Sodium-ion battery positive electrode material Na (2-x) FePO4F (1-x), and preparation method and application thereof

By regulating the ratio of fluorine atoms to iron atoms of Na2-xFePO4F1-x positive electrode material, the problems of low first-term efficiency and poor cycle stability of existing sodium ion battery materials are solved, high capacity and long cycle performance are achieved, and suitable for energy storage materials.

CN118888747AActive Publication Date: 2024-11-01WUHAN HAOYUAN NEW ENERGY CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410916015.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-01
Estimated Expiration
2044-07-09

AI Technical Summary

Technical Problem

The existing sodium ion battery positive electrode material Na2FePO4F has low first-term efficiency, poor cycle stability and specific capacity, resulting in unstable structure during charging and discharging, affecting cycling performance.

Method used

By regulating the chemical formula of the positive electrode material of sodium ion battery is Na2-xFePO4F1-x, the x value range is 0.02≤x≤0.08, and the hydrothermal heat is used as structural regulators for phosphorus, iron, sodium, carbon and sodium fluoride as structural regulators for hydrothermal heat Reaction and sintering preparation, regulate the ratio of fluorine atoms to iron atoms, and improve the structural stability and electrochemical properties of the material.

Benefits of technology

The first reversible capacity and cycle stability of the positive electrode material of sodium ion battery has been significantly improved. The first reversible discharge capacity reaches 123.04mAh/g. The capacity retention rate reaches 91.86% after 100 cycles. The material structure is stable and suitable for energy storage materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118888747A_ABST
    Figure CN118888747A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of sodium ion batteries, and particularly relates to a sodium ion battery positive electrode material Na (2-x) FePO4F (1-x) and a preparation method and application thereof. The invention provides a sodium ion battery positive electrode material Na (2-x) FePO4F (1-x), wherein x is more than or equal to 0.02 and less than or equal to 0.08. The preparation method comprises the following steps: dissolving a phosphorus source, an iron source, a sodium source, a structure regulating agent and a carbon source in water to form a mixed solution, sanding, carrying out a hydrothermal reaction, drying to obtain a precursor material, and finally sintering to obtain the Na (2-x) FePO4F (1-x) positive electrode material. The invention provides a preparation technology of a low-cost, high-safety, long-cycle and high-first-effect positive electrode material, and the prepared positive electrode material has an extremely wide application value, is a battery material with an extremely good market prospect, and particularly brings dawn to the market of energy storage materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of sodium ion batteries, and more specifically, relates to a sodium ion battery positive electrode material Na 2- x FePO4F 1-x , its preparation method and application. Background Art

[0002] In 2022, global lithium mines continued to rise, reaching as high as 600,000 yuan / ton. Although lithium mines have suffered a parabolic plunge since 2023 and have now fallen to nearly 100,000 yuan / ton, they are still much higher than sodium ore resources represented by sodium carbonate. It is worth mentioning that as elements of the same main group, sodium and lithium have very similar physical and chemical properties, but their resource distribution is very different. The crustal abundance of sodium resources is 2.75%, while lithium resources are only 0.0065%. With the rapid development of new energy vehicles and energy storage materials, the resource-rich sodium-ion battery industry chain will usher in new opportunities and challenges. At the same time, many studies have found that sodium-ion batteries and lithium-ion batteries are very similar in working principles, key technologies, etc. Therefore, under the policy orientation of the country's strong support and development of energy storage materials, sodium-ion batteries with abundant resources, low costs and higher safety performance have attracted much attention. In particular, in the past two years, many scientific researchers have focused on sodium-ion batteries with abundant resources, lower costs, stable electrochemical properties and higher safety performance. It is expected that sodium-ion batteries will be widely used in energy storage batteries, base station backup power supplies, low-speed four-wheel vehicles, electric two-wheel vehicles and other fields, forming a complementary pattern with lithium batteries.

[0003] However, although sodium-ion batteries have received much attention, their larger ionic radius will inevitably inhibit the sodium ion deintercalation rate during the charge and discharge process, thereby reducing the chemical reaction kinetic rate. In addition, in order to further improve the cycle stability of sodium-ion batteries, it is necessary not only to consider the effect of the larger ionic radius on the ion transport of battery materials, but also to analyze the phase change problem of battery materials during the charge and discharge process, as well as structural deformation, etc. As we all know, the positive electrode materials of sodium-ion batteries mainly include layered oxide compounds, Prussian blue compounds and polyanion compounds. Although layered oxide positive electrode materials have a significant advantage of high specific capacity, poor cycle performance is their pain point; as Prussian blue compounds with higher specific capacity, they are extremely toxic, which also restricts the application of this type of battery materials. In comparison, polyanion positive electrode materials are slightly insufficient in specific capacity, but because of their long cycle life and safety and stability, they will definitely have a place in the energy storage market.

