Electret material, filter, and master batch

By using a combination of thermoplastic resin and specific charge reinforcers in electret materials, the problem of insufficient capture performance of existing materials is solved, efficient capture and simplified manufacturing process, and cost reduction.

CN118891093APending Publication Date: 2024-11-01DAIKIN INDUSTRIES LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028340.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-18
Filing Date
2023-03-16
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

There are shortcomings in the capture performance of existing electret materials, especially in terms of the efficiency of trapping particles such as NaCl and PAO, and the manufacturing process is complex and costly.

Method used

Using electret materials containing thermoplastic resins and specific charge enhancers, the charge enhancer consists of low molecular weight polytetrafluoroethylene and vinylidene fluoride polymers, combined with metal soap and low molecular amide compounds, and manufactured by melt-kneading, simplifying Manufacturing steps and improve capture performance.

Benefits of technology

The efficient capture performance of particles such as NaCl and PAO is achieved, which simplifies the manufacturing process, reduces costs, and improves the heat resistance and mechanical strength of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005047247910000051
    Figure BDA0005047247910000051
  • Figure BDA0005047247910000052
    Figure BDA0005047247910000052
  • Figure BDA0005047247910000181
    Figure BDA0005047247910000181
Patent Text Reader

Abstract

The purpose of the present disclosure is to provide an electret material having excellent collection performance, a filter using the electret material, and a master batch for manufacturing the electret material. The present invention relates to an electret material comprising a thermoplastic resin and a charge enhancer contained in the thermoplastic resin, and more specifically, to an electret material comprising a thermoplastic resin and a charge enhancer contained in the thermoplastic resin, the charge intensifier includes at least one fluorine-based charge intensifier selected from the group consisting of polytetrafluoroethylene and vinylidene fluoride polymers, and at least one hydrocarbon-based charge intensifier.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to electret materials, filters, and masterbatches. Background Art

[0002] The use of materials obtained by electretizing melt-blown fibers for use in air filters and the like is well known.

[0003] Patent Document 1 describes an electret fiber mixed with an additive such as polyvinylidene fluoride.

[0004] Patent Document 2 describes an electret fiber sheet in which a perfluoroalkyl compound such as an acrylic compound is mixed.

[0005] Patent Document 3 describes a method of making nC by vapor deposition or the like. 10 F 22 The electret is formed by compounds such as ions attached to the surface of the carrier.

[0006] Patent Documents 4 and 5 describe electret fibers in which a fatty acid metal salt and a hindered amine compound are mixed.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Laid-Open No. 5-049824

[0010] Patent Document 2: Japanese Patent Application Publication No. 2018-071018

[0011] Patent Document 3: International Publication No. 2015 / 152207

[0012] Patent Document 4: Japanese Patent Application Laid-Open No. 63-123414

[0013] Patent Document 5: International Publication No. 2021 / 033700 Summary of the invention

[0014] Problems to be solved by the invention

[0015] An object of the present disclosure is to provide an electret material having excellent collection performance, a filter using the same, and a masterbatch for producing the electret material.

[0016] Means for solving problems

[0017] The present disclosure relates to an electret material, which comprises a thermoplastic resin and a charge enhancer contained in the thermoplastic resin, wherein:

[0018] The charge enhancer includes at least one fluorine-based charge enhancer selected from the group consisting of polytetrafluoroethylene and vinylidene fluoride polymers, and at least one hydrocarbon-based charge enhancer.

[0019] The fluorine-based charge enhancer is preferably a low molecular weight polytetrafluoroethylene and a vinylidene fluoride polymer.

[0020] The vinylidene fluoride polymer is preferably at least one selected from the group consisting of polyvinylidene fluoride and a vinylidene fluoride / tetrafluoroethylene copolymer.

[0021] The hydrocarbon-based charge enhancer is preferably at least one selected from the group consisting of metal soaps, hindered amine compounds, triazine compounds, transparentizing agents, and low-molecular amide compounds.

[0022] The hydrocarbon-based charge enhancer is preferably a metal soap or a low-molecular amide compound.

[0023] The metal soap is preferably a salt of a metal of Group 2 of a fatty acid.

[0024] The low molecular weight amide compound is preferably at least one selected from the group consisting of fatty acid amides and fatty acid bisamides.

[0025] The mass ratio of the fluorine-based charge enhancer to the hydrocarbon-based charge enhancer (fluorine-based / hydrocarbon-based) is preferably 1 / 99 to 99 / 1.

[0026] The thermoplastic resin is preferably a polyolefin-based resin.

[0027] The ratio of the F element content to the C element content (F / C) on the surface of the electret material measured by XPS (X-ray photoelectron spectroscopy) is preferably 0.20% or less.

[0028] The total amount of the charge enhancer is preferably 0.01% by mass to 5.0% by mass based on the thermoplastic resin.

[0029] The electret material is preferably a fiber sheet.

[0030] The present disclosure also relates to a filter using the above electret material.

[0031] The filter is preferably a filter for a dust mask.

[0032] The present disclosure also relates to a masterbatch, which is a masterbatch for manufacturing an electret material, wherein:

[0033] The masterbatch comprises: a thermoplastic resin, and a charge enhancer contained in the thermoplastic resin.

[0034] The charge enhancer comprises: at least one fluorine-based charge enhancer selected from the group consisting of polytetrafluoroethylene and vinylidene fluoride polymers, and at least one hydrocarbon-based charge enhancer,

[0035] The total amount of the charge enhancer is greater than 5.0% by mass and less than or equal to 50% by mass based on the thermoplastic resin.

[0036] Effects of the Invention

[0037] According to the present disclosure, it is possible to provide an electret material having excellent collection performance, a filter using the electret material, and a masterbatch for producing the electret material. DETAILED DESCRIPTION

[0038] The present disclosure is described in detail below.

[0039] The present disclosure relates to an electret material, which comprises a thermoplastic resin and a charge enhancer contained in the thermoplastic resin, wherein the charge enhancer comprises at least one fluorine-based charge enhancer selected from the group consisting of polytetrafluoroethylene and vinylidene fluoride polymers, and at least one hydrocarbon-based charge enhancer.

