Preparation method and application of high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst

By preparing scandium-doped ruthenium oxide acid oxygen evolution electrocatalyst, the problem of insufficient stability of noble metal ruthenium-based catalysts in acidic environments is solved, and an electrocatalyst with high catalytic activity and stability in acidic environments is achieved, which is suitable for proton exchange membrane electrolysis. The anode of water hydrogen production technology has promoted the commercial application of electrolytic water hydrogen production technology.

CN118880385APending Publication Date: 2024-11-01EAST CHINA UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411137553.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

In the existing proton exchange membrane electrolytic water anode oxygen evolution reaction, noble metal ruthenium-based catalysts are easily oxidized and dissolved in an acidic environment, resulting in insufficient stability and activity, limiting the further application of electrolytic water hydrogen production technology.

Method used

Using a high-performance scandium-doped ruthenium oxide acidic oxygen electrocatalyst, the hydrated ruthenium trichloride and hydrated scandium chloride are stirred and mixed in anhydrous ethanol, then dried on a heating stage and grinded with potassium nitrate. Then calcined in a muffle furnace and dissolved with ionic water, a highly catalytically active electrocatalyst was prepared that operates stably in an acidic environment.

Benefits of technology

The prepared high-performance scandium-doped ruthenium oxide acidic acid electrocatalyst is required to reach a current density of 10mA/cm² in 0.5mol/L sulfuric acid, which requires an overpotential range of 200 to 260mV, with good activity and current at 10mA/cm². The stable operation time is more than 100 hours under density conditions, and it is suitable for the anode of the proton exchange membrane electrolytic hydrogen production device, which promotes the commercial application of electrolytic hydrogen production technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880385A_ABST
    Figure CN118880385A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst, ruthenium trichloride hydrate and scandium chloride hydrate are dissolved in absolute ethyl alcohol, stirred and mixed, and a uniform mixed solution is obtained; placing the mixed solution on a heating table for heating and drying to obtain a powder sample; grinding and mixing the powder sample and potassium nitrate to obtain a precursor sample; calcining the precursor sample in a muffle furnace to obtain a sample; adding deionized water into the sample for ultrasonic dissolution, washing with water for multiple times, and drying to obtain the high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst. The high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst is applied to water electrolysis hydrogen production. The method has the beneficial effects that the catalyst performance is improved and has important research significance; an important experimental basis is provided for further researching the influence of the ruthenium oxide crystal face on the catalyst reaction; the high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst has good activity and excellent stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hydrogen evolution by proton exchange membrane water electrolysis, and in particular to a preparation method and application of a high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst. Background Art

[0002] Global energy and environmental issues are hot topics in human development. Hydrogen, as an ideal energy carrier with high energy density, clean and pollution-free, is an important way to solve the energy crisis and environmental pollution.

[0003] Proton exchange membrane water electrolysis is an intermittent sustainable hydrogen production technology with the advantages of high current density, high hydrogen purity, fast response, high power density and high energy efficiency. It is considered to be one of the most promising hydrogen production technologies. The high anode potential and acidic environment of proton exchange membrane water electrolysis pose great challenges to the stability and activity of materials, limiting the further application of proton exchange membrane water electrolysis. At present, ruthenium-iridium-based catalysts are the best electrocatalysts for the anode oxygen evolution reaction of proton exchange membrane water electrolysis, while the global annual production of iridium metal is less than ten tons, and the price is about ten times that of metallic ruthenium. In contrast, precious metal ruthenium has higher activity and is cheaper, and has more research value and application potential. However, ruthenium-based catalysts are easily oxidized and dissolved in acidic media. Therefore, the development of ruthenium-based electrocatalysts with high catalytic activity that can operate stably in acidic environments is a key point and difficulty that the water electrolysis hydrogen production industry urgently needs to overcome. Summary of the invention

[0004] In order to solve the above problems, especially to address the deficiencies in the prior art, the present invention provides a method for preparing a high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst and its application, which can solve the above problems.

