Application of amino acid material, perovskite solar cell and preparation method thereof

By modifying the perovskite absorption layer with a variety of amino acid materials, the crystal defects and stability problems in perovskite solar cells are solved, the photoelectric conversion efficiency and environmental stability are improved, and more efficient and stable perovskite solar energy is achieved. Battery performance.

CN118890911APending Publication Date: 2024-11-01SOLARSPACE NEW ENERGY (CHUZHOU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410958738.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

钙钛矿太阳能电池在生长过程中存在晶体缺陷,导致效率和稳定性降低,且现有氨基酸材料官能团种类和数量有限,影响器件的重复性和环境稳定性。

Method used

The perovskite absorption layer is modified by amino acid materials containing Fmoc protective groups and a variety of different types of amino acids. By introducing amino (-NH2) and carboxyl (-COOH) functional groups, a dense passivation layer is formed to improve the perovskite material. stability and photoelectric conversion efficiency.

Benefits of technology

It significantly improves the photoelectric conversion efficiency and stability of perovskite solar cells, increases the grain size of perovskite crystals, reduces the defect state density and interface contact resistance, and improves the environmental stability and repeatability of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118890911A_ABST
    Figure CN118890911A_ABST
Patent Text Reader

Abstract

The invention discloses amino acid material modified perovskite, a perovskite solar cell and a preparation method. The invention relates to an amino acid material, the amino acid material comprises an Fmoc protecting group and two or more different types of amino acids, the general formula of the amino acid material is Fmoc-ABCD...-end group, the end group comprises-NH2 or-COOH, and the Fmoc-ABCD... comprises any one of Fmoc-Gly-OH, Fmoc-HM-OH, Fmoc-HVM-OH and Fmoc-LMH-OH. According to the invention, the amino acid material containing various functional groups is used for passivating the defects of the perovskite interface, the defect state density of the surface of the perovskite material is reduced, non-radiative recombination is inhibited, the photoelectric conversion efficiency is improved, and the efficiency of the perovskite cell is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of perovskite solar cells, and specifically relates to the application of an amino acid material to modify a perovskite absorption layer, a perovskite solar cell and a preparation method thereof. Background Art

[0002] As the global demand for renewable energy grows, solar energy has attracted widespread attention as a clean and sustainable form of energy. Among many photovoltaic devices, perovskite solar cells have attracted much attention for their unique photoelectric conversion properties. Perovskite materials have excellent light absorption properties and high photoelectric conversion efficiency, which makes perovskite solar cells have broad application prospects in the photovoltaic field.

[0003] Organic-inorganic hybrid halide perovskite materials have excellent properties, but the growth of perovskite crystals inevitably causes harmful crystal defects inside, at grain boundaries and on the surface, which ultimately leads to a decrease in the efficiency and stability of perovskite solar cells. Among these methods, surface passivation is considered to be the most commonly used and effective method.

[0004] As a natural organic compound, amino acids have rich functional groups and excellent biocompatibility. In perovskite solar cells, amino acids can chemically bond with the surface of perovskite materials through their specific functional groups to form a dense passivation layer. This passivation layer can not only reduce the defect state density on the surface of perovskite materials, inhibit non-radiative recombination, and improve the photoelectric conversion efficiency, but also enhance the stability of perovskite materials and resist the erosion of environmental factors.

[0005] Therefore, existing perovskite solar cells have the following problems;

[0006] 1) The stability of perovskite materials is a major challenge. Since perovskite materials are sensitive to environmental factors such as humidity, temperature and light, their performance can easily deteriorate, thus affecting the long-term stable operation of solar cells.

[0007] 2) The types and quantities of functional groups contained in a single amino acid are limited, and the device as a whole exhibits low repeatability and high deviation.

[0008] 3) Without packaging, the environmental stability is low.

[0009] Therefore, using amino acid materials containing multiple functional groups to passivate the defects of the perovskite interface can greatly improve the efficiency of perovskite cells. Summary of the invention

[0010] The purpose of the present invention is to provide an application of an amino acid material, a perovskite solar cell and a preparation method thereof. The present invention provides an amino acid material passivated perovskite absorption layer, which can further improve the efficiency and stability of the solar cell.

