Positive pole piece as well as preparation method and application thereof

By introducing a sandwich structure into the positive electrode, the problem of uneven distribution of conductive agent is solved, which improves the conductivity and rate performance of lithium-ion batteries and extends the battery's lifespan.

CN118888680APending Publication Date: 2024-11-01HUIZHOU TOPBAND ELECTRICAL TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410998726.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

In traditional positive electrode sheets, the conductive agent is unevenly distributed during the coating process, resulting in poor conductivity and affecting the rate performance of lithium-ion batteries.

Method used

A sandwich structure is introduced into the positive electrode, including a positive current collector, a first active layer, a conductive layer and a second active layer. The conductive layer is composed of a first conductive agent and a dispersant to ensure uniform distribution of the conductive agent.

Benefits of technology

It improves the overall conductivity of the positive electrode, enhances the rate performance of the battery, reduces temperature rise during high-rate discharge, and extends the cycle life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118888680A_ABST
    Figure CN118888680A_ABST
Patent Text Reader

Abstract

The invention relates to a pole piece as well as a preparation method and application thereof. The positive pole piece comprises a positive current collector, and a first active layer, a conductive layer and a second active layer which are sequentially stacked on the surface of the positive current collector, materials of the conductive layer include a first conductive agent and a dispersant. The positive pole piece comprises a first active layer, a conductive layer and a second active layer which are sequentially stacked on the surface of a positive current collector, namely, the positive pole piece has a sandwich structure. The conductive layer is additionally arranged between the first active layer and the second active layer, so that the overall conductivity of the positive pole piece can be improved. When the positive pole piece is applied to the battery, the rate capability of the battery can be improved, and meanwhile, the battery can have a relatively low temperature rise value during high-rate discharge, so that the battery has relatively long cycle life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of secondary batteries, and in particular to a positive electrode plate and a preparation method and application thereof. Background Art

[0002] At present, lithium-ion batteries have two major development directions, one is the direction of high energy density, and the other is the direction of high rate. Among them, the performance of high-rate lithium-ion batteries is greatly affected by the positive electrode of the battery. The reason is that the positive electrode material is usually a lithium-containing metal oxide, which has relatively poor electronic conductivity. In the preparation process of traditional positive electrode sheets, during the drying process after the positive electrode slurry is coated, part of the conductive agent in the positive electrode slurry will be brought to the surface of the coating as the solvent evaporates, resulting in uneven distribution of the conductive agent in the coating, resulting in insufficient conductive agent inside the coating, affecting the conductivity of the positive electrode sheet, and thus affecting the rate performance of the battery. Summary of the invention

[0003] Based on this, it is necessary to provide a positive electrode sheet and a preparation method and application thereof. The positive electrode sheet of the present application has good conductivity and can achieve good rate performance of the battery.

[0004] In a first aspect, the present application provides a positive electrode plate, including a positive electrode current collector, and a first active layer, a conductive layer and a second active layer sequentially stacked on the surface of the positive electrode current collector; the material of the conductive layer includes a first conductive agent and a dispersant.

[0005] In some embodiments, the material of the first active layer includes a first active material, a second conductive agent, and a first binder.

[0006] In some embodiments, the material of the second active layer includes a second active material, a third conductive agent, and a second binder.

[0007] In some embodiments, based on the mass percentage of the first active layer, the mass percentage of the first active material is 90%-96%, the mass percentage of the second conductive agent is 2%-6%, and the mass percentage of the first binder is 2%-4%.

[0008] In some embodiments, the mass ratio of the first conductive agent to the dispersant is (2-5):1.

[0009] In some embodiments, based on the mass percentage of the second active layer, the mass percentage of the second active material is 90%-96%, the mass percentage of the third conductive agent is 2%-6%, and the mass percentage of the second binder is 2%-4%.

[0010] In some embodiments, the surface density of the first active layer is 4 mg / cm 2 ~8mg / cm 2 .

[0011] In some embodiments, the surface density of the conductive layer is 0.1 mg / cm 2 ~1mg / cm 2 .

[0012] In some embodiments, the surface density of the second active layer is 4 mg / cm 2 ~8mg / cm 2 .

