Composite sodium supplement as well as preparation method and application thereof
By combining sodium carbonate with sodium ion battery layered oxide and using mechanical ball milling method, the problems of cumbersome sodium carbonate process and low battery stability in the existing technology are solved, and efficient sodium supplementation performance and energy density improvement are achieved. Suitable for industrial production.
Patent Information
- Application Number
- CN202410939637.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-15
AI Technical Summary
The process of using sodium carbonate as a sodium supplement in the prior art is cumbersome and the battery stability is low, resulting in limited application in industrial production.
By combining sodium carbonate with sodium ion battery layered oxide, a composite sodium supplement agent with a particle size less than 5μm was prepared, and mixed with mechanical ball milling method was used to reduce the decomposition voltage of sodium carbonate, improve its decomposition efficiency, and reduce inactive Residue of matter.
Effectively reduce the decomposition voltage of sodium carbonate, improve its decomposition efficiency and volume specific capacity, and build an efficient composite pre-sodium system, which can effectively supplement the irreversible capacity loss of active sodium ions, increase the energy density of the battery, and simplify the process flow. , suitable for large-scale production.
Smart Images

Figure CN118888752A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion batteries, and more specifically to a composite sodium supplement and a preparation method and application thereof. Background Art
[0002] Sodium-ion batteries are one of the most promising technologies in the field of large-scale energy storage. With the continuous deepening of research on sodium-ion battery technology in recent years, the electrochemical performance of sodium-ion batteries has been greatly improved. In the sodium-ion battery full cell actually used, due to the common problem of low initial coulombic efficiency of the negative electrode, some sodium ions are irreversibly deintercalated on the negative electrode side, consuming active sodium ions during the cycle, which leads to the overall capacity decay and energy density of the battery. The loss of active sodium ions has become one of the most critical issues restricting the large-scale application of sodium-ion batteries. Pre-sodium technology introduces additional active sodium ions to compensate for the irreversible loss of active sodium ions, thereby maximizing the release of the energy density of the battery. The positive electrode sodium supplement method is a commonly used pre-sodium method. The sodium supplement in the positive electrode is electrochemically oxidized and decomposed during the first charge process, releasing excess active sodium ions, and irreversibly migrating to the electrolyte and the negative electrode, thereby increasing the active sodium ion content during the cycle and improving the overall energy density of the battery. Sodium carbonate, as a positive electrode sodium supplement, has a high theoretical specific capacity (505mAh·g -1 ), low price, safe and non-toxic, and stable in nature; however, sodium carbonate is an extremely poor conductor of electrons and ions, with a wide band gap of 2.52eV, high decomposition voltage, low decomposition efficiency, and an actual decomposition capacity of only 21mAhg -1 , and it can be decomposed in small amounts in repeated cycles, which seriously hinders its application in actual industrial production (Chem. Mater. 2017, 29, 14, 5948-5956).
[0003] At present, in the field of pre-sodium, the main means of applying sodium carbonate is to catalyze it using carbon or transition metal oxides that are not electrochemically active. In sodium ion capacitors, researchers reduced the decomposition voltage of sodium carbonate to 4.25V by mixing sodium carbonate, activated carbon and conductive carbon in a ratio of 4:4:1, and the first-cycle decomposition rate was increased to 82.6%; but too high a carbon content would lead to a serious decrease in its volumetric capacity, limiting its application in positive electrode additives (J. Powder Sources, 2021, 515, 230628).
[0004] The prior art proposes to combine sodium carbonate with different carbon materials to reduce the decomposition voltage of sodium carbonate; however, the process is too complicated and not conducive to expansion into industrial production. There is also the prior art that uses a composite material of sodium carbonate, metal oxide and carbon to exert some of the electrochemical activity of sodium carbonate; however, the use of a large amount of metal oxides results in an excessively high amount of residual inactive substances after the sodium supplementation process is completed, which is not conducive to the subsequent stable cycle of the battery. Summary of the invention
[0005] The invention provides a composite sodium supplement and a preparation method and application thereof, which are used to solve the problems of complicated process and low battery stability in the prior art of using sodium carbonate as a sodium supplement.
