Carbon-based perovskite solar cell based on interface passivation layer

By using dodecyl acetate as an interface passivator in perovskite solar cells, the problem of poor interface contact between the perovskite layer and the carbon electrode is solved, and the efficiency and stability of the solar cell are improved.

CN118890912APending Publication Date: 2024-11-01NINGBO INST OF NORTHWESTERN POLYTECHNICAL UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410961514.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The carbon-based perovskite solar cells have low efficiency, and there are problems such as poor interface contact between the perovskite layer and the carbon electrode, many defects in the light absorbing layer, and high non-radiation recombination rate.

Method used

Dodecyl acetate is used as an interface passivator to passivate the defects on the surface of the perovskite layer through ionic bonds and hydrogen bonds, improve the quality of the interface contact, and enhance the stability of the battery through hydrophobic dodecyl chains.

Benefits of technology

The surface defect density of the perovskite layer is reduced, the interface contact between the perovskite layer and the carbon electrode is improved, and the efficiency and stability of the solar cell is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to a carbon-based perovskite solar cell based on an interface passivation layer, and belongs to the field of perovskite solar cells, the cell structure sequentially comprises a glass substrate, an electron transport layer, a perovskite layer, a passivation layer and a carbon electrode from bottom to top, the surface passivation of the perovskite layer is carried out by using dodecyl acetate, the surface defect density of the perovskite layer is effectively reduced, and the performance of the perovskite solar cell is improved. According to the passivation agent, the interface contact condition between the perovskite layer and the carbon electrode is improved, the dodecyl chain has hydrophobicity, the stability of the carbon-based perovskite solar cell can be improved, and through experimental testing, the efficiency and repeatability of a device optimized through the passivation agent are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of perovskite solar cells, and mainly relates to a dodecyl acetate-passivated carbon-based perovskite solar cell and a preparation method thereof. Background Art

[0002] In recent years, people in various countries have accelerated the development and utilization of clean and renewable energy. Solar energy, as a renewable energy source with abundant raw materials and green environmental protection, has attracted widespread attention. As a major way to utilize solar energy, solar cells can convert light energy into electrical energy. At present, researchers have developed various types of solar cells. Among them, perovskite solar cells have become a research hotspot in recent years because of their strong photoelectric conversion ability, adjustable band gap, and simple manufacturing process. Since 2009, the efficiency of perovskite solar cells has developed from 3.8% to 26%, which can be regarded as a new hope in the photovoltaic field.

[0003] Compared with the traditional structure of perovskite solar cells, carbon-based perovskite solar cells without hole transport layer have simple process, low cost, good stability, and do not require expensive hole transport layer materials and precious metal electrodes, and have greater development potential. However, this structure also has some problems, such as poor interface contact between the perovskite layer and the carbon electrode, many defects in the light absorption layer, high non-radiative recombination rate, and low efficiency. Therefore, the development of new interface modification layers is of great significance to reduce defects and improve efficiency. Summary of the invention

[0004] In order to solve the problem of low efficiency of carbon-based perovskite solar cells, the object of the present invention is to provide a carbon-based perovskite solar cell based on an interface passivation layer.

[0005] In order to achieve the above object, the present invention is implemented in the following ways:

[0006] A carbon-based perovskite solar cell based on an interface passivation layer, characterized in that the cell structure comprises, from bottom to top, a glass substrate, an electron transport layer, a perovskite layer, a passivation layer, and a carbon electrode;

[0007] The specific steps of preparation are as follows:

[0008] S1, cleaning the glass substrate;

[0009] S2, spin coating an electron transport layer on the cleaned glass substrate;

[0010] S3. Prepare perovskite precursor solution:

[0011] Lead iodide (PbI2), methylammonium iodide (MAI), methylammonium hydroiodide (FAI), and cesium iodide (CsI) are dissolved in 1 mL of an organic solvent and stirred for 5 to 8 hours. The molar concentrations are 1.5 mol / L of lead iodide, 1.3 mol / L of methylammonium iodide, 0.15 mol / L of methylammonium hydroiodide, and 0.05 mol / L of cesium iodide. The organic solvent is a mixed solvent of dimethylformamide (DMF) and dimethyl sulfoxide (DMSO) in a volume ratio of 4:1 to 9:1.

