Preparation method of carbon-based hole-transport-layer-free perovskite solar cell
By adopting carbon-based hole-free transport layer and low-temperature preparation methods in perovskite solar cells, the high cost and complex process problems of hole-transport layer and metal electrode materials in perovskite solar cells are solved, and low cost and high quality are achieved Preparation of perovskite solar cells with efficiency and high performance.
Patent Information
- Application Number
- CN202410961566.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-18
AI Technical Summary
The high cost and complex processes of hole transport layers and metal electrode materials in conventional perovskite solar cells are difficult to ensure the stability of the device, hindering its commercial development.
Using the preparation method of carbon-based hole-free transport layer, electron transport layer, perovskite layer and carbon electrode are deposited on the glass substrate by spin coating, and the additives such as 1,3-propylene diamine hydrochloride and cesium iodide are optimized. Perovskite precursor solution reduces defect density and improves crystallinity. Instead of metal materials, carbon materials are used as electrodes, and the whole process is carried out at low temperatures.
It reduces production costs, simplifies process flow, improves device stability and performance, and realizes the preparation of low-cost and high-efficiency perovskite solar cells.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of perovskite solar cells, and mainly relates to a preparation method and application of a carbon-based perovskite solar cell with low cost and high efficiency. Background Art
[0002] Solar cells use the photovoltaic effect to convert light energy into electrical energy. It is an efficient energy utilization technology. Various types of photovoltaic devices have been developed. Among them, perovskite solar cells have become the focus of research due to their superior photoelectric conversion ability, adjustable band gap, abundant raw materials, and simple preparation process. In just over a decade, the photoelectric performance has increased rapidly, and its photoelectric conversion efficiency has increased from 3.8% to the current 26.1%. The rapid development of perovskite solar cells shows great development potential and commercial prospects. However, the hole transport layer and back electrode used in conventional perovskite structures are not only expensive, but also complex in deposition process, and prone to ion migration, making it difficult to ensure the stability of the device, which hinders its further commercial development. Summary of the invention
[0003] The purpose of the present invention is to provide a method for preparing a carbon-based perovskite solar cell without a hole transport layer, so as to solve the cost and process problems caused by hole transport layer materials and metal electrode materials, and to prepare a perovskite solar cell with excellent efficiency, good stability and low cost.
[0004] To achieve the above object, the present invention is implemented as follows:
[0005] A method for preparing a carbon-based perovskite solar cell without a hole transport layer, characterized in that:
[0006] From bottom to top, the perovskite solar cell includes a glass substrate, an electron transport layer, a perovskite layer, and a carbon electrode. The specific steps of preparation are as follows:
[0007] S1 cleans the glass substrate;
[0008] S2 deposits an electron transport layer on the cleaned glass substrate by spin coating;
[0009] S3 prepares perovskite precursor solution:
[0010] Lead iodide, methylammonium iodide (MAI), methylammonium hydroiodide (FAI), cesium iodide and 1,3-propylenediamine hydrochloride (PDADCl) are dissolved in an organic solvent and stirred for 5 to 8 hours, wherein the molar concentrations are 1 to 1.5 mol / L of lead iodide, 0.8 to 1.3 mol / L of methylammonium iodide, 0.1 to 0.3 mol / L of methylammonium hydroiodide, 0.02 to 0.1 mol / L of cesium iodide, and 0.01 to 0.03 mol / L of 1,3-propylenediamine hydrochloride; the organic solvent is a mixed solvent of dimethylformamide (DMF) and dimethyl sulfoxide (DMSO) in a volume ratio of 4:1 to 9:1;
[0011] S4: uniformly coating the perovskite precursor solution prepared in S3 on the surface of the electron transport layer by spin coating, and annealing the perovskite wet film to obtain a perovskite layer;
[0012] S5: coating the carbon slurry on the perovskite layer by scraping, and obtaining the carbon electrode after annealing.