[0006] In a first aspect, the present invention provides a composite sodium supplement, which is composed of a sodium ion battery layered oxide and sodium carbonate in a mass ratio of 1:0.1 to 10.
[0007] As a possible implementation, the particle size of the composite sodium supplement is less than 5 μm.
[0008] As a possible implementation method, the chemical formula of the sodium ion battery layered oxide is Na x TMO2, wherein 0.1≤x<1, and TM is one or a combination of Ca, V, Ti, Cr, Mn, Fe, Co, Ni, Cu, Nb, Mo, Sn, Mg, and Li.
[0009] In a second aspect, the present invention provides a method for preparing a composite sodium supplement, comprising the following steps: mixing the raw material components according to the formula components of the composite sodium supplement described in any possible implementation mode of the first aspect in proportion and then grinding to obtain the composite sodium supplement.
[0010] As a possible implementation method, the grinding step includes: adding ball milling beads in a sealed ball mill and grinding at 200 to 700 rpm / min. -1 Ball mill at a speed of 10 to 70 hours.
[0011] In a third aspect, the present invention provides use of the composite sodium supplement described in any possible implementation of the first aspect or the composite sodium supplement prepared by the preparation method described in any possible implementation of the second aspect in preparing a sodium ion battery.
[0012] In a fourth aspect, the present invention provides a sodium ion battery, wherein the positive electrode active material comprises the composite sodium supplement described in any possible implementation of the first aspect or the composite sodium supplement prepared by the preparation method described in any possible implementation of the second aspect.
[0013] As a possible implementation manner, the mass of the composite sodium supplement is 0.1 wt% to 20 wt% of the mass of the positive electrode active material.
[0014] As a possible implementation, the positive electrode active material further includes one or a combination of sodium ion battery layered oxides, polyanionic compounds, Prussian blue and Prussian blue analogs.
[0015] As a possible implementation, the preparation method includes the following steps: mixing the active material with a conductive agent and a binder to prepare a slurry, and coating the slurry on a current collector; sequentially performing drying and slicing operations to prepare a positive electrode sheet; and assembling the sodium ion battery using the positive electrode sheet as the positive electrode and sodium as the negative electrode.
[0016] Sodium carbonate has a large theoretical specific capacity, but its electrochemical decomposition potential is too high, making it difficult to be directly applied to pre-sodium; when layered oxides are used alone as positive electrode sodium supplements, there is a problem of residual inactive substances. The composite sodium supplement provided by the present invention effectively reduces the decomposition voltage of sodium carbonate and improves its decomposition efficiency by compounding sodium carbonate with layered oxides. While the composite sodium supplement exerts the electrochemical activity of sodium carbonate, there are fewer inactive substances remaining after de-sodiumization. In the composite sodium supplement provided by the present invention, both sodium carbonate and layered oxide can release active sodium ions, and the introduction of inactive carbon is avoided, thereby increasing the volumetric specific capacity of the sodium supplement and constructing an efficient composite pre-sodium system that can exert excellent sodium supplement performance, effectively supplement the irreversible capacity loss of active sodium ions in the full battery, and increase the energy density of the battery.
[0017] The preparation method of the composite sodium supplement provided by the invention comprises the following steps: mixing sodium carbonate and layered oxide by mechanical ball milling to obtain the composite sodium supplement; the preparation method is simple and easy to operate, environmentally friendly and pollution-free, and suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0019] Figure 1 This is a SEM image of untreated sodium carbonate provided by an embodiment of the present invention.
[0020] Figure 2 This is a SEM image of product H provided in an embodiment of the present invention.
[0021] Figure 3The first five charge-discharge curves of the product D provided in the embodiment of the present invention.
[0022] Figure 4 The charge and discharge curves of the experimental group and control group batteries provided in the embodiments of the present invention. DETAILED DESCRIPTION
[0023] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] In order to solve the problems of complicated process and low battery stability in the prior art of using sodium carbonate as a sodium supplement, the embodiment of the present invention provides a composite sodium supplement and a preparation method thereof.