[0011] Embodiments of the present invention provide amino acid material modified perovskite, perovskite solar cell and preparation method, an amino acid material modified perovskite, characterized in that the amino acid material comprises an Fmoc protecting group and two or more different types of amino acids, the general formula of the amino acid material is Fmoc-ABCD...-end group, and the end group comprises an amino group (-NH2) or a carboxyl group (-COOH).

[0012] In one or more embodiments of the present invention, the Fmoc-ABCD... includes any one of Fmoc-Gly-OH, Fmoc-HM-OH, Fmoc-HVM-OH and Fmoc-LMH-OH.

[0013] A perovskite solar cell comprises a light-absorbing layer of the amino acid material modified perovskite according to claim 1, wherein the perovskite solar cell is an inverted structure perovskite solar cell.

[0014] In one or more embodiments of the present invention, the inverted structure perovskite solar cell comprises a conductive substrate, a hole transport layer, a perovskite light absorbing layer, an electron transport layer and a metal electrode stacked in sequence from bottom to top, characterized in that the perovskite light absorbing layer comprises a perovskite material and an amino acid;

[0015] The chemical composition of the perovskite material is ABX3, wherein A is CH3NH3 + 、NH2CHNH2 + 、C(NH2)3 + , Cs + , Li + 、Na + , K + , Rb + or at least one of organic amine cations having a carbon number of not less than 3; B is Pb 2+ , Cu 2+ Sn 2+ , Mn 2+ 、Zn 2 + 、Cd 2+ ,Ge 2+ , Sr 2+ 、Bi 3+ 、Eu 2+ , Yb 2+ , Sb 3+ , Tl 3+ 、In3+ , Cu + 、Ag + , Pd 2+ , Pd 4+ At least one of; X is Cl - ,Br - , I - , SCN - At least one of .

[0016] The amino acid is any one of claim 2.

[0017] A method for preparing a perovskite solar cell, wherein the inverted structure perovskite solar cell comprises the following steps:

[0018] S1. Prepare a substrate; etch and clean the conductive glass, blow dry it with an air gun, and then treat its surface with ultraviolet ozone to obtain a substrate;

[0019] S2. Preparation of a nickel oxide hole transport layer: preparing a nickel oxide solution, using a coating machine to spin coat and using a pipette to absorb the nickel oxide solution and drop it on the substrate, and annealing;

[0020] S3, preparing a perovskite light-absorbing layer; preparing a perovskite precursor solution, and after the preparation is completed, using a sizing machine to drop the perovskite precursor solution on the hole transport layer by spin coating, and then drop ethyl acetate dissolved in amino acids of different concentrations, and after the spin coating is completed, the conductive glass is placed on a hot stage for heating to obtain a perovskite film;

[0021] S4, preparing an electron transport layer: dissolving a fullerene derivative in chlorobenzene and stirring, using a sizing machine to spin-coat a layer of the chlorobenzene solution of the fullerene derivative on the perovskite light-absorbing layer, and then spin-coating a layer of BCP by spin coating;

[0022] S5. Prepare a metal electrode layer: use a vacuum coating apparatus to evaporate Ag or Au on the electron transport layer.

[0023] In one or more embodiments of the present invention, the substrate is FTO or ITO.

[0024] In one or more embodiments of the present invention, the preparation method of the perovskite precursor solution in S3 is to dissolve FAI, MABr, PbBr2 and PbI2 in 1 mL of a mixed solvent composed of DMSO and DMF in a volume ratio of 1:4, and stir, add 84 uL of CsI solution, stir and filter for later use.

[0025] In one or more embodiments of the present invention, the mass of the FAI is 0.1719 g, the mass of the MABr is 0.0734 g, the mass of the PbBr2 is 0.0734 g, and the mass of the PbI2 is 0.5071 g.

