Monoclinic crystal system crystal form substance as well as preparation method and application thereof
The preparation of TiS2Se single crystals on a large cavity press by high temperature and high pressure method solves the problems of limited doping amount and long preparation period in the prior art, and realizes the preparation of high-quality monoclinic crystal forms, and is also a good example of the preparation of the crystal form of the monoclinic crystal. Semiconductor materials offer new uses.
Patent Information
- Application Number
- CN202411006476.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-01
AI Technical Summary
The prior art has limited doping amount when preparing TiS3 compounds, a long preparation period and consumes power. In addition, the chemical gas phase transport method has the problem that samples are easily volatile and oxidized, making it difficult to prepare high-quality monoclinic crystal forms.
Using a high temperature and high pressure method, a large cavity press was used to prepare TiS2Se single crystals by sintering packaging and hexagonal boron nitride protective cover inclusion under 4-6GPa pressure and 700-950℃, which overcomes the volatility and oxidation problems of the single selenium , ensuring crystal quality.
High-quality TiS2Se single crystal was successfully prepared, and it was confirmed that it was free of impurities by single crystal X-ray diffraction, which simplified the preparation of monoclinic structures, reduced costs, and was suitable for the application of semiconductor materials.
Smart Images

Figure CN118880425A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of new material preparation, and in particular to a monoclinic crystal form and a preparation method and application thereof. Background Art
[0002] In recent years, transition metal trichalcogenides (TX3) of groups IVB, VB, and VIB have attracted increasing attention due to their diverse physical properties. The chain structure of TX3 compounds exhibits novel physical properties, such as superconductivity and charge density waves.
[0003] As an emerging two-dimensional semiconductor material, TiS3 currently has very broad application prospects. Its electrical transport test shows that it is an n-type semiconductor, but it has characteristics different from traditional semiconductors, such as higher carrier mobility and anisotropic thermal and electrical properties.
[0004] TiS3 can be prepared using chemical vapor transport, but there is no experimental report on the effect of doping on physical properties. 3-x Se x The maximum Se doping amount in the sample is only x=0.24 (8%). [Nanoscale, 2018, 10, 15654-15660]. In addition, the chemical vapor transport method takes a long time (starting from one week), the sample preparation cycle is long, and it consumes a lot of electricity resources. Summary of the invention
[0005] In view of the above-mentioned shortcomings of the prior art, the object of the present invention is to provide a monoclinic crystal form and a preparation method and use thereof, so as to solve the problems in the prior art.
[0006] To achieve the above-mentioned and other related purposes, the present invention provides a monoclinic crystal form, wherein the molecular formula of the monoclinic crystal form is TiS2Se; the monoclinic crystal form includes the following unit cell parameters: β=97.61(8)°; lattice parameters of the monoclinic crystal form: space group: P21 / m.
[0007] Preferably, each Ti atom in the monoclinic crystal form is surrounded by S atoms and Se atoms, the total number of which is 8.
[0008] The present invention also provides a method for preparing the aforementioned monoclinic crystal form, the method comprising multiple of the following steps:
[0009] 1) Mixing elemental titanium and elemental sulfur, sintering and packaging, and then firing to obtain a TiS2 precursor;
[0010] 2) grinding, mixing, and tableting the TiS2 precursor obtained in step 1) and pure Se powder, and then wrapping them with a hexagonal boron nitride protective cover to prepare an inclusion;
[0011] 3) The inclusions in step 2) are reacted under the conditions of 4-6 GPa pressure and 700-950° C. to obtain a monoclinic crystal.
[0012] As described above, the monoclinic crystal form and the preparation method and use thereof of the present invention have the following beneficial effects:
[0013] The high temperature and high pressure conditions in the preparation method of the monoclinic crystal provided by the present invention can overcome the limitations of high vapor pressure of elemental selenium, easy volatilization, and easy explosion of quartz tubes, thereby preparing TiS2Se single crystals with a simple monoclinic structure. The above-mentioned crystals have good crystallization quality and are confirmed to be single-phase by single crystal X-ray diffraction. The results of single crystal X-ray diffraction show that there are no impurities and Luan crystals in the single crystals. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 Shown is a schematic diagram of a device for synthesizing samples at high temperature and high pressure according to the present invention.
