Semi-solid battery and preparation method and application thereof
By curing and decomposing the semi-solid battery, a stable electrolyte structure is formed, which solves the problem of poor low-temperature performance and achieves good use performance and energy density in cold areas.
Patent Information
- Application Number
- CN202411116775.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-01
AI Technical Summary
The performance of semi-solid state batteries in low temperature environments is limited, which limits their popularity and use in cold areas. Existing solutions such as configuring a cyclic heating device can increase the operating temperature but reduce the energy density.
The battery after injection was cured at a temperature of 50-70°C and a pressure of 500-2000 kg/f, and then the chemical processing was performed to control the mass percentage content and chemical temperature of lithium salts such as LiPF6 to form a stable electrolyte Structure, reduces the fluidity and volatility of the electrolyte, reduces the internal resistance of the battery, and improves the low-temperature conductivity.
The excellent performance of semi-solid state batteries in low temperature environments is achieved, ensuring good performance in cold areas, and avoiding the reduction of energy density by the heating device.
Smart Images

Figure CN118888993A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a semi-solid battery and a preparation method and application thereof, belonging to the technical field of batteries. Background Art
[0002] Semi-solid batteries are a special type of battery that contains both liquid and solid electrolytes. During the charging and discharging process, ions are transferred through solid and liquid electrolytes to achieve the purpose of storing and releasing energy. Semi-solid batteries have the advantages of high energy density, high temperature stability, fast charging and excellent cycle performance, and are favored in the field of automotive power batteries and energy storage.
[0003] However, the low-temperature performance of semi-solid batteries is low, which limits the popularization of such batteries in cold regions. The current common solution is to increase the operating temperature of semi-solid batteries by configuring a circulating heating device outside the battery, thereby improving the discharge performance of such batteries in low-temperature environments. However, this method only physically heats the semi-solid battery, and adding a heating device will reduce the energy density of the semi-solid battery.
[0004] Therefore, it is urgent to explore technical solutions to fundamentally solve the low-temperature performance of semi-solid-state batteries. Summary of the invention
[0005] The invention provides a method for preparing a semi-solid battery. The preparation method is simple to operate, and the prepared semi-solid battery has excellent low-temperature performance.
[0006] The present invention provides a semi-solid-state battery, which is prepared by the above-mentioned preparation method and has excellent low-temperature performance.
[0007] The present invention also provides an electronic device, which includes the semi-solid battery, so the electronic device has excellent performance even in a low-temperature environment.
[0008] In one aspect, the present invention provides a method for preparing a semi-solid-state battery, comprising the following steps:
[0009] 1) curing the battery after injection at 50-70° C. and 500-2000 kg / f for 12-48 hours to obtain a cured battery;
[0010] 2) Performing a formation treatment on the cured battery to obtain a semi-solid battery.
[0011] In the preparation method as described above, in step 1), the curing treatment temperature is 60-70° C., the pressure is 1000-2000 kg / f, and the time is 12-24 h.
[0012] In the preparation method as described above, the electrolyte before solidification treatment includes lithium salt, solvent and additives.
[0013] In the preparation method as described above, the lithium salt includes LiPF6, and the mass percentage of LiPF6 is 9-13wt.%.
[0014] In the preparation method as described above, in step 2), the chemical formation temperature of the chemical formation treatment is 35-45° C., and the extrusion pressure is 1000 kg / f (4-6 h).
[0015] The preparation method as described above further includes a first standing treatment before the curing treatment, wherein the temperature of the first standing treatment is 20-30° C. and the standing time is 24-72 hours.
[0016] The preparation method as described in any one of the above items further comprises a second static treatment after the chemical formation treatment, the temperature of the second static treatment is 25° C., and the static treatment is performed for 24-72 hours.
[0017] According to the preparation method described above, the battery after injection includes a positive electrode sheet, and the positive electrode sheet includes a positive electrode slurry.
[0018] The positive electrode slurry comprises lithium iron phosphate, conductive carbon black, conductive slurry, a binder and 1%-2% of LATP.
[0019] Another aspect of the present invention provides a semi-solid-state battery prepared by the preparation method described above.
[0020] According to another aspect of the present invention, there is provided an electronic device, comprising the semi-solid-state battery as described above.