[0013] In some embodiments, the first active material and the second active material are each independently selected from one or more of lithium iron phosphate, lithium iron manganese phosphate, lithium nickel cobalt manganese oxide, lithium cobalt oxide, and lithium manganese oxide.

[0014] In some embodiments, the first conductive agent, the second conductive agent and the third conductive agent are each independently selected from one or more of carbon black, acetylene black, carbon fiber, flake graphite, carbon nanotubes and graphene.

[0015] In some embodiments, the first binder and the second binder are each independently selected from one or more of polyvinylidene fluoride, polytetrafluoroethylene, and polyacrylic acid.

[0016] In some embodiments, the first active layer, the conductive layer, and the second active layer are sequentially stacked on two opposite surfaces of the positive electrode current collector.

[0017] In a second aspect, the present application provides a method for preparing a positive electrode sheet, comprising the following steps:

[0018] Forming a first active layer, a conductive layer and a second active layer stacked in sequence on the surface of the positive electrode current collector;

[0019] Wherein, the material of the conductive layer includes a first conductive agent and a dispersant.

[0020] In some embodiments, the first active layer is prepared by the following method: using a first slurry to prepare the first active layer on the surface of the positive electrode collector; the first slurry includes a first mixed raw material and a dispersion medium, and the first mixed raw material includes 90% to 96% by mass of a first active material, 2% to 6% by mass of a second conductive agent, and 2% to 4% by mass of a first binder.

[0021] In some embodiments, the conductive layer is prepared by the following method: using a second slurry to prepare the conductive layer on the surface of the first active layer; the second slurry includes a second mixed raw material and a dispersion medium, and in the second mixed raw material, the mass ratio of the first conductive agent to the dispersant is (2~5):1.

[0022] In some embodiments, the second active layer is prepared by the following method: the second active layer is prepared on the surface of the conductive layer using a third slurry; the third slurry includes a third mixed raw material and a dispersion medium, and the third mixed raw material includes 90% to 96% by mass of the second active material, 2% to 6% by mass of the third conductive agent, and 2% to 4% by mass of the second binder.

[0023] In some embodiments, the mass percentage of the first mixed raw material to the first slurry is 10% to 60%.

[0024] In some embodiments, the mass percentage of the second mixed raw material in the second slurry is 1.5% to 12%.

[0025] In some of the embodiments, the mass percentage of the third mixed raw material to the third slurry is 10% to 60%.

[0026] In a third aspect, the present application provides a secondary battery, comprising the positive electrode sheet described in any one of the above items or a positive electrode sheet prepared by the method for preparing the positive electrode sheet described in any one of the above items.

[0027] In a fourth aspect, the present application provides an electrical device, comprising the above-mentioned secondary battery.

[0028] The positive electrode sheet includes a first active layer, a conductive layer and a second active layer stacked in sequence on the surface of the positive electrode current collector, that is, the positive electrode sheet has a sandwich structure. Adding a conductive layer between the first active layer and the second active layer can improve the overall conductivity of the positive electrode sheet. When the positive electrode sheet is applied to a battery, it can improve the rate performance of the battery. At the same time, it can also enable the battery to have a lower temperature rise value when discharged at a high rate, so that the battery has a longer cycle life. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] FIG1 is a schematic diagram of the structure of a positive electrode sheet provided in one embodiment of the present application;

[0030] FIG2 is a schematic diagram comparing the cycle performance of lithium iron phosphate batteries in Example 1, Example 2 and Comparative Example 1 of the present application;

[0031] 3 is a schematic diagram comparing the cycle performance of the nickel cobalt manganese oxide lithium batteries in Example 3, Example 4 and Comparative Example 2 of the present application.

[0032] Description of Reference Numerals

[0033] 10. Positive electrode current collector; 20. First active layer; 30. Conductive layer; 40. Second active layer. DETAILED DESCRIPTION

[0034] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.

[0035] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0036] In the description of the present application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.

[0037] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one of the features. In the description of this application, "plurality" means at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0038] As shown in FIG1 , an embodiment of the present application provides a positive electrode plate, including a positive electrode current collector 10, and a first active layer 20, a conductive layer 30 and a second active layer 40 sequentially stacked on the surface of the positive electrode current collector 10; the material of the conductive layer 30 includes a first conductive agent and a dispersant.