[0040] In the electret material disclosed in the present invention, by using a specific fluorine-based charge enhancer and a hydrocarbon-based charge enhancer together, the particle capture performance (for example, PF value) of particles such as NaCl particles and PAO (poly-α-olefin) particles is excellent.

[0041] Examples of the thermoplastic resin include polyolefin resins such as polyethylene and polypropylene; polyester resins such as polyethylene terephthalate, polypropylene terephthalate, polybutylene terephthalate, and polylactic acid; polycarbonate resins; polystyrene resins; polyphenylene sulfide resins; fluorine resins; thermoplastic elastomers such as polystyrene elastomers, polyolefin elastomers, polyester elastomers, polyamide elastomers, and polyurethane elastomers; and copolymers or mixtures thereof.

[0042] Among these, polyolefin resins are preferably used. Polyolefin resins have high volume resistivity and low water absorption, so they have strong chargeability and charge retention when fiberized, so that high collection efficiency can be achieved.

[0043] As the kind of polyolefin resin, homopolymers such as polyethylene, polypropylene, polybutene and polymethylpentene can be enumerated. In addition, copolymers having different components in these homopolymers and two or more different polymer blends can also be used. Among these, from the aspect of charge retention, polypropylene and polymethylpentene are preferably used. In addition, from the aspect that can be utilized at low cost, polypropylene is more preferably used.

[0044] In the above-mentioned polypropylene, from the viewpoint of obtaining a melt-blown nonwoven fabric having good spinnability and good mechanical strength such as tensile strength, the melt flow rate (MFR) is preferably 600 g / 10 min or more, more preferably 800 g / 10 min or more, and further preferably 1100 g / 10 min or more, and is preferably 2500 g / 10 min or less, more preferably 1800 g / 10 min or less, and further preferably 1500 g / 10 min or less.

[0045] The MFR is measured in accordance with ASTM D-1238 under the conditions of 230° C. and a load of 2160 g.

[0046] The charge enhancer includes at least one fluorine-based charge enhancer selected from the group consisting of polytetrafluoroethylene (PTFE) and vinylidene fluoride (VdF) polymers. The fluorine-based charge enhancer has excellent heat resistance.

[0047] The above-mentioned PTFE is preferably low-molecular-weight PTFE.

[0048] The melt viscosity of the low molecular weight PTFE at 380°C is 1.0×10 2 ~7.0×10 5 Pa·s. In the present disclosure, "low molecular weight" means that the above-mentioned melt viscosity is within the above-mentioned range.

[0049] The above melt viscosity is preferably 1.5×10 3 Pa·s or more, and preferably 3.0×10 5 Pa·s or less, more preferably 1.0×10 5 Pa·s or less.

[0050] The melt viscosity is measured in accordance with ASTM D 1238 using a flow tester (manufactured by Shimadzu Corporation) and The value is obtained by measuring a 2 g sample heated in advance at 380°C for 5 minutes using a -8L die and maintaining the sample at the above temperature under a load of 0.7 MPa.

[0051] The melting point of the low molecular weight PTFE is preferably 320 to 340°C, more preferably 324°C or higher, and more preferably 336°C or lower.

[0052] Regarding the above melting point, a differential scanning calorimeter (DSC) was used. After temperature correction was performed in advance using indium and lead as standard samples, about 3 mg of low molecular weight PTFE was placed in an aluminum dish (covered container), and the temperature was increased at a rate of 10°C / min in a temperature range of 250 to 380°C under an air flow of 200 ml / min. The minimum point of the heat of fusion in the above range was taken as the melting point.

[0053] From the perspective of suppressing clogging of the meltblowing die, the low molecular weight PTFE preferably has an average particle size of 0.1 to 100 μm. The average particle size is more preferably 50 μm or less, further preferably 10 μm or less, particularly preferably 6 μm or less, and more preferably 0.5 μm or more, further preferably 1.0 μm or more.

[0054] The above average particle size is measured using a laser diffraction particle size distribution measuring device (HELOS & RODOS) manufactured by JEOL Ltd. at a dispersion pressure of 1.0 bar without using a cascade. The above average particle size is equal to the particle size corresponding to 50% of the particle size distribution integral (volume basis).

[0055] The low-molecular-weight PTFE may be a TFE homopolymer composed of only tetrafluoroethylene (TFE) units, or may be a modified PTFE containing TFE units and modified monomer units based on a modifying monomer copolymerizable with TFE.

[0056] In the above-mentioned modified PTFE, the content of the above-mentioned modified monomeric unit is preferably 0.001~1 mass % of all monomeric units, more preferably more than 0.01 mass %, and more preferably below 0.5 mass %, further preferably below 0.1 mass %. In this specification, the above-mentioned modified monomeric unit is a part of the molecular structure of modified PTFE, refers to the part from the modified monomer, and all monomeric units refer to the part from all monomers in the molecular structure of modified PTFE. The content of the above-mentioned modified monomeric unit can be obtained by known methods such as Fourier transform infrared spectroscopy (FT-IR).

[0057] As the above-mentioned modified monomer, there is no particular limitation as long as it can be copolymerized with TFE, and examples thereof include: perfluoroolefins such as hexafluoropropylene [HFP]; fluorochloroolefins such as trifluorochloroethylene [CTFE]; hydrogen-containing fluoroolefins such as trifluoroethylene and vinylidene fluoride [VDF]; perfluorovinyl ether; perfluoroalkylethylene; ethylene, etc. In addition, the modified monomer used may be one kind or two or more kinds.

[0058] The perfluorovinyl ether is not particularly limited, and examples thereof include the following general formula (1):

[0059] CF2=CF-ORf (1)

[0060] (wherein Rf represents a perfluoro organic group) and the like. In the present specification, the above-mentioned "perfluoro organic group" refers to an organic group in which all hydrogen atoms bonded to carbon atoms are replaced by fluorine atoms. The above-mentioned perfluoro organic group may have an ether oxygen.

[0061] Examples of the perfluorovinyl ether include perfluoro(alkyl vinyl ether) [PAVE] in which Rf in the general formula (1) represents a perfluoroalkyl group having 1 to 10 carbon atoms. The perfluoroalkyl group preferably has 1 to 5 carbon atoms.