[0004] By consulting a large number of literature, it has been reported that cation doping, carbon coating and other methods can be used to solve the problems of specific capacity, rate performance, cycle stability and so on. Although sodium vanadium phosphate, which has attracted much attention from researchers, has good cycle performance, the toxicity of the material itself cannot be ignored. In recent years, sodium iron phosphate, which has low raw material cost and extremely wide sources, has become the focus of research. For example, Zhou et al. synthesized sodium iron phosphate positive electrode material by high-temperature solid phase method, and coated the material with sucrose as carbon source. The material after carbon coating had an initial discharge capacity of 121mAh / g at 0.05. In addition, Rui et al. reported a carbon-coated rod-shaped Na2FePO4F / C positive electrode material synthesized by solvothermal method, with an initial discharge capacity of 114.3mAh / g at 0.1C. At the same time, Gui et al. also reported a Na2FePO4F material synthesized by rheological phase method, with a discharge capacity of 110mAh / g at 0.1C. At the same time, an existing patent document on the positive electrode material Na2FePO4F has a first-cycle discharge capacity of 120mAh / g at a rate of 0.1C. It can be seen that most of the currently reported Na2FePO4F positive electrode materials are charge and discharge specific capacities at 0.1C, which shows that its synthesis technology still has some shortcomings, and the specific capacity, rate performance, cycle stability and safety need to be improved. It is worth mentioning that the most prominent problems of the reported Na2FePO4F positive electrode materials are low first efficiency and unstable structure. These problems are the crucial factors affecting the cycle stability and specific capacity of the positive electrode material. Therefore, it is urgent to develop a new technology that can adjust the structure of battery materials to solve the problems of low first efficiency, unstable structure and poor cycle performance of materials. Then, a green, environmentally friendly, low-cost and long-cycle sodium ion battery positive electrode material is synthesized and applied to energy storage materials, low-speed electric vehicles and other fields. Summary of the invention

[0005] In view of the defects of the prior art, the present invention is to provide a sodium ion battery positive electrode material Na 2- x FePO4F 1-x , its preparation method and application are intended to solve the technical problems of low initial efficiency, poor cycle stability and specific capacity of the existing Na2FePO4F positive electrode material.

[0006] To achieve the above object, the present invention provides a sodium ion battery positive electrode material, the chemical formula of which is Na 2- x FePO4F 1-x , the value range of x is 0.02≤x≤0.08.

[0007] According to another aspect of the present invention, there is provided a method for preparing the positive electrode material, comprising the following steps:

[0008] (1) mixing a phosphorus source, an iron source, a sodium source, a carbon source and a structure regulator with deionized water to form a mixed solution, and sand-milling to obtain a mixed salt system; the structure regulator is sodium fluoride; the molar ratio of the iron element in the iron source to the fluorine element in the structure regulator is 1:0.92-0.98;

[0009] (2) subjecting the mixed salt system described in step (1) to a hydrothermal reaction;

[0010] (3) drying the mixed salt system after the hydrothermal reaction in step (2) to obtain a precursor of a positive electrode material for a sodium ion battery;

[0011] (4) Sintering the sodium ion battery positive electrode material precursor described in step (3) to obtain the sodium ion battery positive electrode material.

[0012] Preferably, the particle size of the mixed salt in the mixed salt system in step (1) is 0.1 to 10 μm.

[0013] Preferably, in step (1), the molar ratio of the sodium source, the iron source and the phosphorus source is 2:1:1 to 1:1:1, and the molar ratio of the iron element in the iron source to the fluorine element in the structure regulating agent is 1:0.94 to 0.96.

[0014] According to another aspect of the present invention, a sodium ion battery is provided, comprising a positive electrode, a negative electrode and a separator, wherein the active material of the positive electrode comprises the positive electrode material Na 2-x FePO4F 1-x .

[0015] In general, the above technical solution conceived by the present invention has the following technical advantages compared with the prior art:

[0016] (1) The present invention provides a new sodium ion battery positive electrode material Na 2-x FePO4F 1-x , x ranges from 0.02≤x≤0.08. By adjusting the ratio of fluorine atoms to iron atoms in the chemical formula of the positive electrode material, the structure of the positive electrode material is adjusted. Experiments have shown that when the ratio of fluorine atoms to iron atoms is less than 1, the first reversible capacity and cycle stability of the positive electrode material are greatly improved within a certain range.

[0017] (2) The present invention prepares a sodium ion battery positive electrode precursor material by dissolving a phosphorus source, an iron source, a sodium source and a carbon source in water in a certain proportion, performing a hydrothermal reaction after sand grinding, and finally sintering to obtain Na 2-x FePO4F 1-xPositive electrode material. During the preparation process, by regulating the fluorine source within a suitable range, the first reversible capacity and cycle stability of the prepared positive electrode material are significantly improved compared with the existing NaFePO4F.

[0018] (3) The present invention mainly regulates the positive electrode material Na of the sodium ion battery 2-x FePO4F 1-x structure to improve the first efficiency and cycle stability. The sodium ion battery positive electrode material prepared in the preferred embodiment of the present invention is assembled into a battery. The first reversible discharge capacity at 1C can reach 123.04mAh / g, and the first cycle efficiency is 96.03%, which is close to the theoretical specific capacity. After 100 cycles, the specific capacity is still 113.02mAh / g, and the capacity retention rate is 91.86%. It can be seen that the first efficiency and cyclability are significantly improved. Therefore, the sodium ion battery positive electrode material Na prepared in the present invention 2-x FePO4F 1-x It has great application value, will be a good energy storage material, and is expected to become a leader in the new generation of energy storage materials.

[0019] (4) The structure-adjustable positive electrode material Na prepared in the present invention 2-x FePO4F 1-x The raw materials are widely available, the synthesis technology route is simple, and it is easy to industrialize.

