Guanidine phosphite nonlinear optical crystal as well as preparation method and application thereof
By using guanidine phosphate [C(NH2)3]2HPO3 nonlinear optical crystals, different process methods are used to grow crystals with excellent performance, which solves the shortcomings of existing short-wavelength nonlinear optical crystals in birefringence and growth difficulty. , realizes the efficient preparation of large-size transparent crystals, and is suitable for the manufacturing of laser devices.
Patent Information
- Application Number
- CN202410921320.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-10
AI Technical Summary
Existing short-wavelength nonlinear optical crystals such as KBe2BO3F2, BaB2O4 and LiB3O5 have shortcomings in terms of small birefringence and difficulty in growing large-sized crystals, which limits their application.
Guanidine phosphite [C(NH2)3]2HPO3 is used as a new nonlinear optical crystal, and crystals are grown by melt method, high-temperature melt method or vacuum encapsulation method to prepare nonlinear with monoclinic crystal system and moderate birefringence. Optical crystals are optimized by evaporation, hydrothermal or room temperature solution method to obtain large-size transparent crystals.
It is achieved to obtain guanidine phosphate nonlinear optical crystals with large second-order nonlinear coefficient, wide light transmission range, short cut-off edges and moderate birefringence. It has a fast growth rate and low cost, and is suitable for the manufacturing of laser devices.
Smart Images

Figure CN118880467A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a guanidine phosphite [C(NH2)3]2HPO3 nonlinear optical crystal, a preparation method and application thereof. Background Art
[0002] Short-wavelength nonlinear optical crystals can use their frequency conversion properties to convert near-infrared, visible and other band lasers into short-wavelength lasers, and have important application value in the fields of medical treatment, communication, scientific research, etc. As we all know, the current short-wavelength nonlinear optical crystals are Chinese brand crystals KBe2BO3F2 (KBBF), BaB2O4 (BBO) and LiB3O5 (LBO), but these crystals have shortcomings such as low birefringence and difficulty in growing large-sized crystals, which limit their application to a certain extent. Therefore, the preparation and synthesis of new short-wavelength nonlinear optical crystal materials with excellent comprehensive performance is of great significance and practical value.
[0003] When designing and developing new short-wavelength nonlinear optical crystals, people hope to obtain crystals with large second-order nonlinear coefficients, wide light transmission range, short cutoff edges, and moderate birefringence. Summary of the invention
[0004] The present invention aims to provide a guanidine phosphite nonlinear optical crystal, the chemical formula of the crystal is [C(NH2)3]2HPO3, the molecular weight is 200.15, belongs to the monoclinic system, the space group is Cm, and the unit cell parameters are α=90°,β=119.607(3)°,γ=90°,the unit cell volume is
[0005] Another object of the present invention is to provide a method for preparing guanidine phosphite [C(NH2)3]2HPO3 nonlinear optical crystals, which adopts a melt method, a high-temperature melt method or a vacuum packaging method to grow the crystals.
[0006] Another object of the present invention is to provide the use of guanidine phosphite [C(NH2)3]2HPO3 nonlinear optical crystal.