[0013] Furthermore, the cleaning described in step S1 refers to ultrasonically cleaning the glass substrate using ethanol, daily detergent, deionized water, isopropanol and ethanol in sequence for 10 to 20 minutes, then drying it at 50 to 70° C. for 10 to 15 minutes, and continuing to use ultraviolet ozone (UV) treatment for 10 to 20 minutes.
[0014] Furthermore, the depositing of the electron transport layer in step S2 refers to mixing a 15-17 wt% tin dioxide aqueous dispersion and deionized water in a volume ratio of 1:5 to obtain a tin oxide solution, and then taking the tin oxide solution and evenly coating it on a glass substrate, 1×1 cm 2 40-60 μL of tin oxide solution was coated on a glass substrate, and a coating machine was started. The spin coating speed was 4000 r / min and the spin coating time was 30 s. After the spin coating was completed, the electron transport layer was heated at 130-150° C. for 20-30 min to obtain a electron transport layer.
[0015] Furthermore, the coating of the perovskite precursor solution in step S4 refers to: filtering the stirred perovskite precursor solution with a disposable sterile syringe with a polytetrafluoroethylene organic filter membrane, and then coating it evenly on the electron transport layer, 1×1 cm 2 50 μL of perovskite precursor solution was coated on the electron transport layer, and the coating machine was started. The spin coating speed was 4000 r / min and the spin coating time was 30 s. During the high-speed rotation for 6 to 8 s, the anti-solvent chlorobenzene was added dropwise, and the added volume was 4 times the volume of the perovskite precursor solution.
[0016] Furthermore, the perovskite wet film annealing treatment described in step S4 refers to heating the deposited perovskite wet film at 100-120° C. for 12-18 minutes.
[0017] Furthermore, the carbon slurry used in step S5 is a commercial conductive carbon slurry, which is scraped onto the surface of the perovskite layer using a scraper and heated at 100 to 120° C. for 15 to 20 minutes.
[0018] The positive effects of the present invention are:
[0019] (1) The present invention effectively reduces defect density, optimizes film quality, and improves device performance by adding 1,3-propylenediamine hydrochloride (PDADCl) additive during the preparation of the perovskite precursor solution. The amino part in PDADCl can passivate Pb in the perovskite. 2+ Vacancy and MA + Vacancy, reducing negative charge defects, while Cl- can combine with I- vacancies in perovskite, passivate positive charge defects, increase solubility, and chloride ion additives help regulate the formation of perovskite film, thereby improving crystallinity and improving film quality. At the same time, the invention prepares a tri-cation mixed perovskite solution. By adding a small amount of cesium iodide to the perovskite precursor solution, it can fill the cation vacancies formed by the volatilization of organic cations, reduce defect density, reduce the precipitation of lead iodide, and effectively improve the device performance and stability.
[0020] (2) The entire preparation process of the carbon-based hole transport layer-free perovskite solar cell of the present invention is carried out at low temperature, without the need for high-temperature calcination. No expensive hole transport layer materials are required in the preparation process, and carbon materials are used instead of metal materials as electrodes, which greatly reduces production costs and simplifies the process flow. The preparation method of the perovskite solar cell is simple, low-cost, and highly repeatable, and has reference significance for the future production of low-cost, high-performance perovskite solar cells. DETAILED DESCRIPTION
[0021] Example 1
[0022] A method for preparing a carbon-based perovskite solar cell without a hole transport layer, wherein the perovskite solar cell comprises, from bottom to top, a glass substrate, an electron transport layer, a perovskite layer, and a carbon electrode;
[0023] The specific steps of preparation are as follows:
[0024] Step S1, cleaning the glass substrate. 2 The indium tin oxide (ITO) glass substrate was ultrasonically cleaned in 200 ml of ethanol, daily detergent, deionized water, isopropanol and ethanol for 15 minutes, then dried in an oven at 70°C for 15 minutes, and then treated with ultraviolet ozone (UV) for 10 minutes.
