Scintillator panel, radiation detector, method for manufacturing scintillator panel, and method for manufacturing radiation detector
By introducing a combination of flexible support substrate, columnar crystal scintillator layer and intermediate layer into the scintillator panel, the problem of cracks and inappropriate contact of the scintillator layer is solved, and a more stable radiation detection effect is achieved.
Patent Information
- Application Number
- CN202280093830.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-24
- Filing Date
- 2022-10-26
- Publication Date
- 2024-11-01
AI Technical Summary
When the existing scintillator panels come into contact with the light-receiving surface of the sensor panel, cracks in the scintillator layer may easily occur, and the contact is inappropriate, affecting the radiation detection effect.
A scintillator panel is designed, which includes a flexible support substrate, a plurality of columnar crystal scintillator layers and an intermediate layer. The intermediate layer is arranged between the support substrate and the scintillator layer, and through the combination of a metal layer and an organic layer, it is ensured that Stability and contact appropriateness of the scintillator layer and, if necessary, add protective layers to prevent cracks.
It effectively suppresses the cracks in the scintillator layer, ensures the appropriate contact between the sensor panel and the scintillator panel, and improves the image quality of radiation detection and the stability of the equipment.
Smart Images

Figure CN118891683A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a scintillator panel, a radiation detector, a method for manufacturing a scintillator panel, and a method for manufacturing a radiation detector. Background Art
[0002] There is known a scintillator panel including a support substrate and a scintillator layer formed on the support substrate by a vapor deposition method (for example, see Patent Document 1). Such a scintillator panel is sometimes arranged on a light-receiving surface of a sensor panel in a state where the support substrate is located on the opposite side of the sensor panel relative to the scintillator layer, thereby constituting a radiation detector.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Patent No. 4451843 Summary of the invention
[0006] Technical problem to be solved by the invention
[0007] In the scintillator panel as described above, unlike the case where the scintillator layer is formed on the light-receiving surface of the sensor panel by vapor deposition, proper contact with the light-receiving surface of the sensor panel is required. In addition, in the scintillator panel as described above, if the supporting substrate is flexible, it becomes easy to arrange the scintillator panel on the light-receiving surface of the sensor panel, but on the other hand, there is a concern about the generation of cracks in the scintillator layer.
[0008] An object of the present disclosure is to provide a scintillator panel and a method for manufacturing the scintillator panel that can optimize contact with a light receiving surface of a sensor panel and suppress the occurrence of cracks in a scintillator layer, as well as a radiation detector including such a scintillator panel and a method for manufacturing the scintillator panel.
[0009] Means for solving technical problems
[0010] A scintillator panel according to one aspect of the present disclosure comprises: a supporting substrate which is flexible; a scintillator layer which includes a plurality of columnar crystals; and an intermediate layer which is arranged between the supporting substrate and the scintillator layer, the plurality of columnar crystals including: a plurality of first ends on the supporting substrate side, and a plurality of second ends on the side opposite to the supporting substrate, each of the plurality of first ends becomes thinner toward the supporting substrate side, each of the plurality of second ends has an end face along a plane, and a portion of the intermediate layer is at least arranged in the area between the plurality of first ends.
[0011] In the above-mentioned scintillator panel, each of the multiple second ends included in the multiple columnar crystals has an end face along the plane. Thus, in a state where the supporting substrate is located on the opposite side of the sensor panel relative to the scintillator layer, when the scintillator layer is arranged on the light-receiving surface of the sensor panel, the contact between the light-receiving surface of the sensor panel and the scintillator panel is optimized. In addition, in the above-mentioned scintillator panel, a part of the intermediate layer is arranged in the area between the multiple first ends included in the multiple columnar crystals. Thus, even if the scintillator panel is bent, the generation of cracks in the scintillator layer is suppressed. Thus, according to the above-mentioned scintillator panel, the contact with the light-receiving surface of the sensor panel can be optimized and the generation of cracks in the scintillator layer can be suppressed.
[0012] In the scintillator panel according to one aspect of the present disclosure, a portion of the intermediate layer may be disposed at least in the entire region between the plurality of first end portions. Thereby, the occurrence of cracks in the scintillator layer can be reliably suppressed.
[0013] In the scintillator panel of one aspect of the present disclosure, when the distance between the support substrate and the scintillator layer is set to D, a portion of the intermediate layer may reach a position that is advanced from the plurality of front ends of the plurality of first end portions by more than D. This can more reliably suppress the occurrence of cracks in the scintillator layer.
[0014] In the scintillator panel of one aspect of the present disclosure, when the thickness of the scintillator layer is T, a portion of the intermediate layer may reach a position that is advanced by 0.2 T or more from the plurality of leading ends of the plurality of first end portions. This can more reliably suppress the occurrence of cracks in the scintillator layer.
[0015] In the scintillator panel of one aspect of the present disclosure, the intermediate layer may include: a metal layer formed along the surface of each of the plurality of first end portions; and an organic layer disposed at least in a region between the plurality of first end portions via the metal layer, wherein the metal layer has a light reflecting function or a light absorbing function. Thus, it is possible to realize an intermediate layer that can exert a light reflecting function or a light absorbing function and suppress the generation of cracks in the scintillator layer.
[0016] In one aspect of the scintillator panel of the present disclosure, the intermediate layer may include an organic layer at least disposed in a region between the plurality of first end portions, the organic layer having a light reflecting function or a light absorbing function. Thus, it is possible to realize an intermediate layer that exhibits a light reflecting function or a light absorbing function and can suppress the generation of cracks in the scintillator layer.