[0021] The preparation method of the semi-solid battery provided by the present invention realizes the solidification treatment of the battery after liquid injection by controlling the specific pressure and temperature, and then performs a formation treatment on the solidified battery to obtain the semi-solid battery, which has excellent low-temperature performance.
[0022] The semi-solid-state battery provided by the present invention is prepared by the above-mentioned preparation method and has excellent low-temperature performance.
[0023] The electronic device provided by the present invention includes the above-mentioned semi-solid-state battery, and thus can still exert good performance in a low-temperature environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 A comparison chart of 5°C low-temperature charging of the semi-solid-state battery provided in Examples 1-4 of the present invention;
[0025] Figure 2 This is a comparison chart of 5°C low-temperature discharge of the semi-solid-state batteries provided in Examples 1-4 of the present invention. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] On one hand, the present invention provides a method for preparing a semi-solid battery, comprising the following steps: 1) subjecting the battery after liquid injection to a curing treatment at 50-70°C and 500-2000kg / f for 12-48h to obtain a cured battery; 2) subjecting the cured battery to a formation treatment to obtain a semi-solid battery.
[0028] The preparation method provided by the present invention is used to prepare a semi-solid battery. The curing treatment of the battery is achieved by controlling the temperature and pressure, and then the cured battery is subjected to a formation treatment to obtain a semi-solid battery. The semi-solid battery has excellent low-temperature performance.
[0029] In detail, in step 1), the temperature of the curing treatment includes but is not limited to 50°C, 52°C, 54°C, 56°C, 58°C, 60°C, 62°C, 64°C, 66°C, 68°C, 70°C or a range between any two of them, and the pressure of the curing treatment includes but is not limited to 500kg / f, 800kg / f, 1000kg / f, 1200kg / f, 1400kg / f, 1600kg / f, 1800kg / f, 2000kg / f or a range between any two of them.
[0030] It is understood that the positive electrode sheet, the negative electrode sheet, the separator and the current collector need to be assembled first to form an assembled battery. The present invention does not limit the specific process of assembling the battery, and the conventional process in the art can be used for assembly.
[0031] The assembled battery is subjected to a liquid injection treatment, that is, an electrolyte is injected into the assembled battery to obtain a liquid-injected battery. The present invention also does not limit the specific process of the liquid injection treatment.
[0032] In a specific embodiment, the soft-pack battery is injected with liquid. First, a monomer solution containing a certain lithium salt concentration is prepared, and then a thermal initiator is added to the above solution to obtain a precursor solution. Then, the battery is assembled according to the assembly method of the liquid battery. The specific injection amount of each battery cell is 20-25g.
[0033] During the curing process, the battery can be basically cured within this temperature range by disassembling the cured battery, or the hardness of the soft-pack battery cell can be felt by hand. If the battery cell is hard, it has been effectively cured and the curing process can be stopped. At this time, the electrolyte in the battery is in a stable state, which improves the stability of the electrolyte inside the battery.
[0034] In step 2), the cured battery is subjected to a formation treatment so that the positive and negative electrodes of the battery form a stable structure under the wrapping of the electrolyte, ensuring that the electrodes can effectively embed and release ions and achieve good charge and discharge cycle performance.
[0035] The preparation method provided by the present invention can prepare a semi-solid battery with relatively excellent low-temperature performance. The inventor analyzed this and believed that the reason may be that: during the preparation process, the battery after injection is pressurized and heated for curing, and at a certain temperature and pressure, the curing is more complete and thorough, so that the electrolyte forms a more stable structure, that is, the thermal initiation method, which reduces the fluidity and volatility of the electrolyte in a low-temperature environment, and can further reduce the internal resistance of the battery and improve the low-temperature conductivity of the battery; on the other hand, pressurized and heated curing can compress a small amount of gas generated during the curing process into the airbag, avoid the impedance caused by the gas, and further reduce the internal resistance of the battery.
[0036] Furthermore, in a specific embodiment of the present invention, the curing treatment temperature is 60-70° C., the pressure is 500-1000 kg / f, and the time is 12-24 hours.
[0037] In detail, the temperature of the curing treatment includes but is not limited to 60°C, 61°C, 62°C, 63°C, 64°C, 65°C, 66°C, 67°C, 68°C, 69°C, 70°C or a range between any two of them.
