Thickened alkylated urethane copolymers

Thickened urethane copolymer prepared by double-branched alkyl Gelbert reaction solves the viscosity change and pigment compatibility problems during storage of aqueous coating compositions, and achieves viscosity stability and pigment compatibility The improvement in performance ensures the functional and aesthetic performance of the paint.

CN118891301APending Publication Date: 2024-11-01COATEX SA
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202380027781.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-18
Filing Date
2023-03-10
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The viscosity of existing aqueous coating compositions changes or decreases during storage, resulting in failure of functional characteristics, especially under a wide range of shear gradients, making it difficult to maintain stability and pigment compatibility, resulting in uneven color or fading.

Method used

Non-alkoxylated Guerbet alcohol prepared by bibranched alkylguerbet reaction as copolymer, combined with isocyanate compounds and polyhydroxy compounds for polymerization to form thickened urethane Copolymers for improving rheological characteristics and pigment compatibility.

Benefits of technology

Viscosity stability and pigment compatibility under a wide range of shear gradients are achieved, the viscosity loss of coating composition is prevented, the storage and application stability of the coating is improved, and the consistency of color and aesthetic effect is ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005043085420000111
    Figure BDA0005043085420000111
Patent Text Reader

Abstract

The present invention relates to thickened urethane copolymers prepared with non-alkoxylated Guerbet alcohols comprising double branched alkyl groups. The invention also relates to a method for preparing said copolymers and to the use thereof in aqueous compositions, in particular in coating compositions.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to thickened urethane copolymers prepared using non-alkoxylated Guerbet alcohols containing a doubly branched alkyl group. The present invention also relates to a process for preparing said copolymers and to their use in aqueous compositions, in particular in coating compositions.

[0002] Many technical fields require the use of aqueous compositions. Aqueous compositions include in particular aqueous hydraulic adhesive compositions, aqueous adhesive compositions, aqueous detergent compositions, aqueous cosmetic compositions, aqueous ink compositions, aqueous paper coating compositions, aqueous coating compositions, in particular aqueous varnish compositions or aqueous paint compositions, such as aqueous decorative paint compositions or aqueous industrial paint compositions. In addition to their functional properties, these aqueous compositions must also have a texture that is adapted to their use or their storage. In particular, they must have a suitable viscosity. In addition, it must be possible to use these aqueous compositions under very different conditions. In particular, the viscosity of these aqueous compositions may change or decrease. If the rheological behavior of these aqueous compositions is not adapted, for example to prevent sedimentation or phase separation phenomena during their storage, their functional properties may be altered as a result, which can also be manifested as a change in viscosity. Such changes or reductions are particularly harmful or destructive to aqueous hydraulic binder compositions, aqueous adhesive compositions, aqueous detergent compositions, aqueous cosmetic compositions, aqueous ink compositions, aqueous paper coating compositions, aqueous coating compositions, and especially aqueous varnish compositions or aqueous paint compositions.

[0003] Therefore, there is a need to have aqueous compositions which do not have these disadvantages or which do not cause these problems.

[0004] In particular, aqueous coating compositions, especially aqueous varnish compositions or aqueous paint compositions, which can have a viscosity adapted to maintain the uniformity and integrity of their functional properties are particularly useful. For a wide range of shear gradients, it should be possible to maintain the viscosity of these aqueous compositions and limit the loss of their viscosity.

[0005] Therefore, many aqueous coating compositions use rheology-modifying polymers. These polymers should be able to impart the desired rheological properties to the aqueous compositions over a wide range of shear rates. These polymers should also improve their shear thinning by imparting sufficient pseudoplastic behavior to these aqueous compositions, ensure stability and uniformity during their storage, facilitate their transfer to application tools, and help limit the appearance of droplets once applied. The compatibility of the various ingredients in the aqueous coating composition must also be considered. It is particularly important that the thickening copolymer has appropriate compatibility with the pigment and adhesive used.

[0006] It is also important to improve the pigment compatibility of aqueous coating compositions, especially paint compositions, especially for the addition of pigment concentrates for coloring. Without good pigment compatibility, the rheological properties of the composition can be severely degraded. Insufficient pigment compatibility can also lead to reduced tinting strength, resulting in uneven or faded color, which can lead to higher pigment usage or aesthetic defects in the final coating.

[0007] Document WO 2019091819 describes an aqueous composition comprising a surfactant compound and a polyurethane polymer prepared from a Guerbet alcohol obtained by condensing two linear alcohols. Document EP 1806386 describes a composition comprising two thickening polymers, the two thickening polymers being prepared by condensing a hydrophobic compound obtained by condensing two linear alcohols. Document WO 2022023621 describes a diurethane compound prepared from polyethoxylated Guerbet alcohols.

[0008] Known polymers used as thickeners do not always provide satisfactory solutions to these various problems. Therefore, there is a need for improved rheology-modifying copolymers. The copolymers according to the invention can provide solutions to all or part of the problems of the polymers of the prior art.