[0026] The invention provides an application of an amino acid in a perovskite layer of a perovskite solar cell. The amino acid comprises one of Fmoc-Gly-OH, Fmoc-HM-OH, Fmoc-HVM-OH and Fmoc-LMH-OH. An amino acid material having two functional groups, an amino group (-NH2) and a carboxyl group (-COOH), is introduced to passivate defects at the perovskite interface to improve the efficiency and stability of the device, and has a great influence on the crystal structure of the perovskite, wherein large-sized grains of the perovskite are significantly increased, defect state density and interface contact resistance are reduced, and the device has good environmental stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 is the XRD diagram of amino acid perovskite films with different concentrations prepared based on Example 1 and Example 2;

[0028] Figure 2 are scanning electron microscope images b and c of the perovskite thin films prepared in Example 1 and Example 2 and a cross section of the perovskite solar cell in Example 2;

[0029] Figure 3 Figure a is the absorption spectrum and figure b of the steady-state fluorescence spectrum of the perovskite film with different concentrations of amino acids prepared in Example 1 and Example 2;

[0030] Figure 4 is a JV curve diagram of the perovskite solar cells passivated with amino acids of different concentrations prepared in Example 1 and Example 2;

[0031] Figure 5 The molecular structure of Fmoc-Gly-OH is a and the structure of the trans-perovskite solar cell is b;

[0032] Figure 6 It is a process flow chart of the preparation of amino acid modified perovskite film;

[0033] Figure 7 This is a statistical chart of the performance parameters of perovskite solar cells modified with amino acids at different concentrations. DETAILED DESCRIPTION

[0034] The specific implementation modes of the present invention are described in detail below in conjunction with the accompanying drawings, but it should be understood that the protection scope of the present invention is not limited by the specific implementation modes.

[0035] Unless explicitly stated otherwise, throughout the specification and claims, the term “comprise” or variations such as “include” or “comprising”, etc., will be understood to include the stated elements or components but not to exclude other elements or components.

[0036] Embodiment 1;

[0037] A method for preparing a perovskite solar cell without amino acid modification comprises the following steps:

[0038] S1. Prepare the substrate; use FTO as the substrate and prepare the perovskite solar cell on the conductive glass.

[0039] S11. Cut the conductive glass into squares of 19*19mm. Make sure there are no scratches on the conductive surface, and mark and record the non-conductive surface.

[0040] S12. Place the cut glass pieces into a glass cleaning rack and then use ultrasonic cleaning for five times, using deionized water with detergent, deionized water, 95% anhydrous ethanol, isopropanol, and 99% ethanol as cleaning agents, respectively, for half an hour each time.

[0041] S13. Blow dry with an air gun.

[0042] S2. Prepare a nickel oxide hole transport layer on the substrate.

[0043] S21. Prepare a nickel oxide solution.

[0044] Dissolve 0.727 g Ni(NO3)2·6H2O in 5 mL ethylene glycol solution, then add 0.15 g ethylenediamine and stir with a magnetic stirrer until dissolved to obtain NiO x The precursor solution is filtered and set aside. The cleaned glass is blown dry with an air gun, placed on a gel-spinning machine, and the dust on the surface is blown off with an ear-cleaning bulb; then 65 μL of the previously filtered precursor solution is measured with a pipette and dripped onto the FTO.

[0045] S22. Place the finished conductive glass on a hot plate, dry it at 120°C for 10 minutes, and then transfer it to a hot plate at 300°C for annealing for 1 hour.

[0046] S3. Prepare a perovskite light-absorbing layer.

[0047] S31. Prepare a perovskite precursor solution.

[0048] 0.0734g MABr, 0.1719g FAI, 0.5071g PbI2, and 0.0734g PbBr2 were dissolved in 1mL of a mixed solvent consisting of DMSO and DMF in a volume ratio of 1:4. After stirring at room temperature for one hour, 84μL of CsI dissolved in DMSO was added, and the concentration was 1.5mol / L. The perovskite chemical formula was Cs 0.1 (MA 0.12 FA 0.88 ) 0.9 Pb(I 0.95 Br 0.05 )3. Stir and filter for later use.