[0012] S4, coating the perovskite precursor solution prepared in S3 uniformly on the surface of the electron transport layer by spin coating, and annealing the perovskite wet film to obtain a perovskite layer;

[0013] S5. Prepare a passivation agent solution and spin-coat a passivation layer on the surface of the perovskite layer:

[0014] Dissolve dodecylamine acetate in isopropanol and stir evenly to a concentration of 1g / L-3g / L, then evenly coat it on the perovskite layer, 1×1cm 2 40-60 μL of passivation agent solution is coated on the perovskite layer, and the coating machine is started. The spin coating speed is 4000 r / min, and the spin coating time is 30 s. After the spin coating is completed, it is heated at 100° C. for 5-10 min to obtain a passivation layer;

[0015] S6. Scrape carbon slurry on the perovskite layer and obtain a carbon electrode after annealing.

[0016] Furthermore, in step S1, the glass substrate is cleaned by ultrasonically cleaning the glass substrate for 15-20 minutes using anhydrous ethanol, daily detergent, deionized water, isopropanol and anhydrous ethanol in sequence, and then drying the glass substrate at 50-60°C for 10-15 minutes, and then treating the glass substrate with ultraviolet ozone (UV) for 10-20 minutes. Furthermore, in step S2, the electron transport layer is spin-coated by mixing a 15wt% tin dioxide aqueous dispersion and deionized water in a volume ratio of 1:4 to obtain a tin oxide solution, and then taking the tin oxide solution and coating it by spin coating on a 1×1 cm 2 45ul of tin oxide solution was spin-coated on a glass slide, and the coating machine was started. The coating speed was 4000r / min and the coating time was 30s. After the coating was completed, the electron transport layer was heated at 130-150°C for 20-30min to obtain the electron transport layer.

[0017] Furthermore, in step S4, the perovskite precursor solution is applied by filtering the stirred perovskite precursor solution with a disposable sterile syringe with a polytetrafluoroethylene organic filter membrane, and then evenly applying the solution on the electron transport layer, 1×1 cm 250 μL of perovskite precursor solution was coated on the electron transport layer, and the coating machine was started. The spin coating speed was 4000 r / min and the spin coating time was 30 s. During the high-speed rotation for 8-10 s, the anti-solvent chlorobenzene was added dropwise, and the added volume was 4 times the volume of the perovskite precursor solution.

[0018] Furthermore, in step S4, the perovskite wet film is annealed by heating at 100-120° C. for 10-15 min to obtain the perovskite layer.

[0019] Furthermore, the carbon slurry in step S6 is a commercial conductive carbon slurry, and the carbon slurry is directly scraped onto the surface of the perovskite layer using a filter, and heated at 100 to 120° C. for 15 to 20 minutes to obtain a carbon electrode. The positive effects of the present invention are:

[0020] (1) The dodecyl acetate passivated carbon-based perovskite solar cell prepared by the present invention has a simple preparation process, low cost and good stability.

[0021] (2) The present invention uses dodecyl acetate to passivate the surface of the perovskite layer. The carboxylic acid group can interact with the cations on the surface of the perovskite layer through ionic bonds to passivate the surface positive charge defects. At the same time, the amino ions can passivate the negative charge defects on the surface of the perovskite layer through ionic bonds and hydrogen bonds, thereby effectively reducing the surface defect density of the perovskite layer and improving the interface contact between the perovskite layer and the carbon electrode. The dodecyl chain is hydrophobic and can improve the stability of the carbon-based perovskite solar cell. Through experimental tests, the efficiency and repeatability of the device after passivation agent optimization are improved. Specific implementation plan

[0022] Example 1

[0023] A carbon-based perovskite solar cell based on an interface passivation layer, wherein the cell structure includes a glass substrate, an electron transport layer, a perovskite layer, a passivation layer, and a carbon electrode from bottom to top;

[0024] The specific steps of preparation are as follows:

[0025] Step S1, cleaning the glass substrate. The substrate was ultrasonically cleaned for 15 minutes using anhydrous ethanol, daily detergent, deionized water, isopropanol, and anhydrous ethanol in sequence, then dried in an oven at 60° C. for 10 minutes, and then treated with ultraviolet ozone (UV) for 10 minutes.