[0009] The present invention therefore provides a copolymer P which is prepared by polymerization of at least one of:

[0010] ● At least one isocyanate independently selected from diisocyanate compounds (a1), polyisocyanate compounds (a2) and combinations thereof

[0011] Ester compound (a);

[0012] ● at least one polyhydroxylated compound (b);

[0013] ● At least one compound (c) obtained by dimerization of two identical or different compounds of formula I via a Guerbet reaction:

[0014] R-CH[(CH2)mCH3]-(CH2) n -OH (I)

[0015] in:

[0016] - R independently represents a linear C4 to C9-alkyl group;

[0017] -m independently represents 0 or 1;

[0018] -n independently represents a number from 2 to 7.

[0019] Preferably, for the copolymer P according to the present invention, the isocyanate compound (a) is a diisocyanate compound (a1) selected from:

[0020] - Symmetrical aromatic diisocyanate compounds, preferably:

[0021] 2,2'-diphenylmethylene diisocyanate (2,2'-MDI) and 4,4'-diphenylmethylene diisocyanate (4,4'-MDI);

[0022] 4,4'-Dibenzyl diisocyanate (4,4'-DBDI);

[0023] 2,6-Toluene diisocyanate (2,6-TDI);

[0024] m-Xylylene diisocyanate (m-XDI);

[0025] - a symmetrical alicyclic diisocyanate compound, preferably methylenebis(4-cyclohexyl isocyanate) (H 12 MDI);

[0026] - Symmetrical aliphatic diisocyanate compounds, preferably hexamethylene diisocyanate (HDI), pentamethylene diisocyanate

[0027] Ester (PDI);

[0028] - an asymmetric aromatic diisocyanate compound, preferably:

[0029] 2,4'-Methylene diphenyl diisocyanate (2,4'-MDI);

[0030] 2,4'-Dibenzyl diisocyanate (2,4'-DBDI);

[0031] 2,4-Toluene diisocyanate (2,4-TDI);

[0032] - an asymmetric alicyclic diisocyanate compound, preferably isophorone diisocyanate (IPDI).

[0033] Preferably, according to the present invention, the compound (a1) is selected from IPDI, HDI, H 12 MDI and its combinations.

[0034] Also preferably, for the copolymer P according to the invention, the isocyanate compound (a) may be a polyisocyanate compound (a2) strictly comprising more than 2 isocyanate groups or more than 2.2 isocyanate groups or even more than 2.5 isocyanate groups. More preferably, the polyisocyanate compound (a2) comprises more than 2.6 isocyanate groups or more than 2.7 isocyanate groups or more than 3 isocyanate groups. Also more preferably, the polyisocyanate compound (a2) comprises 2.2 to 6 isocyanate groups, 2.2 to 4 isocyanate groups, 2.2 to 3.5 isocyanate groups, 2.5 to 6 isocyanate groups, 2.2 to 5 isocyanate groups, 2.5 to 4 isocyanate groups, 2.5 to 3.5 isocyanate groups, in particular 2.6 to 3.3 isocyanate groups.

[0035] Also preferably, the polyisocyanate compound (a2) is selected from:

[0036] ○Triphenylmethane-4,4',4"-triisocyanate or 1,1',1"-methylene tris(4-isocyanate benzene);

[0037] o Isocyanurate compounds, in particular isocyanurate compounds selected from the following compounds:

[0038] - Symmetrical aromatic diisocyanate compounds, preferably:

[0039] 2,2'-diphenylmethylene diisocyanate (2,2'-MDI) and 4,4'-diphenylmethylene diisocyanate (4,4'-MDI);

[0040] 4,4'-Dibenzyl diisocyanate (4,4'-DBDI);

[0041] 2,6-Toluene diisocyanate (2,6-TDI);

[0042] m-Xylylene diisocyanate (m-XDI);

[0043] - a symmetrical alicyclic diisocyanate compound, preferably methylenebis(4-cyclohexyl isocyanate) (H 12 MDI);

[0044] - Symmetrical aliphatic diisocyanate compounds, preferably hexamethylene diisocyanate (HDI) and pentamethylene diisocyanate (PDI);

[0045] - an asymmetric aromatic diisocyanate compound, preferably:

[0046] 2,4'-Methylene diphenyl diisocyanate (2,4'-MDI);

[0047] 2,4'-Dibenzyl diisocyanate (2,4'-DBDI);

[0048] 2,4-Toluene diisocyanate (2,4-TDI);

[0049] o Biuret trimer compounds, in particular biuret trimer compounds selected from the group consisting of:

[0050] - Symmetrical aromatic diisocyanate compounds, preferably:

[0051] 2,2'-diphenylmethylene diisocyanate (2,2'-MDI) and 4,4'-diphenylmethylene diisocyanate (4,4'-MDI);

[0052] 4,4'-Dibenzyl diisocyanate (4,4'-DBDI);

[0053] 2,6-Toluene diisocyanate (2,6-TDI);

[0054] m-Xylylene diisocyanate (m-XDI);

[0055] - a symmetrical alicyclic diisocyanate compound, preferably methylenebis(4-cyclohexyl isocyanate) (H 12 MDI);

[0056] - Symmetrical aliphatic diisocyanate compounds, preferably hexamethylene diisocyanate (HDI) and pentamethylene diisocyanate (PDI);

[0057] - an asymmetric aromatic diisocyanate compound, preferably:

[0058] 2,4'-Methylene diphenyl diisocyanate (2,4'-MDI);

[0059] 2,4'-Dibenzyl diisocyanate (2,4'-DBDI);

[0060] 2,4-Toluene diisocyanate (2,4-TDI);

[0061] - an asymmetric alicyclic diisocyanate compound, preferably isophorone diisocyanate (IPDI); preferably, the compound (a2) is selected from triphenylmethane-4,4',4"-triisocyanate, 1,1',1"-methylenetris(4-isocyanatebenzene), HDI isocyanurate, IPDI isocyanurate, PDI isocyanurate, HDI biuret trimer and IPDI biuret trimer, PDI biuret trimer.

