composition by mass percentage is: Si 0.3-0.5%, Mg 0.4-0.6%, Cu 0.02-0.05%, Mn 0.02-0.5%, Ti 0.01-0.015%, B 0.002-0.003%, Fe 0.1-0.3%, the balance is Al and unavoidable impurity elements, a single impurity ≤ 0.05%, a total impurity ≤ 0.15%, room temperature tensile strength ≥ 250MPa, yield strength ≥ 210MPa, elongation after fracture ≥ 12%, 20℃ resistivity ≤ 0.03Ω·mm 2 / m, electrical conductivity ≥57.5%IACS, thermal conductivity ≥195W / (m·K).

[0006] CN118127384A discloses a high thermal conductivity aluminum alloy of Al-Si-Fe-Mg series, containing 5-8% Si, 0.4-0.8% Fe, 0.001-0.05% Cu, 0.05-0.4% Mg, 0.005-0.04% Sr, 0.001-0.05% Zn, 0.001-0.05% Ni, 0-0.1% Co, 0-0.01% Be, 0.0001-0.1% Re, with a thermal conductivity greater than 200 W / (m·K), a yield strength greater than 130Mpa, and an elongation greater than 16%. Current research has improved the thermal conductivity of aluminum alloys through current heat treatment methods, but due to the contradiction between the thermal conductivity and mechanical properties of the alloy, the problems of low strength and elongation of the alloy have not been effectively solved. Summary of the invention

[0007] The object of the present invention is to overcome at least one disadvantage of the prior art and to provide a high thermal conductivity and high strength cast Al-Si-Mg-Cu-Sb-Fe alloy and a preparation method thereof.

[0008] The technical solution adopted by the present invention is: In a first aspect, the present invention provides a high thermal conductivity and high strength Al-Si-Mg-Cu-Sb-Fe alloy, which comprises the following composition, in mass percentage: Si 4.0-6.0%, Mg 0.9-1.1%, Cu 0.5-0.6%, Sb 0.05-0.3%, Fe 0.2-0.3%, Ag 0.05-0.1%, Ho 0.05-0.1%, and the balance is Al.

[0009] In some examples, the mass percentage content of Si is 5.0-6.0%.

[0010] In some examples, the mass percentage of Sb is 0.05-0.1%.

[0011] In some examples, the high thermal conductivity and high strength Al-Si-Mg-Cu-Sb-Fe alloy further contains ≤0.1% of unavoidable impurity elements.

[0012] In some examples, the high thermal conductivity and high strength Al-Si-Mg-Cu-Sb-Fe alloy has a tensile strength of ≥400 MPa, a yield strength of ≥250 MPa, an elongation after fracture of ≥20%, and a thermal conductivity of ≥190 W / (m·K).

[0013] In a second aspect, the method for preparing the Al-Si-Mg-Cu-Sb-Fe alloy provided in the first aspect of the present invention comprises the following steps: 1) Weighing raw materials according to alloy composition and smelting to obtain alloy ingots; 2) Taking the alloy ingot prepared in step 1), performing high and low temperature cycle aging treatment to obtain the high thermal conductivity and high strength Al-Si-Mg-Cu-Sb-Fe alloy.

[0014] In some examples, the high and low temperature cycle aging treatment steps are: first high temperature aging treatment at 220-230°C for 2-3 hours, then cooling to -50--40°C, keeping warm for 1-2 hours, and then cycling this operation.

[0015] In some examples, the single cycle time of the high and low temperature cyclic aging treatment is 3 to 5 hours.

[0016] In some examples, the high and low temperature cyclic aging treatment has a cycle frequency of 12 to 16 times.

[0017] In some examples, the total time of the high and low temperature cycle aging is 60 to 80 h.

[0018] The beneficial effects of the present invention are: In view of the problems of low thermal conductivity, contradiction between strength and thermal conductivity of existing aluminum alloys, the present invention invents a cast Al-Si-Mg-Cu-Sb-Fe alloy containing transition element Ag and rare earth Ho. The alloy has high strength and excellent thermal conductivity and can be used for various shells, structural parts, and heat dissipation parts. It effectively avoids the problems of severe heating, insufficient high-temperature service performance, reduced use efficiency, etc. caused by insufficient heat dissipation of electronic communication equipment, and at the same time improves the mechanical and thermal conductivity of the alloy.

