Full-high-entropy perovskite solar cell and preparation method thereof
By constructing full high entropy perovskite solar cells, the configuration entropy of high-entropy materials is used to improve stability, and the stability problem of perovskite solar cells in harsh environments is solved, achieving efficient photoelectric conversion and stability improvement.
Patent Information
- Application Number
- CN202411274042.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-01
AI Technical Summary
Perovskite solar cells have limited thermodynamic and environmental stability under high temperature, ultraviolet, strong acidic, alkaline environments and high humidity conditions, which limits their commercial applications.
Using full high entropy perovskite material, the high entropy metal oxide hole transport layer, high entropy 3D perovskite absorbing layer, high entropy 2D perovskite modified layer and high entropy metal oxide electrons are constructed in turn on the conductive glass substrate. The transport layer is prepared by hydrothermal method and spin coating method to increase the configuration entropy of the material to improve stability.
It significantly improves the photoelectric conversion efficiency and stability of perovskite solar cells, reduces the need for doping inactive elements, expands the range of material properties modulation, and enhances thermal stability and chemical stability.
Smart Images

Figure CN118890907A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of perovskite solar cells, and in particular relates to a full high entropy perovskite solar cell and a preparation method thereof. Background Art
[0002] Using clean and sustainable resources to generate electricity and protecting the environment are two major challenges facing mankind in the 21st century. Since the Industrial Revolution, mankind has become increasingly dependent on fossil fuels, including coal, natural gas and oil, the combustion of which has led to climate change. In order to reduce dependence on fossil fuels, renewable green energy, such as solar energy, has become an inevitable choice.
[0003] In order to effectively convert light energy into electrical energy, it is necessary to rationally develop and utilize solar cells. Solar cells are small in size, easy to move, and are not restricted by geographical location. At present, the solar cells that dominate the market are mainly monocrystalline silicon and polycrystalline silicon solar cells, and the production technology of these two types of cells is relatively mature. However, silicon-based solar cells have strict requirements on raw materials, and the purity is generally above 99.9999%. In addition, there is little room for cell efficiency to increase, the manufacturing process is complex, and the manufacturing cost is high, which greatly restricts the further reduction of power generation costs. In recent years, perovskite materials have been widely used in solar cells, light-emitting diodes, detectors, lasers, catalytic solid oxide cells and other fields. Among them, perovskite solar cells have been widely studied and applied by enterprises and research institutes in recent years due to their extremely high photoelectric conversion efficiency and low manufacturing cost.
[0004] Perovskites have a general ABX3-type structure, where A is a highly positive alkaline, alkaline earth or rare earth metal cation, B is a transition metal cation, and X is an oxygen or halogen anion. Since the A and B sites can flexibly accommodate different elements, the properties of perovskites can be adjusted as needed. However, perovskite materials have limited thermodynamic and environmental stability and will be severely degraded under adverse conditions, including high temperature, ultraviolet light, strong acidity, alkaline environment, high humidity and other conditions. Two strategies are usually used to improve the stability of perovskites. The first method is to introduce a protective layer (such as hydrophobic or heat / light / ultraviolet insulation, etc.) to protect the perovskite from the harsh environment. The other is to dope the perovskite with less active elements or passivating additive materials to regulate the perovskite crystal growth kinetics and passivate various types of defects. However, the existing methods are still limited in significantly improving the stability, making the commercialization of perovskite solar cells full of obstacles.