[0062] Examples of the perfluoroalkyl group in the PAVE include perfluoromethyl, perfluoroethyl, perfluoropropyl, perfluorobutyl, perfluoropentyl, and perfluorohexyl. Preferably, the perfluoroalkyl group is perfluoro(propyl vinyl ether) [PPVE] in which the perfluoroalkyl group is perfluoropropyl.

[0063] Examples of the perfluorovinyl ether include those in which Rf in the general formula (1) is a perfluoro(alkoxyalkyl) group having 4 to 9 carbon atoms, and Rf is the following formula:

[0064] [Chemistry 1]

[0065]

[0066] (wherein m represents 0 or an integer of 1 to 4) and Rf is the following formula:

[0067] [Chemistry 2]

[0068]

[0069] (wherein n represents an integer of 1 to 4) and the like.

[0070] The perfluoroalkylethylene is not particularly limited, and examples thereof include (perfluorobutyl)ethylene (PFBE), (perfluorohexyl)ethylene, and (perfluorooctyl)ethylene.

[0071] The modifying monomer in the modified PTFE is preferably at least one selected from the group consisting of HFP, CTFE, VDF, PPVE, PFBE and ethylene, and more preferably at least one selected from the group consisting of PPVE, HFP and CTFE.

[0072] The VdF polymer is preferably at least one selected from the group consisting of polyvinylidene fluoride (PVdF) and a VdF / TFE copolymer.

[0073] The PVdF may be a homopolymer composed only of polymerized units based on VdF, or may be a polymerized unit containing polymerized units based on VdF and polymerized units based on a monomer (α) copolymerizable with VdF.

[0074] The monomer (α) may have an ethylenically unsaturated double bond. Specific examples of the monomer (α) include: fluorine-containing monomers [e.g., vinyl fluoride (VF), trifluoroethylene (TrFE), hexafluoropropylene (HFP), 1-chloro-1-fluoroethylene (1,1-CFE), 1-chloro-2-fluoroethylene (1,2-CFE), 1-chloro-2,2-difluoroethylene (CDFE), chlorotrifluoroethylene (CTFE), trifluoroethylene monomer, 1,1,2-trifluorobutene-4-bromo-1-butene, 1,1,2-trifluorobutene-4-silane-1-butene, perfluoropropyl] Vinyl ether (PPVE), perfluoroacrylate, 2,2,2-trifluoroethyl acrylate, 2-(perfluorohexyl)ethyl acrylate)], non-fluorinated monomers [such as α-olefins (such as ethylene, propylene); unsaturated dicarboxylic acids or their derivatives (such as maleic acid, maleic anhydride); vinyl ethers (such as ethyl vinyl ether); allyl ethers (such as allyl glycidyl ether); vinyl esters (such as vinyl acetate); acrylic acid or its esters; methacrylic acid or its esters], and combinations of one or more of them.

[0075] In the PVdF, the repeating unit derived from the monomer (α) may be contained in an amount of, for example, 10 mol% or less, preferably 5 mol% or less, and preferably 0.01 mol% or more, among the repeating units derived from all monomers.

[0076] The weight average molecular weight (in terms of polystyrene) of the PVdF is preferably 50,000 to 2,000,000. The weight average molecular weight is more preferably 80,000 or more and more preferably 1,900,000 or less.

[0077] The weight average molecular weight can be measured by gel permeation chromatography (GPC) at 50° C. using N,N-dimethylformamide as a solvent.

[0078] The number average molecular weight (in terms of polystyrene) of the PVdF is preferably 150,000 to 1,400,000. The number average molecular weight is more preferably 200,000 or more and more preferably 1,300,000 or less.

[0079] The number average molecular weight can be measured by gel permeation chromatography (GPC) using N,N-dimethylformamide as a solvent at 50°C.

[0080] In the above-mentioned VdF / TFE copolymer, the molar ratio ((-CH2-CF2-) / (-CF2-CF2-)) of the repeating unit (-CH2-CF2-) derived from VdF and the repeating unit (-CF2-CF2-) derived from TFE is not limited, and can be, for example, in the range of 50 / 50 to 99 / 1. The above-mentioned molar ratio is preferably 55 / 45 or more, more preferably 60 / 40 or more, and further preferably 70 / 30 or more, and is preferably 97 / 3 or less, more preferably 95 / 5 or less, and further preferably 90 / 10 or less.

[0081] The VdF / TFE copolymer may be a copolymer consisting of only VdF and TFE or a copolymer consisting essentially of VdF and TFE. The VdF / TFE copolymer may further include a repeating unit derived from a monomer (β) copolymerizable with VdF and TFE.

[0082] Examples of the monomer (β) include the same monomers as those described above for the monomer (α) in connection with the PVdF.

[0083] In the VdF / TFE copolymer, the repeating unit derived from the monomer (β) may be contained in an amount of, for example, 10 mol% or less, preferably 5 mol% or less, and preferably 0.01 mol% or more, among the repeating units derived from all monomers.

[0084] The weight average molecular weight (polystyrene equivalent) of the VdF / TFE copolymer is preferably 50,000 to 2,000,000. The weight average molecular weight is more preferably 80,000 or more, further preferably 100,000 or more, and more preferably 1,950,000 or less, further preferably 1,500,000 or less.

[0085] The weight average molecular weight can be measured by gel permeation chromatography (GPC) at 50° C. using N,N-dimethylformamide as a solvent.

[0086] The number average molecular weight (polystyrene equivalent) of the VdF / TFE copolymer is preferably 10000 to 1400000. The number average molecular weight is more preferably 16000 or more, further preferably 20000 or more, and more preferably 1300000 or less, further preferably 1200000 or less.

[0087] The number average molecular weight can be measured by gel permeation chromatography (GPC) using N,N-dimethylformamide as a solvent at 50°C.

[0088] As the VdF polymer, the VdF / TFE copolymer is preferred.

[0089] In addition, as the VdF polymer, it is also preferred to mix the PVdF and the VdF / TFE copolymer. In this case, the mass ratio [(VdF / TFE copolymer) / PVdF] is preferably 5 / 95 or more, more preferably 10 / 90 or more, further preferably 20 / 80 or more, and preferably 90 / 10 or less, more preferably 85 / 15 or less.

[0090] The fluorine-based charge enhancer is preferably the PTFE and the VdF polymer, more preferably the low-molecular-weight PTFE and the VdF polymer, and still more preferably the low-molecular-weight PTFE, the PVdF, and the VdF / TFE copolymer.