[0062] Preferably, for the copolymer P according to the invention, the polyhydroxylated compound (b) is a compound (b1) of formula II:

[0063] HO-L p -OH (II)

[0064] in:

[0065] -L independently represents an oxyalkylene residue;

[0066] -p independently represents a number from 30 to 1000.

[0067] Preferably, for the copolymer P according to the invention, the polyhydroxylated compound (b) is a compound (b1) of formula II, wherein:

[0068] -L independently represents an oxyethylene residue; or

[0069] -p independently represents a number from 50 to 400, preferably a number from 100 to 300.

[0070] More preferably, for the copolymer P according to the invention, the polyhydroxylated compound (b) is a compound (b1) of formula II, wherein L independently represents an oxyethylene residue and p independently represents a number from 50 to 400, preferably a number from 100 to 300.

[0071] According to the present invention, the compound (b1) of formula II may be combined with a non-alkoxylated compound (b2) comprising at least three hydroxyl groups. Preferably, according to the present invention, the compound (b2) comprises three hydroxyl groups. More preferably, the compound (b2) is selected from glycerol, pentaerythritol and combinations thereof.

[0072] According to the present invention, the polyhydroxylated compound (b) may also be a polyethoxylated pentaerythritol or a polyalkoxylated compound (b3) comprising at least three hydroxyl groups. Preferably, according to the present invention, the compound (b3) is different from the compound (b2) and comprises three hydroxyl groups. More preferably, the compound (b3) is a polyethoxylated glycerol.

[0073] Advantageously, according to the invention, the copolymer P can be prepared using one or a combination of more than one of compound (b1), compound (b2) and compound (b3).

[0074] Preferably, according to the present invention, the compound (b), compound (b1) or compound (b3) independently have a molar mass (Mw) of 1500 g / mol to 40000 g / mol, preferably 2000 g / mol to 20000 g / mol, more preferably 2000 g / mol to 15000 g / mol or 2000 g / mol to 12000 g / mol measured by SEC. According to the present invention, the molar mass of the compound (b), compound (b1) or compound (b3) is measured by size exclusion chromatography (SEC), also referred to as "gel permeation chromatography" (GPC). This technology uses a "Waters" liquid chromatograph equipped with a detector. The detector is a "Waters" 2414 refractive index detector. The liquid chromatograph is equipped with two size exclusion columns to separate polymers or compounds of various molecular weights studied. The liquid elution phase is an organic phase comprising THF (HPLC grade, not stabilized). In the first step, about 25 mg of the compound was dissolved in 5 mL of THF, to which 0.1 mol% of water was added as an internal flow marker. The solution was then filtered through a 0.2 μm filter. 50 μL was then injected into the chromatographic instrument (eluent: THF, HPLC grade, not stabilized). The liquid chromatographic instrument had an isobaric pump ("Waters" 515), with a flow rate set to 0.3 ml / min. The chromatographic instrument also included a column oven, which included a column system arranged in sequence: an "Agilent" PLgelMiniMIX-A with a column length of 250 mm and a diameter of 4.6 mm, followed by an "Agilent" PLgel MiniMIX-B with a column length of 250 mm and a diameter of 4.6 mm. The detection system included a "Waters" 2414RI refractive index detector. The chromatographic column was maintained at a temperature of 35 ° C and the refractometer was heated to 35 ° C. The chromatographic instrument was calibrated using a polymethyl methacrylate standard ("EasiVial" PMMA) certified by the supplier "Agilent".

[0075] Basically, according to the present invention, the compound (c) is obtained by dimerization of two compounds of formula I. This dimerization is a Guerbet reaction carried out with the two alcohols of formula I. The dimerization reaction and the conditions for carrying it out are known per se. The Guerbet reaction is usually carried out at high temperature and pressure, in an alkaline medium and in the presence of a catalyst. The compound (c) can be prepared using the same compound of formula I or using two different compounds of formula I.

[0076] Preferably, according to the present invention, two identical compounds of formula I dimerize to produce a homodimer (c1). Also preferably, according to the present invention, the compound (c) is a homodimer (c1) obtained by dimerizing two identical compounds of formula I, wherein:

[0077] -R represents a straight-chain C5 to C7-alkyl group;

[0078] -m represents 0 or 1, preferably 0;

[0079] -n represents a number from 2 to 7.

[0080] More preferably, according to the present invention, the compound (c) is a homodimer (c1) obtained by dimerization of two identical compounds of formula I, wherein

[0081] - R represents a straight-chain C4 to C9-alkyl group, preferably a straight-chain C5 to C7-alkyl group;

[0082] -m represents 0 or 1, preferably 0;

[0083] -n represents a number from 5 to 7, preferably a number from 4 to 6, and more preferably 4 or 5.

