Silicone release polyester film and method of making same

By using the release layer of the silicone aqueous dispersion of platinum-based catalyst and crosslinking reaction inhibitor in the ceramic capacitor, the problem of high fracture and defect rate of ceramic green sheets during the peeling process is solved, and light peeling and uniformity are achieved , reduces cost and safety risks and meets the high reliability needs of ceramic capacitors.

CN118891315APending Publication Date: 2024-11-01TOYOBO CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380027877.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-28
Filing Date
2023-03-15
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The release film of existing ceramic capacitors can easily lead to the cracking and failure rate of ceramic green sheets during the peeling process. The traditional method has high cost and safety risks, and the uniform coating ability is poor, making it difficult to meet the high reliability requirements of ceramic green sheets. .

Method used

The coating composition for mold release of aqueous dispersions with specific silicone crosslinking reaction catalysts and inhibitors is used to form a coating layer with a platinum-based catalyst content between 120 ppm and 600 ppm, and the peel strength and uniformity are adjusted through the crosslinking reaction, using Water is used as a solvent to avoid the use of organic solvents.

Benefits of technology

The light peelability and uniformity of the ceramic green sheets in ceramic capacitors are achieved, the peel strength is reduced, the molding quality and production efficiency of the ceramic green sheets are improved, and the safety and cost problems are avoided due to the use of organic solvents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005044023960000181
    Figure BDA0005044023960000181
  • Figure BDA0005044023960000191
    Figure BDA0005044023960000191
  • Figure BDA0005044023960000201
    Figure BDA0005044023960000201
Patent Text Reader

Abstract

The purpose of the present invention is to provide: a silicone release polyester film having excellent light release properties and layer uniformity; a method for producing the silicone release polyester film; and the like. A silicone mold release polyester film having a coating layer on at least one surface of a polyester film, the coating layer being formed using a mold release coating composition of an aqueous dispersion, the coating composition for mold release of the aqueous dispersion includes an aqueous dispersion of an alkenyl group-containing silicone, an aqueous dispersion of a silicone having a hydrogen atom directly bonded to an Si atom represented by an Si-H group, and a platinum-based catalyst, the amount of elemental platinum in the platinum-based catalyst being more than 120 ppm but less than 600 ppm with respect to the weight of the alkenyl group-containing silicone. The platinum-based catalysts include a platinum-based catalyst containing a crosslinking reaction inhibitor and a platinum-based catalyst not containing a crosslinking reaction inhibitor, and the thickness of the coating layer is 5 nm or more and 70 nm or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a silicone release polyester film. More specifically, it relates to a silicone release polyester film having light peelability that is most suitable for molding ceramic green sheets used in manufacturing laminated ceramic capacitors and can prevent peeling of ceramic green sheets, cracking of sheets during lamination, and the generation of pinholes, and a method for producing the same, as well as a protected body formed by laminating the silicone release polyester film. Background Art

[0002] In the manufacture of multilayer ceramic capacitors, a release film is used as a carrier film for molding ceramic green sheets. As the base material of the release film, polyester film is used, especially in terms of dimensional stability and heat resistance. In recent years, the miniaturization and high capacity of multilayer ceramic capacitors have been promoted, while on the other hand, high reliability is required for automotive use, and the demand for improved quality of ceramic green sheets has gradually increased.

[0003] With the thinning and high reliability of ceramic green sheets, the thickness of the sheets after drying has become less than a few μm. Therefore, the carrier film is particularly required to have easy peeling properties. However, due to the thinning, the rigidity of the ceramic green sheet decreases, and when the green sheet is peeled off with the peeling force of the existing release film, cracks and deformations will occur, and the chip defect rate will increase. Therefore, in order to avoid this, easy peeling properties are required.

[0004] Therefore, it is required to reduce the peeling force of the release film, and for example, a method of adjusting the peeling force by controlling the cross-linking structure of silicone has been proposed (for example, refer to Patent Document 1). However, such a method of controlling the cross-linking structure of the release layer requires a new design of a polymer or a cross-linking agent with a special structure, or sometimes requires stronger energy when irradiated with ultraviolet light or electron beams, which has the problem of increased costs. In addition, a release layer formed of a silicone resin with a cross-linking structure and a silicone resin without a cross-linking structure has been proposed (for example, refer to Patent Document 2). However, in this method, the solvent of the coating agent used to form the release layer is an organic solvent, so the organic solvent processing equipment during coating and drying becomes huge, and the operating cost of the volatilized organic solvent processing is also consumed, resulting in a problem of increased costs. Furthermore, there are problems with the working environment and safety issues such as explosions and fires of organic solvents.

[0005] In addition, a method without using an organic solvent has been proposed (for example, see Patent Document 3), but in this method, the operation becomes complicated due to the increase in the viscosity of the coating, and there is a problem that it is difficult to apply uniformly. In addition, a method based on a water-based silicone emulsion has been proposed (for example, see Patent Document 4), but in this method, the type of surfactant (or emulsifier) ​​used is not clearly shown, and no reaction inhibitor is used. Therefore, there is a problem that the stability of the emulsion is poor and uniform coating cannot be performed. In the thin filming of ceramic green sheets, the surface of the release layer is required to have very high uniformity, and these methods are not sufficient.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2006-7689

[0009] Patent Document 2: Japanese Patent Application Publication No. 2008-254207

[0010] Patent Document 3: Japanese Patent Application Publication No. 2003-192987

[0011] Patent Document 4: Japanese Patent Application No. 2009-518499 Summary of the invention

[0012] Problem that the invention aims to solve

[0013] In view of the above circumstances, an object of the present invention is to provide a silicone release polyester film having excellent easy release properties and uniformity of a release layer (film), a method for producing the same, and a protected body laminated with the silicone release polyester film.

[0014] Solutions for solving problems

[0015] The present inventors have conducted intensive research to solve the above-mentioned problems. As a result, they have found that the above-mentioned problems can be solved by using a specific organosilicon and a catalyst for the organosilicon cross-linking reaction and a cross-linking reaction inhibitor to maximize the cross-linking density during the release layer formation process, thereby completing the present invention.

[0016] That is, the present invention provides the following silicone release polyester film (silicone release polyester film).