[0091] When the fluorine-based charge enhancer is the PTFE and the VdF polymer, the mass ratio of the PTFE to the VdF polymer (PTFE / VdF polymer) is preferably 1 / 99 to 70 / 30 from the perspective of further improving the collection performance. The mass ratio is more preferably 5 / 95 or more, more preferably 10 / 90 or more, and particularly preferably 15 / 85 or more. In addition, the mass ratio is more preferably 60 / 40 or less, more preferably 50 / 50 or less, further more preferably 40 / 60 or less, and particularly preferably 30 / 70 or less.

[0092] The charge enhancer includes at least one hydrocarbon-based charge enhancer. The hydrocarbon-based charge enhancer may be a non-fluorine-based charge enhancer.

[0093] Examples of the hydrocarbon-based charge enhancer include metal soaps, hindered amine-based compounds, triazine-based compounds, transparentizing agents, and low-molecular amide compounds.

[0094] The metal soap may be a fatty acid metal salt. It is believed that the fatty acid metal salt effectively captures the charge reaching the composition from, for example, an ion flow released from a corona electrode when the thermoplastic resin composition is electretized.

[0095] The carbon number of the fatty acid in the fatty acid metal salt is preferably 10 to 50, more preferably 12 or more, further preferably 16 or more, and more preferably 30 or less, further preferably 22 or less.

[0096] Examples of the fatty acid include linear saturated fatty acids such as lauric acid, myristic acid, palmitic acid, stearic acid, and behenic acid; and linear unsaturated fatty acids such as oleic acid and erucic acid. Among them, linear saturated fatty acids are preferred, and stearic acid is more preferred.

[0097] Examples of the metal in the fatty acid metal salt include metals of Group 2 of the Periodic Table such as magnesium and calcium, metals of Group 12 of the Periodic Table such as zinc, and metals of Group 13 of the Periodic Table such as aluminum. Of these, metals of Group 2 of the Periodic Table are preferred, magnesium or calcium is more preferred, and magnesium is further preferred.

[0098] The melting point of the fatty acid metal salt is preferably 80° C. or higher, more preferably 100° C. or higher, and may be 300° C. or lower. The thermal decomposition temperature is preferably 200° C. or higher, and may be 300° C. or lower.

[0099] The number of fatty acid chains bonded to the metal may be 1 to 3, preferably 2.

[0100] The above-mentioned metal soap is preferably a metal salt of Group 2 of the Periodic Table of fatty acids, more preferably a metal salt of Group 2 of the Periodic Table of straight-chain saturated fatty acids, further preferably a magnesium salt or a calcium salt of straight-chain saturated fatty acids, further more preferably magnesium stearate or calcium stearate, and particularly preferably magnesium stearate.

[0101] The above-mentioned metal soap is also preferably a fatty acid magnesium salt.

[0102] Examples of the hindered amine compound include poly[(6-(1,1,3,3-tetramethylbutyl)imino-1,3,5-triazine-2,4-diyl)((2,2,6,6-tetramethyl-4-piperidyl)imino)hexamethylene((2,2,6,6-tetramethyl-4-piperidyl)imino)] (e.g., Chimassorb (registered trademark) 944LD manufactured by BASF Japan Co., Ltd.), dimethyl succinate-1-(2-hydroxyethyl)-4-hydroxy-2,2,6,6-tetramethylpiperidinyl condensate (e.g., Tinuvin (registered trademark) 622LD manufactured by BASF Japan Co., Ltd.), and 2-(3,5-di-tert-butyl-4-hydroxybenzyl)-2-n-butylmalonic acid bis(1,2,2,6,6-pentamethyl-4-piperidyl) (e.g., BASF "Tinuvin" (registered trademark) 144) manufactured by Japan Co., Ltd., etc.

[0103] The hindered amine compound is preferably a compound having a triazine structure, and more preferably poly[(6-(1,1,3,3-tetramethylbutyl)imino-1,3,5-triazine-2,4-diyl)((2,2,6,6-tetramethyl-4-piperidinyl)imino)hexamethylene((2,2,6,6-tetramethyl-4-piperidinyl)imino)] (for example, "Chimassorb" (registered trademark) 944LD manufactured by BASF Japan Co., Ltd.).

[0104] Examples of the triazine compounds include poly[(6-(1,1,3,3-tetramethylbutyl)imino-1,3,5-triazine-2,4-diyl)((2,2,6,6-tetramethyl-4-piperidinyl)imino)hexamethylene((2,2,6,6-tetramethyl-4-piperidinyl)imino)] (e.g., “Chimassorb” (registered trademark) 944LD manufactured by BASF Japan Co., Ltd.), and 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-((hexyl)oxy)-phenol (e.g., “Tinuvin” (registered trademark) 1577FF manufactured by BASF Japan Co., Ltd.).

[0105] The triazine compound may not have a hindered amine structure.

[0106] The transparentizing agent may be a crystal nucleating agent.

[0107] Examples of the crystal nucleating agent include sorbitol nucleating agents, nonitol nucleating agents, xylitol nucleating agents, phosphoric acid nucleating agents, triaminobenzene derivative nucleating agents, and carboxylic acid metal salt nucleating agents.

[0108] Examples of the sorbitol-based nucleating agent include dibenzylidene sorbitol (DBS), monomethyldibenzylidene sorbitol (e.g., 1,3:2,4-bis(p-methylbenzylidene)sorbitol (p-MDBS)), dimethyldibenzylidene sorbitol (e.g., 1,3:2,4-bis(3,4-dimethylbenzylidene)sorbitol (3,4-DMDBS)), and 1,3:2,4-bis-O-(4-methylbenzylidene)-D-sorbitol. Examples of commercially available products include "Millad" (registered trademark) 3988 (manufactured by Milliken Japan Co., Ltd.) and "GEL ALL" (registered trademark) E-200 (manufactured by Shin Nippon Rika Co., Ltd.).

[0109] Examples of the nonitol-based nucleating agent include 1,2,3-trideoxy-4,6:5,7-bis-[(4-propylphenyl)methylene]-nonitol, and commercially available products include "Millad" (registered trademark) NX8000 (manufactured by Milliken Japan Co., Ltd.).