[0025] The composite sodium supplement provided by the present invention effectively reduces the decomposition voltage of sodium carbonate and improves its decomposition efficiency by combining sodium carbonate with layered oxides. The composite sodium supplement exerts the electrochemical activity of sodium carbonate while leaving less inactive substances remaining after de-sodiumization. In the composite sodium supplement provided by the present invention, both sodium carbonate and layered oxide can release active sodium ions, and the introduction of inactive carbon is avoided, thereby improving the volumetric capacity of the sodium supplement, constructing an efficient composite pre-sodium system, being able to exert excellent sodium supplement performance, and being able to effectively supplement the irreversible capacity loss of active sodium ions in a full battery.
[0026] Furthermore, in the preparation of a composite sodium supplement provided by the present invention, a comparative experiment was also carried out on the selection of sodium salt, and the results showed that only when sodium carbonate was compounded with layered oxides, the obtained sodium supplement could achieve the ideal effect; other sodium salts, even sodium oxalate whose anion element composition is the same as carbon and oxygen, the effect of the sodium supplement obtained by compounding with layered oxides was not ideal. It can be seen that the sodium carbonate compounded with the layered oxide in the present invention has an irreplaceable role.
[0027] Furthermore, the present invention provides an electrochemical performance test experiment of the composite sodium supplement, which verifies that the composite sodium supplement provided by the present invention has better capacity and electrochemical performance in application and exerts a better sodium supplement effect.
[0028] The technical solution of the present invention will be further described below in conjunction with specific embodiments.
[0029] Example 1
[0030] This example provides an experiment for preparing a composite sodium supplement.
[0031] Sodium carbonate and NaCrO2 were mixed in a mass ratio of 9:1 and placed in a ball mill. After adding ball mill beads, the ball mill was sealed and milled at 300 rpm min. -1 The product A was obtained by ball milling for 20 h.
[0032] Sodium carbonate and NaCrO2 were mixed in a mass ratio of 8:2, put into a ball mill, and sealed after adding ball mill beads. -1 The product was ball milled at a speed of 20 h to obtain product B.
[0033] Sodium carbonate and NaCrO2 were mixed in a mass ratio of 7:3, put into a ball mill, and sealed after adding ball mill beads. -1 The product C was obtained by ball milling for 20 h.
[0034] Sodium carbonate and NaCrO2 were mixed in a mass ratio of 6:4 and placed in a ball mill. After adding ball mill beads, the ball mill was sealed and milled at 300 rpm min. -1 The product D was obtained by ball milling for 20 h.
[0035] Sodium carbonate and NaCrO2 were mixed in a mass ratio of 5:5, put into a ball mill, and sealed after adding ball mill beads. -1 The product E was obtained by ball milling at a speed of 20 h.
[0036] Sodium carbonate and NaCrO2 were mixed in a mass ratio of 6:4 and placed in a ball mill. After adding ball mill beads, the ball mill was sealed and milled at 200 rpm min. -1 The product F was obtained by ball milling at a speed of 20 h.
[0037] Sodium carbonate and NaCrO2 were mixed in a mass ratio of 6:4 and placed in a ball mill. After adding ball mill beads, the ball mill was sealed and milled at 700 rpm min. -1 The product G was obtained by ball milling at a speed of 20 h.
[0038] Sodium carbonate and NaCrO2 were mixed in a mass ratio of 6:4 and placed in a ball mill. After adding ball mill beads, the ball mill was sealed and milled at 300 rpm min. -1 The product H was obtained by ball milling for 10 h.
[0039] Sodium carbonate and NaCrO2 were mixed in a mass ratio of 6:4 and placed in a ball mill. After adding ball mill beads, the ball mill was sealed and milled at 300 rpm min. -1 The product was ball milled at a speed of 70 h to obtain product I.
[0040] Sodium carbonate and Na(Fe) in a mass ratio of 6:4 1 / 3 Ni 1 / 3Mn 1 / 3 )O2, put it into a ball mill, add ball mill beads, seal the ball mill, and grind at 300 rpm min -1 The product J was obtained by ball milling at a speed of 20 h.