[0015] Figure 2 Shown is an optical photograph of the TiS2Se single crystal sample and geometric dimensions of the present invention.
[0016] Figure 3 Shown is the energy dispersive X-ray spectrum of the TiS2Se sample of the present invention.
[0017] Figure 4 Shown is the X-ray diffraction pattern of the TiS2Se single crystal sample of the present invention.
[0018] Figure 5 Shown are schematic diagrams of the simple monoclinic TiS2Se crystal structure of the present invention along different crystallographic axes (left: c-axis; right: b-axis).
[0019] Figure 6 Shown is the resistance-temperature curve of the TiS2Se sample of the present invention. DETAILED DESCRIPTION
[0020] The inventors of the present invention have found through a large number of experiments that the difficulties in the prior art can be overcome by adopting a synthesis method of suitable high temperature and high pressure assembly. The large cavity press has the advantages of physical and mechanical pressurization, eight-sided wrapping of magnesium oxide and pyrophyllite sealing, which can provide a sealed and high-strength sample cavity for the sample. The physical pressure provided by the large cavity press is much greater than the vapor pressure of the sample at high temperature. Therefore, the large cavity press is very suitable for sealing chemical reactants that are easy to oxidize or volatilize at high temperatures, plays an extremely important role in the research and exploration of new materials, and is an important means for preparing metal-rich sulfur / selenium compounds. The present invention uses a high temperature and high pressure method on a 2000-ton Kawai type large cavity press to synthesize a TiS2Se single crystal sample with a simple monoclinic structure for the first time. On this basis, the present invention is completed.
[0021] The present invention provides a monoclinic crystal form, wherein the molecular formula of the monoclinic crystal form is TiS2Se; the monoclinic crystal form includes the following unit cell parameters: β=97.61(8)°; lattice parameters of the monoclinic crystal form: space group: P21 / m, and the crystal system of the monoclinic crystal form is simple monoclinic.
[0022] In some specific embodiments, each Ti atom in the monoclinic crystal form is surrounded by S atoms and Se atoms, the total number of which is 8.
[0023] In some specific embodiments, the monoclinic crystal form is gray-black elongated crystals.
[0024] In the present invention, the testing and single crystal analysis methods are not particularly limited, and single crystal testing instruments known to those skilled in the art can be used. In some specific embodiments, the single crystal data of the monoclinic crystal form is collected at 290K on a Bruker D8 Venture dual-target small molecule X-ray single crystal diffractometer, wherein the single crystal diffractometer tube voltage when collecting data: 50kV, tube current 30mA. ShelXT 2018 / 3 (Sheldrick, 2018) was used to analyze the crystal structure, the least squares method was used to correct the structural parameters and identify the atomic species, and the geometric calculation method and the difference Fourier method were used to obtain all atomic positions, and the final reliability factor R1=0.0396, wR2=0.0843, and the goodness factor was 1.203.
[0025] The molecular formula of the monoclinic crystal form described in the present invention is further determined by X-ray energy dispersion spectrum analysis, and the molecular formula is TiS2Se.
[0026] The present invention also provides a method for preparing the aforementioned monoclinic crystal form, the method comprising multiple of the following steps:
[0027] 1) Mixing elemental titanium and elemental sulfur, sintering and packaging, and then firing to obtain a TiS2 precursor;
[0028] 2) grinding, mixing, and tableting the TiS2 precursor obtained in step 1) and pure Se powder, and then wrapping them with a hexagonal boron nitride protective cover to prepare an inclusion;
[0029] 3) The inclusions in step 2) are reacted under the conditions of 4-6 GPa pressure and 700-950° C. to obtain a monoclinic crystal.