[0017] [1] A silicone release polyester film having a coating layer (also referred to as "release layer" in this specification) on at least one side of the polyester film, wherein the coating layer is formed using a release coating composition in the form of an aqueous dispersion, wherein the release coating composition in the form of an aqueous dispersion comprises an aqueous dispersion of an alkenyl-containing silicone, an aqueous dispersion of an silicone having hydrogen atoms directly bonded to Si atoms represented by a Si-H group, and a platinum-based catalyst,

[0018] The amount of platinum in the platinum-based catalyst is more than 120 ppm and less than 600 ppm relative to the weight of the alkenyl-containing organosilicon.

[0019] The platinum-based catalysts include: platinum-based catalysts containing a cross-linking reaction inhibitor and platinum-based catalysts not containing a cross-linking reaction inhibitor.

[0020] The coating layer has a thickness of 5 nm to 70 nm.

[0021] [2] The silicone release polyester film according to [1], wherein the amount of platinum element (P0) of the platinum-based catalyst not containing a crosslinking reaction inhibitor is 50 ppm or more and less than 400 ppm relative to the weight of the alkenyl-containing silicone,

[0022] The amount of platinum element (P1) in the platinum-based catalyst containing the cross-linking reaction inhibitor is 40 ppm or more and less than 400 ppm based on the weight of the alkenyl group-containing silicone.

[0023] [3] The silicone release polyester film according to [1] or [2], wherein the platinum-based catalyst comprises the amount of platinum element (P0) of the platinum-based catalyst not containing a crosslinking reaction inhibitor and the amount of platinum element (P1) of the platinum-based catalyst containing a crosslinking reaction inhibitor,

[0024] The ratio (P0 / (P1+P0)) of the amount of platinum element (P0) of the platinum-based catalyst not containing a cross-linking reaction inhibitor to the total weight of platinum elements (P1+P0) is 0.3 or more and 0.8 or less.

[0025] [4] The silicone release polyester film according to any one of [1] to [3], wherein the alkenyl group of the alkenyl group-containing silicone is a vinyl group.

[0026] [5] The silicone release polyester film according to any one of [1] to [4], which is used for molding ceramic green sheets in the production of laminated ceramic capacitors.

[0027] Furthermore, the present invention provides the following protected objects.

[0028] [6] The above-mentioned protected body, wherein the silicone release polyester film described in any one of [1] to [5] is laminated on the protected body at the coating layer or the release layer.

[0029] [7] The protected body according to [6], wherein the protected body is a ceramic green sheet.

[0030] Furthermore, the present invention provides the following method for producing a silicone release polyester film.

[0031] [8] A method for producing a silicone release polyester film, comprising the following steps:

[0032] A coating layer is formed on at least one side of a polyester film using a mold release coating composition in the form of an aqueous dispersion, wherein the mold release coating composition comprises an aqueous dispersion of an alkenyl-containing silicone, an aqueous dispersion of silicone having hydrogen atoms directly bonded to Si atoms represented by Si-H groups, and a platinum-based catalyst.

[0033] The amount of platinum in the platinum-based catalyst is more than 120 ppm and less than 600 ppm relative to the weight of the alkenyl-containing organosilicon.

[0034] The platinum-based catalysts include: platinum-based catalysts containing a cross-linking reaction inhibitor and platinum-based catalysts not containing a cross-linking reaction inhibitor.

[0035] The coating layer has a thickness of 5 nm to 70 nm.

[0036] Effects of the Invention

[0037] The silicone release polyester film of the present invention has the above-mentioned structure, so it has a moderately low peel strength and excellent uniformity of the release layer. The silicone release polyester film of the present invention having the above-mentioned characteristics can be used as a carrier film for molding ceramic green sheets used in ceramic laminated capacitors.

[0038] Furthermore, since the protected body is laminated with the silicone release polyester film having the above-mentioned properties, it can be suitably used when, for example, a ceramic green sheet is used as the protected body.

[0039] Furthermore, the method for producing the silicone release polyester film of the present invention can efficiently and simply produce the silicone release polyester film having the above-mentioned properties. DETAILED DESCRIPTION

[0040] Hereinafter, embodiments of the present invention will be described in detail, but the present invention is not limited to these embodiments.

[0041] <Silicone release polyester film>

[0042] The silicone release polyester film of the present invention is a silicone release polyester film having a coating layer on at least one side of a polyester film, wherein the coating layer is formed using a water-dispersed release coating composition, wherein the water-dispersed release coating composition comprises a water dispersion of an alkenyl-containing silicone, a water dispersion of silicone having hydrogen atoms directly bonded to Si atoms represented by Si-H groups, and a platinum-based catalyst.

[0043] The amount of platinum in the platinum-based catalyst is more than 120 ppm and less than 600 ppm relative to the weight of the alkenyl-containing organosilicon.

[0044] The platinum-based catalysts include: platinum-based catalysts containing a cross-linking reaction inhibitor and platinum-based catalysts not containing a cross-linking reaction inhibitor.

[0045] The coating layer has a thickness of 5 nm to 70 nm.

[0046] 〔Polyester film〕

[0047] For the polyester film of the present invention, known polyesters can be suitably used. For example, the following polyesters can be suitably used.

[0048] (Polyester)

[0049] The polyester constituting the polyester film used as the substrate film (hereinafter, sometimes referred to as the substrate) in the present invention is not particularly limited, and a film formed by molding a polyester generally used as a substrate for a release film can be used. Preferably, a crystalline linear saturated polyester formed from an aromatic dibasic acid component and a diol component, such as polyethylene terephthalate, polyethylene isophthalate, polyethylene 2,6-naphthalate, polybutylene naphthalate, poly(1,4-cyclohexylene dimethylene terephthalate), polytrimethylene terephthalate, or a copolymer having the constituent components of these resins as the main component is further suitable. Among them, a polyester film formed from polyethylene terephthalate is particularly suitable. Polyethylene terephthalate is as follows: The repeating unit of ethylene terephthalate is preferably 90 mol% or more, more preferably 95 mol% or more, and other dicarboxylic acid components and diol components may also be copolymerized in small amounts. For example, from the aspect of cost, it is preferred to produce only from terephthalic acid and ethylene glycol.

[0050] Furthermore, known additives such as antioxidants, light stabilizers, ultraviolet absorbers, crystallizing agents, etc. may be added within the range not impairing the effects of the release film of the present invention. The polyester film is preferably a biaxially oriented polyester film because of the high elastic modulus in both directions.