[0025] Step S2, prepare an electron transport layer on the substrate described in S1. Mix 200 μL of 15wt% aqueous dispersion of tin dioxide (SnO2) with 1 mL of deionized water, and stir thoroughly to obtain a tin oxide solution. Then take 45 μL of the tin oxide solution and apply it on the ITO glass substrate of S1, start the coating machine, the spin coating speed is 4000 r / min, the spin coating time is 30 s, and anneal at 150°C for 30 min to obtain a tin dioxide electron transport layer.
[0026] Step S3, prepare a perovskite precursor solution. Weigh 1.5mmol lead iodide, 1.3mmol methylammonium iodide (MAI), 0.15mmol methylammonium hydroiodide (FAI), 0.05mmol cesium iodide (CsI) and 0.03mmol 1,3-propylenediamine hydrochloride (PDADCl) and dissolve them in a mixed solvent of 100μL dimethyl sulfoxide (DMSO) and 900μL dimethylformamide (DMF) (the total amount of the mixed solvent is 1mL) to form a perovskite precursor solution, and stir it thoroughly for 8h. Step S4, spin-coat the perovskite precursor solution described in S3 on the electron transport layer to prepare a perovskite layer. Filter the evenly stirred perovskite precursor solution with a disposable sterile syringe with a polytetrafluoroethylene organic filter membrane, and use a pipette to draw 50μL of the perovskite precursor solution and apply it to the 1×1cm of S2. 2 The film was spin-coated on a glass substrate at a speed of 4000 r / min for 30 s, 200 μL of anti-solvent chlorobenzene was dropped on the electron transport layer within 6 to 8 s of high-speed rotation, and then annealed at 120 ° C for 12 min to obtain the perovskite layer.
[0027] Step S5: Use a glass slide to dip a small amount of carbon slurry and directly scrape it onto the surface of the S4 perovskite layer to completely cover the perovskite layer, and anneal it at 100° C. for 20 minutes to obtain a carbon electrode.
[0028] The performance of the prepared carbon-based perovskite solar cells without hole transport layer is shown in Table 2.
[0029] Example 2-Example 4, Comparative Examples 1-4
[0030] Each step refers to Example 1, and the formula of the perovskite precursor solution is shown in Table 1.
[0031] Table 1
[0032] Lead iodide Methylammonium iodide Methylchloride Cesium iodide 1,3-Propylenediamine hydrochloride Example 1 1.5 1.3 0.15 0.05 0.03 Example 2 1.5 1.1 0.3 0.1 0.03 Example 3 1.2 1 0.18 0.02 0.02 Example 4 1 0.8 0.1 0.1 0.01 Comparative Example 1 1.5 1.3 0.15 0.05 / Comparative Example 2 1.5 1.1 0.3 0.1 / Comparative Example 3 1.5 1.3 0.2 / / Comparative Example 4 1.5 1.1 0.4 / /
[0033] Battery performance indicators are shown in Table 2.
[0034] Example 5
[0035] The preparation method of the carbon-based perovskite solar cell without hole transport layer, the specific steps of the preparation are as follows:
[0036] Step S1, cleaning the glass substrate. 2 The indium tin oxide (ITO) glass substrate was ultrasonically cleaned in 200 ml of ethanol, daily detergent, deionized water, isopropanol and ethanol for 20 minutes, then dried in an oven at 50°C for 12 minutes, and then treated with ultraviolet ozone (UV) for 20 minutes.
[0037] Step S2, prepare an electron transport layer on the substrate described in S1. Mix 200 μL of 17 wt% aqueous dispersion of tin dioxide (SnO2) with 1 mL of deionized water, and stir thoroughly to obtain a tin oxide solution. Then take 40 μL of the tin oxide solution and apply it on the ITO glass substrate of S1, start the coating machine, the spin coating speed is 4000 r / min, the spin coating time is 30 s, and anneal at 130 ° C for 20 min to obtain a tin dioxide electron transport layer.
[0038] Step S3, preparing a perovskite precursor solution. Lead iodide, methylammonium iodide (MAI), methylammonium hydroiodide (FAI), cesium iodide (CsI) and 1,3-propylenediamine hydrochloride (PDADCl) were weighed in the same amount as in Example 1, dissolved in a mixed solvent of 200 μL dimethyl sulfoxide (DMSO) and 800 μL dimethylformamide (DMF) (the total amount of the mixed solvent was 1 mL) to form a perovskite precursor solution, and stirred thoroughly for 6 hours.