[0041] Sodium carbonate and conductive carbon were mixed in a mass ratio of 6:4 and placed in a ball mill. After adding ball mill beads, the ball mill was sealed and milled at 300 rpm min. -1 The product K was obtained by ball milling for 20 h.
[0042] Untreated pure sodium chromate powder was used as product L.
[0043] Scanning electron microscopy analysis of sodium carbonate without ball milling revealed the following Figure 1 The SEM image shown; Scanning electron microscopy analysis of product D yielded the following Figure 2 SEM images shown.
[0044] contrast Figure 1 and Figure 2 It can be seen that ball milling significantly reduces the particle size of sodium carbonate, helps to accelerate the migration of ions and electrons during electrochemical decomposition, and significantly improves its kinetic process.
[0045] Example 2
[0046] This embodiment provides an electrochemical performance test experiment of a composite sodium supplement.
[0047] The sodium supplement, conductive agent and binder to be tested were mixed and ground in a mass ratio of 8:1:1, and then a solvent was added and stirred to form a uniform slurry. The slurry was coated on the current collector, dried at 110°C in a vacuum drying oven for 12 hours, and then cut into a 12mm diameter disc, i.e., the positive electrode sheet. The positive electrode sheet was used as the positive electrode, the metal sodium was used as the negative electrode, the glass fiber was used as the separator, and 1mol·L -1 NaClO4 (EC:PC=1:1, with 5% FEC) was used as the electrolyte to assemble button cells.
[0048] In this example, KB was used as the conductive agent, PVDF was used as the binder, NMP was used as the solvent, and aluminum foil was used as the current collector. The products A to K prepared in Example 1 were used as the sodium supplement to be tested, respectively, to prepare batteries A to K. In the voltage range of 2.0 to 4.2 V (2.0 to 4.6 V for battery K), the battery was charged with 45 mAh·g -1 The current density was used for charge and discharge test, and the results are shown in Table 1 and Figure 3 The electrochemical performance results of the battery are shown.
[0049] Table 1 Decomposition voltage and decomposition capacity of composite sodium supplement
[0050]
[0051] As shown in Table 1, the operation of mixing sodium carbonate and layered oxides by ball milling can effectively promote the electrochemical decomposition of sodium carbonate and reduce the decomposition voltage of sodium carbonate. Therefore, the composite sodium supplement exhibits a higher capacity during the first cycle of charging. At the same time, layered oxides represented by sodium chromate all leave non-electrochemically active solids (such as Na 1-x CrO2), while the decomposition product of sodium carbonate is only carbon dioxide gas. The composite sodium supplement provided by the present invention has less solid residue after decomposition, which is beneficial to the stability of the battery. Figure 3 It can be seen that the composite sodium supplement can irreversibly release a large amount of active sodium ions during the first cycle of charging and discharging, while only a small amount of sodium ions are embedded during the discharge process, which is beneficial to replenish the consumption of active sodium ions.
[0052] Example 3
[0053] This embodiment provides a verification experiment on the improvement of battery charge and discharge performance by a composite sodium supplement.
[0054] The positive electrode active material, conductive agent and binder were mixed and ground in a mass ratio of 8:1:1, and a solvent was added to stir to form a uniform slurry. The slurry was coated on the positive electrode collector, dried in a vacuum oven at 110°C for 12 hours, and then cut into discs with a diameter of 12 mm, namely the positive electrode sheet. The hard carbon, conductive agent and binder were mixed and ground in a mass ratio of 90:5:5, and a solvent was added to stir to form a uniform slurry. The slurry was coated on the negative electrode collector, dried in a vacuum oven at 80°C for 12 hours, and then cut into discs with a diameter of 12 mm, namely the negative electrode sheet. The positive electrode sheet was used as the positive electrode, the negative electrode sheet was used as the negative electrode, the glass fiber was used as the separator, and 1 mol·L -1 NaClO4 (EC:PC=1:1, with 5% FEC) was used as the electrolyte to assemble button cells.