[0019] The Si content in the high thermal conductivity and high strength cast Al-Si-Mg-Cu-Sb-Fe alloy of the present invention is preferably 5.0-6.0%. In aluminum alloys, Si can increase the fluidity of molten alloys and reduce solidification shrinkage, but for thermally conductive aluminum alloys, due to lattice distortion caused by silicon in solid solution and the splitting of the matrix by eutectic silicon, the thermal conductivity decreases as the Si content increases.

[0020] The high thermal conductivity and high strength cast Al-Si-Mg-Cu-Sb-Fe alloy of the present invention mainly contains α-Al, eutectic Si, α-Al8Fe2Si, β-Al5FeSi, π-Al8Si6Mg3Fe, β-Mg2Si, Q-Al5Cu2Mg8Si6 and θ-Al2Cu phases. After high temperature aging treatment, the eutectic Si particles are fragmented, spheroidized and partially dissolved, and the Q, θ and β-Mg2Si phases are completely dissolved in the Al matrix. Due to the strong interaction between Mg and Cu atoms, Cu can be incorporated into Mg-Si clusters and refine these clusters, resulting in accelerated precipitation kinetics. Secondly, the addition of Cu promotes the formation of quaternary Q phase and its precursor (Q' phase) during the aging process. At the same time, the formation of nano-sized θ' phase can further improve the hardening potential of the alloy. After aging treatment, the precipitation of Mg and Cu atoms reduces the degree of lattice distortion and reduces the scattering of electrons, thereby improving the thermal conductivity of the alloy. The formation of a large number of nano-sized Q' and θ' phases also significantly improves the mechanical properties of the alloy.

[0021] The Sb content in the high thermal conductivity and high strength cast Al-Si-Mg-Cu-Sb-Fe alloy of the present invention is preferably: 0.05-0.1%. Sb can effectively modify α-Al and eutectic silicon, and improve the mechanical properties of the alloy. This improvement can be attributed to the transformation of coarse dendrite α-Al grains into refined equiaxed grains, and the secondary dendrite arm spacing (SDAS) gradually decreases. Sb reacts with Al to form AlSb compounds, which are adsorbed around eutectic silicon to reduce the growth temperature of eutectic Si, thereby inhibiting its growth and refinement. The eutectic silicon changes from coarse flakes before modification to fine needles.

[0022] The Ag element is added to the high thermal conductivity and high strength cast Al-Si-Mg-Cu-Sb-Fe alloy of the present invention. When the Ag addition amount is 0.05-0.1%, silver acts as a nucleation particle to promote the precipitation of Mg and Si, and reduce the scattering effect of the distortion stress field on electrons. During the cyclic aging treatment, the high-temperature aging treatment accelerates the precipitation of the β-Mg2Si phase, thereby improving the hardening strength of the alloy. The low-temperature aging treatment is performed by rapidly cooling the temperature to inhibit the coarsening of the Mg2Si phase, thereby improving the yield strength and tensile strength of the alloy.

[0023] Ho element is added to the high thermal conductivity and high strength cast Al-Si-Mg-Cu-Sb-Fe alloy of the present invention. When the Ho addition amount is 0.05-0.1%, the rare earth Ho has the refining and purification effects, so that the alloy casting defects are significantly reduced, and the grain boundaries that are continuously distributed in a network are changed into discontinuous islands and fishbone shapes, which reduces the scattering effect on electron phonons and has a favorable effect on the thermal conductivity of the alloy; secondly, the rare earth Ho also has a metamorphic effect, and as a nucleation particle of the precipitated phase, it promotes the formation of the Q' phase, which is an important strengthening phase, thereby improving the mechanical properties of the alloy. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is the metallographic microstructure diagram of the Al-Si-Mg-Cu-Sb-Fe alloy prepared in Example 1 of the present invention.

[0025] Figure 2 This is the SEM microstructure image of the Al-Si-Mg-Cu-Sb-Fe alloy prepared in Example 1 of the present invention.

[0026] Figure 3 This is the SEM microstructure diagram of the Al-Si-Mg-Cu-Sb-Fe alloy prepared in Example 7 of the present invention. DETAILED DESCRIPTION

[0027] The following disclosure provides many different embodiments or examples for implementing different solutions of the present invention.

