Metal-doped core-shell structure silicon-carbon composite material and preparation method thereof

By doping lithium in mesoporous carbon and depositing silicon nitride film to form a silicon-carbon composite material with a core-shell structure, the problem of poor rate performance and cycle performance of silicon-carbon materials in lithium-ion batteries is solved, and more efficient Electrochemical properties and lower expansion rates.

CN118888705APending Publication Date: 2024-11-01ZHIHUA NEW ENERGY TECH (ZHEJIANG) CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410659355.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-27
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Existing silicon-carbon materials have problems such as deviation in rate performance, large expansion and poor circulation performance in lithium-ion batteries, mainly due to poor electronic conductivity and insufficient uniformity of pore structure.

Method used

Lithium-doped mesoporous carbon is used as the core and nanosilicon and silicon nitride films are deposited on it. The silicon-carbon composite material with a core-shell structure is formed through PECVD technology to improve the electronic conductivity and structural stability of the material and reduce expansion.

Benefits of technology

It significantly improves the rate performance and cycling performance of the material, reduces silicon expansion during charging and discharging, and improves first-time efficiency and high-temperature storage performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118888705A_ABST
    Figure CN118888705A_ABST
Patent Text Reader

Abstract

The invention discloses a composite silicon-carbon material and a preparation method thereof, the silicon-carbon composite material has a core-shell structure, the core is a lithium-silicon doped mesoporous carbon material, and the shell is a silicon nitride film. According to the composite material, the uniformity of deposited silicon of the material is improved by utilizing the uniform aperture of mesoporous carbon, the electronic conductivity of the material is improved and the defects of a core of the material are reduced by utilizing lithium-doped mesoporous carbon, and the high-temperature storage performance is improved by passivating the surface of the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of lithium ion battery material preparation, and specifically relates to a metal-doped core-shell structured silicon-carbon composite material and a preparation method thereof. Background Art

[0002] Silicon-carbon materials are used in high-energy-density lithium-ion batteries and other fields due to their high specific capacity, wide material sources, large expansion, and poor electronic conductivity. At present, there are two types of commercial silicon-carbon materials, sand-milled silicon-carbon and silane cracking silicon-carbon. The sand-milled silicon-carbon material has a moderate specific capacity (1250mAh / g), large expansion at full charge (300%), and poor cycle performance; the silane cracking silicon-carbon material has a high specific capacity (1800-1900mAh / g), small expansion at full charge (100%), and good cycle performance, but because the material matrix is ​​a porous structure with poor electronic conductivity, its rate performance deviation is caused, and the porous carbon material has poor pore structure uniformity, resulting in poor consistency of silicon-carbon materials. Mesoporous carbon has good consistency in pore structure, relatively uniform pores, slightly larger pore size, and high strength, so that it can uniformly deposit nanosilicon and reduce expansion. However, due to the poor electronic conductivity of mesoporous carbon itself, it needs to be doped to improve the rate performance of the material. Summary of the invention

[0003] In order to improve the rate performance of silicon-carbon materials, reduce expansion and improve the consistency of materials, the present invention prepares lithium-doped mesoporous carbon, and deposits nano-silicon in its core and silicon nitride on the surface to improve the rate performance and cycle performance of the material.

[0004] The first aspect of the present invention provides a silicon-carbon composite material for lithium-ion batteries, wherein the silicon-carbon composite material presents a core-shell structure, wherein the core is a lithium-silicon doped mesoporous carbon material, and the shell is a silicon nitride film, and the mass ratio of the shell is 1-10wt% calculated based on the mass ratio of the composite material being 100%. The inner layer of lithium-silicon doped mesoporous carbon material is prepared by mixing lithium-doped mesoporous carbon material with silane gas. The lithium-doped mesoporous carbon material is composed of 1-5wt% lithium and 95-99% mesoporous carbon, and the pore size of the mesoporous carbon is 5-10nm.

[0005] A second aspect of the present invention provides a method for preparing a silicon-carbon composite material for a lithium-ion battery, characterized in that it comprises the following steps:

[0006] Step S1: according to the mass ratio of carbon-based precursor: pore-forming agent: lithium amide: organic solvent = 100: 1-5: 1-5: 500-1000, the carbon-based precursor, pore-forming agent and lithium amide are added to the organic solvent and dispersed evenly, spray dried, and cured at a temperature of 300-600°C for 1-6h to obtain a mesoporous carbon precursor; then transferred to a tubular furnace, heated to 500-800°C, and introduced acidic gas for 1-6h to obtain lithium-doped mesoporous carbon.