[0049] S32. After the configuration is completed, a coating machine is used to drop the perovskite precursor solution onto the hole transport layer by spin coating, wherein the coating machine is set to rotate at 1000 rpm and the duration is 10 s.

[0050] S33. After the addition is completed, 200 μL of ethyl acetate is added dropwise by spin coating using a gel spreader, wherein the speed of the gel spreader is set to 4000 rpm and the duration is 30 s.

[0051] S34. After the spin coating is completed, place the conductive glass on a hot stage and set the hot stage temperature to 70°C for 3 minutes.

[0052] S35, then set the temperature of the hot stage to 100°C and the duration is 10 minutes.

[0053] S4. preparing an electron transport layer.

[0054] S41. Dissolve 45 μL of filtered 25 mg / mL PCBM in chlorobenzene.

[0055] S42. Drop onto the cooled perovskite layer and rotate at 3000r for 30s.

[0056] S43, take 0.5mg / mL BCP solution dissolved in ethanol, add 45μL dropwise onto the electron transport layer, rotate at 3000r for 30s in the same way. Then use γ-butyrolactone to wipe off 5mm of the prepared functional layer on both sides of the battery until the FTO is exposed.

[0057] S5. Prepare the electrode layer. Place the sample on the template in the vacuum coating machine, increase the current to melt the silver block after vacuuming, and start evaporating silver after the silver block is completely melted. Increase every 15-20 seconds Then increase every 8-12 seconds Until

[0058] The substrate may be FTO or ITO.

[0059] Embodiment 2:

[0060] A method for preparing a perovskite solar cell having a perovskite absorption layer modified with amino acids of different concentrations comprises the following steps:

[0061] S1. Prepare the substrate; use FTO as the substrate and prepare the perovskite solar cell on the conductive glass.

[0062] S11. Cut the conductive glass into squares of 19*19mm. Make sure there are no scratches on the conductive surface, and mark and record the non-conductive surface.

[0063] S12. Place the cut glass pieces into a glass cleaning rack and then use ultrasonic cleaning for five times, using deionized water with detergent, deionized water, 95% anhydrous ethanol, isopropanol, and 99% ethanol as cleaning agents, respectively, for half an hour each time.

[0064] S13. Blow dry with an air gun.

[0065] S2. Prepare a nickel oxide hole transport layer on the substrate.

[0066] S21. Prepare a nickel oxide solution.

[0067] Dissolve 0.727 g Ni(NO3)2·6H2O in 5 mL ethylene glycol solution, then add 0.15 g ethylenediamine and stir with a magnetic stirrer until dissolved to obtain NiO x The precursor solution is filtered and set aside. The cleaned glass is blown dry with an air gun, placed on a gel-spinning machine, and the dust on the surface is blown off with an ear-cleaning bulb; then 65 μL of the previously filtered precursor solution is measured with a pipette and dripped onto the FTO.

[0068] S22. Place the finished conductive glass on a hot plate, dry it at 120°C for 10 minutes, and then transfer it to a hot plate at 300°C for annealing for 1 hour.

[0069] S3. Prepare a perovskite light-absorbing layer.

[0070] S31. Prepare a perovskite precursor solution.

[0071] 0.0734g MABr, 0.1719g FAI, 0.5071g PbI2, and 0.0734g PbBr2 were dissolved in 1mL of a mixed solvent consisting of DMSO and DMF in a volume ratio of 1:4. After stirring at room temperature for one hour, 84μL of CsI dissolved in DMSO was added, and the concentration was 1.5mol / L. The perovskite chemical formula was Cs 0.1 (MA 0.12FA 0.88 ) 0.9 Pb(I 0.95 Br 0.05 )3. Stir and filter for later use.

[0072] S32. After the configuration is completed, a coating machine is used to drop the perovskite precursor solution onto the hole transport layer by spin coating, wherein the coating machine is set to rotate at 1000 rpm and the duration is 10 s.