[0110] Examples of the xylitol-based nucleating agent include bis-1,3:2,4-(5′,6′,7′,8′-tetrahydro-2-naphthaldehydebenzylidene)1-allyl xylitol and the like.

[0111] Examples of the phosphoric acid-based nucleating agent include bis(4,4',6,6'-tetra-tert-butyl-2,2'-methylenediphenyl-phosphate)aluminum hydroxide, and commercially available products include "ADKSTAB" (registered trademark) NA-11 (manufactured by ADEKA Corporation) and "ADKSTAB" (registered trademark) NA-21 (manufactured by ADEKA Corporation).

[0112] Examples of the triaminobenzene derivative nucleating agent include 1,3,5-tris(2,2-dimethylpropionamide)benzene, and examples of commercially available products include "Irgaclear" (registered trademark) XT386 (manufactured by BASF Japan Co., Ltd.).

[0113] Examples of the carboxylic acid metal salt nucleating agent include sodium benzoate and 1,2-cyclohexanedicarboxylic acid calcium salt.

[0114] As the above-mentioned transparent agent, at least one selected from the group consisting of sorbitol nucleating agents, nonitol nucleating agents, xylitol nucleating agents, phosphoric acid nucleating agents, triaminobenzene derivative nucleating agents and carboxylic acid metal salt nucleating agents is preferred, at least one selected from the group consisting of sorbitol nucleating agents and phosphoric acid nucleating agents is more preferred, sorbitol nucleating agents are further preferred, and 1,3:2,4-bis-O-(4-methylbenzylidene)-D-sorbitol is particularly preferred.

[0115] The molecular weight of the low molecular weight amide compound is preferably 100 to 1000, more preferably 200 or more, further preferably 500 or more, and is preferably 800 or less, further preferably 700 or less.

[0116] The above molecular weight can be obtained from the molecular structure (chemical formula).

[0117] Examples of the low-molecular amide compound include fatty acid amides and fatty acid bisamides.

[0118] The carbon number of the fatty acid in the fatty acid amide and the fatty acid bisamide is preferably 8 to 60, more preferably 10 or more, further preferably 20 or more, particularly preferably 30 or more, and more preferably 50 or less, further preferably 40 or less.

[0119] Examples of the fatty acid include straight-chain saturated fatty acids such as lauric acid, myristic acid, palmitic acid, stearic acid, and behenic acid; branched-chain saturated fatty acids such as isostearic acid; straight-chain unsaturated fatty acids such as oleic acid and erucic acid, etc. Among them, straight-chain saturated fatty acids are preferred, and stearic acid is more preferred.

[0120] Examples of the fatty acid amide include lauryl amide, palmitamide, stearyl amide, behenyl amide, hydroxystearyl amide, N-lauryl lauryl amide, N-palmityl palmitamide, N-stearyl stearyl amide, N-stearyl-hydroxystearyl amide, and oleic acid amide.

[0121] Among them, stearamide is preferred.

[0122] Examples of the fatty acid bisamides include methylene bisstearamide, methylene bislauramide, methylene bishydroxystearamide, ethylene bisoctylamide, ethylene biscapramide, ethylene bislauramide, ethylene bisstearamide, ethylene bisisostearamide, ethylene bishydroxystearamide, ethylene bisbehenamide, hexamethylene bisstearamide, hexamethylene bisbehenamide, hexamethylene bishydroxystearamide, butylene bishydroxystearamide, N,N'-distearyl adipamide, N,N'-distearyl sebacamide, methylene bisoleamide, ethylene bisoleamide, ethylene biserucamide, hexamethylene bisoleamide, N,N'-dioleyl adipamide, N,N'-dioleyl sebacamide, m-xylylene bisstearamide, and N,N'-distearyl isophthalamide.

[0123] Among them, alkylenebisfatty acid amides such as ethylenebisstearamide are preferred.

[0124] The low molecular weight amide compound is preferably at least one selected from the group consisting of fatty acid amides and fatty acid bisamides, more preferably fatty acid bisamides, further preferably alkylene bisfatty acid amides, and particularly preferably ethylene bisstearamide.

[0125] The hydrocarbon-based charge enhancer is preferably at least one selected from the group consisting of metal soaps, hindered amine compounds, triazine compounds, transparent agents, and low molecular weight amide compounds, more preferably at least one selected from the group consisting of metal soaps, hindered amine compounds, transparent agents, and low molecular weight amide compounds, further preferably at least one selected from the group consisting of metal soaps and low molecular weight amide compounds, and particularly preferably metal soaps and low molecular weight amide compounds. In addition, metal soaps and at least one selected from the group consisting of hindered amine compounds, transparent agents, and low molecular weight amide compounds are also preferred.

[0126] When the hydrocarbon-based charge enhancer is the metal soap and the low-molecular amide compound, the mass ratio of the metal soap to the low-molecular amide compound (metal soap / low-molecular amide) is preferably 30 / 70 to 99 / 1 from the perspective of further improving the collection performance. The mass ratio is more preferably 40 / 60 or more, further preferably 50 / 50 or more, further more preferably 60 / 40 or more, and particularly preferably 70 / 30 or more. In addition, the mass ratio is more preferably 95 / 5 or less, further preferably 90 / 10 or less, and particularly preferably 85 / 15 or less. When the hydrocarbon-based charge enhancer is the metal soap and the hindered amine compound, the mass ratio of the metal soap to the hindered amine compound, and when the hydrocarbon-based charge enhancer is the metal soap and the transparent agent, the mass ratio of the metal soap to the transparent agent are also preferably within the above range.

[0127] In the electret material disclosed in the present invention, from the perspective of further improving the collection performance, the mass ratio of the above-mentioned fluorine-based charge enhancer to the above-mentioned hydrocarbon-based charge enhancer (fluorine-based / hydrocarbon-based) is preferably 1 / 99 to 99 / 1. The above-mentioned mass ratio is more preferably 10 / 90 or more, further preferably 20 / 80 or more, further more preferably 30 / 70 or more, and particularly preferably 40 / 60 or more. In addition, the above-mentioned mass ratio is more preferably 90 / 10 or less, further preferably 80 / 20 or less, further more preferably 70 / 30 or less, and particularly preferably 60 / 40 or less.