[0026] Step S2, spin-coating an electron transport layer on the cleaned glass substrate described in S1. Mix 250 μL of 15 wt% aqueous dispersion of tin dioxide (SnO2) with 1 mL of deionized water, stir thoroughly to obtain a tin oxide solution, and then apply the tin oxide solution on the ITO glass substrate of S1, 1×1 cm 245ul of tin oxide solution was spin-coated on a glass slide, and the coating machine was started. The coating speed was 4000r / min and the coating time was 30s. The tin dioxide electron transport layer was annealed at 150°C for 25min.

[0027] Step S3, preparing a perovskite precursor solution. 1.5 mmol lead iodide, 1.3 mmol methylammonium iodide (MAI), 0.15 mmol methylammonium hydroiodide (FAI), and 0.05 mmol cesium iodide (CsI) were dissolved in a mixed solvent of 100 μL dimethyl sulfoxide (DMSO) and 900 μL dimethylformamide (DMF) (the total amount of the mixed solvent was 1 mL) to form a perovskite precursor solution, which was fully stirred for 5 h.

[0028] Step S4: Spin-coat the perovskite precursor solution in S3 onto the electron transport layer to prepare a perovskite layer. Filter the stirred perovskite precursor solution with a disposable sterile syringe with a polytetrafluoroethylene organic filter membrane, and use a pipette to draw 50 μL of the perovskite precursor solution and apply it to a 1×1 cm 2 The film was spin-coated on a glass substrate at a speed of 4000 r / min for 30 s, 200 μL of anti-solvent chlorobenzene was dropped on the electron transport layer within 8-10 s of high-speed rotation, and then annealed at 120 ° C for 12 min to obtain the perovskite layer.

[0029] Example S5: Prepare a passivation solution and spin coat the perovskite layer. Dissolve 1 mg of dodecylamine acetate in 1 ml of isopropanol to form a passivation solution. Use a pipette to draw 40 ul of the passivation solution and coat it on a 1×1 cm 2 The perovskite layer is spin-coated at a speed of 4000 r / min for 30 seconds, and then annealed at 100° C. for 5 minutes to obtain a passivation layer. Step S6: Use a filter glass to dip a small amount of carbon slurry and directly scrape it onto the surface of the passivation layer in S5 to completely cover the passivation layer, and anneal at 100° C. for 20 minutes to obtain a carbon electrode.

[0030] Example 2-Example 7

[0031] The process parameters of the passivation layer in step S5 are shown in Table 1, and the other steps refer to Example 1.

[0032] Table 1

[0033] Passivation agent concentration Dosage of passivator Passivation layer annealing time Example 1 1mg / mL 40 5 Example 2 2mg / mL 40 5 Example 3 3mg / mL 40 5 Example 4 1mg / mL 50 5 Example 5 1mg / mL 50 10 Example 6 1mg / mL 60 5 Example 7 1mg / mL 60 10

[0034] Example 8

[0035] The preparation steps of carbon-based perovskite solar cells based on interface passivation layer are as follows:

[0036] Step S1, cleaning the glass substrate. The substrate was ultrasonically cleaned for 20 minutes using anhydrous ethanol, daily detergent, deionized water, isopropanol, and anhydrous ethanol in sequence, then dried in an oven at 50° C. for 15 minutes, and then treated with ultraviolet ozone (UV) for 15 minutes.

[0037] Step S2, spin-coating an electron transport layer on the cleaned glass substrate described in S1. Mix 250 μL of 15 wt% aqueous dispersion of tin dioxide (SnO2) with 1 mL of deionized water, stir thoroughly to obtain a tin oxide solution, and then apply the tin oxide solution on the ITO glass substrate of S1, 1×1 cm 2 45ul of tin oxide solution was spin-coated on a glass slide, and the coating machine was started. The coating speed was 4000r / min and the coating time was 30s. The tin dioxide electron transport layer was annealed at 140°C for 20min.