[0039] The above-mentioned positive electrode plate includes a first active layer 20, a conductive layer 30 and a second active layer 40 which are stacked in sequence on the surface of the positive electrode collector 10, that is, the positive electrode plate has a sandwich structure. Adding a conductive layer 30 between the first active layer 20 and the second active layer 40 can improve the overall conductivity of the positive electrode plate. When the positive electrode plate is applied to a battery, the rate performance of the battery can be improved. At the same time, it can also enable the battery to have a lower temperature rise value when discharged at a high rate, so that the battery has a longer cycle life.

[0040] In some embodiments, the material of the first active layer 20 includes a first active material, a second conductive agent, and a first binder.

[0041] In some embodiments, the material of the second active layer 40 includes a second active material, a third conductive agent, and a second binder.

[0042] In some embodiments, based on the mass percentage of the first active layer 20, the mass percentage of the first active material is 90%-96%, the mass percentage of the second conductive agent is 2%-6%, and the mass percentage of the first binder is 2%-4%.

[0043] Optionally, the mass percentage of the first active material is 90%, 91%, 92%, 93%, 94%, 95% or 96% in terms of mass percentage of the first active layer 20. Alternatively, the mass percentage of the first active material may also be within the range between any two of the above mass percentages.

[0044] Optionally, the mass percentage of the second conductive agent is 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5% or 6% based on the mass percentage of the first active layer 20. Alternatively, the mass percentage of the second conductive agent may also be within the range between any two of the above mass percentages.

[0045] Optionally, the mass percentage of the first binder is 2%, 2.5%, 3%, 3.5% or 4% based on the mass percentage of the first active layer 20. Alternatively, the mass percentage of the first binder may also be within the range between any two of the above mass percentages.

[0046] In some embodiments, the mass ratio of the first conductive agent to the dispersant is (2-5):1.

[0047] Optionally, the mass ratio of the first conductive agent to the dispersant is 2: 1, 2.5: 1, 3: 1, 3.5: 1, 4: 1, 4.5: 1 or 5: 1. Alternatively, the mass ratio of the first conductive agent to the dispersant may also be within a range between any two of the above mass ratios.

[0048] In some embodiments, based on the mass percentage of the second active layer 40 , the mass percentage of the second active material is 90%-96%, the mass percentage of the third conductive agent is 2%-6%, and the mass percentage of the second binder is 2%-4%.

[0049] Optionally, the mass percentage of the second active material is 90%, 91%, 92%, 93%, 94%, 95% or 96% in terms of the mass percentage of the second active layer 40. Alternatively, the mass percentage of the second active material may also be within the range between any two of the above mass percentages.

[0050] Optionally, the mass percentage of the third conductive agent is 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5% or 6% based on the mass percentage of the second active layer 40. Alternatively, the mass percentage of the third conductive agent may also be within the range between any two of the above mass percentages.

[0051] Optionally, the mass percentage of the second binder is 2%, 2.5%, 3%, 3.5% or 4% based on the mass percentage of the second active layer 40. Alternatively, the mass percentage of the second binder may also be within the range between any two of the above mass percentages.

[0052] In some embodiments, the first active material and the second active material are each independently selected from one or more of lithium iron phosphate, lithium iron manganese phosphate, lithium nickel cobalt manganese oxide, lithium cobalt oxide, and lithium manganese oxide.

[0053] In some embodiments, the first conductive agent, the second conductive agent and the third conductive agent are each independently selected from one or more of carbon black, acetylene black, carbon fiber, flake graphite, carbon nanotubes and graphene.

[0054] In some embodiments, the dispersant includes polyvinyl pyrrolidone.

[0055] In some embodiments, the first binder and the second binder are each independently selected from one or more of polyvinylidene fluoride, polytetrafluoroethylene, and polyacrylic acid.

[0056] In some embodiments, the surface density of the first active layer 20 is 4 mg / cm 2 ~8mg / cm 2 .