[0005] To achieve the above purpose, the present invention adopts the following technical means:

[0006] A method for preparing a high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst comprises the following steps:

[0007] S1. Dissolve hydrated ruthenium trichloride and hydrated scandium chloride in anhydrous ethanol, stir and mix to obtain a uniform mixed solution;

[0008] S2, placing the mixed solution obtained in step S1 on a heating table for heating and drying to obtain a powder sample;

[0009] S3, grinding and mixing the powder sample obtained in step S2 with potassium nitrate to obtain a precursor sample;

[0010] S4, calcining the precursor sample obtained in step S3 in a muffle furnace to obtain a sample;

[0011] S5. Add deionized water to the sample obtained in step S4 for ultrasonic dissolution, wash with water for multiple times, and dry to obtain a high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst.

[0012] A further embodiment of the present invention is that the molar ratio of hydrated ruthenium trichloride to hydrated scandium chloride in step S1 is 1:0.01-0.1.

[0013] A further solution of the present invention is that the stirring and mixing time in step S1 is 24 hours.

[0014] A further solution of the present invention is that the mass of potassium nitrate added in step S3 is 5 to 100 times the mass of the powder sample dried in S2.

[0015] A further solution of the present invention is that in step S4, the calcination temperature is 350-500° C., the calcination time is 1-3 hours, and the heating rate is 10° C. / min.

[0016] A further solution of the present invention is that in step S5, the sample is added with deionized water for ultrasonic dissolution, centrifuged and washed multiple times, and dried, and the number of centrifugal washings is greater than 6 times.

[0017] A further solution of the present invention is that the specific process of drying in step S5 is: drying at 60° C. for 12 hours.

[0018] Another object of the present invention is to provide a method for preparing a high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst to obtain a high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst.

[0019] Another object of the present invention is to provide an application of a high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst, wherein the high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst is used in hydrogen production by water electrolysis.

[0020] Beneficial effects of the present invention:

[0021] 1. The present invention adopts the molten salt method to introduce scandium into the ruthenium oxide lattice. The synthesis method is simple and is also applicable to other metal-doped ruthenium oxides such as scandium and hafnium. Metal-doped ruthenium oxide has important research significance for further studying the application of ruthenium oxide in proton exchange membrane water electrolysis and improving catalyst performance.

[0022] 2. The high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst prepared by the present invention selectively exposes more rutile ruthenium oxide (101) crystal faces, providing an important experimental basis for further studying the influence of ruthenium oxide crystal faces on catalytic reactions.

[0023] 3. The high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst prepared by the present invention has an overpotential range of 200 to 260 mV required to achieve a current density of 10 mA cm-2 in 0.5 mol L-1 sulfuric acid, and has good activity; in addition, the voltage hardly changes after stable operation for more than 100 hours under the condition of a current density of 10 mV cm-2, and has excellent stability. It can be used as an anode for a proton exchange membrane water electrolysis hydrogen production device, which is of great significance to its accelerated commercialization. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a comparison diagram of the XRD of the high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst and the ruthenium oxide not doped with scandium in Example 1 of the present invention;

[0025] Figure 2 This is a comparison diagram of the OER polarization curves of the high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst of Example 1 of the present invention and commercial ruthenium oxide in 0.5 mol L-1 sulfuric acid;

[0026] Figure 3 This is a comparison chart of the OER stability of the high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst of Example 1 of the present invention and commercial ruthenium oxide at a current density of 10 mA cm-2 in 0.5 mol L-1 sulfuric acid. DETAILED DESCRIPTION

[0027] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] Example 1

[0029] A method for preparing a high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst comprises the following steps:

[0030] S1. Prepare the pre-reaction solution: dissolve 2 mmol of hydrated ruthenium trichloride and 0.02 mmol of hydrated scandium chloride in 20 mL of anhydrous ethanol, and stir magnetically for 24 h to obtain a uniform mixed solution;