[0038] Step S3, preparing a perovskite precursor solution. 1.5 mmol lead iodide, 1.3 mmol methylammonium iodide (MAI), 0.15 mmol methylammonium hydroiodide (FAI), and 0.05 mmol cesium iodide (CsI) were dissolved in a mixed solvent of 200 μL dimethyl sulfoxide (DMSO) and 800 μL dimethylformamide (DMF) (the total amount of the mixed solvent was 1 mL) to form a perovskite precursor solution, which was fully stirred for 6 hours.

[0039] Step S4: Spin-coat the perovskite precursor solution in S3 onto the electron transport layer to prepare a perovskite layer. Filter the stirred perovskite precursor solution with a disposable sterile syringe with a polytetrafluoroethylene organic filter membrane, and use a pipette to draw 50 μL of the perovskite precursor solution and apply it to a 1×1 cm 2 The film was spin-coated on a glass substrate at a speed of 4000 r / min for 30 s, 200 μL of anti-solvent chlorobenzene was dropped on the electron transport layer within 8-10 s of high-speed rotation, and then annealed at 100 °C for 15 min to obtain the perovskite layer.

[0040] Example S5: Prepare a passivation solution and spin coat the perovskite layer. Dissolve 1 mg of dodecylamine acetate in 1 ml of isopropanol to form a passivation solution. Use a pipette to draw 40 ul of the passivation solution and coat it on a 1×1 cm 2 The perovskite layer is spin-coated at a speed of 4000 r / min for 30 seconds, and then annealed at 100° C. for 5 minutes to obtain a passivation layer. Step S6: Use a filter glass to dip a small amount of carbon slurry and directly scrape it onto the surface of the passivation layer in S5 to completely cover the passivation layer, and anneal at 120° C. for 15 minutes to obtain a carbon electrode.

[0041] Example 9

[0042] The preparation steps of carbon-based perovskite solar cells based on interface passivation layer are as follows:

[0043] Step S1, cleaning the glass substrate. The substrate was ultrasonically cleaned for 20 minutes using anhydrous ethanol, daily detergent, deionized water, isopropanol, and anhydrous ethanol in sequence, then dried in an oven at 50° C. for 10 minutes, and then treated with ultraviolet ozone (UV) for 20 minutes.

[0044] Step S2, spin-coating an electron transport layer on the cleaned glass substrate described in S1. Mix 250 μL of 15 wt% aqueous dispersion of tin dioxide (SnO2) with 1 mL of deionized water, stir thoroughly to obtain a tin oxide solution, and then apply the tin oxide solution on the ITO glass substrate of S1, 1×1 cm 2 45ul of tin oxide solution was spin-coated on a glass slide, and the coating machine was started. The coating speed was 4000r / min and the coating time was 30s. The tin dioxide electron transport layer was annealed at 130°C for 30min.

[0045] Step S3, preparing a perovskite precursor solution. 1.5 mmol lead iodide, 1.3 mmol methylammonium iodide (MAI), 0.15 mmol methylammonium hydroiodide (FAI), and 0.05 mmol cesium iodide (CsI) were dissolved in a mixed solvent of 300 μL dimethyl sulfoxide (DMSO) and 700 μL dimethylformamide (DMF) (the total amount of the mixed solvent was 1 mL) to form a perovskite precursor solution, which was fully stirred for 8 h.

[0046] Step S4: Spin-coat the perovskite precursor solution in S3 onto the electron transport layer to prepare a perovskite layer. Filter the stirred perovskite precursor solution with a disposable sterile syringe with a polytetrafluoroethylene organic filter membrane, and use a pipette to draw 50 μL of the perovskite precursor solution and apply it to a 1×1 cm 2 The film was spin-coated on a glass substrate at a speed of 4000 r / min for 30 s, 200 μL of anti-solvent chlorobenzene was dropped on the electron transport layer within 8-10 s of high-speed rotation, and then annealed at 120 ° C for 10 min to obtain the perovskite layer.

[0047] Example S5: Prepare a passivation solution and spin coat the perovskite layer. Dissolve 1 mg of dodecylamine acetate in 1 ml of isopropanol to form a passivation solution. Use a pipette to draw 40 ul of the passivation solution and coat it on a 1×1 cm 2 The perovskite layer is spin-coated at a speed of 4000 r / min for 30 seconds, and then annealed at 100° C. for 5 minutes to obtain a passivation layer. Step S6: Use a filter glass to dip a small amount of carbon slurry and directly scrape it onto the surface of the passivation layer in S5 to completely cover the passivation layer, and anneal at 100° C. for 15 minutes to obtain a carbon electrode.