[0017] In the scintillator panel of one aspect of the present disclosure, it is also possible that, when observed from the thickness direction of the supporting substrate, at least a portion of the outer edge of the supporting substrate, at least a portion of the outer edge of the scintillator layer, and at least a portion of the outer edge of the intermediate layer are consistent. Accordingly, in at least a portion of the outer edge of the supporting substrate, the area where the scintillator layer does not exist can be eliminated. In other words, the area of the scintillator layer can be increased by the amount of the area. In other words, the area of the supporting substrate can be reduced by the amount of the area.
[0018] In the scintillator panel according to one aspect of the present disclosure, the plurality of second end portions may be connected to one another. This can more reliably suppress the occurrence of cracks in the scintillator layer.
[0019] The scintillator panel of one aspect of the present disclosure may further include a protective layer covering the support substrate, the scintillator layer, and the intermediate layer. This can protect the plurality of deliquescent columnar crystals.
[0020] The scintillator panel of one aspect of the present disclosure may further include an adhesive layer disposed on the opposite side of the support substrate with respect to the scintillator layer. Thereby, the scintillator panel can be easily and reliably bonded to the light receiving surface of the sensor panel.
[0021] In the scintillator panel of one aspect of the present disclosure, when the thickness of the scintillator layer is T, the thickness of the support substrate may be greater than 0.2 T. This can prevent cracks from occurring in the scintillator layer due to a local external force acting on a portion of the scintillator panel, for example, during operation of the scintillator panel.
[0022] One aspect of the present disclosure provides a radiation detector including: the above-mentioned scintillator panel; and a sensor panel having a light receiving surface, the scintillator panel being arranged on the light receiving surface in a state where the scintillator layer is located on the sensor panel side with respect to a support substrate.
[0023] In the above radiation detector, the contact between the light receiving surface of the sensor panel and the scintillator panel is optimized. Therefore, according to the above radiation detector, an appropriate radiation image can be acquired.
[0024] A method for manufacturing a scintillator panel according to one aspect of the present disclosure is the above-mentioned method for manufacturing a scintillator panel, which comprises: a first step of forming a scintillator layer on an auxiliary substrate by vapor deposition; a second step of forming an intermediate layer on the scintillator layer after the first step in such a manner that a portion of the intermediate layer is at least arranged in a region between the first end portions; a third step of forming a supporting substrate on the intermediate layer after the second step; and a fourth step of removing the auxiliary substrate from the scintillator layer after the third step.
[0025] According to the above-mentioned method for manufacturing a scintillator panel, it is possible to obtain a scintillator panel in which contact with the light receiving surface of the sensor panel is optimized and generation of cracks in the scintillator layer is suppressed.
[0026] In the manufacturing method of the scintillator panel of one aspect of the present disclosure, a fifth step of cutting at least the scintillator layer, the intermediate layer, and the support substrate along the thickness direction of the support substrate may be further provided after the third step and before the fourth step. Accordingly, the scintillator layer, the intermediate layer, and the support substrate can be cut together in a stable state in which the scintillator layer, the intermediate layer, and the support substrate are supported by the auxiliary substrate.
[0027] In the manufacturing method of the scintillator panel of one aspect of the present disclosure, in the fifth step, the auxiliary substrate may be cut together with the scintillator layer, the intermediate layer and the support substrate in the thickness direction of the support substrate. Thus, the auxiliary substrate may be cut together with the scintillator layer, the intermediate layer and the support substrate.
[0028] In the manufacturing method of the scintillator panel of one aspect of the present disclosure, after the fourth step, a sixth step of cutting the scintillator layer, the intermediate layer, and the support substrate in the thickness direction of the support substrate may be further provided. Thus, the scintillator layer, the intermediate layer, and the support substrate can be easily and reliably cut into predetermined dimensions.
[0029] A method for manufacturing a radiation detector according to one aspect of the present disclosure is the above-mentioned method for manufacturing a radiation detector, which comprises: a first step of preparing a scintillator panel and a sensor panel; and a second step of, after the first step, configuring the scintillator panel on the light receiving surface in such a way that the supporting substrate is located on the opposite side of the sensor panel relative to the scintillator layer.
[0030] According to the above-described method of manufacturing a radiation detector, it is possible to obtain a radiation detector including a scintillator panel in which contact with a light receiving surface of a sensor panel is optimized and generation of cracks in the scintillator layer is suppressed.
[0031] Effects of the Invention
[0032] According to the present disclosure, a scintillator panel and a method for manufacturing the scintillator panel that can optimize contact with a light receiving surface of a sensor panel and suppress the occurrence of cracks in a scintillator layer, and a radiation detector including such a scintillator panel and a method for manufacturing the scintillator panel can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 is a cross-sectional view of a scintillator panel according to one embodiment.
[0034] Figure 2 Yes Figure 1 A cross-sectional view of a radiation detector with a scintillator panel is shown.
[0035] Figure 3 Yes means Figure 1 FIG. 4 is a diagram showing a method for manufacturing a scintillator panel.
[0036] Figure 4 Yes means Figure 1 FIG. 4 is a diagram showing a method for manufacturing a scintillator panel.
[0037] Figure 5 Yes means Figure 1 FIG. 4 is a diagram showing a method for manufacturing a scintillator panel.
[0038] Figure 6 Yes means Figure 1 FIG. 4 is a diagram showing a method for manufacturing a scintillator panel.
[0039] Figure 7 This is a table showing the characteristics of the scintillator panels of Comparative Examples 1 and 2 and Examples 1 and 2.
[0040] Figure 8 is a cross-sectional view of a scintillator panel according to a modified example.
[0041] Fig. 9 is a cross-sectional view of a scintillator panel according to a modified example.
[0042] Fig.10 is a cross-sectional view of a scintillator panel according to a modified example.
[0043] Fig.11 is a cross-sectional view of a scintillator panel according to a modified example.
[0044] Fig.12 is a cross-sectional view of a scintillator panel according to a modified example.
[0045] Fig.13 is a cross-sectional view of a scintillator panel according to a modified example.