[0005] Compared with traditional materials with a single component, high entropy materials composed of disordered multiple components can show enhanced material properties and have attracted more and more attention. High entropy materials have better thermodynamic stability than ordinary materials due to their larger configurational entropy. The first batch of high entropy materials are high entropy alloys (HEAs), which contain 5 or more metal elements with a molar ratio between 5% and 35%. High entropy alloys have a higher configurational entropy, defined as Where R is the universal gas constant, N is the number of elements in the alloy, and x i is the molar fraction of element i. config ≥1.5R, R≤ΔS config ≤1.5R and ΔS config When ≤R, the entropy of the alloy is “high”, “medium”, and “low”, respectively. Similarly, high entropy perovskites (HEPs) can also be defined by configurational entropy, given by Where N and M are the number of positive ions and negative ions, respectively. i (i=1, 2, ..., N) and x j (j = 1, 2, ... M) is the molar fraction of each element in the cation (A or B position) and anion (X position). In general, anions have a small effect on configurational entropy, doping is difficult to control, and there are few elements that can be introduced into the X position. Therefore, high-entropy perovskites are defined as perovskite-type materials that contain five or more cations in the A and B positions, and the content of each cation is at least 5 mol%. In high-entropy perovskites, Gibbs free energy G = H-ΔTS, where H is enthalpy, T is absolute temperature, and S is entropy. When the configurational entropy (a component of S) increases, the Gibbs free energy decreases, resulting in thermodynamic stability. Therefore, high-entropy perovskites can maintain negative G values at high sintering temperatures, prevent phase transitions during cooling, and form energy-stable single-phase structures. These stable structures show excellent chemical and structural stability, making them very suitable for energy applications. In addition, compared with low-entropy perovskites, the incorporation of multiple cations expands the property modulation of high-entropy perovskites and expands the potential application range of high-entropy perovskites. High-entropy perovskites have great potential in solar cells due to their improved stability driven by high configurational entropy. Increasing the entropy of perovskites can improve the stability of photovoltaic devices, so there is no need to dope inactive elements that may cause performance loss. Applying this high-entropy design to perovskite solar cells will result in a series of functional layer devices with high stability guided by high entropy properties, thereby improving the performance of the cell. Summary of the invention
[0006] A full high entropy perovskite solar cell and a method for preparing the same.
[0007] The full high-entropy perovskite solar cell includes, from bottom to top: a conductive glass substrate, a high-entropy metal oxide hole transport layer, a high-entropy 3D perovskite light absorption layer, a high-entropy 2D perovskite modification layer, a high-entropy metal oxide electron transport layer, and a metal electrode layer;
[0008] The high entropy metal oxide hole transport layer is composed of a high entropy metal oxide material containing five or more metal elements, and the metal elements are Ni, Cu, Mo, V, W, Fe, Co, Li, Mg, Ga, Cr, In, and Sc.
[0009] The high entropy 3D perovskite light absorbing layer adopts a high entropy perovskite material containing five or more A-site and B-site cations, wherein the A-site cation has MA + , FA + , Cs + , Rb + , K + , Li + 、Na + , Sr + 、Be + Mg + , Ca + , Ba + , Ra + ,La + , Pr + 、Nd + 、Sm + and Mn + , the B-site cation is Pb + Sn + Mg + , Ca + Sc + 、Ti + 、V + , Fe + 、Co + 、Ni + , Cu + 、Zn + , Ga + 、Al + , Nb + 、Mo + 、Ru + , W + , Ir + , Pt + 、Bi + and Ce + , the anions at the X position are F, Cl, Br, and I.
[0010] The high entropy 2D perovskite modification layer adopts a high entropy perovskite material containing five or more A-position organic cations, wherein the A-position organic cations include OA+ 、PEA + , B.A. + , BDA + 、BEA + 、CMA + , DAT + , GA + , HA + ,PA + , PDA + PEI + 、PeDA + 、PMA + POPA + ThMA + , BdA + , HaD + , OdA + .
[0011] The high entropy metal oxide electron transport layer adopts a high entropy metal oxide material containing five or more metal elements, and the metal elements are Sn, Ti, Zn, Al, Zr, Si, W, Nb, Ce, Sr, Fe, Cr, and Ba.
[0012] The thickness of the high entropy metal oxide hole transport layer is 20-70 nm, specifically 30 nm.
[0013] The thickness of the high entropy 3D perovskite light absorbing layer is 300-900nm, specifically 600nm.
[0014] The thickness of the high entropy 2D perovskite modification layer is 100-700 nm, specifically 300 nm.
[0015] The thickness of the high entropy metal oxide electron transport layer is 20-70 nm, specifically 30 nm.
[0016] The thickness of the counter electrode layer is 100-300 nm, and can be specifically 120 nm. The material of the counter electrode can specifically be Ag.