[0007] Step S2: transfer the lithium-doped mesoporous carbon to a tubular furnace, introduce inert gas to exhaust the air in the tube, and heat to a temperature of 400-600°C, then introduce silane mixed gas at a flow rate of 50-500ml / min and an introduction time of 30-300min to perform nano-silicon deposition to obtain a lithium-silicon mesoporous carbon material; finally, deposit a layer of silicon nitride film on the surface by PECVD to obtain a silicon-carbon composite material.

[0008] Wherein, the carbon-based precursor in step S1 is an amino resin.

[0009] Wherein, the pore-forming agent in step S1 is one or more of polystyrene microspheres, polymethyl methacrylate, and aminocarbamoyl hydrazide.

[0010] Wherein, the organic solvent in step S1 is one or more of acetone, methanol, ethyl acetate and butanone.

[0011] Wherein, the acidic gas in step S1 is one or more of hydrogen sulfide, sulfur dioxide, and hydrogen chloride.

[0012] Wherein, the silane mixed gas in step S2 is a mixed gas of silane and argon, with a volume ratio of 1-5:10.

[0013] Among them, the PECVD test method in step S2 is to transfer the lithium silicon mesoporous carbon material to a tubular furnace, and after evacuating the tubular furnace, maintain the vacuum pressure at 1-5Pa, the deposition temperature is 500-580°C, and then heat the silicon nitride and pass it into the tubular furnace for 10-120 minutes.

[0014] A third aspect of the present invention provides a negative electrode plate for a lithium ion battery, comprising a negative electrode current collector and a negative electrode material coated on at least one surface of the negative electrode current collector, wherein the negative electrode material comprises the above-mentioned silicon-carbon composite material.

[0015] A fourth aspect of the present invention provides a lithium ion battery comprising the above-mentioned negative electrode plate, which also includes a positive electrode plate and a separator between the positive electrode plate and the negative electrode plate.

[0016] Compared with the prior art, the beneficial effects of the present invention are as follows: (1) by doping lithium into mesoporous carbon, the electronic conductivity of the material is improved and the defects of the material are reduced, thereby improving the first efficiency; at the same time, by using acidic gas to modify the amino resin, a carbon structure connected by chemical bonds is generated, thereby improving the stability of the material and improving the cycle performance; at the same time, by doping a pore-forming agent into the carbon-based precursor, the uniformity of the pores during the carbonization process of the material and the size of the pores are improved, thereby reducing the expansion of silicon during the charge and discharge process. (2) by using the PECVD method, silicon nitride is deposited on the outermost layer of the material to avoid side reactions caused by the contact of the inner core nano-silicon with the air. At the same time, the silicon nitride deposited by PECVD has the characteristics of thin thickness and high density, thereby improving the first efficiency of the silicon-carbon composite material and its high-temperature storage performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is the SEM image of the silicon-carbon composite material prepared in Example 1. DETAILED DESCRIPTION

[0018] Embodiment 1:

[0019] A method for preparing a silicon-carbon composite material comprises the following steps:

[0020] Step S1:

[0021] 100g of amino resin, 3g of polystyrene microspheres and 3g of lithium amide were added to 800g of acetone organic solvent and dispersed evenly, spray dried, and cured at 450°C for 3h to obtain a mesoporous carbon precursor; then the mesoporous carbon precursor was transferred to a tube furnace, heated to 600°C, and introduced with hydrogen sulfide acidic gas at a flow rate of 100ml / min for 3h to obtain lithium-doped mesoporous carbon;

[0022] Step S2:

[0023] The lithium-doped mesoporous carbon was transferred to a tube furnace, and argon inert gas was introduced to exhaust the air in the tube, and then a silane mixed gas (volume ratio, silane: argon = 3:10) was introduced, and the heating temperature was 500°C, the flow rate was 100 ml / min, and the introduction time was 120 min to perform nano-silicon deposition to obtain lithium-silicon mesoporous carbon material;

[0024] Then, the PECVD technology is used to transfer the lithium silicon mesoporous carbon material to a tubular furnace, and the vacuum pressure of the tubular furnace is 3Pa after evacuation. Then, the silicon nitride is heated and passed into the tubular furnace. The deposition temperature is 550°C and the time is 60 minutes. A layer of silicon nitride film is deposited on the surface to obtain a silicon-carbon composite material.