[0028] The present invention is described in detail below in conjunction with examples, comparative examples and experimental data, but is not intended to identify the key or decisive elements of the present invention or to limit the scope of protection.

[0029] The chemical composition of the alloy in each embodiment is as follows: Si 4.0-6.0%, Mg 0.9-1.1%, Cu 0.5-0.6%, Sb 0.05-0.3%, Fe 0.2-0.3%, Ag 0.05-0.1%, Ho 0.05-0.1%. The raw materials are pure Al, Mg ingots, Al-30Si, Al-50Cu, Al-10Sb, Al-10Fe, Al-10Ag, Al-10Ho master alloys.

[0030] The compositions of the embodiments and comparative examples are shown in Table 1.

[0031] Table 1 Chemical composition of the embodiments and comparative examples (mass percentage)

[0032] The preparation methods of each embodiment and comparative example are as follows: 1) Raw material preparation: weigh pure Al and Mg ingots, Al-30Si, Al-50Cu, Al-10Sb, Al-10Fe, Al-10Ag, and Al-10Ho master alloys in proportion as raw materials for smelting.

[0033] 2) Melting and casting: taking the aluminum, magnesium ingots and aluminum master alloy prepared in step 1), putting them into a melting furnace, heating and melting, stirring evenly after removing slag, refining with protective gas, standing and filtering after removing slag, casting, and obtaining alloy ingots; 3) Aging treatment: taking the alloy ingot prepared in step 2), and performing high-low temperature cycle aging treatment to obtain the high thermal conductivity and high strength cast Al-Si-Mg-Cu-Sb-Fe alloy.

[0034] During the smelting process, a covering agent and a degassing agent may be added. The covering agent and the degassing agent are commonly used in the art, and the mass ratio of the covering agent to the smelting ingredients is (1-3):100. The composition of the covering agent includes: KCl+ NaCl, mass fraction 1:1; the mass ratio of the degassing agent to the smelting ingredients is 1:100, and the degassing agent is hexachloroethane. The covering agent and the degassing agent themselves have little effect on the properties of the alloy.

[0035] Preferably, the smelting temperature is 740°C to 750°C; the refining temperature is 680°C to 710°C; and the casting temperature is 710°C to 730°C.

[0036] Preferably, the high-temperature aging treatment temperature is 220-230° C., and the insulation time is 2-3 hours; the low-temperature aging treatment temperature is -50--40° C., and the insulation time is 1-2 hours, which is one cycle.

[0037] Preferably, the high-low temperature cyclic aging treatment is performed for 12 to 16 cycles, and the total aging time is 60 to 80 hours.

[0038] The high and low temperature cycle aging treatment parameters of each embodiment and comparative example are shown in Table 2.

[0039] Table 2 High and low temperature cycle aging treatment parameters of the examples and comparative examples

[0040] Comparison of properties of different Al-Si-Mg-Cu-Sb-Fe alloys The alloys obtained in the examples and comparative examples were tested for thermal conductivity and mechanical properties. The thermal conductivity was tested according to GB / T 34482-2017; the strength and elongation test methods were determined according to GB / T 228.1-2010 "Metallic Materials Tensile Test Part 1: Room Temperature Test Method". The performance test results of each example and comparative example are shown in Table 3.

[0041] Table 3 Performance test results of various embodiments and comparative examples

[0042] It can be seen from Table 3 that the tensile strength and thermal conductivity of the aluminum alloys prepared in Examples 7 and 8 are better than those prepared in Comparative Example 2, and the composition of the aluminum alloys in Examples 7 and 8 is similar or almost the same as that of the aluminum alloy in Comparative Example 2, except that Comparative Example 2 did not undergo high and low temperature cyclic aging treatment. In the high temperature aging treatment stage, β-Mg2Si, Q' and θ' phases are precipitated by aging. After the high temperature aging treatment, the precipitation of Mg and Cu atoms reduces the degree of lattice distortion, reduces the scattering of electrons, and thus improves the thermal conductivity of the alloy. The formation of a large number of nano-sized β-Mg2Si, Q' and θ' phases also significantly improves the mechanical properties of the alloy, while improving the mechanical properties and electrical and thermal conductivity of the aluminum alloy. After that, the temperature is rapidly lowered for low temperature aging treatment to inhibit the coarsening of the precipitation strengthening phase during the high temperature aging process, thereby improving the yield strength and tensile strength of the alloy.