[0007] The present invention discloses a guanidine phosphite nonlinear optical crystal, the chemical formula of the crystal is [C(NH2)3]2HPO3, the molecular weight is 200.15, it belongs to the monoclinic system, the space group is Cm, and the unit cell parameters are α=90°,β=119.607(3)°,γ=90°,the unit cell volume is
[0008] The method for preparing the guanidine phosphite nonlinear optical crystal adopts an evaporation method, a hydrothermal method or a room temperature solution method to grow the crystal;
[0009] The evaporation method for growing guanidine phosphite crystals is specifically performed in the following steps:
[0010] a. Mix the compound containing [C(NH2)3] and the compound containing P in a molar ratio of [C(NH2)3]:P=2:1, add 5-25 ml of deionized water, mix and dissolve them fully to obtain a mixed solution, wherein the compound containing [C(NH2)3] is [C(NH2)3]2CO3, [C(NH2)3]NO3, [C(NH2)3]HF2 or [C(NH2)3]Cl, and the compound containing P is H3PO3 or K2HPO3;
[0011] b. placing the mixed solution in step a in a resistance furnace, heating it to 40-90° C. at a rate of 10-20° C. / h, and keeping it at a constant temperature for 5-15 days to evaporate the solvent, and after the crystal growth is completed, a guanidine phosphite nonlinear optical crystal can be obtained;
[0012] The hydrothermal method for growing guanidine phosphite crystals is specifically performed in the following steps:
[0013] a. Mix the compound containing [C(NH2)3] and the compound containing P in a molar ratio of [C(NH2)3]:P=2:1, add 10-30 ml of deionized water, mix and dissolve them fully to obtain a mixed solution, wherein the compound containing [C(NH2)3] is [C(NH2)3]2CO3, [C(NH2)3]NO3, [C(NH2)3]HF2 or [C(NH2)3]Cl, and the compound containing P is H3PO3 or K2HPO3;
[0014] b. Transfer the mixed solution in step a into a polytetrafluoroethylene liner of a hydrothermal reactor with a volume of 23-100 ml, and tighten and seal the reactor; then heat it to 150-220° C. at a rate of 10-20° C. / h, keep it at a constant temperature for 1-3 days, and then cool it to room temperature at a rate of 1-3° C. / h to obtain a guanidine phosphite nonlinear optical crystal;
[0015] The room temperature solution method for growing guanidine phosphite crystals is specifically performed in the following steps:
[0016] a. Mix the compound containing [C(NH2)3] and the compound containing P in a molar ratio of [C(NH2)3]:P=2:1, add 0-150 ml of deionized water, mix and dissolve them fully to obtain a mixed solution, wherein the compound containing [C(NH2)3] is [C(NH2)3]2CO3, [C(NH2)3]NO3, [C(NH2)3]HF2 or [C(NH2)3]Cl, and the compound containing P is H3PO3 or K2HPO3;
[0017] b. Ultrasonic treatment of the mixed solution in step a to fully mix and dissolve the mixed solution to obtain a clear solution, tightly seal the container with a polyvinyl chloride film, place the container in a static environment without shaking, pollution, or air convection, poke several small holes in the sealing film, and leave the container at room temperature for 10-15 days;
[0018] c. When crystals in the solution precipitate and gradually grow, guanidine phosphite nonlinear optical crystals are obtained.
[0019] The guanidine phosphite nonlinear optical crystal is used in preparing harmonic light output of double, triple and quadruple frequency of 1064nm fundamental frequency light output by Nd:YAG laser.
[0020] The guanidine phosphite nonlinear optical crystal is used in preparing ultraviolet frequency-doubled light output below 266nm.
[0021] The guanidine phosphite nonlinear optical crystal is used in preparing a frequency doubling generator, an up or down frequency converter or an optical parametric oscillator.
[0022] The invention discloses a method for preparing a guanidine phosphite nonlinear optical crystal. The container used in the preparation process is a polytetrafluoroethylene beaker, a polytetrafluoroethylene liner, and a hydrothermal kettle with a stainless steel liner equipped with a platinum sleeve. Before use, the container must be cleaned with acid, then rinsed with deionized water, and dried. The resistance furnace used is a muffle furnace or a drying oven.
[0023] By adopting the preparation method of guanidine phosphite nonlinear optical crystal described in the present invention, a centimeter-sized [C(NH2)3]2HPO3 nonlinear optical crystal can be obtained. By using a large-sized container and extending the growth period of the crystal, a corresponding large-sized nonlinear optical crystal [C(NH2)3]2HPO3 can be obtained. During the growth of the [C(NH2)3]2HPO3 nonlinear optical crystal, the crystal is easy to grow, transparent and without wrapping, and has the advantages of fast growth rate, low cost, and easy acquisition of large-sized crystals.