[0051] The intrinsic viscosity of the polyester film is preferably 0.50 dl / g or more and 0.70 dl / g or less, more preferably 0.52 dl / g or more and 0.65 dl / g or less. When the intrinsic viscosity is 0.50 dl / g or more, it is preferred that no large amount of breakage occurs during the stretching process. On the contrary, when it is 0.70 dl / g or less, it is preferred that the cutting property when cutting into a specified product width is good and no dimensional defect occurs. In addition, the raw material pellets are preferably fully vacuum dried.

[0052] In addition, in this specification, when abbreviated as "polyester film", it means the polyester film which has a surface layer A and a surface layer B (laminated).

[0053] The method for producing the polyester film of the present invention is not particularly limited, and a conventionally commonly used method can be used. For example, the polyester is melted in an extruder, extruded into a film, cooled on a rotating cooling drum to obtain an unstretched film, and the unstretched film is biaxially stretched to obtain the film. The biaxially stretched film can be obtained by a method in which a uniaxially stretched film in the longitudinal or transverse direction is biaxially stretched in sequence in the transverse direction or longitudinal direction, or by a method in which an unstretched film is biaxially stretched in the longitudinal and transverse directions simultaneously.

[0054] In the present invention, the stretching temperature during stretching of the polyester film is preferably set to be equal to or higher than the secondary transition point (Tg) of the polyester. The film is preferably stretched by 1 to 8 times, particularly preferably by 2 to 6 times, in each of the longitudinal and transverse directions.

[0055] The thickness of the polyester film is preferably 12 μm or more and 100 μm or less, more preferably 16 μm or more and 50 μm or less, and more preferably 19 μm or more and 33 μm or less. If the thickness of the film is 12 μm or more, there is no worry about deformation due to heat during film production, processing, and molding, and it is preferred. On the other hand, if the thickness of the film is 100 μm or less, the amount of film discarded after use will not increase extremely, and it is preferred in terms of reducing the environmental load.

[0056] The polyester film substrate may be a single layer or a multilayer of two or more layers. For example, the substrate film may be a polyester film having a surface layer A substantially free of particles having a particle size of 1.0 μm or more and a surface layer B containing particles. Preferably, the surface layer A substantially does not contain inorganic particles having a particle size of 1.0 μm or more.

[0057] In this embodiment, particles with a particle size of 1 nm or more and less than 1.0 μm may be present in the surface layer A. The surface layer A substantially does not contain particles with a particle size of 1.0 μm or more, such as inorganic particles, thereby reducing the possibility of defects caused by the particle shape in the substrate being transferred to the resin sheet.

[0058] In one embodiment, by making the surface layer A not contain particles having a particle diameter of less than 1.0 μm, it is possible to more effectively suppress the transfer of the particle shape in the substrate to the resin sheet and the generation of defects.

[0059] In one embodiment, the polyester film substrate is preferably a laminated film having a surface layer A substantially free of inorganic particles on at least one surface. This can more effectively prevent the particle shape in the substrate from being transferred to the resin sheet and causing problems.

[0060] For example, the surface layer A that does not substantially contain particles having a particle size of less than 1.0 μm is preferably a form that does not substantially contain particles having a particle size of 1.0 μm or more.

[0061] Here, in the present invention, "substantially free of particles" means, for example, that in the case of inorganic particles smaller than 1.0 μm, when the inorganic elements are quantitatively analyzed by fluorescent X-ray analysis, the content is 50 ppm or less, preferably 10 ppm or less, and most preferably below the detection limit. This is because even if particles are not actively added to the film, there are cases where contamination components from foreign matter, dirt attached to production lines and devices in the raw resin or film manufacturing process are peeled off and mixed into the film. In addition, "substantially free of particles with a particle size of 1.0 μm or more" means that particles with a particle size of 1.0 μm or more are not actively included.

[0062] In the case of a laminated polyester film having a multilayer structure of two or more layers, it is preferred that a surface layer B containing inorganic particles and the like is provided on the opposite side of a surface layer A containing substantially no inorganic particles.

[0063] As a laminated structure, when the layer on one side of the coating release layer is set as the A layer, the layer on the opposite side is set as the B layer, and the core layer other than these is set as the C layer, the layer structure in the thickness direction can be cited as a laminated structure such as release layer / A / B or release layer / A / C / B. Of course, the C layer can also be a multilayer structure. In addition, the surface layer B may also not contain inorganic particles. In this case, in order to impart the slippage for winding the film into a roll, it is preferred that a coating layer containing at least inorganic particles and a binder is provided on the surface layer B.

[0064] In the polyester film substrate of the present invention, from the viewpoint of the slipperiness and easiness of exhaust of the film, the surface layer B on the opposite side of the surface to which the release layer is applied preferably contains inorganic particles, and silica particles and / or calcium carbonate particles are particularly preferably used. The content of the inorganic particles contained in the surface layer B preferably contains a total of 5000 ppm or more and 15000 ppm or less of the inorganic particles.

[0065] At this time, the regional surface average roughness (Sa) of the film of surface layer B is preferably in the range of more than 1nm and less than 40nm. More preferably, the range is more than 5nm and less than 35nm. When the total amount of silicon dioxide particles and / or calcium carbonate particles is more than 5000ppm and Sa is more than 1nm, when the film is rolled into a roll, air can be uniformly escaped, the winding form is good, and the planarity is good, thus, it is suitable for manufacturing ultra-thin layer ceramic green sheets. In addition, when the total amount of silicon dioxide particles and / or calcium carbonate particles is less than 15000ppm and Sa is less than 40nm, it is not easy to produce the aggregation of lubricants, and no coarse protrusions are formed, so that the quality of ultra-thin layer ceramic green sheets is stable and preferred during manufacturing.

[0066] As the particles contained in the above-mentioned B layer, inactive inorganic particles and / or heat-resistant organic particles can also be used in addition to silicon dioxide and / or calcium carbonate, but from the viewpoint of transparency and cost, silicon dioxide particles and / or calcium carbonate particles are more preferably used. In addition, as inorganic particles that can be used in addition, aluminum oxide-silicon dioxide composite oxide particles, hydroxyapatite color particles, etc. can be cited. In addition, as heat-resistant organic particles, cross-linked polyacrylic acid particles, cross-linked polystyrene particles, benzoguanamine particles, etc. can be cited. In addition, when using silicon dioxide particles, porous colloidal silica is preferred, and when using calcium carbonate particles, from the viewpoint of preventing the lubricant from falling off, it is preferred that light calcium carbonate surface-treated with a high molecular compound of a polyacrylic acid system is used.