[0020] In summary, the sodium ion battery positive electrode material Na prepared by the present invention has a controllable structure. 2-x FePO4F 1-x , the synthesis technology route is simple, the cost is low, the first charge and discharge efficiency is high, the structure is stable, the safety is good, the cycle stability is good, and it can be applied to aqueous solution systems. In view of this, it can be inferred that the new technology for regulating the battery material structure proposed in this patent is expected to be promoted and applied in the field of chemical power source technology. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The sodium ion battery positive electrode material Na obtained in Example 1 of the present invention 2-x FePO4F 1-x Structural diagram based on unit cell parameters;

[0022] Figure 2 The sodium ion battery positive electrode material Na obtained in Example 1 of the present invention 2-x FePO4F 1-x X-ray phase analysis diagram;

[0023] Figure 3 The sodium ion battery positive electrode material Na obtained in Example 1 of the present invention 2-x FePO4F 1-xSEM images of

[0024] Figure 4 The positive electrode material Na obtained in Example 1 and Comparative Example 1 of the present invention 2-x FePO4F 1-x The charge and discharge curve at 1C rate;

[0025] Figure 5 is the positive electrode material Na obtained in Example 1 of the present invention and Comparative Example 1 2-x FePO4F 1-x Cycling stability diagram at 1C rate. DETAILED DESCRIPTION

[0026] The present invention aims to improve the Na 2-x FePO4F 1-x The first efficiency and cycle stability of polyanion cathode materials represented by fluorinated phosphate-containing iron-based sodium ion battery cathode materials have been shown to have a theoretical charge and discharge platform of 3.0V. 2+ / Fe 3+ Redox reaction, through calculation, its maximum discharge specific capacity can reach 124mAh / g. However, the maximum discharge specific capacity of the sodium iron fluorophosphate positive electrode material prepared by the prior art is still far lower than the theoretical maximum value. For example, the first reversible capacity of the Na2FePO4F positive electrode material prepared by the inventor in the prior patent application CN116081594A is only 110mAh / g at most. Although the volume change rate of this type of material is low, the specific capacity decays with the increase of the number of cycles, and the initial efficiency is low. However, if the initial efficiency and cyclability problems of this series of materials can be solved, the fluorinated polyphosphate-type iron-based positive electrode material will be one of the most promising energy storage materials that can replace the current lithium battery system.

[0027] To this end, the present invention provides a sodium positive electrode material, whose chemical formula is Na 2-x FePO4F 1-x , x has a value range of 0.02≤x≤0.08. The present invention provides a controllable fluorine-containing polyphosphate type iron-based sodium ion battery positive electrode material Na 2- x FePO4F 1-x The new technology of structure includes the following steps:

[0028] (1) A phosphorus source, an iron source, a sodium source, a carbon source and a structure regulator are mixed with deionized water to form a mixed solution, and then sand-milled to obtain a mixed salt system; the structure regulator is sodium fluoride; the molar ratio of the iron element in the iron source to the fluorine element in the structure regulator is 1:0.92-0.98,

[0029] (2) subjecting the mixed salt system of step (1) to a hydrothermal reaction at a certain temperature;

[0030] (3) drying the mixed salt after the hydrothermal reaction in step (2) to obtain a positive electrode precursor for a sodium ion battery;

[0031] (4) Sintering the sodium ion battery positive electrode precursor described in step (3) to obtain a structure-adjustable positive electrode material Na 2-x FePO4F 1-x .

[0032] The sodium salt in step (1) is sodium acetate, sodium carbonate, sodium oxalate, sodium chloride, sodium nitrate or sodium citrate; the iron source is ferric phosphate, ferric oxalate or ferrous oxalate; the carbon source is sucrose, oxalic acid, citric acid, maltose, fructose or glucose; the phosphorus source is ferric phosphate, diammonium hydrogen phosphate, ammonium dihydrogen phosphate, ammonium phosphate or phosphoric acid; the mass ratio of the solute to deionized water in the mixed salt system is 30-70:100, preferably 30-50:100, wherein the solute includes the phosphorus source, iron source, sodium source, carbon source and structure regulator.

[0033] In some embodiments, the molar ratio of the sodium source, iron source and phosphorus source in step (1) is 2:1:1 to 1:1:1, and the molar ratio of the iron element in the iron source to the fluorine element in the structure regulating agent is 1:0.92 to 0.98, preferably 1:0.94 to 0.96.

[0034] In a preferred embodiment, the iron source is ferric phosphate dihydrate, the structure regulator is sodium fluoride, and the molar ratio of the iron element in the iron source to the fluorine element in the structure regulator is 1:0.94-0.96.

[0035] In some embodiments of the present invention, ferric phosphate dihydrate is used as an iron source, and the ferric phosphate dihydrate can be purchased from the market or prepared by oneself. The FePO4·2H2O powder used in the present invention has a particle size of 0.1 to 10 μm.

[0036] In some embodiments, step (1) is performed by sand grinding so that the particle size of the mixed salt in the mixed salt system is 0.1 to 10 μm.

[0037] In a preferred embodiment, in order to promote the dissolution of the sodium source, carbon source, etc., the mixed solution is left to stand overnight to promote their dissolution and facilitate subsequent reactions.