[0024] By adopting the preparation method of the guanidine phosphite nonlinear optical crystal described in the present invention, a large-sized [C(NH2)3]2HPO3 nonlinear optical crystal is obtained. According to the crystallographic data of the crystal, the crystal blank is oriented, the crystal is cut according to the required angle, thickness and cross-sectional size, and the light-transmitting surface of the crystal is polished. Then, the crystal can be used as a nonlinear optical device. The [C(NH2)3]2HPO3 nonlinear optical crystal has the advantages of a wide light transmission band, stable physical and chemical properties, and easy processing and storage. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The powder XRD spectrum of the compound [C(NH2)3]2HPO3 of the present invention;
[0026] Figure 2 It is a structural diagram of the [C(NH2)3]2HPO3 crystal of the present invention;
[0027] Figure 3 This is a working principle diagram of the nonlinear optical device made of [C(NH2)3]2HPO3 crystal of the present invention, wherein 1 is a laser, 2 is an emitted light beam, 3 is a [C(NH2)3]2HPO3 crystal, 4 is an output light beam, and 5 is a filter. DETAILED DESCRIPTION
[0028] The present invention is further described below in conjunction with the examples. It should be noted that the following examples cannot be used to limit the scope of protection of the present invention, and any improvements made on the basis of the present invention do not violate the spirit of the present invention. The raw materials or equipment used in the present invention, unless otherwise specified, are all commercially available.
[0029] Example 1
[0030] According to the reaction formula: [C(NH2)3]2CO3+H3PO3→[C(NH2)3]2HPO3+H2O+CO2, the [C(NH2)3]2HPO3 nonlinear optical crystal was prepared by evaporation method:
[0031] a. Mix [C(NH2)3]2CO3 and H3PO3 in a molar ratio of 1:1, add 5 ml of deionized water and mix and dissolve to obtain a mixed solution, and then treat the mixed solution with ultrasound to fully mix and dissolve it to obtain a clear solution;
[0032] b. Place the clarified solution in step a in a resistance furnace, raise the temperature to 90° C. at a rate of 10° C. / h, and keep the temperature constant for 10 days to evaporate the solvent. When the crystal growth is completed, a guanidine phosphite nonlinear optical crystal with a size of Φ5 mm×2 mm×1.3 mm is obtained.
[0033] Example 2
[0034] According to the reaction formula: 2[C(NH2)3]Cl+H3PO3→[C(NH2)3]2HPO3+2HCl, the [C(NH2)3]2HPO3 nonlinear optical crystal was prepared by evaporation method:
[0035] a. Mix [C(NH2)3]Cl and H3PO3 in a molar ratio of 2:1, add 20 ml of deionized water to mix and dissolve to obtain a mixed solution, and then treat the mixed solution with ultrasound to fully mix and dissolve to obtain a clear solution;
[0036] b. Place the clarified solution in step a in a resistance furnace, raise the temperature to 70°C at a rate of 20°C / h, and keep it at a constant temperature for 12 days to evaporate the solvent. When the crystal growth is completed, a guanidine phosphite nonlinear optical crystal with a size of Φ3mm×1mm×0.6mm can be obtained.
[0037] Example 3
[0038] According to the reaction formula: 2[C(NH2)3]HF2+K2HPO3→[C(NH2)3]2HPO3+2KF+2HF, the [C(NH2)3]2HPO3 nonlinear optical crystal was prepared by evaporation method:
[0039] a. Mix [C(NH2)3]HF2 and K2HPO3 in a molar ratio of 2:1, add 25 ml of deionized water, stir evenly to obtain a mixed solution, and treat the mixed solution with ultrasound to make it fully mixed and dissolved to obtain a clear solution;
[0040] b. Place the clarified solution in step a in a resistance furnace, raise the temperature to 60°C at a rate of 10°C / h, and keep it at a constant temperature for 10 days to evaporate the solvent. Crystals will precipitate and gradually grow. When the crystal growth is completed, a [C(NH2)3]2HPO3 nonlinear optical crystal with a size of Φ6mm×2.5mm×2mm is obtained.