[0025] Embodiment 2:

[0026] A method for preparing a silicon-carbon composite material comprises the following steps:

[0027] Step S1:

[0028] 100g of amino resin, 1g of polymethyl methacrylate and 1g of lithium amide were added to 500g of methanol organic solvent and dispersed evenly, spray dried, and cured at 300°C for 6h to obtain a mesoporous carbon precursor; then the mesoporous carbon precursor was transferred to a tube furnace, heated to 500°C, and sulfuric acid dioxide gas was introduced at a flow rate of 200ml / min for 6h to obtain lithium-doped mesoporous carbon;

[0029] Step S2:

[0030] The lithium-doped mesoporous carbon was transferred to a tube furnace, and argon inert gas was introduced to exhaust the air in the tube, and then a silane mixed gas (volume ratio, silane: argon = 1:10) was introduced, and nano-silicon deposition was performed at a heating temperature of 400°C, a flow rate of 500ml / min, and an introduction time of 30min to obtain a lithium-silicon mesoporous carbon material;

[0031] Then, the lithium silicon mesoporous carbon material is transferred to a tubular furnace through PECVD technology, and the vacuum pressure of the tubular furnace is 1Pa after evacuation. Then, the silicon nitride is heated and passed into the tubular furnace. The deposition temperature is 500°C and the time is 120 minutes. A layer of silicon nitride film is deposited on the surface to obtain a silicon-carbon composite material.

[0032] Embodiment 3:

[0033] A method for preparing a silicon-carbon composite material comprises the following steps:

[0034] Step S1:

[0035] 100 g of amino resin, 5 g of carbamoyl hydrazide and 5 g of lithium amide were added to 1000 g of ethyl acetate organic solvent and dispersed evenly, spray dried, and cured at 600° C. for 1 h to obtain a mesoporous carbon precursor; then the mesoporous carbon precursor was transferred to a tube furnace, heated to 800° C., and introduced with hydrochloric acid gas at a flow rate of 50 ml / min for 6 h to obtain lithium-doped mesoporous carbon;

[0036] Step S2:

[0037] The lithium-doped mesoporous carbon was transferred to a tube furnace, and argon inert gas was introduced to exhaust the air in the tube, and then a silane mixed gas (volume ratio, silane: argon = 5:10) was introduced, and the temperature was heated to 600°C, the flow rate was 500ml / min, and the introduction time was 30min to perform nano-silicon deposition to obtain a lithium-silicon mesoporous carbon material;

[0038] Then, the lithium silicon mesoporous carbon material was transferred to a tubular furnace by PECVD method, and the vacuum pressure of the tubular furnace was 5Pa after evacuation. Then, the silicon nitride was heated and passed into the tubular furnace. The deposition temperature was 580°C and the time was 10 minutes. A layer of silicon nitride film was deposited on the surface to obtain a silicon-carbon composite material.

[0039] Comparative Example 1:

[0040] The difference from Example 1 is that lithium amide is not added and hydrogen sulfide gas is not introduced. The other steps are the same as Example 1.

[0041] Comparative Example 2:

[0042] Different from the embodiment, PECVD technology is not used to deposit silicon nitride, but amorphous carbon is deposited on the surface of the lithium silicon mesoporous carbon material by vapor deposition.

[0043] The detailed preparation process is as follows: the lithium-doped mesoporous carbon in step S2 of Example 1 is transferred to a tubular furnace, acetylene gas is introduced, and the mixture is heated to 700° C. and carbonized for 3 h to obtain an amorphous carbon-coated lithium-doped silicon-carbon composite material.

[0044] Test experiment:

[0045] (1) SEM test:

[0046] Figure 1 This is a SEM image of the silicon-carbon composite material prepared in Example 1. It can be seen from the image that the material has a granular structure with a particle size between 5-10 μm, and a layer of granular material is deposited on its surface.

[0047] (2) Physical and chemical properties test:

[0048] The specific surface area and tap density of each silicon-carbon composite material were tested with reference to the national standard GB / T 38823-2020 "Silicon Carbon", and the conductivity of each composite material was tested using a four-probe tester. The pore size, pore volume and powder electronic conductivity of the silicon-carbon composite materials in Examples 1-3 and Comparative Examples 1-2 were also tested respectively; the test results are shown in Table 1 below.