[0084] Particularly preferably, according to the present invention, the dimerization is carried out using two different compounds of formula I and produces a mixture comprising 2 different homodimers (c1) and heterodimers (c2). Preferably, this is a mixture consisting of 2 different homodimers (c1) and heterodimers (c2). Also preferably, the mixture of compound (c) can be obtained by dimerization of two different compounds of formula I, wherein:

[0085] - R independently represents a linear C5 to C7-alkyl group;

[0086] -m independently represents 0 or 1, preferably 0;

[0087] -n independently represents a number from 2 to 7.

[0088] Preferably, according to the present invention, the mixture of compound (c) can be obtained by dimerization of two different compounds of formula I, wherein

[0089] - R independently represents a linear C4 to C9-alkyl group, preferably a linear C5 to C7-alkyl group;

[0090] -m independently represents 0 or 1, preferably 0;

[0091] -n independently represents a number from 5 to 7, preferably a number from 4 to 6, more preferably 4 or 5.

[0092] A preferred mixture of compounds (c) comprises a heterodimeric compound (c2) obtained by dimerization of a first compound of formula I in which R represents a linear C5-alkyl group, m represents 0 and n represents 5 and a different second compound of formula I in which R represents a linear C7-alkyl group, m represents 0 and n represents 4.

[0093] Particularly preferred mixtures of compounds (c) comprise:

[0094] - Heterodimer compounds (c2), obtained by dimerization of a first compound of formula I in which R represents a linear C5-alkyl group, m represents 0 and n represents 5, and a different second compound of formula I in which R represents a linear C7-alkyl group, m represents 0 and n represents 4.

[0095] a first homodimer (c1) obtained by dimerization of a compound of formula I, in which R represents a linear C5-alkyl group, m represents 0 and n represents 5;

[0096] a second homodimer (c1) obtained by dimerization of a different compound of the formula I in which R represents a linear C7-alkyl group, m represents 0 and n represents 4.

[0097] According to the present invention, the dimerization is carried out using two different compounds of formula I, which can produce a mixture containing two different homodimers (c1) and a heterodimer (c2).

[0098] When preparing copolymer P according to the present invention, the amount of compound (a), compound (b) and compound (c) can vary. Preferably, for copolymer P, the polymerization reaction uses relative to the total molar amount of monomer (a), monomer (b), monomer (c):

[0099] 10 mol% to 79.9 mol% or 10 mol% to 74.5 mol%, preferably 10 mol% to 68 mol% or 10 mol% to 60 mol% of monomer (a), or

[0100] 20 mol % to 89.9 mol % or 25 mol % to 89.5 mol %, preferably 30 mol % to 88 mol % or 35 mol % to 85 mol % of monomer (b), or

[0101] 0.1 to 70 mol % or 0.5 to 65 mol %, preferably 2 to 60 mol % or 5 to 55 mol %, of monomers (c).

[0102] Also preferably, according to the present invention, the polymerization reaction may use, relative to the total molar amount of monomer (a), monomer (b), monomer (c):

[0103] 10 mol % to 79.9 mol % or 10 mol % to 74.5 mol %, preferably 10 mol % to 68 mol % or 10 mol % to 60 mol % of monomer (a),

[0104] 20 mol % to 89.9 mol % or 25 mol % to 89.5 mol %, preferably 30 mol % to 88 mol % or 35 mol % to 85 mol % of monomer (b), and

[0105] 0.1 to 70 mol % or 0.5 to 65 mol %, preferably 2 to 60 mol % or 5 to 55 mol %, of monomers (c).

[0106] According to the present invention, the polymerization reaction may be carried out using only compound (a), compound (b) and compound (c), or using one or more than one other additional compound.

[0107] Therefore, the polymerization reaction may also use at least one hydrophobic compound (d) different from said compound (c), which is preferably chosen from compounds of formula (III):

[0108] R 1 -(EO) q -(PO) r -OH (III)

[0109] in:

[0110] -q and r, which are the same or different, independently represent an integer or decimal of 0 or less than 150, and q or r is different from 0;

[0111] -EO independently represents a CH2CH2O group;

[0112] -PO independently represents a group selected from CH(CH3)CH2O and CH2CH(CH3)O,

[0113] -R 1 independently represent a linear or branched C6 to C 40 -alkyl, phenyl, polyphenyl, preferably linear or branched C 10 To C 30 -alkyl, more preferably a straight chain or branched C 12 To C 22 -alkyl, or a group containing 2 to 5 phenyl groups or a tristyrylphenyl group or a pentastyrylcumylphenyl group, preferably, the polymerization reaction uses less than 20 mol %, preferably 0.05 mol % to 20 mol %, in particular 0.1 mol % to 10 mol % of compound (d), relative to the total molar amount of the compounds used.

[0114] The copolymers P according to the invention can be used in many technical fields, in particular as rheology control agents. They can be incorporated into different compositions. Therefore, the present invention provides a rheology control composition comprising at least one copolymer P according to the invention. The rheology control composition of the invention can be acid-treated to a pH below 8, preferably to a pH above 6. The treatment can be carried out with an acid, in particular a carboxylic acid, such as acetic acid or lactic acid.