[0073] S33. After the addition is completed, 200 μL of ethyl acetate dissolved with amino acids of different concentrations is added dropwise by a gel spreader using a spin coating method, wherein the spin spreader is set to a speed of 4000 rpm and the duration is 30 s.

[0074] S34. After the spin coating is completed, place the conductive glass on a hot stage and set the hot stage temperature to 70°C for 3 minutes.

[0075] S35, then set the temperature of the hot stage to 100°C and the duration is 10 minutes.

[0076] S4. preparing an electron transport layer.

[0077] S41. Dissolve 45 μL of filtered 25 mg / mL PCBM in chlorobenzene.

[0078] S42. Drop onto the cooled perovskite layer and rotate at 3000r for 30s.

[0079] S43, take 0.5mg / mL BCP solution dissolved in ethanol, add 45μL dropwise onto the electron transport layer, rotate at 3000r for 30s in the same way. Then use γ-butyrolactone to wipe off 5mm of the prepared functional layer on both sides of the battery until the FTO is exposed.

[0080] S5. Prepare the electrode layer. Place the sample on the template in the vacuum coating machine, increase the current to melt the silver block after vacuuming, and start evaporating silver after the silver block is completely melted. Increase every 15-20 seconds Then increase every 8-12 seconds Until

[0081] Furthermore, the substrate is FTO or ITO.

[0082] Furthermore, under standard test conditions, AM1.5G, 100mW / cm 2 JV performance curve tested under lighting conditions.

[0083] Comparison of the crystal structure and morphology of the perovskite film in Example 1 and Example 2:

[0084] like Figure 1 As shown in the figure, the XRD patterns of perovskite films modified with amino acids at different concentrations. As can be seen from the figure, the diffraction peak positions of the perovskite layer fluorescent film modified with Fmoc-Gly-OH are basically consistent, and the perovskite has good crystallinity.

[0085] like Figure 2 The following are scanning electron microscope images and cross-sections of perovskite solar cells based on perovskite films without amino acid modification and amino acid modification. It can be seen that the crystal grains of the perovskite film modified with Fmoc-Gly-OH are more densely packed and flatter, and the perovskite layer has larger grains and denser packing, indicating that Fmoc-Gly-OH promotes the growth of perovskite, and larger grains indicate fewer grain boundaries, that is, fewer defects.

[0086] Comparison of the optical properties of the perovskite films in Example 1 and Example 2:

[0087] like Figure 3 As shown, the absorption spectra and steady-state fluorescence spectra of the perovskite film modified with different concentrations of amino acids. It can be seen from the figure that in the visible light range of 380-800nm, with the addition of Fmoc-Gly-OH, the light absorption of the perovskite film is also improved, and the PL intensity is constantly increasing, reflecting that the perovskite film modified with Fmoc-Gly-OH has lower defect density and reduced non-radiative recombination.

[0088] Comparison of the photoelectric performance of the perovskite cell devices in Example 1 and Example 2:

[0089] like Figure 4 The battery JV curve shown in the figure can be used to obtain the device performance parameters. The specific changes are as follows Figure 7 shown.

[0090] like Figure 7 As shown in the figure, the PCE, J SC , V OC , FF has different degrees of improvement.

[0091] In summary, a perovskite solar cell and a preparation method according to an embodiment of the present invention have the following benefits:

[0092] 1) The perovskite solar cell made of amino acid material modified perovskite absorption layer reduces the defects between interfaces and accelerates the transfer of charges, thereby significantly improving the photoelectric conversion efficiency and stability.

[0093] 2) Amino acid modification of the perovskite absorber layer has a great influence on the crystal structure of the perovskite, in which the large-size perovskite grains are significantly increased, the defect state density is reduced, and the film quality is improved.

[0094] 3) The best device based on amino acid modified perovskite absorber has an efficiency of 20.61%, an open circuit voltage of 1.16 V, and a short circuit current of 23.02 mA cm -2 , the fill factor is 79%. The device as a whole shows high repeatability and low deviation.