[0041] Example 4
[0042] According to the reaction formula: 2[C(NH2)3]NO3+H3PO3→[C(NH2)3]2HPO3+2HNO3, the [C(NH2)3]2HPO3 nonlinear optical crystal was prepared by evaporation method:
[0043] a. Mix [C(NH2)3]NO3 and H3PO3 in a molar ratio of 2:1, add 10 ml of deionized water, stir evenly to obtain a mixed solution, and then treat the mixed solution with ultrasound to fully mix and dissolve it to obtain a clear solution;
[0044] b. Place the clarified solution in step a in a resistance furnace, raise the temperature to 85°C at a rate of 10°C / h, and keep it at a constant temperature for 10 days to evaporate the solvent. Crystals will precipitate and gradually grow. When the crystal growth is completed, a [C(NH2)3]2HPO3 nonlinear optical crystal with a size of Φ4mm×1.5mm×0.4mm is obtained.
[0045] Example 5
[0046] According to the reaction formula: [C(NH2)3]2CO3+H3PO3→[C(NH2)3]2HPO3+H2O+CO2, the [C(NH2)3]2HPO3 nonlinear optical crystal was prepared by hydrothermal method:
[0047] a. Mix [C(NH2)3]2CO3 and H3PO3 in a molar ratio of 1:1, add 10 ml of deionized water, stir evenly to fully mix and dissolve, and obtain a mixed solution;
[0048] b. Transfer the mixed solution in step a into the polytetrafluoroethylene liner of a hydrothermal reactor with a volume of 23 ml, and tighten and seal the reactor; then heat it to 220° C. at a rate of 10° C. / h, keep it at a constant temperature for 2 days, and then cool it to room temperature at a rate of 1° C. / h to obtain a guanidine phosphite nonlinear optical crystal with a size of 3 mm×1.5 mm×0.6 mm.
[0049] Example 6
[0050] According to the reaction formula: 2[C(NH2)3]Cl+H3PO3→[C(NH2)3]2HPO3+2HCl, the [C(NH2)3]2HPO3 nonlinear optical crystal was prepared by hydrothermal method:
[0051] a. Mix [C(NH2)3]Cl and H3PO3 in a molar ratio of 2:1, add 15 ml of deionized water to mix and dissolve them thoroughly to obtain a mixed solution;
[0052] b. Transfer the mixed solution in step a into the polytetrafluoroethylene liner of a hydrothermal reactor with a volume of 23 ml, and tighten and seal the mouth of the hydrothermal reactor, place it in a constant temperature box, heat it to 180°C at a rate of 20°C / h, keep the temperature constant for 3 days, then cool it to room temperature at a rate of 1°C / h, open the reactor, and you will get a [C(NH2)3]2HPO3 nonlinear optical crystal with a size of 2.4mm×1.4mm×0.6mm.
[0053] Example 7
[0054] According to the reaction formula: 2[C(NH2)3]HF2+K2HPO3→[C(NH2)3]2HPO3+2KF+2HF, the compound [C(NH2)3]2HPO3 nonlinear optical crystal was synthesized by hydrothermal method:
[0055] a. Mix [C(NH2)3]HF2 and K2HPO3 in a molar ratio of 2:1, add 30 ml of deionized water to mix and dissolve them fully to obtain a mixed solution;
[0056] b. Transfer the mixed solution in step a into the polytetrafluoroethylene liner of a hydrothermal reactor with a volume of 100 ml, and tighten and seal the mouth of the hydrothermal reactor, place it in a constant temperature box, heat it to 150°C at a rate of 15°C / h, keep it at a constant temperature for 3 days, then cool it to room temperature at a rate of 2°C / h, open the reactor, and you will get a [C(NH2)3]2HPO3 nonlinear optical crystal with a size of 3.6mm×1.9mm×0.8mm.