[0067] The average particle size of the inorganic particles added to the surface layer B is preferably 0.1 μm or more and 2.0 μm or less, and particularly preferably 0.3 μm or more and 1.0 μm or less. If the average particle size of the inorganic particles is 0.1 μm or more, the slip property of the release film is good and thus it is preferred. In addition, if the average particle size is 2.0 μm or less, there is no concern about adversely affecting the smoothness of the release layer surface, and therefore, there is no concern about pinholes in the ceramic green sheet and thus it is preferred.

[0068] In addition, in order to improve the adhesion of the subsequently coated release layer, etc., or to prevent static electricity, etc., a coating layer can be provided on the surface of the surface layer A and / or the surface layer B before stretching or after uniaxial stretching in the film forming process, or a corona treatment can be performed.

[0069] [Mold release coating composition]

[0070] The silicone release polyester film of the present invention has a coating layer (release layer) formed using a release coating composition, wherein the release coating composition comprises: an aqueous dispersion of an olefin-containing silicone, an aqueous dispersion of silicone having hydrogen atoms directly bonded to Si atoms represented by Si-H groups, a platinum-based catalyst containing a crosslinking reaction inhibitor, and a platinum-based catalyst not containing a crosslinking reaction inhibitor.

[0071] The number average molecular weight of the alkenyl group-containing silicone is 10,000 or more and 40,000 or less.

[0072] The total weight of the platinum element contained as the platinum-based catalyst is 120 ppm or more and 600 ppm or less relative to the weight of the alkenyl group-containing organosilicon.

[0073] (Silicones containing olefin groups)

[0074] As the alkenyl-containing silicone in the present invention, an alkenyl-containing silicone having a number average molecular weight of 10,000 or more and 40,000 or less is used. This can provide excellent mold release properties. If the number average molecular weight of the alkenyl-containing silicone does not meet the lower limit, the crosslinking reaction rate increases, and silicone aggregates are generated. In addition, if the number average molecular weight of the alkenyl-containing silicone exceeds the upper limit, it becomes difficult to disperse in water, and the peel strength at the peeling speed increases.

[0075] Examples of the alkenyl group-containing organosilicon include organopolysiloxane having a structure represented by the following general formula (I).

[0076] R 1 a R 2 b SiO (4-a-b) / 2 ···(I)

[0077] (In formula (I),

[0078] R 1 is an alkenyl group having 2 to 8 carbon atoms, R 2 is a monovalent saturated hydrocarbon group having 1 to 16 carbon atoms selected from an alkyl group or an aryl group,

[0079] Respectively represent integers where a is 1 to 3, b is 0 to 2, and satisfies a+b≤3. )

[0080] The alkenyl group-containing organosilicon may be a linear structure or a branched structure, and may partially have cross-linking or a mixture thereof. 1 Examples of the alkenyl group having 2 to 8 carbon atoms include vinyl, allyl, butenyl, pentenyl, hexenyl, etc. Among these, vinyl is particularly preferred. 2Examples of the alkyl group include methyl, ethyl, propyl, and butyl groups, and examples of the aryl group include phenyl and tolyl groups. 2 80 mol % or more of the substituents are methyl groups.

[0081] In addition, from the perspective of the curing speed and pot life of the composition, it is preferred that the silicon atoms having alkenyl groups are in the range of 0.05 mol% or more and 20 mol% or less relative to all silicon atoms in the above-mentioned alkenyl-containing organosilicon. When the ratio of silicon atoms having alkenyl groups does not meet the lower limit, the curing speed of the composition decreases, and it may become difficult to efficiently form a cured organosilicon film in the thin film formation described later. In addition, when the ratio of silicon atoms having alkenyl groups exceeds the upper limit, the pot life of the composition may become shorter.

[0082] The alkenyl group-containing silicone in the present invention can be produced by a known method. In addition, the alkenyl group-containing silicone in the present invention is contained in the above-mentioned composition in the form of a water dispersion.

[0083] (Silicon containing Si-H group)

[0084] Examples of the organosilicon having a hydrogen atom directly bonded to a Si atom represented by a Si—H group (hereinafter sometimes referred to as Si—H group-containing organosilicon) in the present invention include organohydrogenpolysiloxane having a structure represented by the following general formula (II).

[0085] R 3 c H d SiO (4-c-d) / 2 ···(II)

[0086] (In formula (II),

[0087] R 3 is a monovalent saturated hydrocarbon group having 1 to 16 carbon atoms selected from an alkyl group or an aryl group,

[0088] Respectively represent that c is 0 to 2, d is 1 to 3, and the integers satisfying c+d≤3. )

[0089] The above-mentioned Si-H group-containing organic silicon may be in a linear structure or a branched structure. 3 Examples of the alkyl group include methyl, ethyl, propyl, and butyl groups, and examples of the aryl group include phenyl and tolyl groups. 3 50 mol % or more of the substituents are methyl groups.

[0090] The Si—H group-containing silicone preferably has at least 3 or more, preferably 5 or more, hydrogen atoms bonded to silicon atoms in one silicone molecule from the viewpoint of curing properties.

[0091] The Si-H group-containing silicone can be produced by a known method. In addition, the Si-H group-containing silicone in the present invention is contained in the composition in the form of a water dispersion.

[0092] (Ratio of Si-H groups to olefin groups)

[0093] The ratio of the Si-H radical in the demoulding coating composition in the present invention to the alkenyl number (Si-H radical / alkenyl number) is preferably more than 1.0 and the scope below 2.0. If the above ratio does not meet the lower limit, it remains in the coating layer formed with excessive alkenyl, and therefore, peel strength becomes easy to change over time, and in addition, cross-linking density reduces, and thus, the uniformity of stripping force and residual bonding rate are sometimes reduced. In addition, if the above ratio exceeds the upper limit, it remains in the coating layer formed with reactive high Si-H base, and sometimes causes the increase of stripping force.

[0094] (Silicone content)

[0095] In the demoulding coating composition of the present invention, the total amount of the alkenyl-containing organosilicon solid component and the Si-H-containing organosilicon solid component is preferably 70% by weight or more, based on the weight of the solid content of the above composition. In addition, the more preferred content of each organosilicon solid component is 80% by weight or more and 97% by weight or less. Here, the organosilicon solid component refers to the amount after removing the aqueous solvent, and the solid content weight of the composition refers to the total amount of the solid components of each additive. If the total amount of the above-mentioned organosilicon solid component is less than the lower limit, the area of ​​the thin film surface formed by the organosilicon becomes smaller, the peeling force becomes heavier, and sometimes the peeling force becomes uneven.