[0017] The perovskite solar cell provided by the present invention is prepared according to a method comprising the following steps:
[0018] 1) cleaning the conductive glass substrate, and then drying the conductive glass substrate in a vacuum drying oven for later use;
[0019] 2) preparing a high entropy metal oxide hole transport layer nanocrystalline material by a hydrothermal method, preparing the obtained nanocrystalline material into a precursor solution, and spin-coating it on a conductive glass substrate, and annealing it at 180° C. to form a high entropy metal oxide hole transport layer;
[0020] 3) A high entropy 3D perovskite light absorbing layer was prepared by spin coating on the high entropy metal oxide hole transport layer using a two-step method;
[0021] 4) Spin-coating a solution containing five or more organic cation precursors on the high entropy 3D perovskite light-absorbing layer by a dynamic spin coating method to prepare a high entropy 2D perovskite modified layer;
[0022] 5) preparing a high entropy metal oxide electron transport layer nanocrystalline material by a hydrothermal method, preparing the obtained nanocrystalline material into a precursor solution, and spin-coating it on the high entropy 2D perovskite modified layer, and annealing at 150° C. to form a high entropy metal oxide electron transport layer;
[0023] 6) Preparing a metal electrode layer on the high entropy metal oxide electron transport layer to obtain the full high entropy perovskite solar cell.
[0024] In step 2), the high entropy metal oxide hole transport layer material is synthesized by hydrothermal method. The specific preparation method is: five or more chlorides composed of Ni, Cu, Mo, V, W, Fe, Co, Li, Mg, Ga, Cr, In, Sc metal elements are configured into an aqueous solution, and under the condition of magnetic stirring, concentrated ammonia stock solution is slowly added to a pH value of 7, the reaction solution is transferred into a hydrothermal reactor, placed in a 90°C drying oven for three hours, and the precipitate is washed with deionized water for more than three times to obtain a high entropy metal oxide hole transport layer nanocrystalline material, and a high entropy metal oxide nanocrystal precursor solution is obtained by a water dispersion method. .
[0025] In step 3), the high entropy 3D perovskite light-absorbing layer is prepared by a two-step spin coating method. The specific preparation method is: adding a metal halide to a mixed solvent of DMF and DMSO to obtain a 1-1.8 mM first part of the precursor solution, spin coating it on the high entropy metal oxide hole transport layer, annealing to obtain a metal halide film, spin coating 0.1-0.8 mM A-site cation precursor solution on the metal halide film, and annealing to obtain a high entropy 3D perovskite light-absorbing layer containing five or more A-site and B-site cations.
[0026] In step 4), the high entropy 2D perovskite modification layer is prepared by dynamic spin coating. The specific preparation method is: dynamically spin coating a solution containing 0.01 to 0.5 mM of five or more organic cation halide precursors on the high entropy 3D perovskite light absorbing layer, and annealing at 90°C to obtain a high entropy 2D perovskite modification layer.
[0027] In step 5), the high entropy metal oxide electron transport layer material is synthesized by hydrothermal method. The specific preparation method is: five or more chlorides composed of Sn, Ti, Zn, Al, Zr, Si, W, Nb, Ce, Sr, Fe, Cr, Ba metal elements are configured into an aqueous solution, and under the condition of magnetic stirring, concentrated ammonia stock solution is slowly added to a pH value of 7, the reaction solution is transferred into a hydrothermal reactor, placed in a 90°C drying oven for three hours, and the precipitate is washed with deionized water for more than three times to obtain a high entropy metal oxide electron transport layer nanocrystalline material, and a high entropy metal oxide nanocrystal precursor solution is obtained after dispersion with an isopropanol solvent.
[0028] In step 6), when the material of the counter electrode is Ag, the preparation method may be: vacuum evaporation of Ag on the high entropy hole transport electron transport layer. The evaporation rate of Ag is The vacuum degree is 1.0×10 3 Pa or less, the obtained metal electrode layer.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] The present invention constructs a full high entropy perovskite solar cell, and the incorporation of multiple cations expands the property modulation of high entropy perovskites and expands the potential application range of high entropy perovskites. In addition, due to its improved stability driven by high configuration entropy, high entropy perovskites have great potential in solar cells. Increasing the entropy of perovskites can improve the stability of photovoltaic devices, so there is no need to dope inactive elements that may cause performance loss. This high entropy design is applied to perovskite solar cells to obtain a series of functional layer devices with high stability guided by high entropy properties, thereby improving the performance of the battery.