[0057] Example 8
[0058] According to the reaction formula: 2[C(NH2)3]NO3+H3PO3→[C(NH2)3]2HPO3+2HNO3, the compound [C(NH2)3]2HPO3 nonlinear optical crystal was synthesized by hydrothermal method:
[0059] a. Mix [C(NH2)3]NO3 and H3PO3 in a molar ratio of 2:1, add 25 ml of deionized water, stir evenly, mix and dissolve them fully, and obtain a mixed solution;
[0060] b. Transfer the mixed solution in step a into the polytetrafluoroethylene lining of a hydrothermal reactor with a volume of 80 ml, place the reactor in a constant temperature box, raise the temperature to 145°C at a rate of 15°C / h, keep it at a constant temperature for 2 days, then cool it to room temperature at a rate of 2°C / h, open the high-pressure reactor, and obtain a [C(NH2)3]2HPO3 nonlinear optical crystal with a size of 0.6mm×0.3mm×0.2mm.
[0061] Example 9
[0062] According to the reaction formula: 2[C(NH2)3]Cl+H3PO3→[C(NH2)3]2HPO3+2HCl, [C(NH2)3]2HPO3 nonlinear optical crystal was prepared by room temperature solution method:
[0063] a. Mix [C(NH2)3]Cl and H3PO3 in a molar ratio of 2:1, add 150 ml of deionized water, stir evenly to fully mix and dissolve, and obtain a mixed solution;
[0064] b. Ultrasonic treatment of the mixed solution in step a to fully mix and dissolve the mixed solution to obtain a clear solution, tightly seal the container with a polyvinyl chloride film, place the container in a static environment without shaking, pollution, or air convection, poke a number of small holes in the sealing film, and leave the container at room temperature for 10 days;
[0065] c. Wait for crystals to precipitate out of the solution and grow gradually. When the reaction is finished, a [C(NH2)3]2HPO3 nonlinear optical crystal with a size of 9mm×5mm×2mm is obtained.
[0066] Example 10
[0067] According to the reaction formula: [C(NH2)3]2CO3+H3PO3→[C(NH2)3]2HPO3+H2O+CO2, the [C(NH2)3]2HPO3 nonlinear optical crystal was prepared by the room temperature solution method:
[0068] a. Mix [C(NH2)3]2CO3 and H3PO3 in a molar ratio of 1:1, add 60 ml of deionized water, stir evenly, mix and dissolve them fully, and obtain a mixed solution;
[0069] b. Ultrasonic treatment of the mixed solution in step a to fully mix and dissolve the mixed solution to obtain a clear solution. The container is tightly sealed with a polyvinyl chloride film and placed in a static environment without shaking, pollution, or air convection. Several small holes are punched in the sealing film and the container is left standing at room temperature for 12 days.
[0070] c. When the crystals in the solution precipitate and gradually grow, the reaction is completed, and a [C(NH2)3]2HPO3 nonlinear optical crystal with a size of 5mm×2mm×1mm is obtained.
[0071] Embodiment 11
[0072] According to the reaction formula: 2[C(NH2)3]NO3+H3PO3→[C(NH2)3]2HPO3+2HNO3, [C(NH2)3]2HPO3 nonlinear optical crystal was prepared by room temperature solution method:
[0073] a. Mix [C(NH2)3]NO3 and H3PO3 in a molar ratio of 2:1, add 20 ml of deionized water, stir evenly to fully mix and dissolve, and obtain a mixed solution;
[0074] b. Ultrasonic treatment of the mixed solution in step a to fully mix and dissolve the mixed solution to obtain a clear solution, tightly seal the container with a polyvinyl chloride film, place the container in a static environment without shaking, pollution, or air convection, poke a number of small holes in the sealing film, and leave the container at room temperature for 13 days;
[0075] c. When the crystals in the solution precipitate and gradually grow, the reaction is completed, and a [C(NH2)3]2HPO3 nonlinear optical crystal with a size of 2mm×1.2mm×0.7mm is obtained.