[0046] Fig.14 is a cross-sectional view of a scintillator panel according to a modified example.
[0047] Fig.15 is a cross-sectional view of a scintillator panel according to a modified example.
[0048] Fig.16 It is a cross-sectional view of a radiation detector according to a modified example.
[0049] Fig.17 It is a cross-sectional view of a radiation detector according to a modified example.
[0050] Explanation of symbols
[0051] 1...scintillator panel; 2...support substrate; 3...scintillator layer; 4...intermediate layer; 5...protective layer; 10...radiation detector; 11...sensor panel; 11a...light receiving surface; 12...adhesive layer; 13...auxiliary substrate; 30...columnar crystal; 31...first end; 31a...front end; 32...second end; 32a...end face; 41...metal layer; 42, 49...organic layer; R...region. DETAILED DESCRIPTION
[0052] Hereinafter, the embodiments of the present disclosure will be described in detail with reference to the accompanying drawings. In addition, the same reference numerals are given to the same or corresponding parts in each figure, and repeated descriptions are omitted.
[0053] [Structure of Scintillator Panel]
[0054] like Figure 1 As shown, the scintillator panel 1 includes a supporting substrate 2, a scintillator layer 3, an intermediate layer 4, and a protective layer 5. The intermediate layer 4 is disposed between the supporting substrate 2 and the scintillator layer 3. When observed from the thickness direction of the supporting substrate 2 (hereinafter referred to as "direction A"), the outer edge of the supporting substrate 2, the outer edge of the scintillator layer 3, and the outer edge of the intermediate layer 4 are consistent. That is, the side surface of the supporting substrate 2, the side surface of the scintillator layer 3, and the side surface of the intermediate layer 4 are in a flush state. Figure 2 As shown, the scintillator panel 1 and the sensor panel 11 together constitute a radiation detector 10. In the radiation detector 10, when radiation (e.g., X-rays) is incident on the scintillator panel 1, scintillation light is generated in the scintillator panel 1, and the scintillation light can be detected by the sensor panel 11. The radiation detector 10 is used as a radiation imaging device, for example, in a medical radiation image diagnosis device, a non-destructive inspection device, and the like.
[0055] like Figure 1As shown, the supporting substrate 2 includes an organic layer 21 and an inorganic layer 22. The inorganic layer 22 is formed on the surface 21a of the organic layer 21 and acts as a moisture-proof layer. The material of the organic layer 21 is, for example, PET, PEN, PI, PP, PE, PU, PMMA, etc. The thickness of the organic layer 21 is, for example, 30 μm or more and 250 μm or less. The material of the inorganic layer 22 is, for example, Al, Cu, Ti, Fe, SUS, etc. The thickness of the inorganic layer 22 is, for example, 10 μm or more and 100 μm or less. The supporting substrate 2 is flexible. The supporting substrate 2 can be bent in a manner having a radius of curvature of, for example, 30 mm or more and 120 mm or less. If the thickness of the scintillator layer 3 described later is set to T, the thickness of the supporting substrate 2 is greater than 0.2T. In addition, the supporting substrate 2 can be a substrate consisting of a single layer or a substrate consisting of a plurality of layers. In addition, a functional film such as an easy-adhesion coating, an antistatic coating, and a moisture-proof film (polyparaxylene film) can also be formed on the surface of the supporting substrate 2. In addition, the thickness of the support substrate 2 may be 0.5T or more, or may be T or more.
[0056] The scintillator layer 3 is arranged on one side relative to the supporting substrate 2 (for example, on the side where the inorganic layer 22 is arranged relative to the organic layer 21). The scintillator layer 3 includes a plurality of columnar crystals 30. The plurality of columnar crystals 30 are arranged along a plane perpendicular to the direction A. Each columnar crystal 30 extends along the direction A. The material of the scintillator layer 3 is, for example, CsI:Tl (cesium iodide containing thallium as an activator), CsI:Na (cesium iodide containing sodium as an activator), CsI:Ce (cesium iodide containing cerium as an activator), CsI:Tl,Eu (cesium iodide containing thallium and europium as activators), etc. The thickness of the scintillator layer 3 is, for example, not less than 50 μm and not more than 1000 μm (preferably not less than 50 μm and not more than 400 μm).
[0057] The plurality of columnar crystals 30 include a plurality of first ends 31 on the side of the supporting substrate 2 and a plurality of second ends 32 on the opposite side of the supporting substrate 2. Each first end 31 tapers toward the side of the supporting substrate 2. The height of each first end 31 (the width of each first end 31 in direction A) is, for example, greater than 2 μm and less than 5 μm. The taper angle of each first end 31 is, for example, greater than 60 degrees and less than 100 degrees. Each second end 32 has an end face 32a along a plane perpendicular to direction A. The plurality of second ends 32 are connected to each other. The plurality of end faces 32a are connected to each other in a flush state. In addition, the thickness of the scintillator layer 3 refers to the average value of the length of each columnar crystal 30 in direction A. In other words, the thickness of the scintillator layer 3 refers to the distance between a plane including a plurality of front ends 31a of the plurality of first ends 31 and a plane including a plurality of end faces 32a of the plurality of second ends 32.