[0049] (3) Button battery test:

[0050] The silicon-carbon composite materials corresponding to Examples 1-3 and Comparative Examples 1-2 were used as negative electrode materials for lithium-ion batteries to prepare button batteries according to the following method:

[0051] A binder, a conductive agent and a solvent are added to each corresponding silicon-carbon composite material, stirred to make a slurry, coated on a copper foil, and dried and rolled to obtain a negative electrode sheet; the binder used is LA132, the conductive agent is SP (conductive carbon black), the solvent is NMP, and the usage ratio of the composite material, SP, LA132, and NMP is 95g:1g:4g:220mL; the electrolyte is a solution with LiPF6 as the electrolyte, and the concentration is 1mol / L, wherein the solvent is a mixture of EC and DEC in a volume ratio of 1:1; the metal lithium sheet is the counter electrode, and the diaphragm is a polypropylene (PP) film.

[0052] Each button cell was assembled in an argon-filled glove box, and then the electrochemical performance was tested. Specifically, the electrochemical performance was tested on a Wuhan Blue Electric CT2001A battery tester, with a charge and discharge voltage range of 0.005V to 2.0V and a charge and discharge rate of 0.1C. The test results are shown in Table 1 below.

[0053] The negative electrode sheet of the above button battery was also tested for full-charge expansion. The specific test process is: the thickness D1 of the negative electrode sheet of the rolled button battery was tested, and then the full-charge thickness D2 of the negative electrode sheet was dissected when the button battery was fully charged to 100% SOC, and then the expansion rate was calculated (expansion rate = (D1-D2) / D1*100%); the test results are shown in Table 1 below.

[0054] Table 1

[0055]

[0056] It can be seen from the data in Table 1 above that the specific capacity and the first efficiency of the silicon-carbon composite materials prepared in Examples 1-3 of the present application are significantly better than those in Comparative Examples 1-2; the reason may be that: by doping lithium into the mesoporous carbon, the electronic conductivity of the material is improved and the defects of the material are reduced, the first efficiency and the powder conductivity are improved, and the defects of the material are reduced by PECVD deposition of carbon nitride, which further improves the first efficiency and conductivity of the material.

[0057] (4) Soft pack performance test:

[0058] The silicon-carbon composite materials corresponding to Examples 1-3 and Comparative Examples 1-2 were doped with 90% artificial graphite as negative electrode materials (i.e., negative electrode plates) and positive electrode ternary materials (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2), electrolyte and diaphragm are assembled into a 5Ah soft-pack battery; wherein the diaphragm is celegard 2400, the electrolyte is LiPF6 solution (the solvent is a mixed solution of EC and DEC with a volume ratio of 1:1, and the concentration of LiPF6 is 1.3 mol / L) to prepare the soft-pack battery.

[0059] The following performance tests are performed on each soft pack battery:

[0060] A. Liquid absorption capacity test: Use a 1mL burette and absorb 1mL of electrolyte, add one drop on the surface of each negative electrode, and time until the electrolyte is completely absorbed, and record the time t; the test results are shown in Table 2 below.

[0061] B. Liquid retention rate test: According to the parameters of each negative electrode sheet, calculate the theoretical liquid absorption m1 of the corresponding negative electrode sheet, and weigh the weight of the negative electrode sheet as m2. Then, place the negative electrode sheet in the electrolyte and soak it for 24 hours. Weigh the weight of the negative electrode sheet as m3, and calculate the liquid absorption of the negative electrode sheet as m3-m2, according to the following formula:

[0062] Liquid retention rate = (m3-m2)*100% / m1; the test results are shown in Table 2 below.

[0063] Table 2

[0064] Examples Liquid absorption speed (S) Fluid retention rate Example 1 45 93.3% Example 2 54 92.1% Example 3 41 94.1% Comparative Example 1 78 87.7% Comparative Example 2 65 88.3%

[0065] It can be seen from Table 2 that the liquid absorption and retention capacity of the silicon-carbon composite materials provided in Examples 1-3 is higher than that in Comparative Examples 1-2; the reason may be that the silicon-carbon composite materials provided in the examples of the present application have a larger specific surface area, which can directly improve the liquid absorption and retention capacity of the silicon-carbon composite materials.

[0066] C. Rate and cycle performance test:

[0067] The prepared soft-pack batteries were subjected to cycle performance tests and rate tests; the test conditions for the cycle performance test were as follows: the charge and discharge voltage range was 2.5 to 4.2 V, the temperature was 25 ± 3.0 ° C, the charge and discharge rate was 1.0 C / 1.0 C, and the number of cycles was 500; the test conditions for the rate test were as follows: the constant current ratio of each soft-pack battery was tested under 2C conditions; the test results are shown in Table 3 below.