[0095] Although the above embodiments have been described in detail for the present invention, this is only a part of the many embodiments of the present invention, not all. Without departing from the creative core of the present invention, we can also implement the concept of the present invention in other ways and obtain more embodiments. These different implementations, no matter based on what angle or method, should be regarded as belonging to the protection scope of the present invention.

Claims

1. An amino acid material modified perovskite, characterized in that: The amino acid material comprises an Fmoc protecting group and two or more different kinds of amino acids, and the general formula of the amino acid material is Fmoc-ABCD...-terminal group, and the terminal group comprises an amino group (-NH2) or a carboxyl group (-COOH).

2. An amino acid material according to claim 1, characterized in that: The Fmoc-ABCD... includes any one of Fmoc-Gly-OH, Fmoc-HM-OH, Fmoc-HVM-OH and Fmoc-LMH-OH.

3. A perovskite solar cell, characterized in that: The invention comprises a light-absorbing layer of the amino acid material modified perovskite as claimed in claim 1, wherein the perovskite solar cell is a trans-structured perovskite solar cell.

4. The inverted perovskite solar cell according to claim 3, comprising a conductive substrate, a hole transport layer, a perovskite light absorbing layer, an electron transport layer and a metal electrode stacked in sequence from bottom to top, characterized in that: The perovskite light absorbing layer comprises a perovskite material and an amino acid; The chemical composition of the perovskite material is ABX3, wherein A is CH3NH3 + 、NH2CHNH2 + 、C(NH2)3 + , Cs + , Li + 、Na + , K + , Rb + or at least one of organic amine cations having a carbon number of not less than 3; B is Pb 2+ , Cu 2+ Sn 2+ , Mn 2+ 、Zn 2+ 、Cd 2+ ,Ge 2+ , Sr 2+ 、Bi 3+ 、Eu 2+ , Yb 2+ , Sb 3+ , Tl 3+ 、In 3+ , Cu + 、Ag + , Pd 2+ , Pd 4+ At least one of; X is Cl - ,Br - , I - , SCN - At least one of . The amino acid is any one of claim 2.

5. The method for preparing a perovskite solar cell according to claim 4, characterized in that: The inverted structure perovskite solar cell comprises the following steps: S1. Prepare a substrate; etch and clean the conductive glass, blow dry it with an air gun, and then treat its surface with ultraviolet ozone to obtain a substrate; S2. Preparation of a nickel oxide hole transport layer: preparing a nickel oxide solution, using a coating machine to spin coat and using a pipette to absorb the nickel oxide solution and drop it on the substrate, and annealing; S3, preparing a perovskite light-absorbing layer; preparing a perovskite precursor solution, and after the preparation is completed, using a sizing machine to drop the perovskite precursor solution on the hole transport layer by spin coating, and then drop ethyl acetate dissolved in amino acids of different concentrations, and after the spin coating is completed, the conductive glass is placed on a hot stage for heating to obtain a perovskite film; S4, preparing an electron transport layer: dissolving a fullerene derivative in chlorobenzene and stirring, using a sizing machine to spin-coat a layer of the chlorobenzene solution of the fullerene derivative on the perovskite light-absorbing layer, and then spin-coating a layer of BCP by spin coating; S5. Prepare a metal electrode layer: use a vacuum coating apparatus to evaporate Ag or Au on the electron transport layer.

6. The method for preparing a perovskite solar cell according to claim 5, characterized in that: The substrate is FTO or ITO.

7. The method for preparing a perovskite solar cell according to claim 5, characterized in that: The preparation method of the perovskite precursor solution in S3 is to dissolve FAI, MABr, PbBr2 and PbI2 in 1 mL of a mixed solvent consisting of DMSO and DMF in a volume ratio of 1:4, and stir, add 84 uL of CsI solution, stir, and filter for later use.

8. The method for preparing a perovskite solar cell according to claim 7, characterized in that: The mass of the FAI is 0.1719 g, the mass of the MABr is 0.0734 g, the mass of the PbBr2 is 0.0734 g, and the mass of the PbI2 is 0.5071 g.