[0031] The present invention constructs a full high-entropy perovskite solar cell, increases the overall configuration entropy of each functional layer and reduces the Gibbs free energy, effectively improves the thermal stability of the carrier transport layer and the perovskite film and effectively inhibits the phase change of the material, thereby significantly improving the photoelectric conversion efficiency and stability of the perovskite solar cell. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is a scanning electron microscope image of a high entropy perovskite film in Example 1 of the present invention;
[0033] Figure 2 is a JV curve diagram of a full high entropy perovskite solar cell in Example 1;
[0034] Figure 3 It is a schematic structural diagram of a full high entropy perovskite solar cell of the present invention. DETAILED DESCRIPTION
[0035] This embodiment provides a structure of an inverted perovskite solar cell with a full high entropy structure, which includes, from bottom to top: 1, a conductive glass substrate, 2, a high entropy metal oxide hole transport layer, 3, a high entropy 3D perovskite light absorption layer, 4, a high entropy 2D perovskite modification layer, 5, a high entropy metal oxide electron transport layer, and 6, a metal electrode layer. The high entropy 3D perovskite light absorption layer is prepared by a two-step spin coating method, the high entropy 2D perovskite modification layer is prepared by a dynamic spin coating method, and the high entropy metal oxide electron transport layer material and the high entropy metal oxide hole transport layer material are synthesized by a hydrothermal method and prepared into a thin film by spin coating.
[0036] Example 1
[0037] A full high entropy perovskite solar cell and a preparation method thereof, comprising the following steps:
[0038] S1. The etched ITO conductive glass substrate is cleaned, and the cleaning steps include ultrasonic cleaning with detergent, deionized water, acetone, anhydrous ethanol and isopropanol in sequence, followed by drying with dry nitrogen and performing ultraviolet ozone pretreatment for 15 minutes.
[0039] S2. Prepare a high entropy metal oxide hole transport layer on a clean ITO conductive glass substrate with a film thickness of 25 nm. The specific operation method is: according to the hydrothermal method, CuCl2, NiCl2, MgCl2, ZnCl2, and FeCl3 are prepared in an equal molar ratio to prepare 0.2 mol·L -1 30ml of aqueous solution was added and transferred into a sealed container. Under magnetic stirring, concentrated ammonia solution was slowly added until the pH value was 7. The reaction solution was transferred into a 50ml hydrothermal reactor and placed in a 90° drying oven for three hours. The precipitate was washed with deionized water for more than three times to obtain Cu 0.2 Ni 0.2 Mg 0.2 Zn 0.2 Fe 0.2 O x Nanocrystals. Processing of Cu by water dispersion method 0.2 Ni 0.2 Mg 0.2 Zn 0.2 Fe 0.2 O x After the precursor solution is prepared, it is spin-coated at a speed of 3000 rpm / s for 30 seconds on an ITO conductive glass substrate. After the spin coating is completed, the ITO conductive glass is transferred to a hot stage at 180°C and annealed for 30 minutes to obtain a uniform Cu 0.2 Ni 0.2 Mg 0.2 Zn 0.2 Fe 0.2 O xHole transport layer.
[0040] S3. Prepare a high entropy 3D perovskite light-absorbing layer on the high entropy metal oxide hole transport layer with a film thickness of 500nm. The specific operation method is: prepare it by a two-step spin coating method. In the first step, add PbI2 to a mixed solvent of DMF and DMSO to obtain a 1.5mM first part of the precursor solution, and spin coat it on the high entropy hole transport layer. The spin coating parameters are 2000rpm / s, and the spin coating time is 30 seconds. Anneal at 100°C for 1min to obtain the PbI2 film. MAI:FAI:CsI:RbI is prepared at a molar ratio of 15:3:1:1 to obtain a 0.5mM precursor solution, and then spin coat it on the PbI2 film. The spin coating speed is 3000rpm / s, and the spin coating time is 50s. Anneal at 100°C for 15min to obtain Rb 0.05 Cs 0.05 FA 0.15 MA 0.75 PbI3 perovskite light absorbing layer.