[0038] In some embodiments, the hydrothermal reaction temperature in step (2) is 60-120° C., the reaction time is 10-30 h, and for a large-volume stirred tank, a stirring device is also provided, and the stirring rate is 100-1500 rpm.

[0039] In some embodiments, the drying in step (3) is spray drying; spray drying has a granulation effect and can also control the particle size of the powder. The particle size of the positive electrode material precursor after drying of the present invention is 0.1 to 10 μm. In some embodiments, the outlet temperature during spray drying is 100 to 180°C, and the air inlet volume is 1 to 10 m 3 / min, the feed rate is 200-1000ml / h. In some embodiments, spray drying obtains D 50 It is a precursor of 3-5μm.

[0040] In some embodiments, the sintering conditions in step (4) are: sintering at 200-900° C. for 4-25 hours under an inert atmosphere to obtain the positive electrode material for a sodium ion battery. Preferably, pre-sintering at 200-450° C. for 1-8 hours under an inert atmosphere, and then secondary sintering at 500-900° C. for 3-15 hours to obtain the positive electrode material for a sodium ion battery.

[0041] In some embodiments, the inert atmosphere is nitrogen, argon, a nitrogen-hydrogen mixed atmosphere, an argon-hydrogen mixed atmosphere, or a vacuum atmosphere.

[0042] The synthesis of the present invention obtains a structure-controllable positive electrode material Na 2-x FePO4F 1-x , which can be used as a positive electrode active material of a sodium ion battery. The present invention also provides a sodium ion battery, comprising a positive electrode, a negative electrode and a separator, wherein the active material of the positive electrode comprises the positive electrode material Na 2-x FePO4F 1-x .

[0043] The present invention discloses a method for improving the Na of positive electrode material by regulating the structure. 2-x FePO4F 1-x The use of this technology can promote the rapid development of electrochemical energy storage technology in my country, and to a large extent alleviate the problem of lagging development of energy storage batteries caused by the shortage of lithium resources, and is expected to serve as a beneficial supplement to lithium-ion batteries. In the preparation process of the positive electrode material of the present invention, the addition of sodium fluoride not only introduces fluoride ions with strong electronegativity, and uses its induction effect to improve the electrochemical properties of the prepared active material; it is also added to the reaction system as a structural regulator, and the bond length of Na2-O in the positive electrode material is increased by changing the amount of sodium fluoride, so as to improve the transmission rate of sodium ions and solve the problems of low first efficiency and poor cyclability in the charge and discharge process.

[0044] Some embodiments Specific implementation process: Add a certain amount of deionized water into a plastic bucket, and add a certain amount of FePO4·2H2O, Na2CO3, NaF and sucrose in turn, add materials while stirring, mix evenly, and let stand overnight. Sand grind under certain conditions, and then place in a hydrothermal kettle for constant temperature hydrothermal reaction to obtain the sodium ion battery positive electrode material Na 2-x FePO4F 1-x Precursor; then dilute this precursor with deionized water in a certain proportion and spray dry it under certain conditions. Then, place the dried precursor in a box furnace and sinter it at different temperatures in an inert atmosphere to obtain the positive electrode material Na of the sodium ion battery. 2- x FePO4F 1-x The preparation method of the present invention has a simple synthesis process and is easy for industrial production.

[0045] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme in the embodiment of the present invention will be clearly and completely described in conjunction with the embodiments of the present invention. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention.

[0046] The embodiments of the present invention are implemented on the premise of the technical solution of the present invention, and detailed implementation methods and processes are given, but the protection scope of the present invention is not limited to the following embodiments. The process parameters of the following embodiments that do not specify specific conditions are usually based on conventional conditions.

[0047] The endpoints and any values ​​of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.

[0048] In the present invention, unless otherwise specified and / or described, all numerical values ​​involving the amounts of components are "parts by weight" from beginning to end. The process parameters in the following examples without specifying specific conditions are usually based on conventional conditions.

[0049] The following are examples:

[0050] Example 1

[0051] A new type of sodium ion battery cathode material Na 2-x FePO4F 1-xThe preparation method comprises the following specific steps:

[0052] (1) Weigh 286.0 g NaF and 1080.0 g FePO4·2H2O (D 50 2μm, the same below), 290.0g of sucrose, 380.0g of Na2CO3, add appropriate amount of deionized water to obtain a mixed solution, water accounts for 60% of the total mass of the mixed solution, and stand overnight. The mixed material is placed in a sand mill and fully stirred, and sand milled at 2800rpm for 5h to obtain a uniformly mixed mixed salt with a particle size of 1 to 3μm;

[0053] (2) placing the mixed salt prepared in step (1) in a hydrothermal reaction kettle, setting the reaction temperature to 80° C., the reaction time to 16 h, and the stirring rate to 800 rpm, to obtain a hydrothermal mixed salt;

[0054] (3) spray drying the mixed salt after the hydrothermal reaction in step (2) at an inlet temperature of 220° C., an outlet temperature of 120° C., and a feeding rate of 300 ml / h to obtain a positive electrode precursor for a sodium ion battery;

[0055] (4) The Na prepared in step (3) 2-x FePO4F 1-x The precursor was pre-sintered at 300℃ for 3h and then sintered at 600℃ for 8h in a vacuum box furnace to obtain Na 2-x FePO4F 1-x Positive electrode material.