[0038] The pressure of the curing treatment includes but is not limited to 500kg / f, 550kg / f, 600kg / f, 650kg / f, 700kg / f, 750kg / f, 800kg / f, 850kg / f, 900kg / f, 950kg / f, 1000kg / f or a range between any two of them.
[0039] The curing time includes but is not limited to 12 h, 14 h, 16 h, 18 h, 20 h, 22 h, 24 h or a range between any two of them.
[0040] When the temperature, pressure and time of the curing treatment meet the above-mentioned limitations, during the in-situ polymerization process, the liquid precursor can well infiltrate the electrode to form a closer interface contact. Under the action of external conditions (temperature and pressure) and initiators, the polymerizable functional groups in the precursor solution undergo polymerization reaction, thereby forming a polymer electrolyte in situ, further improving the low-temperature performance of the battery.
[0041] Furthermore, in a specific embodiment of the present invention, the electrolyte before solidification treatment includes lithium salt, solvent, and additives.
[0042] In detail, the lithium salt includes but is not limited to at least one of LiTFSI, LiPF6, LiFSI, LiBOB, LiBF4, LiDFOB, and LiBOB; the solvent includes but is not limited to at least one of PC, EC, DMC, DEC, and EMC; and the additives include but are not limited to at least one of a conductive additive, an overcharge protection additive, and a flame retardant additive.
[0043] In one specific embodiment, the electrolyte before curing includes LiPF6, LiFSI, EC, EMC, DMC, VC, and FEC.
[0044] It is understandable that LiPF6 can provide ionic conductivity and regulate the stability of the electrolyte, and the mass percentage of LiPF6 in the electrolyte is closely related to the performance.
[0045] Furthermore, in a specific embodiment of the present invention, the lithium salt includes LiPF6, and the mass percentage of LiPF6 is 9wt.%-13wt.%.
[0046] In detail, the mass percentage of LiPF6 in the electrolyte includes but is not limited to 9wt.%, 9.5wt.%, 10wt.%, 10.5wt.%, 11wt.%, 11.5wt.%, 12wt.%, 12.5wt.%, 13wt.% or a range between any two of them.
[0047] When the mass percentage of LiPF6 is within the above range, it can not only support ion transfer during battery charging and discharging, but also provide better battery cycle life, charging and discharging efficiency and temperature characteristics, and improve low-temperature performance.
[0048] Furthermore, in a specific embodiment of the present invention, in step 2), the temperature of the chemical conversion treatment is 35-45° C., and the extrusion pressure is 1000 kg / f.
[0049] In detail, the temperature of the chemical conversion treatment includes but is not limited to 35°C, 36°C, 37°C, 38°C, 39°C, 40°C, 41°C, 42°C, 43°C, 44°C, 45°C or a range between any two thereof.
[0050] The chemical formation treatment of the present invention adopts a constant current charging method, and the charging current is 110-550mA.
[0051] The present invention does not limit the time of the chemical formation treatment, and a suitable time can be selected according to actual conditions. In a specific embodiment, the time of the chemical formation treatment is 4-6 hours.
[0052] When the temperature of the formation treatment is within the above range, it can not only prevent the battery from solidifying during the formation stage due to excessively high temperature, but also effectively form the battery. At the same time, the extrusion pressure of 1000kg / f can enable the battery to better form the SEI film through extrusion, making the battery more stable, and further improving the battery's charge and discharge performance and comprehensive performance such as self-discharge and storage.
[0053] Furthermore, in a specific embodiment of the present invention, a first static treatment is further included before the curing treatment, and the temperature of the first static treatment is 20-30° C. and the time is 24-72 hours.
[0054] Specifically, the temperature of the first static treatment includes, but is not limited to, 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, 29°C, 30°C, or a range between any two thereof. The time includes, but is not limited to, 24h, 30h, 35h, 40h, 45h, 50h, 55h, 60h, 65h, 70h, 72h, or a range between any two thereof.
[0055] Performing the first static treatment on the battery before curing treatment within the above temperature and time range can gradually release its internal stress, thereby reducing the internal deformation or stress concentration problems that may occur during the formation or curing process. This helps to improve the manufacturing quality and performance stability of solid-state batteries.
[0056] Furthermore, in a specific embodiment of the present invention, a second static treatment is further included after the chemical formation treatment, and the temperature of the second static treatment is 20-30° C. and the time is 24-72 hours.