[0041] S4. Prepare a high entropy 2D perovskite modification layer on the high entropy 3D perovskite light absorbing layer, with a film thickness of 300nm. The specific operation method is: prepare it by dynamic spin coating. OAI, PEAI, BAI, BDAI, and BEAI are prepared in an equal molar ratio to prepare a 0.05mM high entropy 2D perovskite modification layer precursor solution, and dynamically spin coat the precursor solution on the high entropy 3D perovskite light absorbing layer. The spin coating parameters are 3000rpm / s and the spin coating time is 40 seconds. Then thermally anneal at 90°C for 10 minutes to obtain a uniform OA 0.2 PEA 0.2 BA 0. 2BDA 0.2 BEA 0.2 PbI3 perovskite modified layer.
[0042] S5. Prepare a high entropy metal oxide hole transport layer on the high entropy 2D perovskite modified layer, with a film thickness of 25 nm. The specific operation method is: according to the hydrothermal method, TiCl4, ZnCl2, AlCl3, SnCl4, and FeCl3 are prepared in an equal molar ratio to prepare 0.2 mol·L -1 30ml of aqueous solution was transferred into a sealed container. Under magnetic stirring, concentrated ammonia stock solution was slowly added until the pH value was 7. The reaction solution was transferred into a 50ml hydrothermal reactor and placed in a 90° drying oven for three hours. After washing the precipitate with deionized water for more than three times, Ti 0.2 Zn 0.2 Al 0.2 Sn 0.2 Fe 0.2 O x Nanocrystals. Ti was obtained after dispersion in isopropanol solvent. 0.2Zn 0.2 Al 0.2 Sn 0.2 Fe 0.2 O x The precursor solution was then spin-coated at 3000 rpm / s for 30 s and thermally annealed at 150 °C for 30 min to obtain a uniform Cu 0.2 Ni 0.2 Mg 0.2 Zn 0.2 Fe 0.2 O x Electron transport layer.
[0043] S6. A layer of silver electrode with a thickness of 100 nm is sputtered on the sample prepared in step S5 by magnetron sputtering, thereby obtaining a high-quality perovskite solar cell.
[0044] S7. The photoelectric performance of the prepared perovskite solar cell was tested. The results showed that the open circuit voltage was 1.13V and the short circuit current density was 24.80mA / cm 2 , the filling factor is 0.76, and the photoelectric conversion efficiency reaches 21.66%.
[0045] Example 2
[0046] A method for preparing a full high entropy perovskite solar cell, the steps are the same as those in Example 1, except that in S2, CuCl2, NiCl2, MgCl2, CoCl2, and LiCl are prepared in an equal molar ratio by a hydrothermal method to obtain 0.2 mol·L -1 30ml of aqueous solution was added and transferred into a sealed container. Under magnetic stirring, concentrated ammonia solution was slowly added until the pH value was 7. The reaction solution was transferred into a 50ml hydrothermal reactor and placed in a 90° drying oven for three hours. After the reaction, the precipitate was washed with deionized water for more than three times to obtain Cu 0.2 Ni 0.2 Mg 0.2 Co 0.2 Li 0.2 O x Nanocrystals. Processing of Cu by water dispersion method 0.2 Ni 0.2 Mg 0.2 Co 0.2 Li 0.2 O x After the precursor solution is prepared, it is spin-coated at a speed of 3000 rpm / s for 30 seconds on an ITO conductive glass substrate. After the spin coating is completed, the ITO conductive glass is transferred to a hot stage at 180°C and annealed for 30 minutes to obtain a uniform Cu 0.2 Ni 0.2 Mg 0.2 Co0.2 Li 0.2 O x The electron transport layer has a film thickness of 30 nm.
