Negative electrode active material for secondary battery, and secondary battery

By using silicate composite particles in secondary batteries to adjust their diffraction peak ratio and crystallinity, the cracking problem caused by expansion and contraction of silicon particles is solved, and efficient charge and discharge cycle characteristics and stability are achieved.

CN118891750APending Publication Date: 2024-11-01PANASONIC ENERGY CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380025240.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-09
Filing Date
2023-03-03
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The composite particles of the lithium silicate phase and the silicon particles dispersed in the lithium silicate phase used in existing secondary batteries expand and contract the silicon particles during charging and discharging, resulting in large stress. , resulting in cracks and cracks of composite particles, reducing binding force, affecting the charge and discharge cycle characteristics.

Method used

Silicate composite particles are used, which contain lithium silicate phase, silicon oxide phase and silicon phase. The specific intensity and crystallinity of the silicon oxide phase and silicon phase are adjusted by X-ray diffraction method to ensure silicon oxide near 2θ=26° The ratio of the diffraction peak A of the phase to the diffraction peak B of the silicon phase near 28° is 0.9 or more and 1.4 or less, so that the crystallinity of the silicon oxide phase is improved to suppress cracks and cracks of the composite particles.

Benefits of technology

The excellent charge and discharge cycle characteristics of the negative electrode active material in the secondary battery are achieved, and the cycle stability and capacity density of the battery are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118891750A_ABST
    Figure CN118891750A_ABST
Patent Text Reader

Abstract

The negative electrode active material for a secondary battery comprises silicate composite particles. The silicate composite particles comprise a lithium silicate phase containing lithium, silicon, and oxygen, a silicon oxide phase containing SiO2, and a silicon phase, and the silicon oxide phase and the silicon phase are dispersed in the lithium silicate phase. In a diffraction pattern by X-ray diffraction (XRD), the ratio IA / IB of the maximum intensity IA of a diffraction peak A from the SiO2 (011) plane of a silicon oxide phase appearing near 2 [theta] = 26 DEG to the maximum intensity IB of a diffraction peak B from the Si (111) plane of a silicon phase appearing near 2 [theta] = 28 DEG is 0.9-1.4.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a negative electrode active material for a secondary battery and a secondary battery. Background Art

[0002] Non-aqueous electrolyte secondary batteries, especially lithium-ion secondary batteries, are expected to be used as power sources for small-scale civilian applications, power storage devices, and electric vehicles due to their high voltage and high energy density. In the process of requiring batteries to have higher energy density, materials containing silicon that alloys with lithium are expected to be used as negative electrode active materials with high theoretical capacity density.

[0003] Patent Document 1 proposes using a non-aqueous electrolyte secondary battery having a Li 2z SiO 2+z A negative electrode active material comprising a lithium silicate phase represented by (0<z<2) and silicon particles dispersed in the lithium silicate phase.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: International Publication No. 2016 / 35290 Pamphlet Summary of the invention

[0007] Problems to be solved by the invention

[0008] The composite particles comprising a lithium silicate phase and silicon particles dispersed in the lithium silicate phase and the composite particles (SiO x ) compared to the original, the irreversible capacity accompanying charge and discharge is small, which is beneficial to the improvement of the initial charge and discharge efficiency.

[0009] However, it is known that the above-mentioned composite particles have a large expansion and contraction degree of silicon particles accompanied by the absorption and release of lithium during charge and discharge. Therefore, accompanied by the expansion and contraction of the silicon particles, a large stress is generated in the lithium silicate phase present around the silicon particles, thereby generating cracks and cracks in the composite particles. Accompanying this, the bonding force between the composite particles and the surrounding binding materials becomes weak, and in particular, the broken composite particles lose the conductive path with the surrounding particles and become isolated, causing a reduction in the charge and discharge cycle characteristics.