[0057] Specifically, the temperature of the first static treatment includes, but is not limited to, 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, 29°C, 30°C, or a range between any two thereof. The time includes, but is not limited to, 24h, 30h, 35h, 40h, 45h, 50h, 55h, 60h, 65h, 70h, 72h, or a range between any two thereof.
[0058] After the formation treatment, the second static treatment is carried out at the above temperature and time to ensure that the structure and chemical properties formed during the formation process can be stably present under a wider range of temperature and environmental conditions. At the same time, it helps to further reduce the stress inside the battery and improve the overall stability and performance of the battery.
[0059] Furthermore, in a specific embodiment of the present invention, the battery after injection includes a positive electrode sheet, the positive electrode sheet includes a positive electrode slurry, and the positive electrode slurry includes lithium iron phosphate, conductive carbon black, a binder, and 1%-2% LATP.
[0060] The binder in the present invention includes any one of polyvinylidene fluoride, polyethylene oxide, polyvinyl alcohol, polyurethane, polyacrylic acid, sodium carboxymethyl cellulose or polyacrylonitrile, or a combination of at least two thereof.
[0061] 1%-2% LATP means that the mass percentage of LATP in the positive electrode slurry is 1%-2%. In detail, the mass percentage of LATP in the positive electrode slurry includes but is not limited to 1%, 1.2%, 1.4%, 1.6%, 1.8%, 2.0% or a range composed of any two thereof.
[0062] The present invention does not limit the preparation process of coating the positive electrode slurry on the positive electrode sheet, and conventional processes in the art may be used.
[0063] In one embodiment, the positive electrode slurry is extruded onto the carbon-coated aluminum foil AB surface, and the surface density is 345±4g / m 2 , and bake to avoid baking cracking, lateral cracks and solvent dripping. The LATP doped in the positive electrode slurry has high conductivity, which is conducive to building an ion-conducting network and shortening the diffusion path of electrons and ions. The large specific surface area material helps to pass lithium ions, further accelerate the ion transmission rate, and improve low-temperature performance.
[0064] Another aspect of the present invention provides a semi-solid-state battery prepared by the preparation method described above.
[0065] Since the battery is prepared by the above preparation method, it has good low-temperature performance.
[0066] According to another aspect of the present invention, there is provided an electronic device, comprising the semi-solid-state battery as described above.
[0067] The present invention is not limited to a specific type of electronic device, as long as it includes the semi-solid battery as described above.
[0068] In one specific embodiment, the electronic device is a drone, in another specific embodiment, the electronic device is a new energy vehicle; in another specific embodiment, the electronic device is a smart wearable device.
[0069] Since the electronic device provided by the present invention includes the semi-solid battery as described above, the electronic device still has good performance in relatively cold areas.
[0070] The semi-solid-state battery provided by the present invention is described below through specific embodiments.
[0071] Example 1
[0072] The method for preparing a semi-solid-state battery provided in this embodiment comprises the following steps:
[0073] 1. Injection: Inject electrolyte containing semi-solid additives into the assembled battery, with the mass ratio of additives to electrolyte being 3:97;
[0074] The positive electrode sheet of the assembled battery includes: the main material of the positive electrode sheet is lithium iron phosphate, the binder is polyethylene oxide, and the conductive agent is carbon black, and the mass ratio is 96:2.2:1.8;
[0075] The negative electrode sheet of the assembled battery includes: the main material of the negative electrode sheet is graphite, the binder is styrene-butadiene rubber, and the conductive agent is carbon black, with a mass ratio of 96.1:1.8:2.1;
[0076] The components of the injected electrolyte are EC, EMC, DMC, LiPF6, LiFSI, VC, and FEC in a mass ratio of 34.2:41.8:8.5:9.5:3.0:2.5:0.5.
[0077] 2. Curing: The battery after liquid injection is first placed at 25°C for 48 hours, and then cured at 60°C, with an applied pressure of 1000kg / f and a curing time of 12 hours to obtain a cured battery.
[0078] 3. Formation: The cured battery is charged at a constant current of 110 mA, the formation temperature is 35° C., the extrusion pressure is 1000 kg / f, and the formation time is 5 h to obtain a formed battery.