[0096] (Water-based solvent)

[0097] As the aqueous solvent for forming each of the silicone aqueous dispersions of the present invention, water is preferably used. By using an aqueous solvent, the silicone release layer can be formed in the release film production process without using explosion-proof equipment and organic solvent recovery equipment required for organic solvents.

[0098] (Emulsifier)

[0099] In order to improve the stability and shear resistance of the aqueous dispersion, each silicone aqueous dispersion is prepared using an emulsifier. As the emulsifier, for example, a nonionic emulsifier that does not affect the curing reaction of silicone is preferred. An ionic emulsifier may affect the curing reaction of silicone, and may also be locally present in the coating film, such as oozing out on the surface, and may affect the demolding properties.

[0100] As the nonionic emulsifier, the HLB value is preferably in the range of 8 to 18, and examples thereof include at least one selected from alkylene oxide adducts such as higher alcohols, alkylene oxide adducts of higher fatty acids, esters of alkylene oxide adducts of higher fatty acids and alcohols, alkylene oxide adducts of alkanolamides, alkylene oxide adducts of sorbitan esters, and alkylene oxide adducts of higher fatty acid glycerides. Here, the HLB value is a value calculated according to Griffin's calculation formula.

[0101] As the alkylene oxide, for example, ethylene oxide, propylene oxide, and butylene oxide can be mentioned, and one of them can be used, or multiple types can be used. When using multiple types, regardless of block or random addition forms, the HLB value is preferably in the range of 8 to 18, and more preferably in the range of 10 to 15. Among these nonionic emulsifiers, polyoxyethylene lauryl ether, polyoxyethylene tridecyl ether, etc. can be preferably mentioned. If a nonionic emulsifier having an HLB value exceeding the above range is used as an emulsifier for an organic silicone aqueous dispersion, the emulsification dispersion power and the stability of the aqueous dispersion are sometimes reduced.

[0102] (catalyst)

[0103] In the release coating composition constituting the coating layer of the present invention, an alkenyl-containing organosilicon and a Si-H-containing organosilicon are subjected to an addition reaction, and therefore, a catalyst is preferably used, and a platinum-based catalyst is particularly preferred. As a platinum-based catalyst, a known substance can be used, for example, platinum chloride and chloroplatinic acid can be cited. The above-mentioned platinum-based catalyst can be used in a state of being emulsified in advance using a nonionic emulsifier, or it can be used simultaneously when the organosilicon is emulsified. Furthermore, it can also be added when the cross-linking reaction inhibitor described later is emulsified.

[0104] (Cross-linking Reaction Inhibitor)

[0105] In the present invention, in order to suppress the activity of the platinum-based catalyst at room temperature, the demoulding coating composition contains a crosslinking reaction inhibitor. The crosslinking reaction inhibitor is preferably a crosslinking reaction inhibitor having an acetylene group. If the content of the crosslinking reaction inhibitor is too much, the curing reaction of the silicone is excessively suppressed, and it becomes difficult to form a coating layer (crosslinking reaction). Therefore, the upper limit is not particularly limited as long as the above matters are considered and the range for forming a coating layer is not particularly limited, and relative to the amount of platinum element, it is preferably 6 times or less. More preferably, it is 5 times or less, and particularly preferably 4 times or less.

[0106] The cross-linking reaction inhibitor having an acetylene group is not particularly limited as long as it has an acetylene group. However, in the present invention, an aqueous coating composition is used. Therefore, from the aspects of the balance between the solubility in water and the coordination ability for platinum and volatility, it is preferred to use a cross-linking reaction inhibitor having an acetylene hydroxyl group, for example, represented by 1-ethynylcyclohexanol.

[0107] (Platinum catalysts with and without crosslinking inhibitors)

[0108] In order to efficiently carry out the cross-linking reaction, a platinum-based catalyst containing a cross-linking reaction inhibitor and a platinum-based catalyst not containing a cross-linking reaction inhibitor are used.

[0109] Regarding the mechanism of action that manifests the above-mentioned action effect of the present invention, the following is speculated in the cross-linking reaction of the silicone in the water dispersion system, but the claims of the present invention are not intended to be limited to the following speculation. In the cross-linking reaction of the silicone in the water dispersion system, it is speculated that the following results occur: in the low temperature region, a reaction occurs between the polydimethylsiloxane based on the destruction of the emulsion and the platinum-based catalyst not containing a cross-linking reaction inhibitor, and then in the high temperature region, a reaction occurs between the polydimethylsiloxane based on the complete destruction of the emulsion and the platinum-based catalyst activated by the volatilization of the cross-linking reaction inhibitor in the platinum-based catalyst containing a cross-linking reaction inhibitor.

[0110] In the present invention, the amount of platinum in the platinum catalyst relative to the weight of the alkenyl-containing organosilicon is greater than 120 ppm and less than 600 ppm, for example, greater than 130 ppm and less than 550 ppm, or greater than 150 ppm and less than 500 ppm. By setting the amount within the above range, the organosilicon can be sufficiently cured, and a release film having excellent easy-peel surface properties can be obtained.

[0111] If the weight ratio of the platinum element exceeds the above range, the addition reaction of the alkenyl group and the Si-H group is accelerated, and there is a tendency to produce a gel of the silicone. On the other hand, if the weight of the platinum element is less than 120 ppm, the addition reaction proceeds, but there is a tendency to cause poor curing of the silicone. From the above viewpoint, it is preferably more than 120 ppm.

[0112] The amount of platinum element (P1) in the platinum catalyst containing the crosslinking reaction inhibitor is preferably 40 ppm or more and less than 400 ppm relative to the weight of the olefinic silicone, for example, 40 ppm or more and 370 ppm or more and 60 ppm or less than 300 ppm.

[0113] The amount of platinum element (P0) in the above-mentioned platinum-based catalyst that does not contain a cross-linking reaction inhibitor is preferably 50 ppm or more and less than 400 ppm relative to the weight of the olefinic silicone, for example, 60 ppm or more and 370 ppm or more, 70 ppm or more and 300 ppm or less.