[0056] Example 2

[0057] A new type of sodium ion battery cathode material Na 2-x FePO4F 1-x The preparation method comprises the following specific steps:

[0058] (1) Weigh 290.0 g NaCl, 1080.0 g FePO4·2H2O, 330.0 g glucose, and 580.0 g CH3COONa, add an appropriate amount of deionized water to obtain a mixed solution, in which water accounts for 60% of the total mass of the mixed solution, and let it stand overnight. Place the mixed material in a sand mill and stir it thoroughly, and sand grind it at 2500 rpm for 6 hours to obtain a uniformly mixed mixed salt with a particle size of 1 to 3 μm;

[0059] (2) placing the mixed salt prepared in step (1) in a hydrothermal reactor, setting the reaction temperature to 100° C., the reaction time to 14 h, and the stirring rate to 800 rpm, to obtain a hydrothermal mixed salt;

[0060] (3) spray drying the mixed salt after the hydrothermal reaction in step (2) again, with an inlet temperature of 180° C., an outlet temperature of 100° C., and a feed rate of 280 ml / h to obtain a positive electrode precursor for a sodium ion battery;

[0061] (4) The Na prepared in step (3) 2-x FePO4F 1-x The precursor was placed in a rotary tube furnace and pre-sintered at 350°C for 2 h and then at 650°C for 6 h in an argon atmosphere to obtain Na 2-x FePO4F 1-x Sodium-ion battery cathode materials.

[0062] Example 3

[0063] A new type of sodium ion battery cathode material Na 2-x FePO4F 1-x The preparation method comprises the following specific steps:

[0064] (1) Weigh 280.0 g NaF, 1660.0 g Fe2(C2O4)3·5H2O, 940.0 g (NH)2HPO4, 360.0 g citric acid, and 580.0 g CH3COONa, add appropriate amount of deionized water to obtain a mixed solution, in which water accounts for 60% of the total mass of the mixed solution, and let it stand overnight. Place the mixed material in a sand mill and stir it thoroughly, and sand grind it at 3000 rpm for 5 hours to obtain a uniformly mixed mixed salt with a particle size of 1 to 3 μm;

[0065] (2) placing the mixed salt prepared in step (1) in a hydrothermal reaction kettle, setting the reaction temperature to 120° C., the reaction time to 12 h, and the stirring rate to 800 rpm, to obtain a hydrothermal mixed salt;

[0066] (3) spray drying the mixed salt after the hydrothermal reaction in step (2) again, with an inlet temperature of 200° C., an outlet temperature of 110° C., and a feed rate of 250 ml / h to obtain a positive electrode precursor for a sodium ion battery;

[0067] (4) The Na prepared in step (3) 2-x FePO4F 1-x The precursor was placed in a rotary tube furnace and pre-sintered at 250°C for 4 h and then at 550°C for 6 h in an argon atmosphere to obtain Na 2-x FePO4F 1-x Sodium-ion battery cathode materials.

[0068] Example 4

[0069] A new type of sodium ion battery cathode material Na 2-x FePO4F 1-xThe preparation method comprises the following specific steps:

[0070] (1) Weigh 300.0 g NaCl, 1280.0 g FeC2O4·2H2O, 330.0 g glucose, 940.0 g (NH)2HPO4, and 480.0 g Na2C2O4, add appropriate amount of deionized water to obtain a mixed solution, in which water accounts for 60% of the total mass of the mixed solution, and let it stand overnight. Place the mixed material in a sand mill and stir it thoroughly, and sand grind it at 1000 rpm for 8 hours to obtain a uniformly mixed mixed salt with a particle size of 1 to 3 μm;

[0071] (2) placing the mixed salt prepared in step (1) in a hydrothermal reaction kettle, setting the reaction temperature to 90° C., the reaction time to 10 h, and the stirring rate to 1000 rpm, to obtain a hydrothermal mixed salt;

[0072] (3) spray drying the mixed salt after the hydrothermal reaction in step (2) again, with an inlet temperature of 240° C., an outlet temperature of 125° C., and a feed rate of 350 ml / h to obtain a positive electrode precursor for a sodium ion battery;

[0073] (4) The Na prepared in step (3) 2-x FePO4F 1-x The precursor was placed in a rotary tube furnace and pre-sintered at 200 °C for 4 h and then at 500 °C for 10 h in an argon atmosphere to obtain Na 2-x FePO4F 1-x Sodium-ion battery cathode materials.

[0074] Example 5

[0075] A new type of sodium ion battery cathode material Na 2-x FePO4F 1-x The preparation method comprises the following specific steps:

[0076] (1) Weigh 290.0 g NaCl, 1280.0 g FeC2O4·2H2O, 290.0 g sucrose, 820.0 g NH4H2PO4, and 380.0 g Na2CO3, add appropriate amount of deionized water to obtain a mixed solution, in which water accounts for 60% of the total mass of the mixed solution, and let it stand overnight. Place the mixed material in a sand mill and stir it thoroughly, and sand grind it at 2000 rpm for 7 hours to obtain a uniformly mixed mixed salt with a particle size of 1 to 3 μm;

[0077] (2) placing the mixed salt prepared in step (1) in a hydrothermal reactor, setting the reaction temperature to 60° C., the reaction time to 16 h, and the stirring rate to 800 rpm, to obtain a hydrothermal mixed salt;

[0078] (3) spray drying the mixed salt after the hydrothermal reaction in step (2) again, with an inlet temperature of 230° C., an outlet temperature of 120° C., and a feed rate of 320 ml / h to obtain a positive electrode precursor for a sodium ion battery;

[0079] (4) The Na prepared in step (3) 2-x FePO4F 1-x The precursor was placed in a rotary tube furnace and pre-sintered at 400 °C for 1 h and then at 700 °C for 6 h in an argon atmosphere to obtain Na 2-x FePO4F 1-x Sodium-ion battery cathode materials.