[0058] The intermediate layer 4 includes a metal layer 41, an organic layer 42, and an adhesive layer 43. The metal layer 41 is formed along the surface of each first end 31. The metal layer 41 is directly formed on the surface of each first end 31. The metal layer 41 has a light reflection function (a function of reflecting scintillation light) or a light absorption function (a function of absorbing scintillation light). The metal layer 41 is, for example, Al, Cr, Ni, Ag, Ti, Cu, Au, etc. The thickness of the metal layer 41 is, for example, not less than 10 nm and not more than 1000 nm. The organic layer 42 is arranged in the region R between the plurality of first ends 31 via the metal layer 41, and covers the plurality of first ends 31. The material of the organic layer 42 is, for example, polyparaxylene. The thickness of the portion of the organic layer 42 located on the support substrate 2 side relative to the plane including the plurality of front ends 31a is, for example, not less than 0.5 μm and not more than 20 μm. The adhesive layer 43 is arranged between the support substrate 2 and the organic layer 42. The support substrate 2 is bonded to the organic layer 42 via the adhesive layer 43. The material of the adhesive layer 43 is a binder (not cured after bonding) or an adhesive (cured after bonding). The thickness of the adhesive layer 43 is, for example, 0.1 μm to 100 μm (preferably 25 μm or less).
[0059] A portion of the intermediate layer 4 is at least arranged in a region R between the plurality of first end portions 31. In the present embodiment, a portion of the organic layer 42 is arranged in the entire region R between the plurality of first end portions 31, and enters between the plurality of columnar crystals 30 via the region R. Here, if the distance between the supporting substrate 2 and the scintillator layer 3 (the distance between "the surface on the scintillator layer 3 side in the supporting substrate 2" and "the plane including the plurality of front ends 31a") is set to D, a portion of the organic layer 42 reaches a position that has advanced by more than D from the plurality of front ends 31a. In addition, if the thickness of the scintillator layer 3 is set to T, a portion of the organic layer 42 reaches a position that has advanced by more than 0.2T from the plurality of front ends 31a. As an example, D is greater than 10 μm and less than 20 μm, T is greater than 50 μm and less than 400 μm, and a portion of the organic layer 42 reaches a position that has advanced by a distance of greater than 100 μm and less than 200 μm from the plurality of front ends 31a. In the present embodiment, a portion of the organic layer 42 reaches the plurality of second end portions 32 between the plurality of columnar crystals 30.
[0060] The protective layer 5 covers the support substrate 2, the scintillator layer 3, and the intermediate layer 4. The material of the protective layer 5 is, for example, polyparaxylene. The thickness of the protective layer 5 is, for example, about 5 μm.
[0061] [Structure of the radiation detector]
[0062] like Figure 2As shown, the radiation detector 10 includes the above-mentioned scintillator panel 1, a sensor panel 11, and an adhesive layer 12. The sensor panel 11 has a light receiving surface 11a. A plurality of photoelectric conversion elements (not shown) are provided along the light receiving surface 11a of the sensor panel 11. Each photoelectric conversion element constitutes a pixel and outputs an electrical signal corresponding to the incident scintillation light.
[0063] The scintillator panel 1 is arranged on the light receiving surface 11a when the scintillator layer 3 is located on the sensor panel 11 side relative to the supporting substrate 2. The adhesive layer 12 is arranged between the light receiving surface 11a and the scintillator panel 1. The scintillator panel 1 is bonded to the sensor panel 11 through the adhesive layer 12. The material of the adhesive layer 12 is a light-transmitting organic material, such as OCA (Optical Clear Adhesive) or the like. The thickness of the adhesive layer 12 is, for example, not less than 0.1 μm and not more than 100 μm (preferably not more than 25 μm). In addition, the scintillator panel 1 may also have an adhesive layer 12 arranged on the opposite side of the supporting substrate 2 relative to the scintillator layer 3.
[0064] [Method for manufacturing scintillator panel]
[0065] The manufacturing method of the above-mentioned scintillator panel 1 is described. Figure 3 As shown in (a), prepare the auxiliary substrate 13. The material of the auxiliary substrate 13 is, for example, PET, PEN, PI, PMMA, AL, SUS, Glass, etc. In order to improve the smoothness and peelability, a coating such as acrylic, fluorine, silicone, aluminum oxide, ITO, SiO2, etc. may also be applied to the auxiliary substrate 13. The thickness of the auxiliary substrate 13 is, for example, not less than 0.1 mm and not more than 0.5 mm. Next, as Figure 3 As shown in (b), a scintillator layer 3 is formed on the auxiliary substrate 13 by vapor deposition (first step). In this embodiment, the scintillator layer 3 is formed on the auxiliary substrate 13 by evaporation. As a result, in the plurality of columnar crystals 30, a plurality of second end portions 32 are located on the auxiliary substrate 13 side, and a plurality of first end portions 31 are located on the opposite side of the auxiliary substrate 13. In addition, as an example of a vapor deposition method other than the evaporation method, there is a sputtering method.
[0066] Then, if Figure 4 As shown in (a) of FIG. 1 , a metal layer 41 is formed on the surface of each first end portion 31 by vapor deposition. Figure 4 As shown in (b), an organic layer 42 is formed by CVD to cover the auxiliary substrate 13, the scintillator layer 3 and the metal layer 41 (second step). Thus, a portion of the organic layer 42 is disposed in the entire region R between the plurality of first end portions 31 and also enters between the plurality of columnar crystals 30 through the region R.
[0067] Then, if Figure 5 As shown in (a), the support substrate 2 is bonded to the organic layer 42 via the adhesive layer 43. That is, the support substrate 2 is formed on the intermediate layer 4 composed of the metal layer 41, the organic layer 42 and the adhesive layer 43 (third step). Figure 5 As shown in (b), the auxiliary substrate 13, the scintillator layer 3, the intermediate layer 4 and the supporting substrate 2 are cut along the direction A (the fifth step). As a result, the side surfaces of the auxiliary substrate 13, the scintillator layer 3, the intermediate layer 4 and the supporting substrate 2 are flush with each other.
[0068] Then, if Figure 6 As shown in (a), the auxiliary substrate 13 is removed from the scintillator layer 3 (the fourth step). As a result, a plurality of end faces 32a of the plurality of second end portions 32 appear. Figure 6 As shown in (b) of FIG. 1 , the protective layer 5 is formed by the CVD method so as to cover the supporting substrate 2 , the scintillator layer 3 , and the intermediate layer 4 . In this way, the scintillator panel 1 is obtained.