[0114] In addition, the platinum-based catalyst includes the amount of platinum (P0) of the platinum-based catalyst not containing a crosslinking reaction inhibitor and the amount of platinum (P1) of the platinum-based catalyst containing a crosslinking reaction inhibitor. The ratio of the amount of platinum (P0) of the platinum-based catalyst not containing a crosslinking reaction inhibitor to the total weight of the platinum element (P1+P0) is preferably 0.3 or more and 0.8 or less, for example, 0.31 or more and 0.75 or less, for example, 0.32 or more and 0.70 or less. In particular, the crosslinking reaction at low temperature affects the final high crosslinking density. Therefore, when the weight ratio of the platinum in the platinum-based catalyst not containing a crosslinking reaction inhibitor does not satisfy 0.3, the crosslinking reaction at low temperature is insufficient, and thus, a film with a high crosslinking density is not obtained in the end, and the peeling force becomes high. In addition, if the weight ratio of the platinum in the platinum-based catalyst not containing a crosslinking reaction inhibitor exceeds 0.8, a film with a high crosslinking density is obtained, but the reaction is carried out after the coating liquid is prepared, so the coating appearance is deteriorated due to the gelation of the coating liquid.

[0115] (Other ingredients)

[0116] The mold release coating composition of the present invention may further contain, for example, an adhesiveness-imparting agent to a substrate, a colorant, an ultraviolet absorber, particles, an antistatic agent, and the like, within a range not impairing the subject matter of the present invention.

[0117] (Preparation of Silicone Aqueous Dispersion)

[0118] When preparing each of the organosilicon aqueous dispersions of the present invention, a method of emulsifying the above-mentioned organosilicon component, aqueous solvent and emulsifier can be cited. These components can be emulsified by a known method, for example, a method of mechanically emulsifying the pre-prepared organosilicon, emulsifier and other components as needed in an aqueous medium using a stirring device such as a homogenizer, vacuum emulsifier (AGI-HOMO MIXER), super planetary mixer, etc.

[0119] The particle size of the aqueous dispersion can be adjusted by adjusting the size of the stirring blade, the stirring speed and the stirring time. The average particle size of each silicone aqueous dispersion of the present invention is preferably 200 nm or less, more preferably 100 nm or more and 200 nm or less.

[0120] 〔Coating layer〕

[0121] In the present invention, a coating layer (release layer) is formed on at least one surface of a polyester film using the release coating composition of the present invention. The coating layer (release layer) of the present invention is formed as follows: the release coating composition is applied to the polyester film and then dried to form a coating layer.

[0122] In the present invention, the coating layer thickness is preferably 5 nm or more and 70 nm or less in terms of thickness after drying. If the coating layer thickness does not meet the lower limit, the demoulding property may become insufficient, and if it exceeds the upper limit, the peel strength increases, and there is a tendency that the coating solution has a high concentration or the coating amount needs to be increased, thereby becoming difficult to apply.

[0123] When applying the demoulding coating composition of the present invention on a polyester film, an aqueous coating liquid containing the above-mentioned composition is prepared. For the solid content concentration of the aqueous coating liquid, the weight of the above-mentioned coating liquid is set as a benchmark, preferably 20 weight % or less, more preferably 1 weight % or more and 10 weight % or less. If the solid content concentration in the aqueous coating liquid does not meet the lower limit, the coating property of the polyester film is sometimes insufficient. In addition, if the solid content concentration exceeds the upper limit, the stability of the coating liquid and the appearance of the coating layer are sometimes deteriorated. As an aqueous solvent for adjusting the solid content concentration, water is preferably used.

[0124] The aqueous coating liquid may be applied to the polyester film at any stage, but is preferably applied during the production process of the polyester film, and more preferably applied to the polyester film before the crystal orientation is completed.

[0125] Here, the polyester film before the completion of crystal orientation includes: an unstretched film, a uniaxially oriented film in which the unstretched film is oriented in the longitudinal direction (hereinafter, sometimes referred to as the film continuous film forming direction, the length direction, the MD direction) or the transverse direction (hereinafter, sometimes referred to as the direction orthogonal to the longitudinal direction, the width direction, the TD direction), and a film that is further stretched and oriented at a low ratio in the longitudinal and transverse directions (finally stretched in the longitudinal or transverse direction to complete the crystal orientation before the biaxially stretched film). Among them, it is preferred to apply the aqueous coating liquid of the above-mentioned composition on the unstretched film or the uniaxially stretched film oriented in one direction, and directly implement longitudinal stretching and / or transverse stretching and heat setting, so-called online coating. The coating layer can be dried by a stretching process or a heat setting treatment after coating, and a drying process can be further applied as needed. In addition, when the composition is cured using a catalyst to obtain a cured coating, it can be cured by a stretching process or a heat setting treatment, and a curing process can be further applied as needed.

[0126] When the aqueous coating liquid is applied to a polyester film, for example, as a pretreatment for improving coating properties, it is preferred to subject the film surface to a physical treatment such as corona surface treatment, flame treatment, or plasma treatment, or to use the aforementioned emulsifier together with the composition as a wetting agent.

[0127] As the coating method, any known coating method can be applied, for example, roll coating, gravure coating, roll brush coating, spray coating, air knife coating, impregnation, curtain coating, etc. can be used alone or in combination.

[0128] <Method for producing silicone release polyester film>

[0129] The method for producing the silicone release polyester film of the present invention comprises the following steps:

[0130] A coating layer is formed on at least one side of a polyester film using a mold release coating composition in the form of an aqueous dispersion, wherein the mold release coating composition comprises an aqueous dispersion of an alkenyl-containing silicone, an aqueous dispersion of silicone having hydrogen atoms directly bonded to Si atoms represented by Si-H groups, and a platinum-based catalyst.

[0131] The amount of platinum in the platinum-based catalyst is more than 120 ppm and less than 600 ppm relative to the weight of the alkenyl-containing organosilicon.

[0132] The platinum-based catalysts include: platinum-based catalysts containing a cross-linking reaction inhibitor and platinum-based catalysts not containing a cross-linking reaction inhibitor.

[0133] The coating layer has a thickness of 5 nm to 70 nm.

[0134] The method for producing the silicone release polyester film of the present invention can efficiently and simply produce a silicone release polyester film having the above-mentioned properties. It should be noted that the production method shown here is an example, and the present invention is not limited thereto.

[0135] In the above-mentioned production method, the description concerning the above-mentioned silicone release polyester film and the like in this specification can be appropriately applied to each structure.