[0115] The rheology control composition according to the invention may also contain at least one solvent, in particular water or a coalescing solvent, such as glycols, butyl glycol, diethylene glycol butyl ether, monopropylene glycol, ethylene glycol, diethylene glycol, the "Dowanol" product with CAS No. 34590-94-8, the "Texanol" product with CAS No. 25265-77-4; or in combination with at least one additive selected from amphiphilic compounds, in particular surfactant compounds, preferably hydroxylated surfactant compounds, such as alkyl-polyalkylene glycols, in particular alkyl-polyethylene glycol and alkyl-polypropylene glycol; polysaccharide derivatives, such as cyclodextrins, cyclodextrin derivatives, polyethers, alkyl-glycosides; hydrophilic compounds, defoamers, antimicrobial agents and combinations thereof.

[0116] The rheology control composition according to the invention is particularly suitable for facilitating the use of pigments, in particular organic pigments or mineral pigments, in aqueous media. It can be incorporated into specific pigment preparations. Thus, the invention provides an aqueous preparation comprising:

[0117] - at least one rheology-controlling composition according to the invention; optionally

[0118] at least one organic or mineral pigment or organic, organometallic or mineral particles, such as calcium carbonate, talc, kaolin, mica, silicates, silicon dioxide, metal oxides, in particular titanium dioxide, iron oxides; and optionally

[0119] - at least one agent selected from particle spacing agents, dispersants, steric stabilizers, electrostatic stabilizers, opacifiers, colorants, solvents, coalescing agents, defoamers, preservatives, antimicrobial agents, spreading agents, thickeners, film-forming copolymers and mixtures thereof.

[0120] Preferably, the preparation according to the invention is a coating preparation, in particular an ink preparation, a varnish preparation, an adhesive preparation, a paint preparation, for example a decorative paint preparation or an industrial paint preparation.

[0121] The copolymers P according to the invention can also be used in the printing sector, in particular textile printing. The invention therefore also provides a concentrated aqueous pigment paste comprising at least one copolymer P according to the invention and at least one colored organic pigment or colored mineral pigment.

[0122] The present invention also provides a method for controlling the viscosity of an aqueous composition, which comprises adding to the composition at least one copolymer P according to the invention. The viscosity control method according to the invention is used for an aqueous composition, which is an aqueous preparation according to the invention.

[0123] Advantageous, particular or preferred features of the copolymers P according to the invention define likewise advantageous, particular or preferred rheology-controlling compositions, aqueous preparations, pigment slurries and viscosity-controlling methods according to the invention.

[0124] The following examples illustrate various aspects of the invention. Example

[0125] Example 1: Preparation and characterization of copolymer (P1) according to the invention:

[0126] In a 3L glass reactor equipped with a mechanical stirring rod, a vacuum pump and a nitrogen inlet and heated with a double jacket using oil circulation, compound (b) (polyethylene glycol-molecular weight 10000 g / mol) (148.6 g) was introduced and heated to 95°C under vacuum. Under stirring and inert atmosphere, 200 ppm of a bismuth carboxylate type catalyst (K Kat B221) was added to the medium, and then compound (c) (prepared by dimerization of a compound of formula I in which R represents a linear C5-alkyl, m represents 0 and n represents 5 and a compound of formula I in which R represents a linear C7-alkyl, m represents 0 and n represents 4 by Guerbet reaction, non-ethoxylated-"Isofol" 2426S) (16.4 g) was added within 5 minutes. Then, diisocyanate compound (a1) (isophorone diisocyanate, IPDI) (9.9 g) was introduced with a syringe under stirring at 150 rpm. The reaction was continued at 100°C for 1 hour.

[0127] The isocyanate level is then checked by reverse measurement to ensure that it is zero. Collect 1 gram of reaction medium and add excess dibutylamine (e.g. 1 mole), which can react with any isocyanate groups that may be present in the medium. Then analyze any unreacted dibutylamine with hydrochloric acid (e.g. 1 equivalent concentration). The number of isocyanate groups present in the reaction medium can then be inferred. If this value is not zero, the reaction continues with a cycle of 15 minutes until the reaction is complete. When the level reaches zero, a copolymer P1 is obtained, which comprises 14 mol % of compound a, 43 mol % of compound b and 43 mol % of compound c. It is formulated with an ethoxylated alcohol surfactant compound ("Emulan" HE 51 "Basf") (95g), 1000ppm of an antimicrobial agent ("Biopol" SMV "Chemipol"), 1000ppm of a defoamer ("Tego" 1488 "Evonik") and water (730g). An aqueous composition consisting of 17.5% by mass of the copolymer P1 according to the invention, 9.5% by mass of a surfactant compound and 73% by mass of water was obtained.

[0128] Example 2: Preparation and characterization of an aqueous paint formulation according to the invention:

[0129] The matt paint formulation according to the invention was prepared by mixing the various ingredients with stirring. The compounds and the amounts (g) used are listed in Table 1.

[0130] Ingredients in Matte Paint Preparations Dosage(g) "Ecodis" P50 ("Coatex" dispersant) 2.00 "Tego" 810 ("Tego" defoamer) 0.51 "Acticide" MBS ("Thor" fungicide) 1.00 <![CDATA["Tiona”568("Tronox”TiO2)]]> 40.01 <![CDATA["Omyacoat”850OG("Omya”CaCO3)]]> 110.00 <![CDATA["Durcal”2AV("Omya”CaCO3)]]> 150.29 "Acronal" S790 ("Basf" adhesive) 65.00 Monopropylene glycol 5.06 "Texanol" ("Eastman" film former) 5.02 NaOH (20% in water) 0.41 Aqueous compositions of copolymers P1 according to the invention 6.29 water 114.41 total 500.00

[0131] Table 1

[0132] The paint formulation was then pigmented by adding 5% by weight of black pigment ("Colanyl" N500 black "Clariant") to give formulation F1 according to the invention.