[0030] In some specific embodiments, based on the total volume of the reaction system in step 1), the molar ratio (amount ratio) of elemental titanium to elemental sulfur in step 1) is 1:1.5-2.5. Specifically, the molar ratio is 1:1.5-2 or 1:2-2.5.
[0031] In some specific embodiments, based on the total volume of the reaction system in step 2), the molar ratio of the TiS2 precursor in step 2) to the pure Se powder is 1:0.5-1.5. Specifically, the molar ratio is 1:0.5-1 or 1:1-1.5.
[0032] In some embodiments, the mixing in step 1) or step 2) can occur in a glove box under protective gas conditions. The protective gas is an inert gas. Preferably, the protective gas is selected from one or more of argon, helium, neon, krypton or xenon.
[0033] In some specific embodiments, the cylinder formed by tableting in step 2) has a diameter of 3-4 mm and a height of 3.5-4.5 mm. Specifically, the diameter is 3-3.5 or 3.5-4 mm; the height is 3.5-4 or 4-4.5 mm.
[0034] In some specific embodiments, in step 2), the hexagonal boron nitride protective sleeve can be composed of hexagonal boron nitride sheets and / or hexagonal boron nitride tubes. Among them, the wall thickness of the hexagonal boron nitride tube can be 0.2-0.25 mm or 0.25-0.3 mm, and the inner diameter can be 3-3.5 mm or 3.5-4 mm; the thickness of the hexagonal boron nitride sheet can be 0.45-0.5 mm or 0.5-0.55 mm, and the diameter can be 3.5-4 mm or 4-4.5 mm. Since the elemental Se reacts with the noble metal Ag or Pt under high temperature and high pressure, therefore, unlike the samples wrapped with noble metals in the existing high temperature and high pressure experiments, the sample reactants in the present invention are wrapped with hexagonal boron nitride that is resistant to high temperature and high pressure and has stable chemical properties, reducing the probability of generating impurities. In addition, the price of hexagonal boron nitride is lower than that of noble metals, which can reduce the cost of sample preparation and facilitate batch preparation of samples.
[0035] In some specific embodiments, the reaction temperature in step 3) is 700-750°C, 750-800°C, 800-850°C, 850-900°C or 900-950°C.
[0036] In some specific embodiments, the reaction pressure in step 3) is 4-4.5 GPa, 4.5-5 GPa, 5-5.5 GPa or 5.5-6 GPa.
[0037] In some specific embodiments, step 3) includes a pressure increasing step, wherein the pressure increasing step is from a starting temperature of 15-42° C. and a pressure increasing rate of 80-120 tons / h until the pressure of the sample chamber reaches a preset pressure. Specifically, the pressure increasing rate is 80-90 tons / h, 90-100 tons / h, 100-110 tons / h or 110-120 tons / h.
[0038] In some specific embodiments, in step 3), when the reaction pressure reaches a preset pressure, a heating program is started to a preset temperature.
[0039] In some specific embodiments, the reaction time of step 3) under the conditions of 4-6 GPa pressure and 700-950° C. is 100-180 min. Specifically, the reaction time is 100-110 min, 110-120 min, 120-130 min, 130-140 min, 140-160 min or 160-180 min.
[0040] In some specific embodiments, step 3) further comprises an annealing step, wherein the annealing step is to cool the sample slowly to 580-750°C at a rate of 1.5-1.8°C / min after the reaction is completed under the conditions of 4-6GPa pressure and 700-950°C. Specifically, the annealing step is to cool the sample to 580-600°C, 600-620°C, 620-650°C, 650-700°C or 700-750°C at a rate of 1.5-1.67 or 1.67-1.8°C / min after the reaction is completed under the conditions of 4-6GPa pressure and 700-950°C.
[0041] In some specific implementation steps, step 3) further comprises a quenching step, wherein the quenching step is provided after the annealing step, and the temperature of the sample is cooled down to 15-42°C.