[0039] Step S4: Spin-coat the perovskite precursor solution in S3 onto the electron transport layer to prepare a perovskite layer. Filter the stirred perovskite precursor solution with a disposable sterile syringe with a polytetrafluoroethylene organic filter membrane, and use a pipette to draw 50 μL of the perovskite precursor solution and apply it to a 1×1 cm 2 The film was spin-coated on a glass substrate at a speed of 4000 r / min for 30 s, 200 μL of anti-solvent chlorobenzene was dropped on the electron transport layer within 6 to 8 s of high-speed rotation, and then annealed at 100°C for 18 min to obtain the perovskite layer.
[0040] Step S5: Use a glass slide to dip a small amount of carbon slurry and directly scrape it onto the surface of the S4 perovskite layer to completely cover the perovskite layer, and anneal it at 100° C. for 15 minutes to obtain a carbon electrode.
[0041] Battery performance indicators are shown in Table 2.
[0042] Example 6
[0043] The preparation method of the carbon-based perovskite solar cell without hole transport layer, the specific steps of the preparation are as follows:
[0044] Step S1, cleaning the glass substrate. 2The indium tin oxide (ITO) glass substrate was ultrasonically cleaned in 200 ml of ethanol, daily detergent, deionized water, isopropanol and ethanol for 10 minutes, then dried in an oven at 60°C for 10 minutes, and then treated with ultraviolet ozone (UV) for 15 minutes.
[0045] Step S2, prepare an electron transport layer on the substrate described in S1. Mix 200 μL of 16 wt% aqueous dispersion of tin dioxide (SnO2) with 1 mL of deionized water, and stir thoroughly to obtain a tin oxide solution. Then take 50 μL of the tin oxide solution and apply it on the ITO glass substrate of S1, start the coating machine, the spin coating speed is 4000 r / min, the spin coating time is 30 s, and anneal at 140 ° C for 25 min to obtain a tin dioxide electron transport layer.
[0046] Step S3, preparing a perovskite precursor solution. Lead iodide, methylammonium iodide (MAI), methylammonium hydroiodide (FAI), cesium iodide (CsI) and 1,3-propylenediamine hydrochloride (PDADCl) were weighed in the same amount as in Example 1, dissolved in a mixed solvent of 300 μL dimethyl sulfoxide (DMSO) and 700 μL dimethylformamide (DMF) (the total amount of the mixed solvent was 1 mL) to form a perovskite precursor solution, and stirred thoroughly for 5 hours.
[0047] Step S4: Spin-coat the perovskite precursor solution in S3 onto the electron transport layer to prepare a perovskite layer. Filter the stirred perovskite precursor solution with a disposable sterile syringe with a polytetrafluoroethylene organic filter membrane, and use a pipette to draw 50 μL of the perovskite precursor solution and apply it to a 1×1 cm 2 The film was spin-coated on a glass substrate at a speed of 4000 r / min for 30 s, 200 μL of anti-solvent chlorobenzene was dropped on the electron transport layer within 6 to 8 s of high-speed rotation, and then annealed at 110°C for 15 min to obtain the perovskite layer.
[0048] Step S5: Use a glass slide to dip a small amount of carbon slurry and directly scrape it onto the surface of the S4 perovskite layer to completely cover the perovskite layer, and anneal it at 120° C. for 15 minutes to obtain a carbon electrode.
[0049] Battery performance indicators are shown in 2.
[0050] Example 7
[0051] The preparation method of the carbon-based perovskite solar cell without hole transport layer, the specific steps of the preparation are as follows:
[0052] Step S1, cleaning the glass substrate. 2The indium tin oxide (ITO) glass substrate was ultrasonically cleaned in 200 ml of ethanol, daily detergent, deionized water, isopropanol and ethanol for 20 minutes, then dried in an oven at 50°C for 12 minutes, and then treated with ultraviolet ozone (UV) for 20 minutes.