[0057] It is understood that the surface density in this application refers to the weight of dry material per unit area of ​​each layer. Optionally, the surface density of the first active layer 20 is 4 mg / cm 2 , 4.5mg / cm 2 , 5mg / cm 2 , 5.5mg / cm 2 , 6mg / cm 2 、6.5mg / cm 2 , 7mg / cm 2 、7.5mg / cm 2 or 8mg / cm 2 Alternatively, the surface density of the first active layer 20 may also be within the range between any two of the above surface densities.

[0058] In some embodiments, the surface density of the conductive layer 30 is 0.1 mg / cm 2 ~1mg / cm 2 .

[0059] Optionally, the surface density of the conductive layer 30 is 0.1 mg / cm 2 , 0.2mg / cm 2 , 0.3mg / cm 2 , 0.4mg / cm 2 , 0.5mg / cm 2 , 0.6mg / cm 2 , 0.7mg / cm 2 , 0.8mg / cm 2 , 0.9mg / cm 2 or 1mg / cm 2 Alternatively, the surface density of the conductive layer 30 may also be within the range between any two of the above surface densities.

[0060] In some embodiments, the surface density of the second active layer 40 is 4 mg / cm 2 ~8mg / cm 2 .

[0061] Optionally, the surface density of the second active layer 40 is 4 mg / cm 2 , 4.5mg / cm 2 , 5mg / cm 2 , 5.5mg / cm 2 , 6mg / cm 2 、6.5mg / cm 2 , 7mg / cm 2 、7.5mg / cm 2 or 8mg / cm 2Alternatively, the surface density of the second active layer 40 may also be within the range between any two of the above surface densities.

[0062] Referring again to FIG. 1 , in some embodiments, a first active layer 20 , a conductive layer 30 , and a second active layer 40 stacked in sequence are disposed on two opposite surfaces of the positive electrode current collector 10 .

[0063] Another embodiment of the present application provides a method for preparing a positive electrode sheet, comprising the following steps:

[0064] A first active layer 20 , a conductive layer 30 , and a second active layer 40 are sequentially stacked on the surface of the positive electrode current collector 10 ; wherein the material of the conductive layer 30 includes a first conductive agent and a dispersant.

[0065] In some embodiments, the first active layer 20 is prepared by the following method: the first active layer 20 is prepared on the surface of the positive electrode collector 10 using a first slurry; the first slurry includes a first mixed raw material and a dispersion medium, and the first mixed raw material includes 90% to 96% by mass of a first active material, 2% to 6% by mass of a second conductive agent, and 2% to 4% by mass of a first binder.

[0066] In some embodiments, the conductive layer 30 is prepared by the following method: the conductive layer 30 is prepared on the surface of the first active layer 20 using a second slurry; the second slurry includes a second mixed raw material and a dispersion medium, and in the second mixed raw material, the mass ratio of the first conductive agent to the dispersant is (2~5):1.

[0067] In some embodiments, the second active layer is prepared by the following method: the second active layer is prepared on the surface of the conductive layer 30 using a third slurry; the third slurry includes a third mixed raw material and a dispersion medium, and the third mixed raw material includes 90% to 96% by mass of the second active material, 2% to 6% by mass of the third conductive agent, and 2% to 4% by mass of the second binder.

[0068] In some embodiments, the mass percentage of the first mixed raw material to the first slurry is 10% to 60%.

[0069] Optionally, the mass percentage of the first mixed raw material to the first slurry is 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55% or 60%. Alternatively, the mass percentage of the first mixed raw material to the first slurry may also be within the range between any two of the above mass percentages.

[0070] In some of the embodiments, the mass percentage of the second mixed raw material to the second slurry is 1.5% to 12%.

[0071] Optionally, the mass percentage of the second mixed raw material in the second slurry is 1.5%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 10.5%, 11%, 11.5% or 12%. Alternatively, the mass percentage of the second mixed raw material in the second slurry may also be within the range between any two of the above mass percentages.

[0072] In some of the embodiments, the mass percentage of the third mixed raw material to the third slurry is 10% to 60%.

[0073] Optionally, the mass percentage of the third mixed raw material in the third slurry is 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55% or 60%. Alternatively, the mass percentage of the third mixed raw material in the third slurry can also be within the range between any two of the above mass percentages.