[0128] In the electret material disclosed in the present invention, from the perspective of further improving the collection performance, the total amount of the charge enhancer, that is, the total amount of the fluorine-based charge enhancer and the hydrocarbon-based charge enhancer relative to the thermoplastic resin is preferably 0.01 to 5.0% by mass. The total amount is more preferably 0.10% by mass or more, further preferably 0.20% by mass or more, further preferably 0.30% by mass or more, and particularly preferably 0.40% by mass or more. In addition, the total amount is more preferably 1.0% by mass or less, further preferably 0.8% by mass or less, further preferably 0.7% by mass or less, and particularly preferably 0.6% by mass or less.

[0129] The charge enhancer is contained in the thermoplastic resin. The electret material thus constituted can be produced by mixing the thermoplastic resin and the charge enhancer, so that it is not necessary to attach the charge enhancer by post-processing such as vapor deposition or impregnation, thereby simplifying the production process. In addition, it is also possible to prevent the reduction of the collection performance due to the peeling of the charge enhancer from the surface.

[0130] The charge enhancer may be dispersed in the thermoplastic resin.

[0131] In the electret material disclosed herein, the ratio of the F element content to the C element content (F / C) on the surface of the electret material measured by XPS (X-ray photoelectron spectroscopy) is preferably 0.20% or less, more preferably 0.10% or less, further preferably 0.03% or less, and is preferably 0.0005% or more, more preferably 0.0006% or more, and further preferably 0.0008% or more.

[0132] The fact that the ratio (F / C) is within the above range means that the charge enhancer is contained in the thermoplastic resin (the charge enhancer is not attached to the surface by post-processing).

[0133] The above ratio (F / C) can be calculated by the following method using a value measured by XPS (X-ray photoelectron spectroscopy).

[0134] Ratio (F / C) = A / B

[0135] A: Peak area value of F element

[0136] B: Peak area value of C element

[0137] The electret material of the present disclosure may contain other components within a range that does not impair the effect. Examples of the other components include delustering agents, pigments, mildewproofing agents, antibacterial agents, flame retardants, heat stabilizers, weathering agents, polymerization inhibitors, and the like.

[0138] The above-mentioned thermoplastic resin, the above-mentioned charge enhancer, and other components as necessary are mixed to prepare a resin composition, and then the resin composition is subjected to an electret treatment to produce the electret material of the present disclosure.

[0139] The thermoplastic resin and the charge enhancer may be mixed by mixing a masterbatch containing the thermoplastic resin and the charge enhancer with the thermoplastic resin. The masterbatch is as follows.

[0140] The resin composition may be processed into a desired shape before and / or after the electret treatment.

[0141] As a method for mixing the thermoplastic resin and the charge enhancer, melt kneading is preferred. When the master batch is used, the master batch and the thermoplastic resin are preferably melt kneaded.

[0142] The melt kneading can be performed by a known method, for example, using a single-screw or twin-screw extruder, an open roll mill, a kneader, a Banbury mixer, or the like.

[0143] The temperature of the melt kneading is preferably higher than the melting point of the thermoplastic resin, and more preferably 5° C. or more higher than the melting point of the thermoplastic resin.

[0144] As the method of the above-mentioned electret treatment, it can be arbitrarily selected from the methods of applying corona charging method, liquid contact charging method, friction charging method, electric field charging method, thermoelectric field charging method, electron beam irradiation method and other known charging methods. As a specific electret method, it is preferred to use methods based on electrical action such as polarization based on high voltage, collision of charged ions, injection of charged particles; methods based on interaction with solids such as friction and collision; methods using contact and collision with liquids and other existing known methods.

[0145] The shape of the electret material disclosed in the present invention is not particularly limited, and may be in the form of fibers, sheets, films, particles, rods, tubes, or the like.

[0146] The electret material disclosed in the present invention is preferably in a fibrous form, more preferably in a fibrous sheet.

[0147] The average fiber diameter of the fibers constituting the fiber sheet is preferably 0.001 μm or more, more preferably 0.1 μm or more, further preferably 0.2 μm or more, and particularly preferably 0.5 μm or more. In addition, it is preferably 100 μm or less, more preferably 20 μm or less, further preferably 10 μm or less, and particularly preferably 5 μm or less. When the average fiber diameter of the fibers is thicker than 100 μm, it is difficult to obtain practical collection efficiency, and the efficiency during charge decay is significantly reduced. When the average fiber diameter of the fibers is thinner than 0.001 μm, it is difficult to produce an electret with a charge.

[0148] The above average fiber diameter is measured as follows. Using a scanning electron microscope (trade name: SU8020, manufactured by HITACHI), observe an arbitrary 25 μm × 20 μm area in an electron microscope photograph taken at a magnification of 5000 times, draw vertical and horizontal orthogonal straight lines, use a ruler to measure the diameters of all fibers intersecting each straight line, perform scale conversion, and calculate the fiber diameter (μm). Next, for the cumulative frequency distribution of the obtained fiber diameter, draw a logarithmic normal plot on a logarithmic probability paper using the fiber diameter on the horizontal axis and the cumulative frequency on the vertical axis, and take the value with a cumulative frequency of 50% as the average fiber diameter (median diameter).

[0149] The fiber sheet may be a uniform product made of a single production method and material, or may be a mixture of two or more materials different in production method, material and fiber diameter.

[0150] From the perspective of obtaining an electret fiber sheet having excellent air permeability and collection properties, the basis weight of the fiber sheet is preferably 3 g / m 2More preferably 5g / m 2 More preferably, 10 g / m 2 In addition, it is preferably 100g / m 2 Below, more preferably 70g / m 2 Below, more preferably 50g / m 2 the following.

[0151] From the perspective of obtaining an electret fiber sheet having excellent air permeability and collection characteristics, the thickness of the fiber sheet is preferably 0.01 mm or more, more preferably 0.05 mm or more, and further preferably 0.1 mm or more. In addition, it is preferably 1.0 mm or less, more preferably 0.7 mm or less, and further preferably 0.5 mm or less.

[0152] The fiber sheet is preferably a nonwoven fabric.