[0048] Example 10

[0049] The preparation steps of carbon-based perovskite solar cells based on interface passivation layer are as follows:

[0050] Step S1, cleaning the glass substrate. The substrate was ultrasonically cleaned for 20 minutes using anhydrous ethanol, daily detergent, deionized water, isopropanol, and anhydrous ethanol in sequence, then dried in an oven at 60° C. for 15 minutes, and then treated with ultraviolet ozone (UV) for 20 minutes.

[0051] Step S2, spin-coating an electron transport layer on the cleaned glass substrate described in S1. Mix 250 μL of 15 wt% aqueous dispersion of tin dioxide (SnO2) with 1 mL of deionized water, stir thoroughly to obtain a tin oxide solution, and then apply the tin oxide solution on the ITO glass substrate of S1, 1×1 cm 2 45ul of tin oxide solution was spin-coated on a glass slide, and the coating machine was started. The coating speed was 4000r / min and the coating time was 30s. The tin dioxide electron transport layer was annealed at 150°C for 25min.

[0052] Step S3, preparing a perovskite precursor solution. 1.5 mmol lead iodide, 1.3 mmol methylammonium iodide (MAI), 0.15 mmol methylammonium hydroiodide (FAI), and 0.05 mmol cesium iodide (CsI) were dissolved in a mixed solvent of 400 μL dimethyl sulfoxide (DMSO) and 600 μL dimethylformamide (DMF) (the total amount of the mixed solvent was 1 mL) to form a perovskite precursor solution, which was fully stirred for 6 hours.

[0053] Step S4: Spin-coat the perovskite precursor solution in S3 onto the electron transport layer to prepare a perovskite layer. Filter the stirred perovskite precursor solution with a disposable sterile syringe with a polytetrafluoroethylene organic filter membrane, and use a pipette to draw 50 μL of the perovskite precursor solution and apply it to a 1×1 cm 2 The film was spin-coated on a glass substrate at a speed of 4000 r / min for 30 s, 200 μL of anti-solvent chlorobenzene was dropped on the electron transport layer within 8-10 s of high-speed rotation, and then annealed at 110 °C for 15 min to obtain the perovskite layer.

[0054] Example S5: Prepare a passivation solution and spin coat the perovskite layer. Dissolve 1 mg of dodecylamine acetate in 1 ml of isopropanol to form a passivation solution. Use a pipette to draw 40 ul of the passivation solution and coat it on a 1×1 cm 2The perovskite layer is spin-coated at a speed of 4000 r / min for 30 seconds, and then annealed at 100° C. for 5 minutes to obtain a passivation layer. Step S6: Use a filter glass to dip a small amount of carbon slurry and directly scrape it onto the surface of the passivation layer in S5 to completely cover the passivation layer, and anneal at 110° C. for 20 minutes to obtain a carbon electrode.

[0055] Comparative Example

[0056] Carbon-based perovskite solar cells, the cell structure includes a glass substrate, an electron transport layer, a perovskite layer, and a carbon electrode from bottom to top;

[0057] The specific preparation steps, steps S1-S4 are the same as in Example 1.

[0058] Step S5: Use a filter to dip a small amount of carbon slurry and directly scrape it onto the surface of the perovskite layer of S4 to completely cover the perovskite layer, and anneal it at 100° C. for 20 minutes to obtain a carbon electrode.

[0059] The performance of the prepared carbon-based perovskite solar cells is shown in Table 2.

[0060] Table 2

[0061]

[0062] As shown in Table 2, by comparing the data of Examples 1-3 and the comparative example, it can be found that after the surface of the perovskite layer is passivated with dodecylamine acetate, the open circuit voltage and fill factor of the device are significantly improved, indicating that the passivator reduces the defect density on the surface of the perovskite film, improves the interface contact between the perovskite layer and the carbon electrode, reduces the recombination of carriers, improves the transport capacity of carriers, and improves the efficiency and stability of the solar cell. By comparing the data of the embodiments, the passivator concentration and process parameters used in Example 1 are optimal.