[0074] In some embodiments, the dispersion medium includes water or N-methylpyrrolidone.

[0075] Yet another embodiment of the present application provides a secondary battery, comprising any of the above-mentioned positive electrode sheets or a positive electrode sheet prepared by any of the above-mentioned methods for preparing a positive electrode sheet.

[0076] In some embodiments, the secondary battery further includes a negative electrode sheet, an electrolyte, and a separator.

[0077] In some embodiments, the negative electrode sheet includes a negative electrode current collector and a third active layer located on a surface of the negative electrode current collector, and the material of the third active layer includes a third active material, a fourth conductive agent, and a third binder.

[0078] In some embodiments, based on the mass percentage of the third active layer, the mass percentage of the third active material is 92%-96%, the mass percentage of the fourth conductive agent is 1%-3%, and the mass percentage of the third binder is 3%-5%.

[0079] Optionally, the mass percentage of the third active material in the third active layer is 92%, 92.5%, 93%, 93.5%, 94%, 94.5%, 95%, 95.5% or 96%. Alternatively, the mass percentage of the third active material may also be within the range between any two of the above mass percentages.

[0080] Optionally, the mass percentage of the fourth conductive agent is 1%, 1.2%, 1.4%, 1.6%, 1.8%, 2%, 2.2%, 2.4%, 2.6%, 2.8% or 3%. Alternatively, the mass percentage of the fourth conductive agent may also be within the range between any two of the above mass percentages.

[0081] Optionally, the mass percentage of the third binder is 3%, 3.2%, 3.4%, 3.6%, 3.8%, 4%, 4.2%, 4.4%, 4.6%, 4.8% or 5%. Alternatively, the mass percentage of the third binder may also be within the range between any two of the above mass percentages.

[0082] In some embodiments, the third active material includes one or more of artificial graphite, natural graphite, mesophase carbon microbeads, soft carbon, and hard carbon.

[0083] In some embodiments, the fourth conductive agent includes one or more of carbon black, acetylene black, carbon fiber, flake graphite, carbon nanotube, and graphene.

[0084] In some embodiments, the third binder includes at least one of polyvinylidene fluoride, sodium carboxymethyl cellulose and styrene-butadiene rubber.

[0085] In some embodiments, the surface density of the third active layer is 3.5 mg / cm 2 ~9mg / cm 2 .

[0086] Optionally, the surface density of the third active layer is 3.5 mg / cm 2 , 4mg / cm 2 , 4.5mg / cm 2 , 5mg / cm 2 , 5.5mg / cm 2 , 6mg / cm 2 、6.5mg / cm 2 , 7mg / cm 2 、7.5mg / cm 2 , 8mg / cm 2 、8.5mg / cm 2 or 9mg / cm 2 Alternatively, the surface density of the third active layer may also be within the range between any two of the above surface densities.

[0087] In some embodiments, the third active layer is prepared by the following method: using a fourth slurry to prepare the third active layer on the surface of the negative electrode current collector, the fourth slurry includes a fourth mixed raw material and a dispersion medium; the fourth mixed raw material includes 92% to 96% by mass of the third active material, 1% to 3% by mass of the fourth conductive agent, and 3% to 5% by mass of the third binder.

[0088] In some of the embodiments, the mass ratio of the dispersion medium to the fourth mixed raw material is (0.8-1.5):1.

[0089] Optionally, the mass ratio of the dispersion medium to the fourth mixed raw material is 0.8: 1, 0.9: 1, 1: 1, 1.1: 1, 1.2: 1, 1.3: 1, 1.4: 1 or 1.5: 1. Alternatively, the mass ratio of the dispersion medium to the fourth mixed raw material may also be within the range between any two of the above mass ratios.

[0090] In some embodiments, the electrolyte includes a lithium salt and an organic solvent.

[0091] In some embodiments, the lithium salt includes at least one of LiPF6, LiBF4, LiBOB and LiFSI.

[0092] In some embodiments, the concentration of the lithium salt in the electrolyte is 1.1 mol / L to 1.5 mol / L.