[0010] Means for solving problems

[0011] In view of the above, one aspect of the present invention relates to a negative electrode active material for a secondary battery, comprising a silicate composite particle, wherein the silicate composite particle comprises a lithium silicate phase, a silicon oxide phase and a silicon phase, wherein the lithium silicate phase comprises lithium, silicon and oxygen, the silicon oxide phase comprises SiO2, the silicon oxide phase and the silicon phase are dispersed in the lithium silicate phase, and in a diffraction pattern of the silicate composite particle based on X-ray diffraction (XRD), a maximum intensity I of a diffraction peak A from the SiO2 (011) plane of the silicon oxide phase appearing near 2θ = 26° is A The maximum intensity I of the diffraction peak B originating from the Si(111) plane of the silicon phase appears near 2θ=28° B Ratio I A / I B It is 0.9 or more and 1.4 or less.

[0012] Another aspect of the present invention relates to a secondary battery comprising a positive electrode, a negative electrode, an electrolyte, and a separator interposed between the positive electrode and the negative electrode, wherein the negative electrode comprises a current collector and a negative electrode active material layer, and the negative electrode active material layer comprises the negative electrode active material for the secondary battery.

[0013] Effects of the Invention

[0014] By using the negative electrode active material for a secondary battery of the present invention, a secondary battery having excellent charge and discharge cycle characteristics can be realized.

[0015] The novel features of the present invention are described in the scope of the appended claims, but the present invention in both structure and content together with other objects and features of the present invention should be more fully understood through the following detailed description with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is a diagram schematically showing a cross section of a negative electrode active material according to one embodiment of the present invention.

[0017] Figure 2 This is a schematic perspective view showing a partially cutaway portion of a secondary battery according to an embodiment of the present invention.

[0018] Figure 3 This is a graph showing the diffraction patterns of the silicate composite particles used in the secondary batteries of Example 1 and Comparative Example 1, obtained by X-ray diffraction (XRD). DETAILED DESCRIPTION

[0019] Hereinafter, the embodiments of the present invention will be described with examples, but the present invention is not limited to the examples described below. In the following description, specific numerical values ​​and materials are sometimes exemplified, but other numerical values ​​and materials may also be applied as long as the effect of the present invention can be obtained. In this specification, the description of "numerical value A to numerical value B" includes numerical value A and numerical value B, and may be renamed as "numerical value A or more and numerical value B or less". In the following description, when the lower limit and upper limit of numerical values ​​for specific physical properties, conditions, etc. are exemplified, as long as the lower limit is not above the upper limit, any one of the exemplified lower limits may be arbitrarily combined with any one of the exemplified upper limits. When multiple materials are exemplified, one may be selected and used alone, or two or more may be used in combination.

[0020] In addition, the present invention includes a combination of matters recorded in two or more claims arbitrarily selected from a plurality of claims recorded in the scope of the attached claims. That is, as long as no technical contradiction occurs, matters recorded in two or more claims arbitrarily selected from a plurality of claims recorded in the scope of the attached claims may be combined.

[0021] [Negative electrode active material for secondary batteries]

[0022] The negative electrode active material for a secondary battery according to an embodiment of the present invention comprises silicate composite particles. The silicate composite particles comprise a lithium silicate phase containing lithium (Li), silicon (Si) and oxygen (O), a silicon oxide phase containing SiO2 and a silicon phase (silicon particles), wherein the silicon oxide phase and the silicon phase are dispersed in the lithium silicate phase. It should be noted that "silicate composite particles" will be referred to as "composite particles" in some places hereinafter.

[0023] In the diffraction pattern of the silicate composite particles of the present embodiment based on the X-ray diffraction method (XRD), peaks from the silicon oxide phase, the silicon phase and the lithium silicate phase may appear. Specifically, in the range of 2θ=25° to 27° (hereinafter referred to as 2θ=26° or thereabouts), a diffraction peak A from the SiO2(011) plane of the silicon oxide phase is observed. In addition, in the range of 2θ=27° to 30° (hereinafter referred to as 2θ=28° or thereabouts), a diffraction peak B from the Si(111) plane of the silicon phase is observed. In addition, in the range of 2θ=23° to 25°, a peak from the lithium silicate phase (Li2Si2O5) may appear. However, since the lithium silicate phase contains many amorphous phases, its peak intensity is small. It should be noted that the X-rays used in the XRD method use Cu Kα rays.