[0080] Example 6

[0081] A new type of sodium ion battery cathode material Na 2-x FePO4F 1-x The preparation method comprises the following specific steps:

[0082] (1) Weigh 280.0 g NaF, 1080.0 g FePO4·2H2O, 330.0 g glucose, and 480.0 g Na2C2O4, add appropriate amount of deionized water to obtain a mixed solution, in which water accounts for 60% of the total mass of the mixed solution, and let it stand overnight. Place the mixed material in a sand mill and stir it thoroughly, and sand grind it at 1500 rpm for 7.5 hours to obtain a uniformly mixed mixed salt with a particle size of 1 to 3 μm;

[0083] (2) placing the mixed salt prepared in step (1) in a hydrothermal reactor, setting the reaction temperature to 100° C., the reaction time to 12 h, and the stirring rate to 1200 rpm, to obtain a hydrothermal mixed salt;

[0084] (3) spray drying the mixed salt after the hydrothermal reaction in step (2) again, with an inlet temperature of 160° C., an outlet temperature of 100° C., and a feed rate of 240 ml / h to obtain a positive electrode precursor for a sodium ion battery;

[0085] (4) The Na prepared in step (3) 2-x FePO4F 1-x The precursor was placed in a rotary tube furnace and pre-sintered at 350°C for 2 h and then at 650°C for 6 h in an argon atmosphere to obtain Na 2-x FePO4F 1-x Sodium-ion battery cathode materials.

[0086] Comparative Example 1

[0087] (1) Weigh 300.7 g NaF, 1080.0 g FePO4·2H2O, 290.0 g sucrose, and 380.0 g Na2CO3, add appropriate amount of deionized water to obtain a mixed solution, in which water accounts for 60% of the total mass of the mixed solution, and let it stand overnight. Place the mixed material in a sand mill and stir it thoroughly, and sand grind it at 2800 rpm for 5 hours to obtain a uniformly mixed mixed salt with a particle size of 1 to 3 μm;

[0088] (2) The mixed salt prepared in step (1) was placed in a hydrothermal reactor, the reaction temperature was set to 80°C, the reaction time was 16 hours, and the stirring rate was 800 rpm to obtain Na 2-x FePO4F 1-x Precursor;

[0089] (3) The mixed salt after the hydrothermal reaction in step (2) was spray dried again, with an inlet temperature of 220° C., an outlet temperature of 120° C., and a feed rate of 300 ml / h to obtain a positive electrode precursor for a sodium ion battery.

[0090] (4) The Na prepared in step (3) 2-x FePO4F 1-x The precursor was pre-sintered at 300℃ for 3h and then sintered at 600℃ for 8h in a vacuum box furnace to obtain Na 2-x FePO4F 1-x Sodium-ion battery cathode materials.

[0091] The other conditions are the same as those of Comparative Example 1, except that the amount of sodium fluoride is changed from 300.7 g to 315.7 g, 330.8 g, 345.8 g, 360.8 g, 270.6 g, 276.6 g, 282.6 g, 288.7 g, 294.7 g, 255.6 g and 150.3 g, to obtain Comparative Example 2, Comparative Example 3, Comparative Example 4, Comparative Example 5, Comparative Example 6, Example 7, Example 8, Example 9, Example 10, Comparative Example 7, Comparative Example 8 and Comparative Example 9. It should be noted that Comparative Example 9 has many impurity peaks and was not refined, so there is no data corresponding to this comparative example in the following table.

[0092] After XRD refinement, the unit cell parameters of the positive electrode materials obtained in the embodiments and comparative examples before charge and discharge are specifically listed in Table 1 below.

[0093] Table 1 Cell parameters and Na2-O distance of positive electrode materials in embodiments and comparative examples

[0094]

[0095] It can be seen from Table 1 that the unit cell parameters of Example 1 and the comparative examples are different, and Example 1 has the largest volume and the largest Na2-O distance. This further illustrates that the Na2-O distance is different with different fluorine dosages, and the larger the Na2-O distance, the more favorable it is for the sodium ions to escape and embed, and the higher the material specific capacity.

[0096] In addition, in order to further illustrate the volume change of the positive electrode material after structural regulation during the charge and discharge process, this patent also carried out in-situ XRD testing on the positive electrode materials prepared in Example 1 and Comparative Example 1, that is, the XRD of the positive electrode materials of Example 1 and Comparative Example 1 was tested after one cycle of charge and discharge, and then the unit cell parameters before and after charge and discharge were obtained by refinement, as shown in Table 2 for details.