[0055] In this embodiment, SP is used as the conductive agent, PVDF is used as the binder, NMP is used as the solvent, aluminum foil is used as the positive electrode collector, copper foil is used as the negative electrode collector, and Na(Fe 1 / 3 Ni 1 / 3 Mn 1 / 3 )O2 and the mixture of the product D prepared in Example 1 (the mass of the product D is 5wt% of the mixture) were used as the positive electrode active material of the experimental group to prepare the experimental group battery; Na(Fe 1 / 3 Ni 1 / 3 Mn 1 / 3 )O2 was used as the positive electrode active material of the control group to prepare the control group battery. In the voltage range of 2.0 to 4.5 V, 15 mAh·g -1 After activating for 3 cycles with a current density of 1.5 V, the charge and discharge cycles were carried out in the voltage range of 2.0 to 4.0 V. Figure 4 And the charge and discharge capacities shown in Table 2.
[0056] Table 2 Charge and discharge capacity
[0057]
[0058] From Table 2 and Figure 4 It can be seen that product D can release excess active sodium ions in the full battery and exert an excellent sodium replenishment effect in practical applications.
[0059] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.
[0060] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A composite sodium supplement, characterized in that: The invention is composed of sodium ion battery layered oxide and sodium carbonate in a mass ratio of 1:0.1 to 10.
2. The composite sodium supplement according to claim 1, characterized in that Its particle size is less than 5 μm.
3. The composite sodium supplement according to claim 1, characterized in that The chemical formula of the sodium ion battery layered oxide is Na x TMO2, wherein 0.1≤x<1, and TM is one or a combination of Li, Mg, Ca, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Nb, Mo, and Sn.
4. A method for preparing a composite sodium supplement, characterized in that: The following steps are involved: According to the formula components of the composite sodium supplement according to any one of claims 1 to 3, the raw material components are mixed in proportion and then ground to obtain the composite sodium supplement.
5. The preparation method according to claim 4, characterized in that: The grinding step comprises: adding ball milling beads to a sealed ball mill at 200-700 rpm·min -1 Ball mill at a speed of 10 to 70 hours.
6. Use of the composite sodium supplement according to any one of claims 1 to 3 or the composite sodium supplement prepared by the preparation method according to any one of claims 4 to 5 in the preparation of sodium ion batteries.
7. A sodium ion battery, characterized in that: The positive electrode raw material comprises an active material, and the active material comprises the composite sodium supplement agent described in any one of claims 1 to 3 or the composite sodium supplement agent prepared by the preparation method described in any one of claims 4 to 5.
8. The sodium ion battery according to claim 7, characterized in that: The mass of the composite sodium supplement is 0.1wt% to 20wt% of the mass of the active material.
9. The sodium ion battery according to claim 7, characterized in that: The active material also includes one of a sodium ion battery layered oxide, a polyanionic compound, Prussian blue and a Prussian blue analog.
10. The method for preparing a sodium ion battery according to any one of claims 7 to 9, characterized in that: The following steps are involved: The active material is mixed with a conductive agent and a binder to prepare a slurry, and the slurry is coated on a current collector; Drying and slicing operations are performed in sequence to prepare a positive electrode sheet; The sodium ion battery is assembled by using the positive electrode sheet as the positive electrode and sodium as the negative electrode.
Citation Information
Patent Citations
Sodium-ion battery positive electrode additive of NaCrO2 / C and preparation and application method thereof
CN107785584A
Composite sodium supplement additive and application thereof in sodium ion battery
CN113113681A
Self-sodium-supplementing sodium ion battery positive electrode active material as well as preparation method and application thereof
CN114790013A
Layered oxide positive electrode material of sodium-ion battery as well as preparation method and application of layered oxide positive electrode material
CN115799493A
Sodium-ion battery negative electrode material, preparation method of negative electrode plate and sodium-ion battery
CN116072994A
Cited By
Needle-shaped sodium zirconium phosphate sodium supplement as well as preparation method and application thereof
CN120109196A
Layered transition metal oxide material mediated pre-sodium-modified material and application thereof
CN122338077A