[0136] In the above production method, the step of forming a coating layer using the aqueous release coating composition may be any method as long as the coating layer is formed on a film using the aqueous release coating composition, and a known method may be appropriately used.

[0137] <Protected Body>

[0138] The protected body of the present invention is obtained by laminating the silicone release polyester film on the protected body as the coating layer or the release layer.

[0139] Examples of the protected body include organic resin sheets, inorganic resin sheets, glass plates, metal plates, ceramic sheets, adhesive sheets, etc. The protected body of the present invention is laminated with a silicone release polyester film having the above-mentioned properties, and therefore, for example, can be suitably used when a ceramic green sheet is used as the protected body.

[0140] Example

[0141] The present invention will be specifically described with reference to the examples, but the present invention is not limited to the following examples. It should be noted that the physical properties and characteristics in the examples are measured or evaluated by the following methods. In addition, the expression "parts" refers to "parts by mass".

[0142] Each measurement and evaluation in the examples were performed as follows.

[0143] (1) Ceramic sheet peelability

[0144] 90 parts by weight of barium titanate (BaTiO3), 7 parts by weight of polyvinyl butyral, 1.5 parts by weight of dioctyl phthalate, and 2.5 parts by weight of a polycarboxylic acid-based polymer surfactant were added to a mixed solvent of toluene:ethanol = 1:1 (volume ratio), and dispersed in a ball mill to adjust the slurry. The slurry was evenly applied to the coating layer (release layer) of the release polyester film in a manner to have a thickness of 2 μm after drying, and then dried to form a ceramic sheet.

[0145] The release polyester film formed with the ceramic sheet was cut into 25 mm × 150 mm, and an adhesive tape (manufactured by Nitto Denko Corporation, trade name "31B tape") was attached to the ceramic sheet side to prepare a test piece. The test piece was conditioned at 23°C and 50% humidity for 24 hours, and then the ceramic sheet (31B tape side) was peeled off using a tensile tester at a peeling angle of 90° and a peeling speed of 10 m / min to measure the peel strength.

[0146] The peel strength of the ceramic sheet is judged by the following indexes.

[0147] ○: Peel strength is 0.60g / 25mm or less

[0148] ×: Peel strength exceeds 0.60 g / 25 mm

[0149] (2) Residual bonding rate

[0150] Determine the peel strength after polyester adhesive tape (Nitto Denko system, No.31B) is adhered to the cold-rolled stainless steel plate (SUS304) specified in JIS G4305, as basic bonding force (f0). In addition, the above-mentioned polyester adhesive tape is crimped on the release layer surface of the demoulding polyester film with a 5kg pressing roller, and the adhesive tape is peeled off after maintaining for 30 seconds, and the peel strength after the adhesive tape after the peeling is adhered to the above-mentioned stainless steel plate is measured as residual bonding force (f). By the basic bonding force (f0) and residual bonding force (f) obtained, the residual bonding rate is obtained by the following formula. It should be noted that the peeling angle is set to 180 degrees and the peeling speed is set to 300mm / minute.

[0151] Residual bonding rate (%) = (f) / (f0)×100

[0152] The residual adhesion ratio is preferably 90% or more, indicating that the silicone crosslinking density is high. If it is less than 90%, it indicates that the crosslinking is insufficient.

[0153] (3) Coating thickness

[0154] The film was fixed with an embedding resin, and its cross section was cut with a microtome so that the cross section of the film could be observed. The obtained film was stained with 2% osmic acid at 60°C for 2 hours and observed with a transmission electron microscope (JEM2010 manufactured by JEOL Ltd.) to measure the thickness of the release layer.

[0155] (4) Coating uniformity

[0156] The coating uniformity of the release layer was evaluated by visually observing the surface of the release layer under reflected light according to the following criteria.

[0157] ◎: There are no coating defects and the coating is very uniform.

[0158] ○: There are no coating defects, but slight unevenness of rainbow pattern is observed along the length direction.

[0159] △: Slightly fine coating defects and coating streaks were observed along the length direction.

[0160] ×: There are many fine coating defects, and strong coating streaks are observed along the length direction. It cannot be said that the coating is uniform.

[0161] [Examples 1 to 5, Comparative Examples 1 to 8]

[0162] A molten polyethylene terephthalate ([η]=0.64dl / g, Tg=78°C) containing 0.1% by mass of calcium carbonate particles with an average particle size of 0.7μm was extruded from a die and cooled on a cooling drum according to a conventional method to form an unstretched film. Subsequently, the film was stretched to 3.6 times in the longitudinal direction and the components were mixed in a manner to obtain a solid content ratio as shown in Table 1 to prepare an aqueous coating liquid (aqueous dispersion with a solid content concentration of 5% by mass). The prepared aqueous coating liquid was evenly applied to the surface of the film using a roll coater to form a coating layer (release layer) in a manner such that the coating thickness after drying became 30nm.

[0163] Next, the coated film was dried at 115°C for about 5 seconds and stretched to 4.5 times in the transverse direction at 145°C, and further heat-set at 230°C for about 5 seconds to obtain a 25 μm biaxially stretched polyester film having a coating layer (release layer) shown in Table 1.

[0164] <Alkenyl-containing silicone aqueous dispersion>

[0165] A raw material containing 98% by weight of an organosilicon having an alkenyl group represented by the following formula (1) (number average molecular weight: 28,000) and 2% by weight of polyoxyethylene lauryl ether (Kao Corporation, trade name: Emulgen 109P) as a surfactant was mechanically emulsified in an aqueous medium using an emulsifying device capable of stirring the entire container (NPLabo Co., Ltd., device name: "Super Planetary Mixer") to obtain an aqueous dispersion of an organosilicon containing an alkenyl group having a solid content of 20% by weight. In addition, the particle size of the emulsion was adjusted by adjusting the stirring speed and stirring time during emulsification.

[0166]

[0167] (In formula (1), m is 2, and n is adjusted so that the number average molecular weight becomes 28,000.)

[0168] <Silicon Aqueous Dispersion Containing Si-H Group>

[0169] A raw material containing 98% by weight of a silicone having a hydrogen group represented by the following formula (2) (number average molecular weight: 5000) and 2% by weight of polyoxyethylene lauryl ether (Kao Corporation, trade name "Emulgen 109P") as a surfactant was mechanically emulsified in an aqueous medium using an emulsifier capable of stirring the entire container (NPLabo Co., Ltd., device name "Super Planetary Mixer") to obtain a Si-H group-containing silicone aqueous dispersion having a solid content of 20% by weight. In addition, the particle size of the emulsion was adjusted by adjusting the stirring speed and stirring time during emulsification.