[0042] In some specific embodiments, step 3) further comprises a decompression step, which is provided after the quenching step, and reduces the pressure of the sample chamber from 4-6 GPa to normal pressure (1 standard atmosphere) at a rate of 20-30 tons / h. Specifically, the decompression step reduces the pressure of the sample chamber from 4-6 GPa to normal pressure at a rate of 20-25 or 25-30 tons / h.
[0043] Generally, any reactor that can provide the above-mentioned high temperature and high pressure can be used in the preparation method of the present invention. In some specific implementations, the above reaction can be carried out using a large cavity press, and more preferably a Kawai type large cavity press, and further a 2000-ton Kawai type large cavity press can be selected. When used specifically, Figure 1 As shown, the inclusion is first placed in a heating furnace, the four sides of the inclusion can be sealed with zirconium dioxide insulation plugs, the graphite heating furnace is placed in a zirconium dioxide insulation tube, and finally placed in a pressure medium in a magnesium oxide octahedron doped with 5% cobalt oxide. The sample synthesis is carried out on a 2000-ton Kawai type large cavity press. After controlling the aforementioned high pressure and high temperature conditions, cooling and pressure relief, the sample is taken out from the magnesium oxide octahedron, and gray-black elongated crystals are observed under a microscope.
[0044] In some specific embodiments, before the high pressure experiment in step 3), the pressure and temperature are calibrated first; the pressure is calibrated using the resistance-pressure curve of metal Bi; the temperature is calibrated through the crystal structure phase transition of silicon dioxide, and the heating temperature is controlled by controlling the heating power and measured using a tungsten-rhenium thermocouple.
[0045] The present invention also provides use of the aforementioned monoclinic crystal form in preparing semiconductor materials.
[0046] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0047] Before further describing the specific embodiments of the present invention, it should be understood that the scope of protection of the present invention is not limited to the specific embodiments described below; it should also be understood that the terms used in the examples of the present invention are for describing the specific embodiments rather than for limiting the scope of protection of the present invention; in the present specification and claims, unless otherwise expressly stated herein, the singular forms "a", "an" and "the" include plural forms.
[0048] When the embodiments give numerical ranges, it should be understood that, unless otherwise specified in the present invention, both endpoints of each numerical range and any numerical value between the two endpoints can be selected. Unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those generally understood by those skilled in the art. In addition to the specific methods, equipment, and materials used in the embodiments, according to the grasp of the prior art by those skilled in the art and the record of the present invention, any methods, equipment, and materials of the prior art similar or equivalent to the methods, equipment, and materials described in the embodiments of the present invention can also be used to realize the present invention.
[0049] The process equipment or devices not specifically specified in the examples are all conventional equipment or devices in the art; all pressure values and ranges refer to absolute pressures.
[0050] In addition, it should be understood that one or more method steps mentioned in the present invention do not exclude the existence of other method steps before or after the combination step or the insertion of other method steps between these explicitly mentioned steps, unless otherwise specified; it should also be understood that the combination connection relationship between one or more devices / apparatuses mentioned in the present invention does not exclude the existence of other devices / apparatuses before or after the combination device / apparatus or the insertion of other devices / apparatuses between these explicitly mentioned two devices / apparatuses, unless otherwise specified. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or the scope of the present invention. Changes or adjustments in their relative relationships should also be regarded as the scope of the present invention without substantially changing the technical content.
[0051] Example 1
[0052] 1) Preparation of precursor samples at atmospheric pressure
[0053] Chemically pure elemental titanium and sulfur were mixed evenly in an argon environment of a glove box at a molar ratio of 1:2, vacuum sintered and packaged using a quartz tube, and placed in a muffle furnace and heated to 660°C for pre-calcination for 20 hours to obtain a TiS2 precursor.
[0054] The pre-calcined TiS2 precursor and pure Se powder are ground and mixed in a molar ratio of 1:1, wrapped with copper sheets and pressed into cylindrical shapes. The copper columns containing the powders are then cold-pressed at about 8 to 10 MPa to form cylinders with a height of 4.0 mm and a diameter of 3.5 mm. The copper sheets are then scraped off with a clean blade.