[0024] It should be noted that in the range of 2θ=18° to 20°, a peak derived from lithium silicate Li2SiO3 can be further observed, and in the range of 2θ=20° to 21°, a peak derived from SiO2 can be further observed.

[0025] According to the negative electrode active material for a secondary battery of an embodiment of the present invention, in the diffraction pattern of the silicate composite particles based on X-ray diffraction (XRD), the maximum intensity I of the diffraction peak A originating from the SiO2 (011) plane of the silicon oxide phase appearing near 2θ=26° is A The maximum intensity I of the diffraction peak B from the Si(111) plane of the silicon phase appears near 2θ=28° B Ratio I A / I B is greater than or equal to 0.9 and less than or equal to 1.4. A / I B When the ratio is 0.9 or more, the crystallinity of the silicon oxide phase in the silicate composite particles can be improved. Thus, the hardness of the silicate composite particles is improved, and cracks and fissures in the composite particles can be suppressed.

[0026] Than I A / I B The upper limit is not particularly limited to 0.9 or more. However, from the perspective of easy manufacture of silicate composite particles and easy realization of secondary batteries with excellent charge-discharge cycle characteristics, the upper limit is preferably 0.9 or more. A / I B It can be below 1.4.

[0027] In the diffraction pattern, the half-value width W of the diffraction peak B from Si contained in the silicon phase is B The half-value width W of the diffraction peak A from SiO2 contained in the silicon oxide phase can be 0.3° or more and 1.5° or less based on 2θ. A Based on 2θ, it can be 0.6° or less, or 0.2° or more and 0.6° or less. If each half-value width is within this range, the cracks and cracks of the silicate composite particles are significantly suppressed, and it is easy to realize a secondary battery with excellent charge and discharge cycle characteristics. In this specification, the half-value width of the diffraction peak refers to the full width at half maximum (FWHM).

[0028] In the diffraction pattern, the integrated intensity S of the diffraction peak A is A The integrated intensity S of the diffraction peak B B The ratio of S A / S B In this case, the content ratio of the silicon phase and the silicon oxide phase dispersed in the lithium silicate phase is appropriate, and a secondary battery having excellent charge and discharge cycle characteristics can be easily realized using the silicate composite particles.

[0029] The maximum intensity, half-value width and integrated intensity of the diffraction peaks A and B are obtained by analyzing the X-ray diffraction pattern using Cu-Kα rays. The diffraction peaks A and B are separated from the X-ray diffraction pattern, and the maximum intensity, half-value width and integrated intensity obtained for the separated diffraction peak A are respectively set as I A , W A and S A The maximum intensity, half-value width and integrated intensity of the separated diffraction peak B are set as I B , W B and S B The intensity of the separated diffraction peak A was integrated within the range of the diffraction angle 2θ of 25° to 27° to obtain S. A The intensity of the separated diffraction peak B was integrated within the range of the diffraction angle 2θ of 27° to 30° to obtain S. B .

[0030] For example, lithium silicate is mixed with silicon particles, the mixture is composited by crushing using a ball mill or the like, and the crushed mixture is sintered to produce silicate composite particles. Lithium silicate can be obtained by mixing and sintering a silicon raw material (such as silicon dioxide) with a lithium raw material. At this time, in the manufacturing process of lithium silicate, if there is too much silicon raw material relative to the lithium raw material, silicon oxide can be generated. Silicon oxide crystallizes in the sintering process after compositeization and precipitates finely in the lithium silicate phase in the form of silicon oxide phase. Crystallized silicon oxide is stable and will not become an important factor in irreversible reactions during charging, and because it is fine, it is not easy to hinder the expansion and contraction of the silicon phase.

[0031] Silicon oxide is harder than lithium silicate phase and has low flexibility. By dispersing a silicon oxide phase with high hardness in the lithium silicate phase, the stress accompanying the expansion and contraction of the silicon phase can be dispersed in the entire lithium silicate phase, and the volume change of the silicate composite particles accompanying the expansion and contraction of the silicon phase can be suppressed. In addition, by improving the crystallinity of the silicon oxide phase, the volume change of the silicate composite particles is further suppressed, and a negative electrode active material with good cycle characteristics can be realized.