[0069] [Method for manufacturing radiation detector]
[0070] The manufacturing method of the radiation detector 10 is described. Figure 2 As shown, the scintillator panel 1 and the sensor panel 11 are prepared (first step). Next, the scintillator panel 1 is bonded to the sensor panel 11 via the adhesive layer 12 in a state where the support substrate 2 is located on the opposite side of the sensor panel 11 relative to the scintillator layer 3. That is, the scintillator panel 1 is arranged on the light receiving surface 11a in a manner that the support substrate 2 is located on the opposite side of the sensor panel 11 relative to the scintillator layer 3 (second step). Thus, the radiation detector 10 is obtained.
[0071] [Function and Effect]
[0072] In the scintillator panel 1, each of the plurality of second ends 32 included in the plurality of columnar crystals 30 has an end face 32a along a plane. Thus, when the scintillator layer 3 is arranged on the light-receiving surface 11a of the sensor panel 11 in a state where the support substrate 2 is located on the opposite side of the sensor panel 11 relative to the scintillator layer 3, the contact between the light-receiving surface 11a of the sensor panel 11 and the scintillator panel 1 is appropriated. In addition, in the scintillator panel 1, a portion of the intermediate layer 4 is arranged in the region R between the plurality of first ends 31 included in the plurality of columnar crystals 30. Thus, even if the scintillator panel 1 is bent, the generation of cracks in the scintillator layer 3 can be suppressed. As a specific example, when the scintillator panel 1 is bent in a manner that the plurality of second ends 32 are separated from each other, the plurality of first ends 31 are suppressed from approaching each other, and when the scintillator panel 1 is bent in a manner that the plurality of second ends 32 are close to each other, the plurality of first ends 31 are suppressed from being separated from each other. As a result, no matter how the scintillator panel 1 is bent, the generation of cracks in the scintillator layer 3 can be suppressed. As described above, according to the scintillator panel 1 , the contact with the light receiving surface 11 a of the sensor panel 11 can be optimized and the occurrence of cracks in the scintillator layer 3 can be suppressed.
[0073] In the scintillator panel 1 , by configuring a portion of the intermediate layer 4 in the region R between the plurality of first end portions 31 included in the plurality of columnar crystals 30 , adhesion between the support substrate 2 and the scintillator layer 3 is improved, and floating of the scintillator layer 3 on the outer edge of the support substrate 2 is suppressed.
[0074] In the scintillator panel 1 , a part of the intermediate layer 4 is disposed over the entire region R between the plurality of first end portions 31 . Thus, the occurrence of cracks in the scintillator layer 3 can be reliably suppressed.
[0075] In the scintillator panel 1 , when the distance between the support substrate 2 and the scintillator layer 3 is D, a portion of the intermediate layer 4 reaches a position that is advanced by more than D from the front ends 31 a of the first end portions 31 . This can more reliably suppress the occurrence of cracks in the scintillator layer 3 .
[0076] In the scintillator panel 1 , when the thickness of the scintillator layer 3 is T, a portion of the intermediate layer 4 reaches a position that is advanced by 0.2T or more from the front ends 31 a of the first end portions 31 . This can more reliably suppress the occurrence of cracks in the scintillator layer 3 .
[0077] In the scintillator panel 1, the intermediate layer 4 includes a metal layer 41 formed along the surface of each of the plurality of first end portions 31, and an organic layer 42 arranged in a region R between the plurality of first end portions 31 via the metal layer 41, and the metal layer 41 has a light reflecting function or a light absorbing function. Thus, it is possible to realize an intermediate layer 4 that exerts a light reflecting function or a light absorbing function and can suppress the generation of cracks in the scintillator layer 3. In addition, in the case where the metal layer 41 is directly formed on the surface of each first end portion 31, even if abnormal growth occurs in a portion of the plurality of columnar crystals 30, it is not easy to form a cavity between the scintillator layer 3 and the metal layer 41.
[0078] In the scintillator panel 1, when viewed from the direction A, the outer edge of the support substrate 2, the outer edge of the scintillator layer 3, and the outer edge of the intermediate layer 4 are aligned. Thus, in the outer edge of the support substrate 2, the region where the scintillator layer 3 does not exist can be eliminated. In other words, the area of the scintillator layer 3 can be increased by the amount of the region. In other words, the area of the support substrate 2 can be reduced by the amount of the region.
[0079] In the scintillator panel 1 , the plurality of second end portions 32 are connected to one another. This makes it possible to more reliably suppress the occurrence of cracks in the scintillator layer 3 .
[0080] In the scintillator panel 1, the support substrate 2, the scintillator layer 3, and the intermediate layer 4 are covered with the protective layer 5. Thus, the plurality of deliquescent columnar crystals 30 can be protected.
[0081] In the scintillator panel 1 , the adhesive layer 12 is disposed on the side opposite to the support substrate 2 with respect to the scintillator layer 3 . Thus, the scintillator panel 1 can be easily and reliably bonded to the light receiving surface 11 a of the sensor panel 11 .
[0082] In the scintillator panel 1 , when the thickness of the scintillator layer 3 is T, the thickness of the support substrate 2 is greater than or equal to 0.2 T. This can suppress cracks in the scintillator layer 3 caused by local external force acting on a part of the scintillator panel 1 , for example, when the scintillator panel 1 is operated.
[0083] In the radiation detector 10, the contact between the light receiving surface 11a of the sensor panel 11 and the scintillator panel 1 is optimized. As a specific example, it is difficult to form a cavity or foreign matter to enter between the light receiving surface 11a and the scintillator panel 1. Therefore, according to the radiation detector 10, it is possible to obtain an appropriate radiation image. For example, when the metal layer 41 has a light reflection function, a high-brightness radiation image can be obtained, and when the metal layer 41 has a light absorption function, a high-resolution radiation image can be obtained.