[0133] Then, for formulation F1, the following data were measured at 25°C:

[0134] Brookfield viscosity at 10 rpm (μB10, mPa.s);

[0135] Brookfield viscosity at 100 rpm (μB100, mPa.s);

[0136] Cone-and-plate viscosity or ICI viscosity measured under high shear gradient (μI, mPa.s);

[0137] Stormer viscosity (μS, Krebs units or KUs) measured under moderate shear gradient using a reference modulus.

[0138] The results were measured immediately after the addition of the black pigment (T=0) and 24 hours after the addition (T=24 hours).

[0139] The pigment compatibility of formulation F1 was assessed on dried paint coatings. The color of the initially white paint was obtained by adding 5% by weight of a colorant based on a black pigment ("Colanyl" N500 black "Clariant"), relative to the white paint formulation.

[0140] The rub-out test is known per se and involves rubbing a 150 micron thick wet colored paint layer on a comparison chart with a finger. This may expose a small portion of the surface of the newly applied colored paint layer to the shearing effect generated by the circular motion of the finger. The shearing effect may change the stability and distribution of the colored pigments in the matrix consisting of the colored paint layer, thereby changing the color intensity of the sheared area.

[0141] When the pigmented paint layer was dry, the color difference between the initial sheared area and the unsheared area of ​​the pigmented paint layer was measured using a "Byk" Spectro-Guide Sphere Gloss spectrophotometer.

[0142] The color difference is quantified by a ΔE value calculated from the known measured parameters corresponding to the L*a*b* color space. Low ΔE values ​​indicate a reduced color difference between sheared and unclipped areas, thus improving pigment compatibility.

[0143] The unsheared area of ​​the colored paint was also measured according to one of the parameters of the L*a*b* color space. The parameter L* quantifies the color intensity. Low L* values ​​indicate reduced lightness and therefore higher black intensity, corresponding to improved pigment compatibility of the paint formulations evaluated using the copolymers according to the present invention. The results are shown in Table 2.

[0144]

[0145] Table 2

[0146] For the formulation F1 according to the invention, the copolymers according to the invention make it possible to control the viscosity of the various ingredients both after preparation and over time. The copolymers according to the invention impart good pigment compatibility to the paint formulation.

Claims

1. A copolymer P prepared by polymerization of at least one of the following: ● at least one isocyanate compound (a) independently selected from diisocyanate compounds (a1), polyisocyanate compounds (a2) and combinations thereof; ● at least one polyhydroxylated compound (b); ● At least one compound (c) obtained by dimerization of two identical or different compounds of formula I via a Guerbet reaction: R-CH(CH 2 ) m CH 3 ]-(CH 2 ) n -OH (I) in: -R independently represents a straight chain C 4 To C 9 -alkyl; -m independently represents 0 or 1; -n independently represents a number from 2 to 7.