[0047] Example 3
[0048] A method for preparing a full high entropy perovskite solar cell, the steps are the same as those in Example 1, the difference is that in S3, a high entropy 3D perovskite light absorbing layer is prepared on a high entropy metal oxide hole transport layer, and the preparation is prepared by a two-step spin coating method. In the first step, PbI2 is added to a mixed solvent of DMF and DMSO to obtain a 1.5mM first part of the precursor solution, which is spin-coated on the high entropy hole transport layer. The spin coating parameters are 2000rpm / s, and the spin coating time is 30 seconds. Annealing at 100°C for 1min obtains a PbI2 film. MAI:FAI:CsI:RbI is prepared at a molar ratio of 12:6:1:1 to obtain a 0.5mM precursor solution, which is then spin-coated on the PbI2 film. The spin coating speed is 3000rpm / s, and the spin coating time is 50s. Annealing at 100°C for 15min obtains Rb 0.05 Cs 0.05 FA 0.3 MA 0.6 PbI3 perovskite light absorbing layer.
[0049] Example 4
[0050] A method for preparing a full high entropy perovskite solar cell, the steps are the same as those in Example 1, the difference is that in S3, a high entropy 3D perovskite light absorbing layer is prepared on a high entropy metal oxide hole transport layer, and the preparation is prepared by a two-step spin coating method. In the first step, PbI2 and SnI4 are added in equal molar ratios to a mixed solvent of DMF and DMSO to obtain a 1.5mM first part of the precursor solution, which is spin-coated on the high entropy hole transport layer. The spin coating parameters are 2000rpm / s, and the spin coating time is 30 seconds. Annealing at 100°C for 1min obtains a metal halide film. MAI:FAI:CsI:RbI is prepared at a molar ratio of 12:6:1:1 to obtain a 0.5mM precursor solution, which is then spin-coated on a metal halide film. The spin coating speed is 3000rpm / s, and the spin coating time is 50s. Annealing at 100°C for 15min obtains Rb 0.05 Cs 0.05 FA 0.3 MA 0.6 Pb 0.5 Sn 0.5 I3 perovskite light-absorbing layer.
[0051] Example 5
[0052] A method for preparing a full high entropy perovskite solar cell, the steps are the same as those in Example 1, the difference is that in S3, a high entropy 3D perovskite light absorbing layer is prepared on a high entropy metal oxide hole transport layer, and the preparation is prepared by a two-step spin coating method. In the first step, PbI2 and SnI4 are added in equal molar ratios to a mixed solvent of DMF and DMSO to obtain a 1.5mM first part precursor solution, which is spin-coated on the high entropy hole transport layer. The spin coating parameters are 2000rpm / s, and the spin coating time is 30 seconds. Annealing at 100°C for 1min obtains a metal halide film. MAI:FAI:CsI is prepared at a molar ratio of 17:2:1 to obtain a 0.5mM precursor solution, which is then spin-coated on a metal halide film. The spin coating speed is 3000rpm / s, and the spin coating time is 50s. Annealing at 100°C for 15min obtains Cs 0.05 FA 0.1 MA 0.85 Pb 0.5 Sn 0.5 I3 perovskite light-absorbing layer.
[0053] Example 6
[0054] A method for preparing a full high entropy perovskite solar cell, the steps are the same as those in Example 1, the difference is that in S4, a high entropy 2D perovskite modification layer is prepared on the high entropy 3D perovskite light absorbing layer by a dynamic spin coating method. The specific operation method is: prepare by dynamic spin coating. PEBr, PEABr, BAI, PAI, and PDAI are prepared in an equimolar ratio to obtain a 0.05mM high entropy 2D perovskite modification layer precursor solution, and the precursor solution is dynamically spin coated on the high entropy 3D perovskite light absorbing layer, the spin coating parameters are 3000rpm / s, and the spin coating time is 40 seconds. Then thermally anneal at 90°C for 10 minutes to obtain a uniform PE 0.2 PEA 0.2 BA 0.2 PA 0.2 PDA 0.2 The PbI3 perovskite modified layer has a film thickness of 300nm.