[0043] Compared with the traditional multi-stage aging treatment, the high and low temperature cyclic aging treatment of the present invention effectively controls the abnormal coarsening and growth of the strengthening phase, ensures that the precipitated phase is finely dispersed in the matrix, and through multiple cyclic aging cycles, prolongs the precipitation time of the aging strengthening phase, increases the volume fraction of the precipitated phase, reduces the solid solubility of each alloy element in the aluminum matrix, and at the same time improves the mechanical properties and thermal conductivity of the aluminum alloy.

[0044] like Figure 1 As shown in the metallographic structure diagram of the alloy prepared in Example 1 of the present invention without adding Ag and Ho, its coarse α-Al matrix makes the strength and elongation of the alloy poor.

[0045] like Figure 2 As shown in the SEM microstructure of the alloy prepared in Example 1 of the present invention without adding Ag and Ho, the precipitated phase is continuously distributed near the grain boundary, and there are a large number of lath-like β-Fe phases, which hinder the transmission of electrons. At the same time, in the tensile test, the alloy is prone to crack formation starting from the lath-like β-Fe phases, which reduces the mechanical properties of the alloy.

[0046] like Figure 3 As shown, the alloy precipitates added with Ag and Ho prepared in Example 7 of the present invention are discontinuous island and fishbone shaped, which reduces the scattering effect on electrons and improves the thermal conductivity of the alloy.

[0047] The above is a further detailed description of the present invention, which should not be regarded as a limitation on the specific implementation of the present invention. For ordinary technicians in the technical field to which the present invention belongs, simple deduction or replacement without departing from the concept of the present invention is within the protection scope of the present invention.

Claims

1. A high thermal conductivity and high strength Al-Si-Mg-Cu-Sb-Fe alloy, characterized in that: The alloy comprises the following composition in percentage by mass: Si 4.0-6.0%, Mg 0.9-1.1%, Cu 0.5-0.6%, Sb 0.05-0.3%, Fe 0.2-0.3%, Ag 0.05-0.1%, Ho 0.05-0.1%, and the balance is Al.

2. The Al-Si-Mg-Cu-Sb-Fe alloy according to claim 1, characterized in that: The mass percentage content of Si is 5.0-6.0%.

3. The Al-Si-Mg-Cu-Sb-Fe alloy according to claim 1, characterized in that: The mass percentage content of Sb is 0.05-0.1%.

4. The Al-Si-Mg-Cu-Sb-Fe alloy according to claim 1, characterized in that: The high thermal conductivity and high strength Al-Si-Mg-Cu-Sb-Fe alloy further contains ≤0.1% of inevitable impurity elements.

5. The Al-Si-Mg-Cu-Sb-Fe alloy according to claim 1, characterized in that: The high thermal conductivity and high strength Al-Si-Mg-Cu-Sb-Fe alloy has a tensile strength of ≥400 MPa, a yield strength of ≥250 MPa, an elongation after fracture of ≥20%, and a thermal conductivity of ≥190 W / (m·K).

6. The method for preparing the Al-Si-Mg-Cu-Sb-Fe alloy according to any one of claims 1 to 5, characterized in that: The following steps are involved: 1) Weigh raw materials according to alloy composition and smelt them to obtain alloy ingots; 2) Taking the alloy ingot prepared in step 1), performing high and low temperature cycle aging treatment to obtain the high thermal conductivity and high strength Al-Si-Mg-Cu-Sb-Fe alloy.

7. The preparation method according to claim 6, characterized in that: The high and low temperature cycle aging treatment steps are: firstly perform high temperature aging treatment at 220-230° C. for 2-3 hours, then cool to -50--40° C., keep warm for 1-2 hours, and then cycle this operation.

8. The preparation method according to claim 6, characterized in that: The single cycle time of the high and low temperature cyclic aging treatment is 3 to 5 hours.

9. The preparation method according to claim 6, characterized in that: The cycle frequency of the high and low temperature cycle aging treatment is 12 to 16 times.

10. The preparation method according to claim 6, characterized in that: The total time of the high and low temperature cycle aging is 60 to 80 hours.

Citation Information

Cited By

  • Method for calculating content threshold value of impurity elements in alloy

    CN118428031A