Claims

1. A carbon-based perovskite solar cell based on an interface passivation layer, characterized in that: The battery structure includes glass substrate, electron transport layer, perovskite layer, passivation layer, and carbon electrode from bottom to top; The specific steps of preparation are as follows: S1, cleaning the glass substrate; S2, spin coating an electron transport layer on the cleaned glass substrate; S3. Prepare perovskite precursor solution: Lead iodide (PbI2), methylammonium iodide (MAI), methylammonium hydroiodide (FAI), and cesium iodide (CsI) are dissolved in 1 mL of an organic solvent and stirred for 5 to 8 hours. The molar concentrations are 1.5 mol / L of lead iodide, 1.3 mol / L of methylammonium iodide, 0.15 mol / L of methylammonium hydroiodide, and 0.05 mol / L of cesium iodide. The organic solvent is a mixed solvent of dimethylformamide (DMF) and dimethyl sulfoxide (DMSO) in a volume ratio of 4:1 to 9:

1. S4, coating the perovskite precursor solution prepared in S3 uniformly on the surface of the electron transport layer by spin coating, and annealing the perovskite wet film to obtain a perovskite layer; S5. Prepare a passivation agent solution and spin-coat a passivation layer on the surface of the perovskite layer: Dissolve dodecylamine acetate in isopropanol and stir evenly to a concentration of 1g / L-3g / L, then evenly coat it on the perovskite layer, 1×1cm 2 40-60 μL of passivation agent solution is coated on the perovskite layer, and the coating machine is started. The spin coating speed is 4000 r / min, and the spin coating time is 30 s. After the spin coating is completed, it is heated at 100° C. for 5-10 min to obtain a passivation layer; S6. Scrape carbon slurry on the perovskite layer and obtain a carbon electrode after annealing.

2. A carbon-based perovskite solar cell based on an interface passivation layer according to claim 1, characterized in that Step S1 is to clean the glass substrate by ultrasonically cleaning the glass substrate using anhydrous ethanol, daily detergent, deionized water, isopropyl alcohol and anhydrous ethanol for 15-20 minutes respectively, then drying it at 50-60° C. for 10-15 minutes, and continuing to use ultraviolet ozone (UV) treatment for 10-20 minutes.

3. A carbon-based perovskite solar cell based on an interface passivation layer according to claim 1, characterized in that Step S2 spin-coating the electron transport layer is to mix 15 wt% tin dioxide aqueous dispersion and deionized water in a volume ratio of 1:4 to obtain a tin oxide solution, and then take the tin oxide solution and apply it by spin coating on a 1×1 cm 2 45ul of tin oxide solution was spin-coated on a glass slide, and the coating machine was started. The coating speed was 4000r / min and the coating time was 30s. After the coating was completed, the electron transport layer was heated at 130~150℃ for 20~30min to obtain the electron transport layer.

4. A carbon-based perovskite solar cell based on an interface passivation layer according to claim 1, characterized in that Step S4 is to apply the perovskite precursor solution, which is stirred evenly, and then filter the perovskite precursor solution with a disposable sterile syringe with a polytetrafluoroethylene organic filter membrane, and then evenly apply it on the electron transport layer, 1×1 cm 2 50 μL of perovskite precursor solution was coated on the electron transport layer, and the coating machine was started. The spin coating speed was 4000 r / min and the spin coating time was 30 s. During the high-speed rotation for 8-10 s, the anti-solvent chlorobenzene was added dropwise, and the added volume was 4 times the volume of the perovskite precursor solution.

5. A carbon-based perovskite solar cell based on an interface passivation layer according to claim 1, characterized in that In step S4, the perovskite wet film is annealed by heating at 100-120° C. for 10-15 minutes to obtain a perovskite layer.

6. A carbon-based perovskite solar cell based on an interface passivation layer according to claim 1, characterized in that The carbon paste in step S6 is a commercial conductive carbon paste. The carbon paste is directly scraped onto the surface of the perovskite layer using a filter, and heated at 100-120° C. for 15-20 min to obtain a carbon electrode.

Citation Information

Cited By

  • Method for preparing high-efficiency carbon-based hole-free perovskite solar cell

    CN119816168A