[0084] According to the manufacturing method of the scintillator panel 1, it is possible to obtain a scintillator panel 1 in which the contact with the light receiving surface 11a of the sensor panel 11 is properly performed and the generation of cracks in the scintillator layer 3 is suppressed. In addition, the adhesion between the scintillator layer 3 and the supporting substrate 2 is improved by the intermediate layer 4, and on the other hand, the adhesion between the scintillator layer 3 and the auxiliary substrate 13 is reduced by each of the plurality of second end portions 32 having an end surface 32a along a plane, so that the auxiliary substrate 13 can be easily and reliably peeled off from the scintillator layer 3.
[0085] In the method for manufacturing the scintillator panel 1 , the auxiliary substrate 13 , the scintillator layer 3 , the intermediate layer 4 , and the supporting substrate 2 are cut along the direction A. Thus, the auxiliary substrate 13 , the scintillator layer 3 , the intermediate layer 4 , and the supporting substrate 2 can be cut together in a stable state in which the scintillator layer 3 , the intermediate layer 4 , and the supporting substrate 2 are supported by the auxiliary substrate 13 .
[0086] According to the method for manufacturing the radiation detector 10 , it is possible to obtain the radiation detector 10 including the scintillator panel 1 in which the contact with the light receiving surface 11 a of the sensor panel 11 is optimized and the occurrence of cracks in the scintillator layer 3 is suppressed.
[0087] Figure 7 : is a table showing the characteristics of the scintillator panels of Comparative Examples 1 and 2 and Examples 1 and 2. The scintillator panel of Comparative Example 1 comprises: a supporting substrate, a scintillator layer formed directly on the supporting substrate by a vapor deposition method, and a polyparaxylene layer covering a plurality of front ends of a plurality of columnar crystals included in the scintillator layer, and the polyparaxylene layer is arranged on the light-receiving surface of the sensor panel via an adhesive layer. The scintillator panel of Comparative Example 2 comprises: a supporting substrate, and a scintillator layer formed directly on the supporting substrate by a vapor deposition method, and a plurality of front ends of a plurality of columnar crystals included in the scintillator layer are arranged on the light-receiving surface of the sensor panel via an adhesive layer. The scintillator panel of Example 1 comprises: a supporting substrate, a scintillator layer arranged in a manner that a plurality of front ends (first ends) of a plurality of columnar crystals are located on the supporting substrate side, and a polyparaxylene layer (intermediate layer) arranged between the supporting substrate and the scintillator layer, and a plurality of roots (second ends) of a plurality of columnar crystals are directly arranged on the light-receiving surface of the sensor panel. The scintillator panel of Example 2 comprises: a supporting substrate, a scintillator layer arranged in a manner such that a plurality of front ends (first ends) of a plurality of columnar crystals are located on the supporting substrate side, and a polyparaxylene layer (middle layer) arranged between the supporting substrate and the scintillator layer, and a plurality of roots (second ends) of the plurality of columnar crystals are arranged on the light receiving surface of the sensor panel via an adhesive layer.
[0088] like Figure 7As shown, the MTF (resolution characteristics at a frequency of 3L / mm) obtained by the scintillator panels of Examples 1 and 2 becomes a value closer to 1 than the MTF obtained by the scintillator panels of Comparative Examples 1 and 2. It can be seen that the scintillator panels of Examples 1 and 2 can obtain higher resolution radiation images than the scintillator panels of Comparative Examples 1 and 2. In addition, the LOP (light output (brightness) characteristics) obtained by the scintillator panels of Examples 1 and 2 becomes a value greater than the LOP obtained by the scintillator panels of Comparative Examples 1 and 2. It can be seen that the scintillator panels of Examples 1 and 2 can obtain higher brightness radiation images than the scintillator panels of Comparative Examples 1 and 2.
[0089] [Modifications]
[0090] The present disclosure is not limited to the above-mentioned embodiments. For example, in the scintillator panel 1, a portion of the intermediate layer 4 only needs to be disposed at least in the region R between the plurality of first end portions 31. Furthermore, in the scintillator panel 1, a portion of the intermediate layer 4 only needs to be disposed at least in a portion of the region R. Figure 8 to Figure 14 The deformability of the intermediate layer 4 will be described.
[0091] like Figure 8 As shown, a portion of the organic layer 42 may not reach the plurality of second end portions 32 between the plurality of columnar crystals 30. Fig. 9 As shown in (a) and (b), the intermediate layer 4 may also include a metal layer 41, an organic layer 42, an inorganic layer 44, an organic layer 45, and an adhesive layer 43. The inorganic layer 44 is arranged between the organic layer 42 and the adhesive layer 43, and acts as a moisture-proof layer. The material of the inorganic layer 44 is, for example, Al, Cr, Ni, Ag, Ti, Cu, Au, SiO2, Al2O3, SiON, SiN, etc. The organic layer 45 is arranged between the inorganic layer 44 and the adhesive layer 43. The material of the organic layer 45 is, for example, polyparaxylene. In this case, the supporting substrate 2 includes the organic layer 21, and may not include the inorganic layer 22. In addition, a portion of the organic layer 42 may be as shown in FIG. Fig. 9 As shown in (a), between the plurality of columnar crystals 30, the plurality of second end portions 32 may also be formed. Fig. 9 As shown in (b), the plurality of second end portions 32 are not reached between the plurality of columnar crystals 30 .
[0092] like Fig.10 As shown in (a), the intermediate layer 4 includes a metal layer 41 and an adhesive layer 43, and may not include an organic layer 42. In this case, a portion of the adhesive layer 43 is disposed in a region R between the plurality of first end portions 31. Fig.10 As shown in (b) , a portion of the organic layer 42 may be disposed only in the region R between the plurality of first end portions 31 .