[0153] As a method for obtaining the above-mentioned nonwoven fabric, the following conventionally known methods can be used: a method of making a sheet of short fibers such as single component fibers, composite fibers such as core-sheath fibers or parallel fibers, split fibers, etc. by carding, air-laying, wet papermaking, etc.; a method of making a sheet of continuous fibers by spunbonding, melt-blowing, electrostatic spinning, centrifugal spinning, etc.; etc. Among them, from the viewpoint of effectively utilizing the mechanical collection mechanism, melt-blowing, electrostatic spinning, and centrifugal spinning, which are easy to obtain dense and fine fineness, are preferred, and from the viewpoint of not requiring residual solvent treatment, melt-blowing, melt electrostatic spinning, and melt centrifugal spinning are more preferred, and melt-blowing is further preferred.

[0154] The fiber sheet is preferably a melt-blown nonwoven fabric.

[0155] The electret material of the present disclosure, preferably the above-mentioned fiber sheet, has excellent collection performance and can therefore be suitably used in a filter. The present disclosure also relates to a filter using the electret material of the present disclosure.

[0156] The filter disclosed in the present invention can be used in dust masks, various air conditioning elements, air cleaners, cabin filters, various devices, etc. for the purpose of dust collection, protection, ventilation, etc. Among them, it can be preferably used for dust masks.

[0157] The present disclosure also relates to a masterbatch for producing an electret material, comprising a thermoplastic resin and a charge enhancer contained in the thermoplastic resin, wherein the charge enhancer comprises at least one fluorine-based charge enhancer selected from the group consisting of polytetrafluoroethylene and vinylidene fluoride polymers, and at least one hydrocarbon-based charge enhancer, and the total amount of the charge enhancer is greater than 5.0% by mass and less than 50% by mass relative to the thermoplastic resin.

[0158] As the thermoplastic resin in the masterbatch of the present disclosure, the same thermoplastic resin as that which can be used in the electret material of the present disclosure can be used.

[0159] As the charge enhancer in the masterbatch of the present disclosure, the same charge enhancer as that used in the electret material of the present disclosure can be used. Also, the same scheme as that of the electret material of the present disclosure can be adopted for the preferred combination of charge enhancers and the preferred ratio when combined.

[0160] In the masterbatch of the present disclosure, the total amount of the charge enhancer is greater than 5.0% by mass and less than 50% by mass relative to the thermoplastic resin. The total amount is more preferably greater than 10% by mass, further preferably greater than 15% by mass, and more preferably less than 40% by mass, further preferably less than 30% by mass.

[0161] The masterbatch of the present disclosure may contain other components as necessary. Examples of other components include the same components as those that can be contained in the electret material of the present disclosure.

[0162] The masterbatch of the present disclosure may be electret-free or electret-free.

[0163] The masterbatch of the present disclosure can be prepared by mixing the thermoplastic resin, the charge enhancer, and other components as necessary. The mixing can be performed using a single-screw or twin-screw extruder, an open mill, a kneader, a Banbury mixer, and the like.

[0164] The masterbatch disclosed in the present invention may be in any form such as powder, granules, pellets, etc., but is preferably a pellet obtained by melt kneading from the viewpoint of maintaining the charge enhancer in a finely dispersed state in the thermoplastic resin.

[0165] The melt kneading temperature is preferably higher than the melting point of the thermoplastic resin, and more preferably 5° C. or more higher than the melting point of the thermoplastic resin.

[0166] The masterbatch of the present disclosure is used to manufacture an electret material. The masterbatch can be used to manufacture an electret material comprising a thermoplastic resin and a charge enhancer contained in the thermoplastic resin, and is preferably used to manufacture the electret material of the present disclosure.

[0167] Example

[0168] Next, the present disclosure will be described in more detail with reference to examples, but the present disclosure is not limited to these examples.

[0169] In Examples and Comparative Examples, the following raw materials were used.

[0170] <Thermoplastic resin>

[0171] Polypropylene (PP) (MFR: 1500g / 10min)

[0172] <Fluorine-based charge enhancer>

[0173] PTFE: Low molecular weight PTFE (average particle size: 4 μm, melt viscosity: 5.0×10 4 Pa·s, melting point: 329°C).

[0174] VdF polymer 1: VdF / TFE copolymer (VdF / TFE (molar ratio) = 81 / 19, weight average molecular weight: 1,300,000).

[0175] VdF polymer 2: a mixture of PVdF (weight average molecular weight: 1,850,000) and a VdF / TFE copolymer (VdF / TFE (molar ratio) = 81 / 19, weight average molecular weight: 1,300,000)) in a mass ratio of 75 / 25.

[0176] <Hydrocarbon-based charge enhancer>

[0177] Metal soap 1: magnesium stearate (StMg)

[0178] Metal soap 2: calcium stearate

[0179] Low molecular weight amide compound 1: Ethylene bisstearamide (EBS)

[0180] Low molecular weight amide compound 2: stearic acid amide

[0181] Hindered amine compounds: poly[(6-(1,1,3,3-tetramethylbutyl)imino-1,3,5-triazine-2,4-diyl)((2,2,6,6-tetramethyl-4-piperidinyl)imino)hexamethylene((2,2,6,6-tetramethyl-4-piperidinyl)imino)]

[0182] Transparent agent: 1,3:2,4-Bis-O-(4-methylbenzylidene)-D-sorbitol

[0183] Various physical properties were measured by the following methods.

[0184] <Surface measurement by XPS (X-ray photoelectron spectroscopy)>

[0185] The surface of the obtained electret fiber sheet was measured by XPS (X-ray photoelectron spectroscopy) using the following method. ESCA3400 (manufactured by SHIMADZU) was used for the measurement. The radiation source used MgKα radiation (1253.6 eV) and the measurement was performed under the conditions of a measurement area diameter of about 3 mm and a detection depth of about 7 nm (photoelectron extraction angle of 90°).

[0186] [Ratio (F / C)]

[0187] The calculation was performed by the following method using the value measured by XPS (X-ray photoelectron spectroscopy).

[0188] Ratio (F / C) = A / B

[0189] A: Peak area value of F element

[0190] B: Peak area value of C element

[0191] <Collection Performance Evaluation>

[0192] The electret fiber sheet was stored in a constant temperature and humidity chamber (temperature 38° C., humidity 85%) for 25 hours, and then the collection performance was evaluated under the following conditions.