[0093] Optionally, the concentration of the lithium salt in the electrolyte is 1.1 mol / L, 1.15 mol / L, 1.2 mol / L, 1.25 mol / L, 1.3 mol / L, 1.35 mol / L, 1.4 mol / L or 1.5 mol / L. Alternatively, the concentration of the lithium salt in the electrolyte may also be within the range between any two of the above concentrations.

[0094] In some embodiments, the organic solvent includes at least one of ethylene carbonate (EC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), diethyl carbonate (DEC), propylene carbonate (PC), ethyl acetate (EA), propyl acetate (PA) and ethyl propionate (EP).

[0095] In some embodiments, the organic solvent includes at least two of EC, EMC, DMC, DEC, PC, EA, PA, and EP.

[0096] In some embodiments, the porosity of the separator is 45% to 55%.

[0097] Optionally, the porosity of the diaphragm is 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54% or 55%. Alternatively, the porosity of the diaphragm may also be within the range between any two of the above porosities.

[0098] In some embodiments, the thickness of the separator is 9 μm to 25 μm.

[0099] Optionally, the thickness of the separator is 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, 20 μm, 21 μm, 22 μm, 23 μm, 24 μm or 25 μm. Alternatively, the thickness of the separator may also be within a range between any two of the above thicknesses.

[0100] Another embodiment of the present application provides an electrical device, including the secondary battery mentioned above.

[0101] The following are specific embodiments

[0102] Example 1

[0103] In this embodiment, the material of the first active layer 20 is a first active material with a mass percentage of 94%, a second conductive agent with a mass percentage of 3.5%, and a first binder with a mass percentage of 2.5%, wherein the first active material is lithium iron phosphate, the second conductive agent is a mixed conductive agent of carbon nanotubes + graphene + carbon black, and the first binder is polyvinylidene fluoride. The first active layer 20 is prepared by coating the first slurry on the two opposite surfaces of the positive electrode current collector 10, drying, and rolling. The dispersion medium in the first slurry is N-methylpyrrolidone, and the mass of N-methylpyrrolidone is 70% of the mass of the first mixed raw material. The surface density of the first active layer 20 is 6mg / cm 2 The second active layer 40 is made of the same material as the first active layer 20, and the surface density of the second active layer 40 is 6 mg / cm 2 The conductive layer 30 is prepared by coating the second slurry on the surface of the first active layer 20, drying and rolling. In the second slurry, the mass percentage of N-methylpyrrolidone is 94%, the dispersant is polyvinylpyrrolidone, the mass percentage is 1%, and the first conductive agent is carbon nanotubes + graphene, the mass percentage is 5%. The surface density of the conductive layer 30 is 0.6 mg / cm 2 . In this embodiment, the third active layer is prepared by coating the fourth slurry on two opposite surfaces of the negative electrode current collector, drying and rolling. The fourth slurry includes water and a fourth mixed raw material. The mass ratio of water to the fourth mixed raw material is 9:10. The fourth mixed raw material includes 95% graphite, 1.5% carbon black, 1.5% sodium carboxymethyl cellulose and 2.0% styrene-butadiene rubber in mass percentages. The surface density of the third active layer is 5.5 mg / cm2 The positive electrode sheet and the negative electrode sheet were assembled into a lithium iron phosphate battery with a capacity of 25Ah, wherein the porosity of the diaphragm was 50%, the thickness was 20μm, the lithium salt of the electrolyte was LiPF6, the concentration was 1.1mol / L, and the solvent of the electrolyte was EC+EMC+DMC+PA.

[0104] Example 2

[0105] The difference between this embodiment and embodiment 1 is that the surface density of the first active layer 20 is 5 mg / cm 2 The surface density of the conductive layer 30 is 0.8 mg / cm 2 The surface density of the second active layer 40 is 8 mg / cm 2 The surface density of the third active layer is 6 mg / cm 2 .