[0093] like Fig.11 As shown in (a) and (b), the intermediate layer 4 includes an organic layer 42, an adhesive layer 46, an organic layer 47, and an adhesive layer 43, and may not include the metal layer 41. The organic layer 47 is arranged between the organic layer 42 and the adhesive layer 43, and has a light reflecting function or a light absorbing function. The organic layer 47 is, for example, a sheet containing a pigment. The material of the sheet is, for example, PET, PEN, PI, PP, PE, PU, PMMA, etc. In the case where the organic layer 47 has a light reflecting function, the pigment is, for example, TiO2, etc. In the case where the organic layer 47 has a light absorbing function, the pigment is, for example, C, etc. The thickness of the organic layer 47 is, for example, not less than 30 μm and not more than 250 μm. The adhesive layer 46 is arranged between the organic layer 42 and the organic layer 47. The organic layer 47 is bonded to the organic layer 42 through the adhesive layer 46. In this case, the supporting substrate 2 can be as shown in Fig.11 As shown in (a), it is bonded to the organic layer 47 through the bonding layer 43, or it can be as shown in Fig.11 As shown in (b), the organic layer 48 formed on the organic layer 47 is bonded to the organic layer 48 via the bonding layer 43. The material of the organic layer 48 is, for example, polyparaxylene.
[0094] like Fig.12 As shown in (a) and (b) of FIG. 1 , the intermediate layer 4 includes the adhesive layer 46 , the organic layer 47 , and the adhesive layer 43 , and may not include the metal layer 41 and the organic layer 42 . Fig.12 In the intermediate layer 4 shown in (a), a portion of the adhesive layer 46 is arranged in the region R between the plurality of first end portions 31. Fig.11 The intermediate layer 4 shown in (a) is different. Fig.12 In the intermediate layer 4 shown in (b), a portion of the adhesive layer 46 is arranged in the region R between the plurality of first end portions 31. Fig.11 The intermediate layer 4 shown in (b) is different.
[0095] like Fig.13 As shown in (a) and (b), the intermediate layer 4 includes an organic layer 42, an organic layer 49, and an adhesive layer 43, and may not include the metal layer 41. The organic layer 49 is arranged between the organic layer 42 and the adhesive layer 43, and has a light reflecting function or a light absorbing function. The organic layer 49 is, for example, a coating film containing a pigment. The material of the coating film is, for example, epoxy, silicone, fluorine, urethane (urethan), acryl (acryl), etc. In the case where the organic layer 49 has a light reflecting function, the pigment is, for example, TiO2. In the case where the organic layer 49 has a light absorbing function, the pigment is, for example, C. The thickness of the organic layer 49 is, for example, not less than 5 μm and not more than 250 μm. In this case, the supporting substrate 2 can be as follows Fig.13As shown in (a), it is bonded to the organic layer 49 through the bonding layer 43, or it can be as shown in Fig.13 As shown in (b), the organic layer 48 formed on the organic layer 49 is bonded via the adhesive layer 43.
[0096] like Fig.14 As shown in (a) and (b) of FIG. 1 , the intermediate layer 4 includes the organic layer 49 and the adhesive layer 43 , and may not include the metal layer 41 and the organic layer 42 . Fig.14 In the intermediate layer 4 shown in (a), a portion of the organic layer 49 is arranged in the region R between the plurality of first end portions 31. Fig.13 The intermediate layer 4 shown in (a) is different. Fig.14 In the intermediate layer 4 shown in (b), a portion of the organic layer 49 is arranged in the region R between the plurality of first end portions 31. Fig.13 Even in this case, the intermediate layer 4 that can exert a light reflection function or a light absorption function and suppress the generation of cracks in the scintillator layer 3 can be realized.
[0097] In addition, in the scintillator panel 1, the intermediate layer 4 may not include a layer having a light reflecting function or a light absorbing function, and the supporting substrate 2 may include a layer having a light reflecting function or a light absorbing function. In addition, in the scintillator layer 3, the plurality of second end portions 32 may not be connected to each other. In addition, the protective layer 5 may also be as shown in FIG. Fig.15 As shown, the surface of the scintillator layer 3 opposite to the support substrate 2 is not covered. In this case, the adhesive layer 12, as a part of the scintillator panel 1, may be directly formed on the surface of the scintillator layer 3 opposite to the support substrate 2. In addition, in the scintillator panel 1, as long as at least a portion of the outer edge of the support substrate 2, at least a portion of the outer edge of the scintillator layer 3, and at least a portion of the outer edge of the intermediate layer 4 are aligned when viewed from the direction A.
[0098] In addition, if Fig.16 As shown, the radiation detector 10 may also include a sealing member 14. The sealing member 14 extends in a frame-like shape in a region surrounding the light-receiving surface 11a on the surface of the sensor panel 11, and covers the side of the scintillator panel 1. The material of the sealing member 14 is, for example, epoxy, silicone, fluorine, urethane, acrylic, etc. The material of the sealing member 14 may also include a filler composed of an inorganic material such as glass. The material of the filler only needs to have a higher moisture resistance than the main material of the sealing member 7, and is, for example, SiO2, Al2O3, TiO2, etc.
[0099] In addition, in the radiation detector 10, as shown in FIG. Fig.17As shown in (a) and (b), the adhesive layer 12 may not be arranged between the sensor panel 11 and the scintillator panel 1. For example, the sensor panel 11 and the scintillator panel 1 may be arranged together with an elastic member 15 such as a sponge in a frame (not shown), thereby maintaining the contact state between the sensor panel 11 and the scintillator panel 1. In addition, in the radiation detector 10, other components such as fiber-optic plates may be arranged between the sensor panel 11 and the scintillator panel 1.