[0055] Example 7
[0056] A method for preparing a full high entropy perovskite solar cell, the steps are the same as those in Example 1, except that in S5, TiCl4, ZnCl2, SiCl4, CrCl3, and FeCl3 are prepared in an equal molar ratio by a hydrothermal method to obtain a 0.2 mol·L -1 30ml of aqueous solution was added and transferred into a sealed container. Under magnetic stirring, concentrated ammonia solution was slowly added until the pH value was 7. The reaction solution was transferred into a 50ml hydrothermal reactor and placed in a 90° drying oven for three hours. After the reaction, the precipitate was washed with deionized water for more than three times to obtain Ti 0.2 Zn0.2 Si 0.2 Cr 0.2 Fe 0.2 O x Nanocrystals. Ti was obtained after dispersion in isopropanol solvent. 0.2 Zn 0.2 Al 0.2 Sn 0.2 Fe 0.2 O x The precursor solution was then spin-coated at 3000 rpm / s for 30 s and thermally annealed at 150 °C for 30 min to obtain a uniform Ti 0.2 Zn 0.2 Si 0.2 Cr 0.2 Fe 0.2 O x The electron transport layer has a film thickness of 30 nm.
[0057] The high entropy perovskite film prepared in Example 1 is flat, has uniform grain size, high film density, and few holes. Figure 1 As shown by scanning electron microscopy.
[0058] The open circuit voltage of a fully high entropy perovskite solar cell prepared in Example 1 is 1.14V and the short circuit current density is 25.01mA / cm 2 , the filling factor is 75.21%, and the photoelectric conversion efficiency reaches 21.48%. Figure 2 shown.
[0059] The above embodiments are only examples for clear explanation and do not limit the implementation method, that is, the present invention is not dependent on the above embodiments to be implemented. Any modification, equivalent replacement and improvement made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A full high entropy perovskite solar cell, characterized in that: The perovskite solar cell includes, from bottom to top, a conductive glass substrate, a high entropy metal oxide hole transport layer, a high entropy 3D perovskite light absorption layer, a high entropy 2D perovskite modification layer, a high entropy metal oxide electron transport layer and a metal electrode layer.
2. A full high entropy perovskite solar cell according to claim 1, characterized in that: The high entropy metal oxide hole transport layer is composed of a high entropy metal oxide material containing five or more metal elements, and the metal elements include Ni, Cu, Mo, V, W, Fe, Co, Li, Mg, Ga, Cr, In, and Sc.
3. The full high entropy perovskite solar cell according to claim 1, characterized in that: The high entropy 3D perovskite light absorbing layer adopts a high entropy perovskite material containing five or more A-site and B-site cations, wherein the A-site cation has MA + , FA + , Cs + , Rb + , K + , Li + 、Na + , Sr + 、Be + Mg + , Ca + , Ba + , Ra + ,La + , Pr + 、Nd + 、Sm + and Mn + , the B-site cation is Pb + Sn + Mg + , Ca + Sc + 、Ti + 、V + , Fe + 、Co + 、Ni + , Cu + 、Zn + , Ga + 、Al + , Nb + 、Mo + 、Ru + , W + , Ir + , Pt + 、Bi + and Ce + , the anions at the X position are F, Cl, Br, and I.
4. The all-high-entropy perovskite solar cell according to claim 1, characterized in that: The high entropy 2D perovskite modification layer adopts a high entropy perovskite material containing five or more A-position organic cations, wherein the A-position organic cations include OA + 、PEA + , B.A. + , BDA + 、BEA + 、CMA + , DAT + , GA + , HA + ,PA + , PDA + PEI + 、PeDA + 、PMA + POPA + ThMA + , BdA + , HaD + , OdA + .
5. The full high entropy perovskite solar cell according to claim 1, characterized in that: The high entropy metal oxide electron transport layer adopts a high entropy metal oxide material containing five or more metal elements, and the metal elements include Sn, Ti, Zn, Al, Zr, Si, W, Nb, Ce, Sr, Fe, Cr, and Ba.
6. The full high entropy perovskite solar cell according to claim 1, characterized in that: The metal electrode layer is one or more of Au, Ag, Cu, Al, and Mg.