[0170]

[0171] (In formula (2), o=40, p=35.)

[0172] <Platinum-based catalysts>

[0173] Platinum catalyst (P1) containing a reaction inhibitor: an aqueous dispersion having a solid content of 10% by weight is prepared by using an isopropanol solution of chloroplatinic acid (in this composition, the amount of platinum metal is 500 ppm by mass), 99.75% by weight of polyoxyethylene lauryl ether (manufactured by Kao Corporation, trade name "Emulgen 109P") as a surfactant, 0.2% by weight of a crosslinking reaction inhibitor (1-ethynylcyclohexanol), and pure water. The platinum catalyst (P1) preferentially coordinates the crosslinking reaction inhibitor, and thus the catalytic effect can be delayed until the reaction inhibitor volatilizes.

[0174] Platinum catalyst (P0) without reaction inhibitor: an aqueous dispersion is prepared using an isopropanol solution of chloroplatinic acid (in this composition, the amount of platinum metal is 500 ppm by mass), 99.95% by weight of polyoxyethylene lauryl ether (manufactured by Kao Corporation, trade name "Emulgen 109P") as a surfactant, and pure water. The platinum catalyst (P0) does not contain a reaction inhibitor, and therefore can exhibit a catalytic effect in a low temperature region.

[0175] <Adjustment of silicone coating liquid>

[0176] As a coating composition for demolding, a composition consisting of 90 parts by weight of an alkenyl-containing silicone water dispersion / 10 parts by weight of an Si-H-containing silicone water dispersion / a platinum-based catalyst (the added amounts are adjusted so that the amount of platinum elements P0+P1 becomes as shown in Table 1) is used, and the coating liquid is prepared by diluting it with water so that the solid content concentration of the coating liquid becomes 5% in a manner to obtain a target coating layer thickness.

[0177] The above formulations and results are shown in Table 1.

[0178] [Table 1]

[0179]

[0180] As shown in Table 1, the film of the embodiment of the present invention has excellent peelability, residual adhesion and appearance. This is because a film with a very high crosslinking density is obtained by combining a catalyst containing a crosslinking reaction inhibitor with a catalyst not containing a crosslinking reaction inhibitor. On the other hand, in Comparative Examples 1 and 2, the total amount of platinum elements is too much, which becomes a gel state, and the coating appearance is also poor. In addition, in Comparative Examples 3 and 4, the total amount of platinum elements is too little and the coating appearance is poor. In addition, in Comparative Example 5, a large amount of crosslinking reaction from the low temperature region is carried out, so the effective amount of platinum elements in the high temperature region is reduced, and the final crosslinking density is also reduced, which is the result of the peeling force becoming larger. In addition, in Comparative Example 6, the effective amount of platinum elements in the low temperature region is reduced, the crosslinking reaction in the low temperature region is not carried out, and it only becomes a crosslinking reaction in the high temperature region, the crosslinking density is reduced, and the peeling force becomes larger. In addition, in Comparative Example 7, the total amount of platinum elements is large, the crosslinking reaction from the low temperature region is excessively carried out, and the coating appearance is also poor. In addition, in Comparative Example 8, the total amount of platinum elements is large, and the crosslinking reaction in the high temperature region is excessively carried out, and the coating appearance is also poor.

Claims

1. A silicone release polyester film having a coating layer on at least one side of the polyester film, wherein the coating layer is formed using a release coating composition of an aqueous dispersion, wherein the release coating composition of the aqueous dispersion comprises an aqueous dispersion of an alkenyl-containing silicone, an aqueous dispersion of an silicone having a hydrogen atom directly bonded to a Si atom represented by a Si—H group, and a platinum-based catalyst. The amount of platinum in the platinum catalyst is greater than 120 ppm and less than 600 ppm relative to the weight of the alkenyl-containing organosilicon. The platinum-based catalyst includes: a platinum-based catalyst containing a cross-linking reaction inhibitor and a platinum-based catalyst not containing a cross-linking reaction inhibitor. The coating layer has a thickness of 5 nm or more and 70 nm or less.

2. The silicone release polyester film according to claim 1, in, The amount of platinum element (P0) of the platinum-based catalyst not containing a crosslinking reaction inhibitor is 50 ppm or more and less than 400 ppm relative to the weight of the alkenyl-containing organosilicon. The amount of platinum element (P1) in the platinum-based catalyst containing the cross-linking reaction inhibitor is 40 ppm or more and less than 400 ppm based on the weight of the alkenyl group-containing organosilicon.

3. The silicone release polyester film according to claim 1 or 2, in, The platinum-based catalyst comprises the amount of platinum elements (P0) of the platinum-based catalyst not containing a cross-linking reaction inhibitor and the amount of platinum elements (P1) of the platinum-based catalyst containing a cross-linking reaction inhibitor, The ratio (P0 / (P1+P0)) of the amount of platinum element (P0) of the platinum-based catalyst not containing a cross-linking reaction inhibitor to the total weight of platinum elements (P1+P0) is 0.3 or more and 0.8 or less.

4. The silicone release polyester film according to any one of claims 1 to 3, in, The alkenyl group of the alkenyl group-containing organosilicon is vinyl group. 5 . The silicone release polyester film according to claim 1 , which is used for molding ceramic green sheets in the production of laminated ceramic capacitors.

6. A protected object, in, The silicone release polyester film according to any one of claims 1 to 5 is laminated on the protected body at the coating layer or the release layer.

7. The protected body according to claim 6, in, The protected body is a ceramic green sheet.

8. A method for producing a silicone release polyester film, comprising the following steps: A coating layer is formed on at least one side of a polyester film using a mold release coating composition in the form of an aqueous dispersion, wherein the mold release coating composition comprises an aqueous dispersion of an alkenyl-containing silicone, an aqueous dispersion of silicone having hydrogen atoms directly bonded to Si atoms represented by Si-H groups, and a platinum-based catalyst. The amount of platinum in the platinum catalyst is greater than 120 ppm and less than 600 ppm relative to the weight of the alkenyl-containing organosilicon. The platinum-based catalyst includes: a platinum-based catalyst containing a cross-linking reaction inhibitor and a platinum-based catalyst not containing a cross-linking reaction inhibitor. The coating layer has a thickness of 5 nm or more and 70 nm or less.