[0100] In addition, in the fifth step of the method for manufacturing the scintillator panel 1, it is sufficient to at least cut the scintillator layer 3, the intermediate layer 4, and the supporting substrate 2 along the direction A. That is, in the fifth step, the auxiliary substrate 13 may not be cut. Even in this case, the scintillator layer 3, the intermediate layer 4, and the supporting substrate 2 can be cut together in a stable state in which the scintillator layer 3, the intermediate layer 4, and the supporting substrate 2 are supported by the auxiliary substrate 13. In addition, in the fifth step, if the auxiliary substrate 13 is not completely cut, a slit may be engraved on the auxiliary substrate 13.
[0101] In addition, in the manufacturing method of the scintillator panel 1, the scintillator layer 3, the intermediate layer 4, and the supporting substrate 2 may be further cut along the direction A (sixth step) after the fourth step of removing the auxiliary substrate 13 from the scintillator layer 3. In this case, the scintillator layer 3, the intermediate layer 4, and the supporting substrate 2 can be easily and reliably cut in a prescribed size. In addition, in the manufacturing method of the scintillator panel 1, the scintillator layer 3, the intermediate layer 4, and the supporting substrate 2 may not be cut before the fourth step of removing the auxiliary substrate 13 from the scintillator layer 3, but the scintillator layer 3, the intermediate layer 4, and the supporting substrate 2 may be cut after the fourth step of removing the auxiliary substrate 13 from the scintillator layer 3.
Claims
1. A scintillator panel, in, have: A supporting substrate having flexibility; a scintillator layer comprising a plurality of columnar crystals; and an intermediate layer disposed between the support substrate and the scintillator layer, The plurality of columnar crystals include: a plurality of first end portions on the support substrate side and a plurality of second end portions on the opposite side to the support substrate. Each of the plurality of first end portions becomes thinner toward the support substrate side, Each of the plurality of second end portions has an end surface along a plane, A portion of the intermediate layer is disposed at least in a region between the plurality of first end portions.
2. The scintillator panel according to claim 1, in, A portion of the intermediate layer is disposed at least in the entire region between the plurality of first end portions.
3. The scintillator panel according to claim 1 or 2, in, If the distance between the support substrate and the scintillator layer is defined as D, the portion of the intermediate layer reaches a position that is advanced by more than D from the plurality of leading ends of the plurality of first end portions.
4. The scintillator panel according to any one of claims 1 to 3, in, When the thickness of the scintillator layer is defined as T, the portion of the intermediate layer reaches a position advanced by 0.2T or more from the plurality of leading ends of the plurality of first end portions.
5. The scintillator panel according to any one of claims 1 to 4, in, The middle layer comprises: a metal layer formed along a surface of each of the plurality of first end portions; and an organic layer, which is arranged at least in the region between the plurality of first end portions via the metal layer, The metal layer has a light reflection function or a light absorption function.
6. The scintillator panel according to any one of claims 1 to 4, in, The intermediate layer includes an organic layer at least disposed in the region between the plurality of first end portions. The organic layer has a light reflecting function or a light absorbing function.
7. The scintillator panel according to any one of claims 1 to 6, in, When viewed in the thickness direction of the support substrate, at least a portion of an outer edge of the support substrate, at least a portion of an outer edge of the scintillator layer, and at least a portion of an outer edge of the intermediate layer coincide with each other.
8. The scintillator panel according to any one of claims 1 to 7, in, The plurality of second end portions are connected to each other.
9. The scintillator panel according to any one of claims 1 to 8, in, A protective layer covering the support substrate, the scintillator layer, and the intermediate layer is further provided.
10. The scintillator panel according to any one of claims 1 to 9, in, The invention further includes an adhesive layer disposed on the side of the scintillator layer opposite to the support substrate.
11. The scintillator panel according to any one of claims 1 to 10, in, If the thickness of the scintillator layer is defined as T, the thickness of the support substrate is equal to or greater than 0.2T.
12. A radiation detector, in, have: The scintillator panel according to any one of claims 1 to 11; and A sensor panel having a light receiving surface, The scintillator panel is disposed on the light receiving surface in a state in which the scintillator layer is located on the sensor panel side with respect to the support substrate.
13. A method for manufacturing a scintillator panel, in, The manufacturing method is a method for manufacturing a scintillator panel according to any one of claims 1 to 11, comprising: The first step is to form the scintillator layer on the auxiliary substrate by vapor deposition; a second step of forming the intermediate layer on the scintillator layer after the first step in such a manner that a portion of the intermediate layer is disposed at least in the region between the first end portions; A third step, after the second step, forming the support substrate on the intermediate layer; as well as A fourth step, after the third step, of removing the auxiliary substrate from the scintillator layer.
14. The method for manufacturing a scintillator panel according to claim 13, in, After the third step and before the fourth step, the method further comprises: In a fifth step, at least the scintillator layer, the intermediate layer, and the support substrate are cut along a thickness direction of the support substrate.
15. The method for manufacturing a scintillator panel according to claim 14, in, In the fifth step, the auxiliary substrate is cut along the thickness direction of the support substrate together with the scintillator layer, the intermediate layer, and the support substrate.
16. The method for manufacturing a scintillator panel according to any one of claims 13 to 15, in, After the fourth step, the method further comprises: In a sixth step, the scintillator layer, the intermediate layer, and the support substrate are cut along a thickness direction of the support substrate.
17. A method for manufacturing a radiation detector, in, The manufacturing method is a method for manufacturing the radiation detector according to claim 12, comprising: The first step is to prepare the scintillator panel and the sensor panel; In a second step, after the first step, the scintillator panel is disposed on the light receiving surface so that the support substrate is located on the opposite side of the sensor panel with respect to the scintillator layer.