[0055] In order to prevent the reactants from chemically reacting with the heating furnace to generate impurities, the reactants need to be wrapped with inclusions. Through literature research, we found that elemental selenium reacts chemically with both precious metals gold and platinum at high temperatures. Therefore, the initial reactants cannot be wrapped with precious metals, but instead hexagonal boron nitride tubes (wall thickness: 0.25 mm; inner diameter 3.5 mm) and discs (thickness: 0.5 mm; diameter: 4.0 mm) that are resistant to high temperature and pressure and have stable chemical properties are used. In addition, the price of hexagonal boron nitride is lower than that of precious metals, which can reduce the cost of sample preparation and facilitate batch preparation of samples.
[0056] 2) Preparation of simple monoclinic TiS2Se single crystals by high temperature and high pressure method
[0057] First, prepare the magnesium oxide octahedron assembly required for sample preparation. Put the above cylindrical sample reactants and hexagonal boron nitride protective sleeve into the graphite heating furnace. Then put the sample into the high-pressure assembly for high-pressure and high-temperature synthesis. The sample synthesis is carried out on a Kawai type large-cavity press with a thrust of 2000 tons. First, slowly increase the pressure to 5GPa (100 tons per hour) at room temperature, then start the heating program to heat to 800℃, and keep it warm for 120 minutes under high temperature and high pressure conditions (5GPa+800℃). In order to prepare single crystal samples, it is necessary to anneal the high-temperature and high-pressure samples. The method is to cool down the sample temperature at a rate of 1.67℃ / minute and slowly cool the sample temperature to 600℃. Finally, turn off the heating power supply and quickly quench the sample to room temperature. After the temperature drops to room temperature, slowly release the pressure of the sample chamber (25 tons per hour) to normal pressure.
[0058] Take out the sample from the magnesium oxide octahedron, and you can see that the sample is gray-black elongated crystals under the microscope (see Figure 2 ).
[0059] In this example, the chemical composition of the sample was analyzed by X-ray energy dispersion spectroscopy. The experimental results are as follows: Figure 3 As shown, the chemical element ratio given by EDX is Ti:S:Se=25.12%:48.37%:27.51%, which is basically consistent with the theoretical chemical ratio of 1:2:1. Single crystal X-ray diffraction analysis was performed on the sample obtained after quenching. Figure 4 It is the diffraction pattern of the TiS2Se single crystal sample of the present invention. Figure 4 It can be seen that the single crystal diffraction spot of the sample is small and bright, and the crystal quality is good. The crystallographic information file (Crystallographic Information File) of the sample was obtained through single crystal analysis software. The lattice parameters are: space group: P21 / m, unit cell parameters are: β=97.61(8)°. The detailed crystal structure refinement parameters are shown in Table 1:
[0060] Table 1. Crystal structure refinement parameters of TiS2Se
[0061]
[0062]
[0063] The atomic coordinates of TiS2Se are shown in Table 2. Based on the crystallographic information file analyzed in this example, we drew a schematic diagram of the crystal structure of a simple monoclinic TiS2Se ( Figure 5 ). Figure 5 (Left) and 5 (right) are schematic diagrams of the crystal structure of the sample along different crystal directions. The blue atoms are Ti, the yellow ones are S, and the green ones are Se. There are 8 total S and Se atoms around each Ti. The TiS(Se) polyhedron forms a layered structure along the bc plane and stacks in the a-axis direction, such as Figure 5 (left) as shown; Figure 5 (Right) Schematic diagram of TiS2Se crystal along the b-axis, forming a one-dimensional infinitely long chain along the b-axis.