[0068] Table 3

[0069]

[0070] It can be seen from Table 3 that the rate and cycle performance of the soft-pack lithium-ion battery prepared using the silicon-carbon composite material provided by Examples 1-3 are significantly better than those of Comparative Examples 1-2. The reason may be that: the example material has a high powder conductivity, which improves the constant current ratio of the material; at the same time, the example material has a high specific surface area, which improves the liquid retention performance of the material, and the carbon nitride coated on the outer layer improves the structural stability of the material and improves the cycle performance.

[0071] It is obvious to those skilled in the art that the present invention is not limited to the details of the above exemplary embodiments, and that the present invention can be implemented in other specific forms without departing from the spirit or essential characteristics of the present invention.

Claims

1. A silicon-carbon composite material for lithium-ion batteries, characterized in that: The silicon-carbon composite material presents a core-shell structure, wherein the core is a lithium-silicon doped mesoporous carbon material and the shell is a silicon nitride film. Calculated based on the mass ratio of the composite material being 100%, the mass ratio of the shell is 1-10wt%.

2. The silicon-carbon composite material according to claim 1, characterized in that: The inner layer lithium-silicon doped mesoporous carbon material is prepared by a mixture of lithium doped mesoporous carbon material and silane gas.

3. The silicon-carbon composite material according to claim 2, characterized in that: The lithium-doped mesoporous carbon material consists of 1-5wt% lithium and 95-99% mesoporous carbon, and the pore size of the mesoporous carbon is 5-10nm.

4. The method for preparing the silicon-carbon composite material according to any one of claims 1 to 3, characterized in that: The steps include: Step S1: adding a carbon-based precursor, a pore-forming agent and lithium amide to an organic solvent and dispersing them uniformly, spray drying, and curing them at a temperature of 300-600° C. for 1-6 hours to obtain a mesoporous carbon precursor; then transferring the precursor to a tube furnace, heating the precursor to 500-800° C., and introducing an acidic gas for 1-6 hours to obtain lithium-doped mesoporous carbon; Step S2: The lithium-doped mesoporous carbon is transferred to a tubular furnace, and an inert gas is introduced to exhaust the air in the tube, and the temperature is heated to 400-600°C, and then a silane mixed gas is introduced at a flow rate of 50-500ml / min and an introduction time of 30-300min to perform nano-silicon deposition to obtain a lithium silicon mesoporous carbon material; finally, a layer of silicon nitride film is deposited on the surface by PECVD (plasma enhanced chemical vapor deposition) to obtain a silicon carbon material.

5. The preparation method according to claim 4, characterized in that: In step S1, the material mass ratio of the carbon-based precursor, the pore-forming agent, lithium amide, and the organic solvent is 100:1-5:1-5:500-1000; the carbon-based precursor is an amino resin; the pore-forming agent is selected from one or more of polystyrene microspheres, polymethyl methacrylate, and aminocarbamoyl hydrazide; and the organic solvent is selected from one or more of acetone, methanol, ethyl acetate, and butanone.

6. The preparation method according to claim 4, characterized in that: The acidic gas in step S1 is selected from one or more of hydrogen sulfide, sulfur dioxide and hydrogen chloride.

7. The preparation method according to claim 4, characterized in that: In step S2, the silane mixed gas is a mixed gas of silane and argon, with a volume ratio of 1-5:

10.

8. The preparation method according to claim 4, characterized in that: The specific operation of the PECVD test method in step S2 is: transfer the lithium silicon mesoporous carbon material to a tubular furnace, evacuate the tubular furnace and maintain the vacuum pressure at 1-5 Pa, the deposition temperature is 500-580°C, and then heat the silicon nitride and pass it into the tubular furnace for 10-120 minutes.

9. A negative electrode plate for a lithium ion battery, characterized in that: The negative electrode plate comprises a negative electrode current collector and a negative electrode material coated on at least one surface of the negative electrode current collector, and the negative electrode material comprises the silicon-carbon composite material according to any one of claims 1-3 or the silicon-carbon composite material prepared according to any one of claims 4-8.

10. A lithium ion battery, characterized in that: The lithium-ion battery comprises a positive electrode sheet, a negative electrode sheet and a separator separated between the positive electrode sheet and the negative electrode sheet, and the negative electrode sheet is the negative electrode sheet according to claim 9.

Citation Information

Cited By

  • High-power silicon-carbon composite material, preparation method and application thereof