[0193] (Pressure loss)

[0194] The electret fiber sheet was placed on an effective area of ​​65 cm 2 The filter holder was fixed, the inlet side was pressurized with a compressor, and the air permeation flow rate was adjusted to 9.6 cm / sec with a flow meter. The pressure loss at this time was then measured with a pressure gauge.

[0195] (Collection efficiency of NaCl particles with a particle size of 0.3 μm)

[0196] According to the method described in JIS B9928 Annex 5 (regulation) "NaCl aerosol generation method (pressurized spray method)", the NaCl particles generated by the sprayer were classified into a particle size of 0.3 μm using an electrostatic classifier (manufactured by TSI), and the particles were charged and neutralized using americium 241. The permeation flow rate was adjusted to 9.6 cm / sec, and the number of particles on the front and rear sides of the fiber sheet as the measurement sample was obtained using a particle counter (manufactured by TSI, CNC), and the collection efficiency was calculated using the following formula. It should be noted that the initial value of the collection efficiency was measured using the fiber sheet in an unused state.

[0197] Transmittance (%) = (CO / CI) × 100

[0198] Collection efficiency (%) = 100 - transmittance (%)

[0199] CO = the number of NaCl particles 0.3 μm counted on the downstream side of the measurement sample (the rear side of the fiber sheet)

[0200] CI = the number of NaCl particles 0.3 μm counted on the upstream side of the measurement sample (front side of the fiber sheet)

[0201] (PF value of NaCl particles with a particle size of 0.3 μm)

[0202] Using NaCl particles with a particle size of 0.3 μm, the PF value was determined according to the following formula from the pressure loss and collection efficiency (collection efficiency of NaCl particles with a particle size of 0.3 μm) of the electret fiber sheet.

[0203] PF value = {-log ((100-collection efficiency (%)) / 100)} / (pressure loss (Pa) / 1000)

[0204] Examples 1 to 18

[0205] [Production of masterbatch]

[0206] PP and the charge enhancer listed in Table 1 or 2 were mixed so that the total amount of the charge enhancer was 10% by mass relative to PP, and the mixture was fed into a twin-screw extruder (Torque Rheometer (LABOPLASTOMILL) 30C150, manufactured by Toyo Seiki Seisaku-sho, Ltd.) and melt-kneaded to obtain masterbatch pellets.

[0207] [Production of electret fiber sheets]

[0208] PP and the masterbatch prepared above were mixed so that the charge enhancer was mixed in the amount described in Table 1 or 2 relative to 100 parts by mass of PP, and the mixture was fed into the raw material feed hopper of the spinning machine. The mixture was sprayed by melt-blowing using a die (hole pitch: 0.9 mm, number of holes: 275 holes, width: 250 mm) in which discharge holes with a diameter of 0.2 mm were arranged in a straight line at intervals, at a polymer discharge rate of 500 g / hour, a nozzle temperature of 220°C, and an air pressure of 0.15 MPa. The speed of the collecting conveyor was adjusted to obtain a basis weight of 25 g / m 2 The obtained meltblown nonwoven fabric sheet was subjected to corona charging treatment to obtain an electret fiber sheet. The obtained electret fiber sheet was evaluated using the above method. The results are shown in Tables 1 and 2.

[0209] Comparative Example 1

[0210] Using only PP, an electret fiber sheet was prepared in the same manner as in Example 1 and evaluated. The results are shown in Table 1.

[0211] Comparative Examples 2 to 5

[0212] The electret fiber sheets were prepared and evaluated in the same manner as in Example except that the charge enhancers listed in Table 1 were used. The results are shown in Table 1.

[0213]

[0214]

Claims

1. An electret material comprising a thermoplastic resin and a charge enhancer contained in the thermoplastic resin, wherein: The charge enhancer includes at least one fluorine-based charge enhancer selected from the group consisting of polytetrafluoroethylene and vinylidene fluoride polymers, and at least one hydrocarbon-based charge enhancer.

2. The electret material according to claim 1, wherein The fluorine-based charge enhancer is a low molecular weight polytetrafluoroethylene and a vinylidene fluoride polymer.

3. The electret material according to claim 1 or 2, wherein: The vinylidene fluoride polymer is at least one selected from the group consisting of polyvinylidene fluoride and a vinylidene fluoride / tetrafluoroethylene copolymer.

4. The electret material according to any one of claims 1 to 3, wherein The hydrocarbon-based charge enhancer is at least one selected from the group consisting of metal soaps, hindered amine compounds, triazine compounds, transparentizing agents, and low-molecular amide compounds.

5. The electret material according to any one of claims 1 to 4, wherein The hydrocarbon-based charge enhancer is a metal soap and a low-molecular amide compound.

6. The electret material according to claim 4 or 5, wherein: The metal soap is a metal salt of Group 2 of the Periodic Table of Fatty Acids.

7. The electret material according to any one of claims 4 to 6, wherein The low molecular weight amide compound is at least one selected from the group consisting of fatty acid amide and fatty acid bisamide.

8. The electret material according to any one of claims 1 to 7, wherein The mass ratio of the fluorine-based charge enhancer to the hydrocarbon-based charge enhancer, ie, fluorine-based / hydrocarbon-based, is 1 / 99 to 99 / 1.

9. The electret material according to any one of claims 1 to 8, wherein The thermoplastic resin is a polyolefin resin.

10. The electret material according to any one of claims 1 to 9, wherein The ratio F / C of the F element content to the C element content on the surface of the electret material measured by X-ray photoelectron spectroscopy XPS is 0.20% or less.

11. The electret material according to any one of claims 1 to 10, wherein The total amount of the charge enhancer is 0.01% by mass to 5.0% by mass based on the thermoplastic resin. 12 . The electret material according to claim 1 , which is a fiber sheet. 13 . A filter using the electret material according to claim 1 .

14. The filter according to claim 13, which is a filter for a dust mask.

15. A masterbatch for producing an electret material, wherein: The masterbatch comprises: a thermoplastic resin, and a charge enhancer contained in the thermoplastic resin. The charge enhancer comprises at least one fluorine-based charge enhancer selected from the group consisting of polytetrafluoroethylene and vinylidene fluoride polymers, and at least one hydrocarbon-based charge enhancer, The total amount of the charge enhancer is greater than 5.0% by mass and less than or equal to 50% by mass relative to the thermoplastic resin.