[0076] Example 12
[0077] According to the reaction formula: 2[C(NH2)3]HF2+K2HPO3→[C(NH2)3]2HPO3+2KF+2HF, [C(NH2)3]2HPO3 nonlinear optical crystal was prepared by room temperature solution method:
[0078] a. Mix [C(NH2)3]HF2 and KH2PO3 in a molar ratio of 2:1, add 30 ml of deionized water, stir evenly, and mix and dissolve them fully to obtain a mixed solution;
[0079] b. Ultrasonic treatment of the mixed solution in step a to fully mix and dissolve the mixed solution to obtain a clear solution, tightly seal the container with a polyvinyl chloride film, place the container in a static environment without shaking, pollution, or air convection, poke a number of small holes in the sealing film, and leave the container at room temperature for 14 days;
[0080] c. Wait for crystals to precipitate out of the solution and grow gradually. When the reaction is finished, a [C(NH2)3]2HPO3 nonlinear optical crystal with a size of 3.2 mm×1.3 mm×0.7 mm is obtained.
[0081] Embodiment 13
[0082] According to the reaction formula: 2[C(NH2)3]HF2+H3PO3→[C(NH2)3]2HPO3+4HF, [C(NH2)3]2HPO3 nonlinear optical crystal was prepared by room temperature solution method:
[0083] a. Mix [C(NH2)3]HF2 and H3PO3 in a molar ratio of 2:1, add 70 ml of deionized water, stir evenly, mix and dissolve them fully, and obtain a mixed solution;
[0084] b. Ultrasonic treatment of the mixed solution in step a to fully mix and dissolve the mixed solution to obtain a clear solution, tightly seal the container with a polyvinyl chloride film, place the container in a static environment without shaking, pollution, or air convection, poke a number of small holes in the sealing film, and leave the container at room temperature for 15 days;
[0085] c. Wait for crystals to precipitate out of the solution and grow gradually. When the reaction is finished, a [C(NH2)3]2HPO3 nonlinear optical crystal with a size of 6.2 mm×4.7 mm×2 mm is obtained.
[0086] Embodiment 14
[0087] Any [C(NH2)3]2HPO3 nonlinear optical crystal obtained in Examples 1-14 is processed in a matching direction, and the attached Figure 3As shown, it is placed at position 3. At room temperature, a Q-switched Nd:YAG laser is used as the light source. The incident wavelength is 1064nm. The infrared light beam 2 with a wavelength of 1064nm emitted by the Q-switched Nd:YAG laser 1 is incident on the [C(NH2)3]2HPO3 single crystal 3, generating green frequency-doubled light with a wavelength of 532nm. The output intensity is about 0.8 times that of KDP under the same conditions. At the same time, under the same experimental setup, purple frequency-doubled light with a wavelength of 266nm is generated, and the output intensity is 0.1 times that of BBO under the same conditions.
Claims
1. A guanidine phosphite nonlinear optical crystal, characterized in that The chemical formula of the crystal is [C(NH2)3]2HPO3, the molecular weight is 200.15, it belongs to the monoclinic system, and the space group is Cm , the unit cell parameters are a =13.0197(14) Å, b =7.3168(7) Å, c =11.7448(19) Å, α= 90°, β= 119.607(3)°, γ= 90°, unit cell volume is 972.8(2)Å 3 .