2. The copolymer P according to claim 1, wherein the isocyanate compound (a) is: ● A diisocyanate compound (a1) selected from: - Symmetrical aromatic diisocyanate compounds, preferably: 2,2'-diphenylmethylene diisocyanate (2,2'-MDI) and 4,4'-diphenylmethylene diisocyanate (4,4'-MDI); 4,4'-Dibenzyl diisocyanate (4,4'-DBDI); 2,6-Toluene diisocyanate (2,6-TDI); m-Xylylene diisocyanate (m-XDI); - a symmetrical alicyclic diisocyanate compound, preferably methylenebis(4-cyclohexyl isocyanate) (H 12 MDI); - Symmetrical aliphatic diisocyanate compounds, preferably hexamethylene diisocyanate (HDI) and pentamethylene diisocyanate (PDI); - an asymmetric aromatic diisocyanate compound, preferably: 2,4'-Methylene diphenyl diisocyanate (2,4'-MDI); 2,4'-Dibenzyl diisocyanate (2,4'-DBDI); 2,4-Toluene diisocyanate (2,4-TDI); - an asymmetric alicyclic diisocyanate compound, preferably isophorone diisocyanate (IPDI), Preferably, the compound (a1) is selected from IPDI, HDI, H 12 MDI and its combination; or a polyisocyanate compound (a2) which strictly comprises more than 2 isocyanate groups or more than 2.2 isocyanate groups or even more than 2.5 isocyanate groups; preferably, the polyisocyanate compound (a2) comprises more than 2.6 isocyanate groups or more than 2.7 isocyanate groups or more than 3 isocyanate groups; more preferably, the polyisocyanate compound (a2) comprises 2.2 to 6 isocyanate groups, 2.2 to 4 isocyanate groups, 2.2 to 3.5 isocyanate groups, 2.5 to 6 isocyanate groups, 2.2 to 5 isocyanate groups, 2.5 to 4 isocyanate groups, 2.5 to 3.5 isocyanate groups, in particular 2.6 to 3.3 isocyanate groups; or a polyisocyanate compound (a2) which is selected from: ○Triphenylmethane-4,4',4"-triisocyanate or 1,1',1"-methylene tris(4-isocyanate benzene); ● Isocyanurate compounds, in particular isocyanurate compounds selected from the following compounds: - Symmetrical aromatic diisocyanate compounds, preferably: 2,2'-diphenylmethylene diisocyanate (2,2'-MDI) and 4,4'-diphenylmethylene diisocyanate (4,4'-MDI); 4,4'-Dibenzyl diisocyanate (4,4'-DBDI); 2,6-Toluene diisocyanate (2,6-TDI); m-Xylylene diisocyanate (m-XDI); - a symmetrical alicyclic diisocyanate compound, preferably methylenebis(4-cyclohexyl isocyanate) (H 12 MDI); - Symmetrical aliphatic diisocyanate compounds, preferably hexamethylene diisocyanate (HDI) and pentamethylene diisocyanate (PDI); - an asymmetric aromatic diisocyanate compound, preferably: 2,4'-Methylene diphenyl diisocyanate (2,4'-MDI); 2,4'-Dibenzyl diisocyanate (2,4'-DBDI); 2,4-Toluene diisocyanate (2,4-TDI); o Biuret trimer compounds, in particular biuret trimer compounds selected from the group consisting of: - Symmetrical aromatic diisocyanate compounds, preferably: 2,2'-diphenylmethylene diisocyanate (2,2'-MDI) and 4,4'-diphenylmethylene diisocyanate (4,4'-MDI); 4,4'-Dibenzyl diisocyanate (4,4'-DBDI); 2,6-Toluene diisocyanate (2,6-TDI); m-Xylylene diisocyanate (m-XDI); - a symmetrical alicyclic diisocyanate compound, preferably methylenebis(4-cyclohexyl isocyanate) (H 12 MDI); - Symmetrical aliphatic diisocyanate compounds, preferably hexamethylene diisocyanate (HDI) and pentamethylene diisocyanate (PDI); - an asymmetric aromatic diisocyanate compound, preferably: 2,4'-Methylene diphenyl diisocyanate (2,4'-MDI); 2,4'-Dibenzyl diisocyanate (2,4'-DBDI); 2,4-Toluene diisocyanate (2,4-TDI); - an asymmetric alicyclic diisocyanate compound, preferably isophorone diisocyanate (IPDI); preferably, the compound (a2) is selected from triphenylmethane-4,4',4"-triisocyanate, 1,1',1"-methylenetris(4-isocyanatebenzene), HDI isocyanurate, IPDI isocyanurate, PDI isocyanurate, HDI biuret trimer and IPDI biuret trimer, PDI biuret trimer.

3. The copolymer P according to any one of claims 1 or 2, wherein the polyhydroxylated compound (b) is selected from: ●Compound (b1) of formula II: HO-L p -OH (II) in: -L independently represents an oxyalkylene residue; -p independently represents a number from 30 to 1000; A compound (b1) of formula II in combination with a non-alkoxylated compound (b2) comprising at least three hydroxyl groups; A polyalkoxylated compound (b3) comprising at least three hydroxyl groups; ●Their combination.

4. The copolymer P according to any one of claims 1 to 3, wherein the compound (b) is selected from: ● a compound (b1) of formula II, in: -L independently represents an oxyethylene residue; or - p independently represents a number from 50 to 400, preferably a number from 100 to 300; or - L independently represents an oxyethylene residue, and p independently represents a number from 50 to 400, preferably a number from 100 to 300; A compound (b2) comprising three hydroxyl groups, which is preferably selected from glycerol, pentaerythritol and combinations thereof; • Polyethoxylated pentaerythritol or a compound (b3) different from said compound (b2) and comprising three hydroxyl groups, preferably, compound (b3) is polyethoxylated glycerol.

5. The copolymer P according to any one of claims 1 to 4, wherein the compound (b), compound (b1) or compound (b3) independently has a molar mass (Mw) measured by SEC of 1500 to 40000 g / mol, preferably 2000 to 20000 g / mol, more preferably 2000 to 15000 g / mol or 2000 to 12000 g / mol.

6. The copolymer P according to any one of claims 1 to 5, in: ● two identical compounds of formula I dimerize to produce a homodimer (c1); or ●Compound (c) is a homodimer (c1) obtained by dimerization of two identical compounds of formula I, wherein: -R represents straight chain C 5 To C 7 -alkyl; -m represents 0 or 1, preferably 0; -n represents a number from 2 to 7; or ●Compound (c) is a homodimer (c1) obtained by dimerization of two identical compounds of formula I, wherein: -R represents straight chain C 4 To C 9 -alkyl, preferably straight chain C 5 To C 7 -alkyl; -m represents 0 or 1, preferably 0; -n represents a number from 5 to 7, preferably a number from 4 to 6, and more preferably 4 or 5.