[0053] Step S2, prepare an electron transport layer on the substrate described in S1. Mix 200 μL of 17 wt% aqueous dispersion of tin dioxide (SnO2) with 1 m of deionized water, and stir thoroughly to obtain a tin oxide solution. Then take 60 μL of the tin oxide solution and apply it on the ITO glass substrate of S1, start the coating machine, the spin coating speed is 4000 r / min, the spin coating time is 30 s, and anneal at 130 ° C for 20 min to obtain a tin dioxide electron transport layer.
[0054] Step S3, preparing a perovskite precursor solution. Lead iodide, methylammonium iodide (MAI), methylammonium hydroiodide (FAI), cesium iodide (CsI) and 1,3-propylenediamine hydrochloride (PDADCl) were weighed in the same amount as in Example 1, dissolved in a mixed solvent of 400 μL dimethyl sulfoxide (DMSO) and 600 μL dimethylformamide (DMF) (the total amount of the mixed solvent was 1 mL) to form a perovskite precursor solution, and stirred thoroughly for 6 hours.
[0055] Step S4: Spin-coat the perovskite precursor solution in S3 onto the electron transport layer to prepare a perovskite layer. Filter the stirred perovskite precursor solution with a disposable sterile syringe with a polytetrafluoroethylene organic filter membrane, and use a pipette to draw 50 μL of the perovskite precursor solution and apply it to a 1×1 cm 2 The film was spin-coated on a glass substrate at a speed of 4000 r / min for 30 s, 200 μL of anti-solvent chlorobenzene was dropped on the electron transport layer within 6 to 8 s of high-speed rotation, and then annealed at 100°C for 18 min to obtain the perovskite layer.
[0056] Step S5: Use a glass slide to dip a small amount of carbon slurry and directly scrape it onto the surface of the S4 perovskite layer to completely cover the perovskite layer, and anneal it at 100° C. for 15 minutes to obtain a carbon electrode.
[0057] Battery performance indicators are shown in 2.
[0058] Table 2
[0059]
[0060]
[0061] By comparing the data of Control Example 1 and Control Example 3, and Control Example 2 and Control Example 4 in Table 2, it can be found that after adding a small amount of Cs to the perovskite precursor solution, the open circuit voltage and filling of the device are significantly improved, indicating that Cs ions can fill organic cation vacancies, thereby reducing negative charge defects, reducing lead iodide precipitation, and improving device performance.
[0062] By comparing the data of Example 1 and Comparative Example 1, and Example 2 and Comparative Example 2 in Table 2, it can be found that the photoelectric performance of the perovskite solar cell with the 1,3-propylenediamine hydrochloride (PDADCl) additive is better than that of the device without the additive, and from the comparison of Examples 1 to 4 and Comparative Examples 1 to 2, it can be seen that for perovskite precursor solutions with different concentrations and cation ratios, the device performance after adding the 1,3-propylenediamine hydrochloride (PDADCl) additive is also better than that of the device without the additive. It shows that the 1,3-propylenediamine hydrochloride (PDADCl) additive selected by the present invention can effectively passivate the positive and negative charge defects in the perovskite, increase the grain size, and improve the film quality, thereby promoting carrier transport and improving battery performance and stability.
[0063] By comparing the data of the examples, the precursor concentration, formula and process parameters adopted in Example 1 are optimal.