2. The method for preparing the guanidine phosphite nonlinear optical crystal according to claim 1, characterized in that Growing crystals by evaporation, hydrothermal or room temperature solution methods; The evaporation method for growing guanidine phosphite crystals is specifically performed in the following steps: a. Mix the compound containing [C(NH2)3] and the compound containing P in a molar ratio of [C(NH2)3]:P=2:1, add 5-25 ml of deionized water, mix and dissolve them fully to obtain a mixed solution, wherein the compound containing [C(NH2)3] is [C(NH2)3]2CO3, [C(NH2)3]NO3, [C(NH2)3]HF2 or [C(NH2)3]Cl, and the compound containing P is H3PO3 or K2HPO3; b. placing the mixed solution in step a in a resistance furnace, heating it to 40-90° C. at a rate of 10-20° C. / h, and keeping it at a constant temperature for 5-15 days to evaporate the solvent, and after the crystal growth is completed, a guanidine phosphite nonlinear optical crystal can be obtained; The hydrothermal method for growing guanidine phosphite crystals is specifically performed in the following steps: a. Mix the compound containing [C(NH2)3] and the compound containing P in a molar ratio of [C(NH2)3]:P=2:1, add 10-30 ml of deionized water, mix and dissolve them fully to obtain a mixed solution, wherein the compound containing [C(NH2)3] is [C(NH2)3]2CO3, [C(NH2)3]NO3, [C(NH2)3]HF2 or [C(NH2)3]Cl, and the compound containing P is H3PO3 or K2HPO3; b. Transfer the mixed solution in step a into a polytetrafluoroethylene liner of a hydrothermal reactor with a volume of 23-100 ml, and tighten and seal the reactor; then heat it to 150-220° C. at a rate of 10-20° C. / h, keep it at a constant temperature for 1-3 days, and then cool it to room temperature at a rate of 1-3° C. / h to obtain a guanidine phosphite nonlinear optical crystal; The room temperature solution method for growing guanidine phosphite crystals is specifically performed in the following steps: a. Mix the compound containing [C(NH2)3] and the compound containing P in a molar ratio of [C(NH2)3]:P=2:1, add 0-150 ml of deionized water, mix and dissolve them fully to obtain a mixed solution, wherein the compound containing [C(NH2)3] is [C(NH2)3]2CO3, [C(NH2)3]NO3, [C(NH2)3]HF2 or [C(NH2)3]Cl, and the compound containing P is H3PO3 or K2HPO3; b. Ultrasonic treatment of the mixed solution in step a to fully mix and dissolve the mixed solution to obtain a clear solution, tightly seal the container with a polyvinyl chloride film, place the container in a static environment without shaking, pollution, or air convection, poke several small holes in the sealing film, and leave the container at room temperature for 10-15 days; c. When crystals in the solution precipitate and gradually grow, guanidine phosphite nonlinear optical crystals are obtained.
3. Use of the guanidine phosphite nonlinear optical crystal as claimed in claim 1 in preparing harmonic light output of 1064nm fundamental frequency light output by Nd:YAG laser for double, triple and quadruple frequency.
4. Use of the guanidine phosphite nonlinear optical crystal as claimed in claim 1 in the preparation of ultraviolet frequency-doubled light output below 266 nm.
5. Use of the guanidine phosphite nonlinear optical crystal as claimed in claim 1 in preparing a frequency doubling generator, an up or down frequency converter or an optical parametric oscillator.
Citation Information
Patent Citations
Nonlinear optical crystal monoflurophospate
CN109208077A
Guanidine tetrafluoroborate nonlinear optical crystal and preparation method and application thereof
CN112760717A
Preparation method and application of nonlinear optical crystal germanium phosphite
CN114032614A
Fire retardant and fireproof processing process
JP1982153072A
Cited By
Compound guanidine calcium nitrate, guanidine calcium nitrate birefringent crystal, preparation method and application
CN119684164A
Compound calcium guanidine nitrate and calcium guanidine nitrate birefringent crystals and preparation method and use thereof
CN119684164B
Compound guanidine difluorophosphate, guanidine difluorophosphate nonlinear optical crystal, and preparation method and application of compound guanidine difluorophosphate nonlinear optical crystal
CN119775171A
Compound guanidine difluorophosphate and guanidine difluorophosphate nonlinear optical crystal as well as preparation method and use thereof
CN119775171B
Dihydroguanidino urea phosphite nonlinear optical crystal as well as preparation method and application thereof
CN120099648A