[0079] 4. Secondary sealing: First, the air bag is punctured by a guillotine and vacuumed at the same time, so that the gas in the air bag and a small part of the electrolyte will be extracted, and then the secondary sealing head will be immediately sealed in the secondary sealing area to ensure the airtightness of the battery, and finally the air bag is cut off from the packaged battery cell.
[0080] 5. Capacity division: The batteries that have completed the second sealing are placed in the capacity division cabinet for capacity division. During the battery manufacturing process, different battery cells may have slight differences. Battery capacity division can accurately measure and classify these differences to improve the overall performance and life of the battery pack, and finally obtain a semi-solid-state battery.
[0081] Example 2
[0082] The preparation method of the semi-solid-state battery provided in this embodiment is basically the same as that in Embodiment 1, except that:
[0083] In step 2), the curing temperature is 70° C. and the applied pressure is 1000 kg / f.
[0084] Example 3
[0085] The preparation method of the semi-solid-state battery provided in this embodiment is basically the same as that in Embodiment 1, except that:
[0086] In step 2), the curing time is 24 hours.
[0087] Example 4
[0088] The preparation method of the semi-solid-state battery provided in this embodiment is basically the same as that in embodiment 2, except that:
[0089] In step 2), the curing time is 24 hours.
[0090] Example 5
[0091] The method for preparing a semi-solid-state battery provided in this embodiment comprises the following steps:
[0092] 1. Injection: Inject electrolyte containing semi-solid additives into the assembled battery, with the mass ratio of additives to electrolyte being 3:97;
[0093] The positive electrode sheet of the assembled battery includes: the main material of the positive electrode sheet is lithium iron phosphate, the binder is polyethylene oxide, and the conductive agent is carbon black, and the mass ratio is 96:2.2:1.8;
[0094] The negative electrode sheet of the assembled battery includes: the main material of the negative electrode sheet is graphite, the binder is styrene-butadiene rubber, and the conductive agent is carbon black, with a mass ratio of 96.1:1.8:2.1;
[0095] The components of the injected electrolyte are EC, EMC, DMC, LiPF6, LiFSI, VC, and FEC in a mass ratio of 34.2:41.8:8.5:9.5:3.0:2.5:0.5.
[0096] 2. Curing: The battery after liquid injection is first placed at 30°C for 48 hours, and then cured at 50°C, with an applied pressure of 1000kg / f and a curing time of 36 hours to obtain a cured battery.
[0097] 3. Formation: The cured battery is charged at a constant current of 110 mA, the formation temperature is 35° C., the extrusion pressure is 1000 kg / f, the formation time is 5 h, and the formed battery is obtained. The formed battery is subjected to a second static treatment at a temperature of 20° C. for 48 h.
[0098] 4. Secondary sealing: First, the air bag is punctured by a guillotine and vacuumed at the same time, so that the gas in the air bag and a small part of the electrolyte will be extracted, and then the secondary sealing head will be immediately sealed in the secondary sealing area to ensure the airtightness of the battery, and finally the air bag is cut off from the packaged battery cell.
[0099] 5. Capacity division: The batteries that have completed the second sealing are placed in the capacity division cabinet for capacity division. During the battery manufacturing process, different battery cells may have slight differences. Battery capacity division can accurately measure and classify these differences to improve the overall performance and life of the battery pack, and finally obtain a semi-solid-state battery.
[0100] Example 6
[0101] The preparation method of the semi-solid-state battery provided in this embodiment is basically the same as that in Embodiment 1, except that:
[0102] In step 2), the curing temperature is 50° C., the pressure is 500 kg / f, and the time is 48 h.
[0103] Example 7
[0104] The preparation method of the semi-solid-state battery provided in this embodiment is basically the same as that in Embodiment 1, except that:
[0105] In step 1), the components of the electrolyte are EC, EMC, DMC, LiPF6, LiFSI, VC, and FEC in a mass ratio of 26.5:45.5:8.5:13.5:3.0:2.5:0.5.
[0106] Example 8
[0107] The preparation method of the semi-solid-state battery provided in this embodiment is basically the same as that in Embodiment 1, except that:
[0108] In step 3), the forming temperature of the forming treatment is 30° C. and the extrusion pressure is 800 kg / f.