[0106] Example 3

[0107] In this embodiment, the material of the first active layer 20 is 95.5% by mass of the first active material, 2.5% by mass of the second conductive agent, and 2% by mass of the first binder, wherein the first active material is lithium nickel cobalt manganese oxide, the second conductive agent is a mixed conductive agent of carbon nanotubes + graphene + carbon black, and the first binder is polyvinylidene fluoride. The first active layer 20 is prepared by coating the first slurry on the two opposite surfaces of the positive electrode current collector 10, drying, and rolling. The dispersion medium in the first slurry is N-methylpyrrolidone, and the mass of N-methylpyrrolidone is 60% of the mass of the first mixed raw material. The surface density of the first active layer 20 is 4 mg / cm 2 The second active layer 40 is made of the same material as the first active layer 20. The surface density of the second active layer 40 is 6 mg / cm 2 The conductive layer 30 is prepared by coating the second slurry on the surface of the first active layer 20, drying and rolling. In the second slurry, the mass percentage of N-methylpyrrolidone is 94%, the dispersant is polyvinylpyrrolidone, the mass percentage is 1%, and the first conductive agent is carbon nanotubes + graphene, the mass percentage is 5%. The surface density of the conductive layer 30 is 0.5 mg / cm 2 . In this embodiment, the third active layer is prepared by coating the fourth slurry on two opposite surfaces of the negative electrode current collector, drying and rolling. The fourth slurry includes water and a fourth mixed raw material. The mass ratio of water to the fourth mixed raw material is 9:10. The fourth mixed raw material includes 95% graphite, 1.5% carbon black, 1.5% sodium carboxymethyl cellulose and 2.0% styrene-butadiene rubber in mass percentages. The surface density of the third active layer is 5.8 mg / cm 2The positive electrode sheet and the negative electrode sheet were assembled into a nickel cobalt manganese oxide lithium battery with a capacity of 25Ah, wherein the porosity of the diaphragm was 52%, the thickness was 16μm, the lithium salt of the electrolyte was LiPF6, the concentration was 1.2mol / L, and the solvent of the electrolyte was EC+EMC+PC+EP.

[0108] Example 4

[0109] The difference between this embodiment and embodiment 3 is that the surface density of the first active layer 20 is 5 mg / cm 2 The surface density of the conductive layer 30 is 0.6 mg / cm 2 The surface density of the second active layer 40 is 7 mg / cm 2 The surface density of the third active layer is 7.2 mg / cm 2 .

[0110] Comparative Example 1

[0111] The difference between Comparative Example 1 and Example 1 is that the positive electrode sheet in Comparative Example 1 does not include the conductive layer 30 and the second active layer 40, and the surface density of the first active layer 20 is 12 mg / cm 2 .

[0112] Comparative Example 2

[0113] The difference between Comparative Example 2 and Example 3 is that the positive electrode sheet in Comparative Example 2 does not include the conductive layer 30 and the second active layer 40, and the surface density of the first active layer 20 is 10 mg / cm 2 .

[0114] The batteries prepared in Examples 1 to 4 and Comparative Examples 1 and 2 were subjected to rate and cycle performance tests, wherein the test results of Example 1, Example 2 and Comparative Example 1 are shown in Table 1 below:

[0115] Table 1

[0116]

[0117] The test results of Example 3, Example 4 and Comparative Example 2 are shown in Table 2 below:

[0118] Table 2

[0119]

[0120] Referring to Figures 2 and 3 and Tables 1 and 2 above, it can be seen that when the lithium iron phosphate battery is discharged at a high rate, the battery in Example 1 and Example 2 uses the positive electrode plate in the present application, and its temperature rise value is significantly lower than that in Comparative Example 1, and high temperature will accelerate the capacity decay of the battery, therefore, the cycle performance of the battery in Example 1 and Example 2 is significantly better than that in Comparative Example 1. When the nickel cobalt manganese oxide lithium battery is discharged at a high rate, the battery in Example 3 and Example 4 uses the positive electrode plate in the present application, and its temperature rise value is significantly lower than that in Comparative Example 2, and the cycle performance of the battery in Example 3 and Example 4 is significantly better than that in Comparative Example 2.

[0121] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0122] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent of the present application shall be subject to the attached claims, and the description and drawings may be used to interpret the contents of the claims.

Claims

1. A positive electrode sheet, characterized in that: The invention comprises a positive electrode current collector, and a first active layer, a conductive layer and a second active layer which are sequentially stacked on the surface of the positive electrode current collector; the material of the conductive layer comprises a first conductive agent and a dispersant.