[0064] Table 2, atomic coordinates of TiS2Se
[0065] Atom x y z Occ. U Wyckoff Ti 0.7146(3) 0.75 0.35020(14) 1.000 0.012 2e S(1) 0.8832(2) 1.25 0.16656(13) 0.445 0.020 2e S(2) 0.4569(3) 1.25 0.17857(16) 0.686 0.020 2e S(3) 0.7631(3) 0.25 0.55045(17) 0.848 0.013 2e Se(1) 0.8832(2) 1.25 0.16656(13) 0.555 0.020 2e Se(2) 0.4569(3) 1.25 0.17857(16) 0.314 0.020 2e Se(3) 0.7631(3) 0.25 0.55045(17) 0.152 0.013 2e
[0066] Example 2
[0067] 1) Preparation of cylindrical reactants of TiS2 and selenium under normal pressure
[0068] TiS2 and selenium were mixed evenly in a glove box at a molar ratio of 1:1, and mortared in an agate mortar for half an hour. The reactant powder was pressed into a cylinder with a height of 4.0 mm and a diameter of 3.5 mm by a powder tablet press (pressure: 8 MPa). Since selenium reacts with both precious metals gold and platinum under high temperature and high pressure, the sample reactant in the present invention is wrapped with hexagonal boron nitride that is resistant to high temperature and high pressure and has stable chemical properties, which reduces the probability of generating impurities.
[0069] 2) Place the above sample and the hexagonal boron nitride protective cover into a graphite heating furnace. Then place the sample into a high-pressure assembly for high-pressure and high-temperature synthesis. The sample synthesis is carried out on a 2000-ton Kawai large-cavity press. First, slowly increase the pressure (100 tons per hour) to 5 GPa at room temperature, then start the heating program and heat to 850°C, keep warm for 3 hours under high temperature and high pressure conditions (5 GPa + 850°C), then cool down at a rate of 100°C per hour, and slowly cool the sample temperature to 650°C. Then turn off the power and quench the sample to room temperature. Finally, slowly unload the pressure (25 tons per hour) to normal pressure. After taking out the sample from the magnesium oxide octahedron, you can see a shiny single crystal sample.
[0070] Similar to Example 1, the sample obtained after quenching also has a single crystal semiconductor with a monoclinic structure. Single crystal X-ray diffraction, EDX and ultraviolet absorption spectrum analysis are performed on it, and it is found that the sample has a monoclinic semiconductor.
[0071] Example 3
[0072] 1) Preparation of cylindrical reactants of TiS2 and selenium under normal pressure
[0073] TiS2 and selenium were mixed evenly in a glove box at a molar ratio of 1:1, and mortared in an agate mortar for half an hour. The reactant powder was pressed into a cylinder with a height of 4.0 mm and a diameter of 3.5 mm by a powder tablet press (pressure: 8 MPa). Since selenium reacts with both precious metals gold and platinum under high temperature and high pressure, the sample reactant in the present invention is wrapped with hexagonal boron nitride that is resistant to high temperature and high pressure and has stable chemical properties, which reduces the probability of generating impurities. The excess selenium acts as a flux.
[0074] 2) Place the above sample and the hexagonal boron nitride protective sleeve together in a graphite heating furnace. Then place the sample into a high-pressure assembly for high-pressure and high-temperature synthesis. The sample synthesis is carried out on a Kawai-type large-cavity press with a thrust of 2,000 tons. First, slowly increase the pressure to 6 GPa (100 tons / hour) at room temperature, then start the heating program and heat to 950°C, keep warm for 3 hours under high temperature and high pressure conditions (6 GPa+950°C), then cool down at a rate of 1.5°C per minute, slowly cool the sample temperature to 750°C, then quench to room temperature, and finally slowly (25 tons per hour) decompress to normal pressure.
[0075] Similar to Example 1, the sample obtained after quenching also has a monoclinic semiconductor single crystal. A single crystal X-ray diffraction study was performed on it, and it was found that the sample has a monoclinic crystal.
[0076] Example 4
[0077] like Figure 6 As shown in the performance test resistance-temperature curve of the TiS2Se sample, the resistance of TiS2Se increases with decreasing temperature, indicating that the TiS2Se sample exhibits semiconductor conductive behavior, and the band gap of the semiconductor sample can be obtained by the resistance-temperature curve in the high temperature section, which is about 80meV. The resistance test is obtained by taking a flat single crystal and adopting a standard four-electrode layout method in the PPMS (physical property measurement system) of Quantum Design. The test temperature range is: 25K-300K. The current size is: 1 microampere. The formula used for the resistivity-bandgap fitting of the semiconductor is: ρ=ρ0exp(Eg / 2k B T), where E g is the fitted band gap value.