7. The full high entropy perovskite solar cell according to claim 1, characterized in that: The thickness of the high entropy metal oxide hole transport layer is 20-70nm, the thickness of the high entropy 3D perovskite light absorption layer is 300-900nm, the thickness of the high entropy 2D perovskite modification layer is 100-700nm, the thickness of the high entropy metal oxide electron transport layer is 20-70nm, and the thickness of the metal electrode layer is 100-300nm.
8. A method for preparing the full high entropy perovskite solar cell as claimed in claim 1, characterized in that: The steps include: 1) cleaning the conductive glass substrate, and then drying the conductive glass substrate in a vacuum drying oven for later use; 2) preparing a high entropy metal oxide hole transport layer nanocrystalline material by a hydrothermal method, preparing the obtained nanocrystalline material into a precursor solution, and spin-coating it on a conductive glass substrate, and annealing it at 180° C. to form a high entropy metal oxide hole transport layer; 3) A high-entropy 3D perovskite light-absorbing layer was prepared on the high-entropy metal oxide hole transport layer by a two-step spin coating method; 4) Spin-coating a solution containing five or more organic cation precursors on the high entropy 3D perovskite light-absorbing layer by a dynamic spin coating method to prepare a high entropy 2D perovskite modified layer; 5) preparing a high entropy metal oxide electron transport layer nanocrystalline material by a hydrothermal method, preparing the obtained nanocrystalline material into a precursor solution, and spin-coating it on the high entropy 2D perovskite modified layer, and annealing at 150° C. to form a high entropy metal oxide electron transport layer; 6) Preparing a metal electrode layer on the high entropy metal oxide electron transport layer to obtain the full high entropy perovskite solar cell.
9. The method for preparing a full high entropy perovskite solar cell according to claim 8, characterized in that: In step 2), the high entropy metal oxide hole transport layer material is synthesized by a hydrothermal method. The specific preparation method is: five or more chlorides composed of Ni, Cu, Mo, V, W, Fe, Co, Li, Mg, Ga, Cr, In, and Sc metal elements are configured into an aqueous solution, and under magnetic stirring, concentrated ammonia stock solution is slowly added dropwise to a pH value of 7, the reaction solution is transferred into a hydrothermal reactor, placed in a 90° C. drying oven for three hours, and the precipitate is washed with deionized water for more than three times to obtain a high entropy metal oxide hole transport layer nanocrystalline material, and a high entropy metal oxide nanocrystal precursor solution is obtained by a water dispersion method; In step 3), the high entropy 3D perovskite light-absorbing layer is prepared by a two-step spin coating method. The specific preparation method is: adding a metal halide to a mixed solvent of DMF and DMSO to obtain a 1-1.8 mM first part precursor solution, spin coating it on the high entropy metal oxide hole transport layer, annealing to obtain a metal halide film, spin coating 0.1-0.8 mM A-site cation precursor solution on the metal halide film, and annealing to obtain a high entropy 3D perovskite light-absorbing layer containing five or more A-site and B-site cations; In step 4), the high entropy 2D perovskite modification layer is prepared by a dynamic spin coating method, and the specific preparation method is: dynamically spin coating a solution containing 0.01 to 0.5 mM of five or more organic cation halide precursors on the high entropy 3D perovskite light absorbing layer, and annealing at 90° C. to obtain a high entropy 2D perovskite modification layer; In step 5), the high entropy metal oxide electron transport layer material is synthesized by a hydrothermal method. The specific preparation method is: five or more chlorides composed of Sn, Ti, Zn, Al, Zr, Si, W, Nb, Ce, Sr, Fe, Cr, and Ba metal elements are configured into an aqueous solution, and under magnetic stirring, concentrated ammonia stock solution is slowly added dropwise to a pH value of 7, the reaction solution is transferred into a hydrothermal reactor, placed in a 90°C drying oven for three hours, and the precipitate is washed with deionized water for more than three times to obtain a high entropy metal oxide electron transport layer nanocrystalline material, and a high entropy metal oxide nanocrystal precursor solution is obtained after dispersion with an isopropanol solvent.
Citation Information
Cited By
High-entropy perovskite relaxor ferroelectric ceramic with ultra-wide-temperature energy storage temperature stability and near-zero hysteresis as well as preparation method and application of high-entropy perovskite relaxor ferroelectric ceramic
CN119977555A