[0097] Table 2 Cell parameters and Na2-O distance of positive electrode materials before and after charge and discharge of Example 1 and Comparative Example 1

[0098]

[0099] It is not difficult to see from Table 2 that the unit cell parameters of Example 1 and Comparative Example 1 have changed after one week of charge and discharge. The volume change rate of Example 1 is 2.80%, which is significantly lower than that of the Na2Fe2O3 doped with magnesium and coated with carbon reported in the existing literature. 0.95 Mg 0.05 The volume change rate of PO4F@C material is 3.4%. The volume change rate of comparative example 1 is 3.68%, which is basically consistent with the 3.70% reported in the literature. Obviously, the volume change rate of example 1 is smaller. It can be inferred that the material will have better cycle stability during the charge and discharge process.

[0100] The sodium ion battery positive electrode material Na prepared in Example 1 2-x FePO4F 1-x Place it on an X-ray diffractometer to obtain the sodium ion battery positive electrode material Na 2-x FePO4F 1-x X-ray diffraction phase analysis of Figure 2 It can be seen that a single peak appears at 2θ = 12.8°, a double peak with obvious splitting appears at 2θ = 29.9° and 2θ = 30.3°, and a triple peak with obvious splitting appears at 2θ = 12.8°, 2θ = 34.2°, 2θ = 34.5° and 2θ = 34.8°. These three groups of peaks are consistent with the characteristic peaks of Na2FePO4F, indicating that Na2FePO4F prepared by this method is 2-x FePO4F 1-x At the same time, after refining the XRD of the material, Na 2-x FePO4F 1-x The structure is as Figure 1 The structure shown, from Figure 1 It can be clearly seen that by controlling the amount of structure regulator sodium fluoride, the distance between Na2-O in the positive electrode material structure is significantly increased.

[0101] The sodium ion battery positive electrode material prepared in Example 1 was observed and processed using a scanning electron microscope, and the Figure 3 The SEM image shown in the figure shows that Na 2-x FePO4F 1-x The material is spherical particles with a particle size of 3 to 6 μm, regular morphology, uniform particle size and good dispersibility.

[0102] XRF analysis was performed on the positive electrode materials prepared in different embodiments and comparative examples. The element stoichiometric ratio was calculated based on the test results to obtain the chemical formula of the positive electrode materials corresponding to different fluorine dosages. The results are shown in Tables 3 and 4.

[0103] Table 3 XRF analysis results of positive electrode materials prepared in different embodiments

[0104]

[0105]

[0106] Table 4 XRF analysis results of positive electrode materials prepared in different comparative examples

[0107]

[0108] As can be seen from Table 3 and Table 4, the positive electrode materials prepared in Examples 1 and Examples 7 to 10 are analyzed by XRF, and the ratio of F atoms to Fe atoms in the chemical formula is less than 1, corresponding to Na 2-x FePO4F 1-x In the examples, x is 0.05, 0.08, 0.06, 0.04 and 0.02 respectively. In the positive electrode materials prepared in Comparative Examples 1, 2, 3, 6 and 7, x is 0, -0.05, -0.10, 0.10 and 0.15 respectively.

[0109] The sodium ion battery positive electrode material Na prepared in Example 1 2-x FePO4F 1-x The electrochemical performance test was carried out. 2-x FePO4F 1-x As the positive electrode active material, blue electricity was used for electrochemical performance testing. Figure 4The charge and discharge curves of the sodium ion battery positive electrode materials prepared in Example 1 and Comparative Example 1 at 1C rate are shown in the figure. It can be clearly seen from the figure that the first cycle discharge capacity of Example 1 is significantly higher than that of Comparative Example 1, and more importantly, the discharge platform of Example 1 is more stable. This result shows that adding an appropriate amount of structure regulator can better maintain the stability of the structure. Figure 5 is the positive electrode material Na obtained in Example 1 of the present invention and Comparative Example 1 2-x FePO4F 1-x Cyclic stability diagram at 1C rate. Tables 5 and 6 are the sodium ion battery positive electrode materials Na prepared in different embodiments and comparative examples. 2-x FePO4F 1-x The cycle performance data and the first efficiency data at 1C rate show that the sodium ion battery positive electrode material Na prepared in Example 1 is 2- x FePO4F 1-x The first reversible charge and discharge specific capacities at a rate of 1C can reach 128.12mAh / g and 123.04mAh / g, respectively, with a first efficiency of 96.03%; Examples 7 to 10 can also obtain higher first reversible charge and discharge specific capacities and cycle performance by controlling the amount of sodium fluoride within a certain range. The first cycle charge and discharge specific capacities of Comparative Example 1 at 1C are described as 117.22mAh / g and 109.90mAh / g, respectively, with a first efficiency of 93.76%. It can be seen that the first cycle discharge capacity and first cycle efficiency of the positive electrode material prepared in Example 1 are significantly better than those in Comparative Example 1, and the first cycle discharge specific capacity is relatively close to the theoretical specific capacity. At the same time, it can be seen from the figure that after 100 cycles at 1C, the discharge specific capacity of Example 1 is still 113.02mAh / g, and the capacity retention rate is 91.86%; while that of Comparative Example 1 is 93.28mAh / g, and the capacity retention rate is 84.88%. The cycle stability data of other embodiments and comparative examples are listed one by one in Table 5 and Table 6. It can also be seen from the table that the cycle stability of Example 1, Example 7, Example 8, Example 9 and Example 10 is better than that of the comparative example. This result once again confirms the conclusion that an appropriate amount of structure regulator can better maintain structural stability. Based on this, we can say that by regulating the material structure, the first-cycle efficiency of the material in the charging and discharging process can be significantly improved and a long cycle can be achieved. It should be particularly noted here that the charging and discharging of the positive electrode material obtained in the present invention are tested at 1C, and the high first-cycle efficiency and long cycle performance it has achieved are at the leading level in the industry. By comparing multiple pairs of test results, it is not difficult to find that the Na prepared by the present invention 2-x FePO4F 1-x The positive electrode material is superior in terms of specific capacity, initial efficiency, cycle stability, safety and rate performance.