[0031] S2, placing the mixed solution obtained in step S1 on a heating table at 100° C. and heating and drying for 5 h to obtain a powder sample;

[0032] S3, grinding and mixing the powder sample obtained in step S2 with 25 times the mass of potassium nitrate to obtain a precursor sample;

[0033] S4, calcining the precursor sample obtained in step S3 in a muffle furnace at a calcination temperature of 350°C, a calcination time of 2h, and a heating rate of 10°C / min to obtain a sample;

[0034] S5. Add deionized water to the sample obtained in step S4 for ultrasonic dissolution, centrifuge and wash with water for 6 times to ensure that potassium nitrate is completely washed away, and dry to obtain a high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst.

[0035] Example 2

[0036] The high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst provided in this embodiment can refer to Example 1, except that the amount of hydrated scandium chloride is 0.06 mmol.

[0037] Example 3

[0038] The high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst provided in this embodiment can refer to Example 1, except that the amount of hydrated scandium chloride is 0.1 mmol.

[0039] Example 4

[0040] The high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst provided in this embodiment can refer to Example 1, except that the amount of hydrated scandium chloride is 0.2 mmol.

[0041] Example 5

[0042] The high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst provided in this embodiment can refer to Example 1, except that the mass of potassium nitrate is 100 times the mass of the powder sample.

[0043] Comparative Example 1:

[0044] like Figures 1 to 3 As shown, the high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst of Example 1 is selected for comparison with commercial ruthenium oxide, and the specific information of the commercial ruthenium oxide is brand: Shengernuo, CAS NO.12036-10-1, model: SRu75. By comparison, it can be seen that the high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst prepared by the present invention has good activity and excellent stability.

[0045] The examples given in the present invention are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here, and the obvious changes or modifications derived therefrom are still within the protection scope of the present invention.

Claims

1. A method for preparing a high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst, characterized in that: The following steps are involved: S1. Dissolve hydrated ruthenium trichloride and hydrated scandium chloride in anhydrous ethanol, stir and mix to obtain a uniform mixed solution; S2, placing the mixed solution obtained in step S1 on a heating table for heating and drying to obtain a powder sample; S3, grinding and mixing the powder sample obtained in step S2 with potassium nitrate to obtain a precursor sample; S4, calcining the precursor sample obtained in step S3 in a muffle furnace to obtain a sample; S5. Add deionized water to the sample obtained in step S4 for ultrasonic dissolution, wash with water for multiple times, and dry to obtain a high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst.

2. The method for preparing a high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst according to claim 1, characterized in that: In step S1, the molar ratio of hydrated ruthenium trichloride to hydrated scandium chloride is 1:0.01-0.

1.

3. The method for preparing a high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst according to claim 2, characterized in that: The stirring and mixing time in step S1 is 24 hours.

4. The method for preparing a high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst according to claim 1, characterized in that: The mass of potassium nitrate added in step S3 is 5 to 100 times the mass of the powder sample dried in S2.

5. The method for preparing a high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst according to claim 1, characterized in that: In step S4, the calcination temperature is 350-500° C., the calcination time is 1-3 hours, and the heating rate is 10° C. / min.

6. The method for preparing a high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst according to claim 1, characterized in that: In step S5, the sample is added with deionized water for ultrasonic dissolution, washed with water by centrifugation for multiple times, and dried, and the number of times of centrifugation and washing with water is greater than 6 times.

7. The method for preparing a high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst according to claim 6, characterized in that: The specific process of drying in step S5 is: drying at 60° C. for 12 hours.

8. A high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst prepared according to the method for preparing a high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst as described in any one of claims 1 to 7.

9. The use of a high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst according to claim 8, characterized in that: The high-performance scandium-doped ruthenium oxide acidic oxygen evolution electrocatalyst is used in the production of hydrogen by electrolysis of water.