7. The copolymer P according to any one of claims 1 to 5, in: ● two different compounds of formula I dimerize to produce a mixture comprising two different homodimers (c1) and a heterodimer (c2); or A mixture of compounds (c) obtained by dimerization of two different compounds of formula I, wherein: -R independently represents a straight chain C 5 To C 7 -alkyl; -m independently represents 0 or 1, preferably 0; -n independently represents a number from 2 to 7; or A mixture of compounds (c) obtained by dimerization of two different compounds of formula I, wherein: -R independently represents a straight chain C 4 To C 9 -alkyl, preferably straight chain C 5 To C 7 -alkyl; -m independently represents 0 or 1, preferably 0; - n independently represents a number from 5 to 7, preferably a number from 4 to 6, more preferably 4 or 5; or ● The mixture of compound (c) comprises a heterodimeric compound (c2) consisting of wherein R represents a linear C 5 -alkyl, m represents 0 and n represents 5, and the first compound of formula I wherein R represents a straight chain C 7 -alkyl, m represents 0 and n represents 4, and a second compound of formula I is obtained by dimerization; or A mixture of compound (c) comprising: ○ Heterodimer compound (c2), wherein R represents a linear C 5 -alkyl, m represents 0 and n represents 5, and the first compound of formula I wherein R represents a straight chain C 7 -alkyl, m represents 0 and n represents 4, and a second compound of formula I is dimerized to give, ○ The first homodimer (c1) obtained by dimerization of the compound of formula I, wherein R represents a linear C 5 -alkyl, m represents 0 and n represents 5, o A second homodimer (c1) obtained by dimerization of a different compound of formula I, wherein R represents a linear C 7 -alkyl, m represents 0 and n represents 4.

8. The copolymer P according to any one of claims 1 to 7, wherein the polymerization reaction uses, relative to the total molar amount of monomer (a), monomer (b) and monomer (c): 10 mol% to 79.9 mol% or 10 mol% to 74.5 mol%, preferably 10 mol% to 68 mol% or 10 mol% to 60 mol% of monomer (a), or 20 mol % to 89.9 mol % or 25 mol % to 89.5 mol %, preferably 30 mol % to 88 mol % or 35 mol % to 85 mol % of monomer (b), or 0.1 to 70 mol % or 0.5 to 65 mol %, preferably 2 to 60 mol % or 5 to 55 mol %, of monomers (c).

9. The copolymer P according to any one of claims 1 to 8, wherein the polymerization reaction also uses at least one hydrophobic compound (d) different from compound (c), which is preferably selected from compounds of formula (III): R 1 -(EO) q -(PO) r -OH(III) in: -q and r, the same or different, independently represent an integer or decimal of 0 or less than 150, q or r is different from 0, -EO independently represents CH 2 CH 2 O group, -PO independently represents a 3 )CH 2 O and CH 2 CH(CH 3 )O group, -R 1 Independently represents a straight or branched chain C 6 To C 40 -alkyl, phenyl, polyphenyl, preferably linear or branched C 10 To C 30 -alkyl, more preferably a straight chain or branched C 12 To C 22 -alkyl, or a group containing 2 to 5 phenyl groups or a tristyrylphenyl group or a pentastyrylcumylphenyl group, preferably, the polymerization reaction uses less than 20 mol %, preferably 0.05 mol % to 20 mol %, in particular 0.1 mol % to 10 mol % of compound (d), relative to the total molar amount of the compounds used.

10. A rheology control composition comprising at least one copolymer P according to any one of claims 1 to 9, optionally acid-treated to a pH below 8, preferably to a pH above 6, for example using an acid, in particular a carboxylic acid such as acetic acid or lactic acid.

11. The rheology control composition according to claim 10, further comprising at least one solvent, in particular water or a coalescing solvent, such as glycols, butyl glycol, diethylene glycol butyl ether, monopropylene glycol, ethylene glycol, diethylene glycol, the "Dowanol" product with CAS No. 34590-94-8, the "Texanol" product with CAS No. 25265-77-4; or in combination with at least one additive selected from amphiphilic compounds, in particular surfactant compounds, preferably hydroxylated surfactant compounds, such as alkyl-polyalkylene glycols, in particular alkyl-polyethylene glycol and alkyl-polypropylene glycol; polysaccharide derivatives, such as cyclodextrins, cyclodextrin derivatives, polyethers, alkyl-glycosides; hydrophilic compounds, defoamers, antimicrobial agents and combinations thereof.

12. An aqueous formulation comprising: - at least one composition according to any one of claims 10 or 11; optionally at least one organic or mineral pigment or organic, organometallic or mineral particles, such as calcium carbonate, talc, kaolin, mica, silicates, silicon dioxide, metal oxides, in particular titanium dioxide, iron oxides; and optionally - at least one agent selected from particle spacing agents, dispersants, steric stabilizers, electrostatic stabilizers, opacifiers, colorants, solvents, coalescing agents, defoamers, preservatives, antimicrobial agents, spreading agents, thickeners, film-forming copolymers and mixtures thereof.

13. The preparation according to claim 12, which is a coating preparation, in particular an ink preparation, a varnish preparation, an adhesive preparation, a paint preparation, for example a decorative paint preparation or an industrial paint preparation.

14. A concentrated aqueous pigment slurry comprising at least one copolymer P according to any one of claims 1 to 9 and at least one coloured organic pigment or coloured mineral pigment.

15. A method for controlling the viscosity of an aqueous composition, comprising adding to the composition at least one copolymer P according to any one of claims 1 to 9.

16. A method according to claim 15, wherein the aqueous composition is an aqueous formulation as defined in any one of claims 12 or 13.

Citation Information

Patent Citations

  • Polymeric additives for reducing the viscosity loss on tinting