[0078] The above examples are for the purpose of illustrating the embodiments disclosed by the present invention and are not to be construed as limiting the present invention. In addition, the various modifications listed herein and the variations of the methods in the invention are obvious to those skilled in the art without departing from the scope and spirit of the present invention. Although the present invention has been specifically described in conjunction with various specific preferred embodiments of the present invention, it should be understood that the present invention should not be limited to these specific embodiments. In fact, various modifications as described above that are obvious to those skilled in the art to obtain the invention should be included within the scope of the present invention.
Claims
1. A monoclinic crystal form, characterized in that: The molecular formula of the monoclinic crystal form is TiS2Se; the monoclinic crystal form includes the following unit cell parameters β=97.61(8)°; The monoclinic crystal form has the characteristics of P21 / m space group.
2. The monoclinic crystal form according to claim 1, characterized in that: In the monoclinic crystal form, each Ti atom is surrounded by S atoms and Se atoms, the total number of which is 8. And / or, the monoclinic crystal form is gray-black elongated crystals.
3. The method for preparing the monoclinic crystal form according to claim 1 or 2, characterized in that: The preparation method comprises multiple of the following steps: 1) Mixing elemental titanium and elemental sulfur, sintering and packaging, and then firing to obtain a TiS2 precursor; 2) mixing the TiS2 precursor obtained in step 1) with Se powder, pressing the tablets, and then wrapping them with a hexagonal boron nitride protective cover to obtain an inclusion; 3) The inclusions in step 2) are reacted under the conditions of 4-6 GPa pressure and 700-950° C. to obtain a monoclinic crystal.
4. The preparation method according to claim 3, characterized in that: The preparation method comprises one or more of the following features: I) Based on the total volume of the reaction system in step 1), the molar ratio of elemental titanium to elemental sulfur in step 1) is 1:1.5-2.5; II) Based on the total volume of the reaction system in step 2), the molar ratio of the TiS2 precursor in step 2) to the pure Se powder is 1:0.5-1.5; III) The mixing in step 1) or step 2) takes place in a glove box under protective gas conditions.
5. The preparation method according to claim 3, characterized in that: The preparation method comprises one or more of the following features: IV) the cylinder formed by tableting in step 2) has a diameter of 3-4 mm and a height of 3.5-4.5 mm; V) in step 2), the hexagonal boron nitride protective cover is composed of a hexagonal boron nitride sheet and / or a hexagonal boron nitride tube; VI) Step 3) The reaction time is 100-180 min at a pressure of 4-6 GPa and a temperature of 700-950° C.
6. The preparation method according to claim 3, characterized in that: Step 3) includes a pressure increasing step, wherein the pressure increasing step is from a starting temperature of 15-42° C. and a pressure increasing rate of 80-120 tons / h until the pressure of the sample chamber reaches a preset pressure.
7. The preparation method according to claim 3, characterized in that: Step 3) also includes an annealing step, wherein after the reaction is completed under the conditions of 4-6 GPa pressure and 700-950°C, the temperature of the sample is slowly cooled to 580-750°C at a rate of 1.5-1.8°C / min.
8. The preparation method according to claim 7, characterized in that: Step 3) further comprises a quenching step, wherein the quenching step is arranged after the annealing step, and the temperature of the sample is cooled to 15-42°C.
9. The preparation method according to claim 8, characterized in that: Step 3) further comprises a decompression step, which is arranged after the quenching step, and reduces the pressure of the sample chamber from 4-6 GPa to normal pressure at a rate of 20-30 tons / h.
10. The preparation method according to claim 3, characterized in that: The reactor used in step 3) is a large cavity press.