2. The positive electrode sheet according to claim 1, characterized in that: The material of the first active layer includes a first active material, a second conductive agent and a first binder; and / or, The material of the second active layer includes a second active material, a third conductive agent and a second binder.

3. The positive electrode sheet according to claim 2, characterized in that: In terms of the mass percentage of the first active layer, the mass percentage of the first active material is 90% to 96%, the mass percentage of the second conductive agent is 2% to 6%, and the mass percentage of the first binder is 2% to 4%; and / or, The mass ratio of the first conductive agent to the dispersant is (2-5):1; and / or, Calculated by mass percentage of the second active layer, the mass percentage of the second active material is 90% to 96%, the mass percentage of the third conductive agent is 2% to 6%, and the mass percentage of the second binder is 2% to 4%.

4. The positive electrode sheet according to claim 3, characterized in that: The first active material and the second active material are each independently selected from one or more of lithium iron phosphate, lithium manganese iron phosphate, lithium nickel cobalt manganese oxide, lithium cobalt oxide, and lithium manganese oxide; and / or, The first conductive agent, the second conductive agent and the third conductive agent are each independently selected from one or more of carbon black, acetylene black, carbon fiber, flake graphite, carbon nanotubes, and graphene; and / or, The dispersant comprises polyvinyl pyrrolidone; and / or, The first binder and the second binder are independently selected from one or more of polyvinylidene fluoride, polytetrafluoroethylene, and polyacrylic acid.

5. The positive electrode sheet according to claim 1, characterized in that: The surface density of the first active layer is 4 mg / cm 2 ~8mg / cm 2 and / or, The surface density of the conductive layer is 0.1 mg / cm 2 ~1mg / cm 2 and / or, The surface density of the second active layer is 4 mg / cm 2 ~8mg / cm 2 .

6. The positive electrode sheet according to any one of claims 1 to 5, characterized in that: The first active layer, the conductive layer, and the second active layer are sequentially stacked on both opposite surfaces of the positive electrode current collector.

7. A method for preparing a positive electrode sheet, characterized in that: The steps include: Forming a first active layer, a conductive layer and a second active layer stacked in sequence on the surface of the positive electrode current collector; Wherein, the material of the conductive layer includes a first conductive agent and a dispersant.

8. The method for preparing a positive electrode sheet according to claim 7, characterized in that: The first active layer is prepared by the following method: using a first slurry to prepare the first active layer on the surface of the positive electrode current collector; the first slurry includes a first mixed raw material and a dispersion medium, the first mixed raw material includes 90% to 96% by mass of a first active material, 2% to 6% by mass of a second conductive agent, and 2% to 4% by mass of a first binder; and / or, The conductive layer is prepared by the following method: using a second slurry to prepare the conductive layer on the surface of the first active layer; the second slurry comprises a second mixed raw material and a dispersion medium, and in the second mixed raw material, the mass ratio of the first conductive agent to the dispersant is (2-5):1; and / or, The second active layer is prepared by the following method: using a third slurry to prepare the second active layer on the surface of the conductive layer; the third slurry includes a third mixed raw material and a dispersion medium, and the third mixed raw material includes 90% to 96% by mass of the second active material, 2% to 6% by mass of the third conductive agent, and 2% to 4% by mass of the second binder.

9. The method for preparing a positive electrode sheet according to claim 8, characterized in that: The mass percentage of the first mixed raw material to the first slurry is 10% to 60%; and / or, The mass percentage of the second mixed raw material to the second slurry is 1.5% to 12%; and / or, The mass percentage of the third mixed raw material to the third slurry is 10% to 60%.

10. A secondary battery, characterized in that: A positive electrode sheet comprising the positive electrode sheet as described in any one of claims 1 to 6 or a positive electrode sheet prepared by the method for preparing the positive electrode sheet as described in any one of claims 7 to 9.

11. An electrical device, characterized in that: The secondary battery according to claim 10 is included.

Citation Information

Cited By

  • Positive electrode sheet, battery, battery pack, and electric device

    WO2026219267A1