[0109] Comparative Example 1
[0110] The preparation method of the semi-solid-state battery provided in this comparative example is basically the same as that in Example 1, except that:
[0111] In step 2), no pressurization is performed during the curing process, and there is no pressure.
[0112] Comparative Example 2
[0113] The preparation method of the semi-solid-state battery provided in this comparative example is basically the same as that in Example 1, except that:
[0114] In step 2), the temperature during the curing process is 45° C., the pressure is 2500 kg / f, and the time is 24 hours.
[0115] Comparative Example 3
[0116] The preparation method of the semi-solid-state battery provided in this comparative example is basically the same as that in Example 1, except that:
[0117] In step 2), the curing temperature is 75° C., the pressure is 450 kg / f, and the time is 12 h.
[0118] Test Case
[0119] The semi-solid batteries provided in all the embodiments and comparative examples are tested, including the following steps:
[0120] a) Initial discharge of battery cells;
[0121] b) The battery cells are placed at (5±2)℃ for 20h;
[0122] c) At (5±2)℃, charge the battery cells at a constant power of P to the charging termination voltage of any cell or module and leave it to stand for 30 minutes;
[0123] d) At (5±2)°C, the battery cell is discharged at a constant power of P to the discharge termination voltage of the battery cell;
[0124] e) Record the charging energy, discharging energy, charging time, discharging time, charging capacity, and discharging capacity of c) and d); calculate the energy efficiency; calculate the energy retention rate of the charging energy and discharging energy relative to the initial charging energy and initial discharging energy, respectively.
[0125] The specific test results are shown in Table 1. Figure 1 This is a comparison chart of 5°C low temperature charging of Examples 1-4. Figure 2 It is a comparison chart of 5°C low-temperature discharge of Examples 1-4.
[0126] Table 1
[0127] Serial number Charge / initial energy Discharge / initial energy Energy efficiency Example 1 90.51% 63.61% 67.55% Example 2 88.04% 61.17% 67.31% Example 3 79.49% 55.15% 61.69% Example 4 74.81% 51.55% 60.46% Example 5 75.25% 53.31% 61.06% Example 6 75.28% 51.68% 61.55% Example 7 76.64% 51.25% 62.24% Example 8 78.62% 54.76% 65.16% Comparative Example 1 74.25% 50.18% 60.26% Comparative Example 2 72.55% 49.44% 59.82% Comparative Example 3 71.36% 48.97% 57.24%
[0128] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a semi-solid battery, characterized in that: The following steps are involved: 1) curing the battery after injection at 50-70° C. and 500-2000 kg / f for 12-48 hours to obtain a cured battery; 2) Performing a formation treatment on the cured battery to obtain a semi-solid battery.
2. The preparation method according to claim 1, characterized in that: In step 1), the curing treatment temperature is 60-70° C., the pressure is 1000-2000 kg / f, and the time is 12-24 hours.
3. The preparation method according to claim 1 or 2, characterized in that: The electrolyte before solidification treatment includes lithium salt, solvent and additives.
4. The preparation method according to claim 3, characterized in that: The lithium salt includes LiPF6, and the mass percentage of LiPF6 is 9wt.%-13wt.%.
5. The preparation method according to any one of claims 1 to 4, characterized in that: In step 2), the chemical treatment temperature is 35-45° C., and the extrusion pressure is 1000 kg / f.
6. The preparation method according to any one of claims 1 to 5, characterized in that: The curing process also includes a first static treatment, wherein the temperature of the first static treatment is 20-30° C. and the static treatment lasts for 24-72 hours.
7. The preparation method according to any one of claims 1 to 6, characterized in that: The chemical formation treatment further includes a second static treatment, wherein the temperature of the second static treatment is 25° C. and the static treatment lasts for 24-72 hours.
8. The preparation method according to any one of claims 1 to 7, characterized in that: The battery after injection includes a positive electrode sheet, and the positive electrode sheet includes a positive electrode slurry. The positive electrode slurry comprises lithium iron phosphate, conductive carbon black, conductive slurry, a binder and 1%-2% of LATP.
9. A semi-solid battery, characterized in that: The preparation method is described in any one of claims 1 to 8.
10. An electronic device, characterized in that: Comprising the semi-solid-state battery as described in claim 9.
Citation Information
Cited By
Semi-solid-state battery, and preparation method therefor and use thereof
WO2026037062A1