Claims
1. A method for preparing a carbon-based perovskite solar cell without a hole transport layer, characterized in that: From bottom to top, the perovskite solar cell includes a glass substrate, an electron transport layer, a perovskite layer, and a carbon electrode; The specific steps of preparation are as follows: S1 cleans the glass substrate; S2 deposits the electron transport layer on the cleaned glass substrate by spin coating; S3 Preparation of perovskite precursor solution: Lead iodide, methylammonium iodide (MAI), methylammonium hydroiodide (FAI), cesium iodide and 1,3-propylenediamine hydrochloride (PDADCl) are dissolved in an organic solvent and stirred for 5-8 hours, wherein the molar concentrations are 1-1.5 mol / L lead iodide, 0.8-1.3 mol / L methylammonium iodide, 0.1-0.3 mol / L methylammonium hydroiodide, 0.02-0.1 mol / L cesium iodide, and 0.01-0.03 mol / L 1,3-propylenediamine hydrochloride; the organic solvent is a mixed solvent of dimethylformamide (DMF) and dimethyl sulfoxide (DMSO) in a volume ratio of 4:1-9:1; S4: uniformly coating the perovskite precursor solution prepared in S3 on the surface of the electron transport layer by spin coating, and annealing the perovskite wet film to obtain a perovskite layer; S5: coating the carbon slurry on the perovskite layer by scraping, and obtaining the carbon electrode after annealing.
2. The method for preparing a carbon-based perovskite solar cell without a hole transport layer according to claim 1, characterized in that The cleaning described in step S1 refers to ultrasonically cleaning the glass substrate using ethanol, daily detergent, deionized water, isopropanol and ethanol in sequence for 10 to 20 minutes, then drying it at 50 to 70° C. for 10 to 15 minutes, and continuing to use ultraviolet ozone (UV) treatment for 10 to 20 minutes.
3. The method for preparing a carbon-based perovskite solar cell without a hole transport layer according to claim 1, characterized in that The deposited electron transport layer in step S2 is to mix a 15-17 wt% tin dioxide aqueous dispersion and deionized water in a volume ratio of 1:5 to obtain a tin oxide solution, and then evenly coat the tin oxide solution on a glass substrate, 1×1 cm 2 40~60μL of tin oxide solution was coated on the glass substrate, and the coating machine was started. The spin coating speed was 4000r / min and the spin coating time was 30s. After the spin coating, it was heated at 130~150℃ for 20~30min to obtain the electron transport layer.
4. The method for preparing a carbon-based perovskite solar cell without a hole transport layer according to claim 1, characterized in that The coating of the perovskite precursor solution in step S4 is as follows: the stirred perovskite precursor solution is filtered with a disposable sterile syringe with a polytetrafluoroethylene organic filter membrane, and then evenly coated on the electron transport layer, 1×1 cm 2 50 μL of perovskite precursor solution was coated on the electron transport layer, and the coating machine was started. The spin coating speed was 4000 r / min and the spin coating time was 30 s. During the high-speed rotation for 6 to 8 s, the anti-solvent chlorobenzene was added dropwise, and the added volume was 4 times the volume of the perovskite precursor solution.
5. The method for preparing a carbon-based perovskite solar cell without a hole transport layer according to claim 1, characterized in that The perovskite wet film annealing treatment described in step S4 refers to heating the deposited perovskite wet film at 100-120° C. for 12-18 minutes.
6. The method for preparing a carbon-based perovskite solar cell without a hole transport layer according to claim 1, characterized in that The carbon slurry used in step S5 is a commercial conductive carbon slurry, which is applied on the surface of the perovskite layer using a scraper and heated at 100-120° C. for 15-20 min.
Citation Information
Patent Citations
Preparation method of hole-free transmission material perovskite thin film heterojunction battery
CN104600197A
Perovskite solar cell and preparation method thereof
CN111403547A
Preparation method of all-inorganic perovskite carbon-based solar cell with high stability and photoelectric property in high-humidity environment
CN113257955A
Solar cell based on quasi two-dimensional-two-dimensional perovskite and preparation method thereof
CN114824092A
Ammonium chloride salt treated perovskite solar cell and preparation method thereof
CN115988889A
Cited By
Omnibearing annealing preparation method of perovskite thin film, perovskite thin film and application of perovskite thin film
CN120112146A
Perovskite crystallization method, lead-based organic-inorganic hybrid perovskite solar cell and preparation method thereof
CN120456785A
Preparation method and application of perovskite thin film in perovskite solar cell
CN121358153A
Perovskite precursor solution preparation method and high open-circuit voltage tandem cell
WO2026183655A1