[0110] Table 5 Electrochemical performance of positive electrode materials prepared in different embodiments at 1C rate

[0111]

[0112] Table 6 Electrochemical performance of positive electrode materials prepared in different comparative examples at 1C rate

[0113]

[0114] In summary, the sodium ion battery positive electrode material Na prepared by the present invention has a controllable structure. 2- x FePO4F 1-x It not only has the characteristics of low cost, high specific capacity and good safety, but also has the advantages of high initial efficiency and good cycle stability. Therefore, the new technology of adjustable battery material structure provided by the present invention can be promoted and applied in the field of chemical power sources.

[0115] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A sodium ion battery positive electrode material, characterized in that: Its chemical formula is Na 2-x FePO4F 1-x , the value range of x is 0.02≤x≤0.

08.

2. The method for preparing the positive electrode material according to claim 1, characterized in that: The steps include: (1) mixing a phosphorus source, an iron source, a sodium source, a carbon source and a structure regulator with deionized water to form a mixed solution, and sand-milling to obtain a mixed salt system; the structure regulator is sodium fluoride; the molar ratio of the iron element in the iron source to the fluorine element in the structure regulator is 1:0.92-0.98; (2) subjecting the mixed salt system described in step (1) to a hydrothermal reaction; (3) drying the mixed salt system after the hydrothermal reaction in step (2) to obtain a precursor of a positive electrode material for a sodium ion battery; (4) Sintering the sodium ion battery positive electrode material precursor described in step (3) to obtain the sodium ion battery positive electrode material.

3. The preparation method according to claim 2, characterized in that: The particle size of the mixed salt in the mixed salt system in step (1) is 0.1 to 10 μm.

4. The preparation method according to claim 1, characterized in that: The sodium salt in step (1) is sodium acetate, sodium carbonate, sodium oxalate, sodium chloride, sodium nitrate or sodium citrate; and / or. The iron source is ferric phosphate, ferric oxalate or ferrous oxalate; and / or. The carbon source is sucrose, oxalic acid, citric acid, maltose, fructose or glucose; and / or. The phosphorus source is ferric phosphate, diammonium hydrogen phosphate, ammonium dihydrogen phosphate, ammonium phosphate or phosphoric acid; and / or. The mass ratio of the solute to deionized water in the mixed salt system is 30-70:100, preferably 30-50:100, wherein the solute includes the phosphorus source, iron source, sodium source, carbon source and structure regulator.

5. The preparation method according to claim 2, characterized in that: In step (1), the molar ratio of the sodium source, the iron source and the phosphorus source is 2:1:1 to 1:1:1, and the molar ratio of the iron element in the iron source to the fluorine element in the structure regulating agent is 1:0.94 to 0.

96.

6. The preparation method according to claim 1, characterized in that: The hydrothermal reaction temperature in step (2) is 60-120° C., the reaction time is 10-30 h, and the stirring rate is 100-1500 rpm.

7. The preparation method according to claim 1, characterized in that: The drying in step (3) is spray drying.

8. The preparation method according to claim 1, characterized in that: The sintering conditions of step (4) are: sintering at 200-900° C. for 4-25 hours under an inert atmosphere to obtain the sodium ion battery positive electrode material.

9. The preparation method according to claim 1, characterized in that: The sintering conditions of step (4) are: pre-sintering at 200-450° C. for 1-8 hours under an inert atmosphere, and then secondary sintering at 500-900° C. for 3-15 hours to obtain the sodium ion battery positive electrode material; and / or. The inert atmosphere is nitrogen, argon, a nitrogen-hydrogen mixed atmosphere, an argon-hydrogen mixed atmosphere or a vacuum atmosphere.

10. A sodium ion battery, characterized in that: The invention comprises a positive electrode, a negative electrode and a separator, wherein the active material of the positive electrode comprises the positive electrode material Na as claimed in claim 1 2-x FePO4F 1-x .

Citation Information

Patent Citations

  • Fluorinion-doped modified ferric sodium pyrophosphate used for sodium-ion battery positive electrode material, and preparation method and application thereof

    CN114057175A

  • Transition metal phosphate sodium ion battery positive electrode material and preparation method and application thereof

    CN115036477A

  • Fluorine ion doped manganese-based layered oxide positive electrode material with air stability and preparation method and application thereof

    CN115188959A

  • Method for preparing carbon-coated sodium ferric fluorophosphate from waste lithium iron phosphate and application of carbon-coated sodium ferric fluorophosphate

    CN115818613A

  • Preparation method of sodium ion battery positive electrode material

    CN116081594A