[0032] The crystallinity of the silicon oxide phase can be controlled by changing the heating and pressurizing conditions during sintering of the composite mixture, thereby controlling the maximum intensity I of the diffraction peak A. A , half-value width W A And the integrated intensity S A During sintering, a hot press may be used for pressurization. For example, the pressurization pressure (surface pressure) is set to 200 to 600 MPa, the heating temperature is set to 600 to 1000°C, and hot pressing is performed for 2 to 8 hours, thereby obtaining a product with a ratio of I A / I BMore preferably, the pressing pressure (surface pressure) is 200 to 600 MPa, the heating temperature is 750 to 950° C., and hot pressing is performed for 2 to 6 hours, thereby making it easier to obtain the target composite particles.

[0033] When synthesizing lithium silicate, highly crystalline silicon dioxide can be used as the silicon raw material. By controlling the input amount and / or crystallinity of silicon dioxide added as the silicon raw material, the crystallinity of the silicon oxide phase dispersed in the lithium silicate phase can be highly controlled in the silicate composite particles, and a particle size ratio of 1. A / I B The silicate composite particles have a particle size of 0.9 or more.

[0034] In the silicate composite particles, the atomic ratio of O to Si in the lithium silicate phase (O / Si ratio) is, for example, greater than 2 and less than 4. When the O / Si ratio is greater than 2 and less than 4 (z in the formula described below is 0<z<2), it is advantageous in terms of stability and lithium ion conductivity. Preferably, the O / Si ratio is greater than 2 and less than 3 (z in the formula described below is 0<z<1). The atomic ratio of Li to Si in the lithium silicate phase (Li / Si ratio) is, for example, greater than 0 and less than 4.

[0035] The lithium silicate phase contains 2z SiO 2+z The oxide layer is represented by (0<z<2). From the viewpoints of stability, ease of production, lithium ion conductivity, etc., z preferably satisfies the relationship of 0<z<1, and z=1 / 2 is more preferred.

[0036] The lithium silicate phase may contain elements other than Li, Si, and O (oxygen). For example, the lithium silicate phase may contain at least one element selected from alkali metal elements (excluding Li) and Group II elements.

[0037] By including alkali metal elements other than Li in the lithium silicate phase, crystallization is difficult to occur, the viscosity in the softened state is low, and the fluidity becomes high. As a result, even in heat treatment at low temperatures, it is easy to fill the gaps between silicon phases and to generate dense composite particles. Since alkali metal elements are cheap, they can be Na and / or K. The atomic ratio of the alkali element X (for example, K) other than Li contained in the lithium silicate phase to Li (X / Li ratio) is, for example, 0.1 to 7.1, or it can be greater than 0.4 and less than 5, or it can be greater than 0.7 and less than 2.

[0038] The lithium silicate phase may contain Group II elements. Generally speaking, the silicate phase exhibits alkalinity, and the Group II elements have the effect of inhibiting the dissolution of alkali metals from the silicate phase. As a result, the viscosity of the slurry is easily stabilized when preparing a slurry containing a negative electrode active material. As a result, the necessity of a treatment (such as an acid treatment) for neutralizing the alkaline component of the silicate composite particles is also reduced. The content of the Group 1I element relative to the total amount of elements other than O contained in the lithium silicate phase is, for example, less than 20 mol%, or less than 15 mol%, or less than 10 mol%.

[0039] The lithium silicate phase may contain element M. Element M may be at least one selected from B, Al, Ca, Mg, Zr, Nb, Ta, La, V, Y, Ti, P, Bi, Zn, Sn, Pb, Sb, Co, Er, F and W. By making the lithium silicate phase contain these elements M, the chemical stability and lithium ion conductivity of the composite particles are improved, and the side reactions caused by the contact between the lithium silicate phase and the non-aqueous electrolyte can be suppressed. Specifically, for example, B has a low melting point, which is beneficial to improve the fluidity during sintering. Although Ca reduces ion conductivity, it has the effect of increasing the hardness of the lithium silicate phase. Al, Zr, Nb, Ta and La can increase the hardness while keeping the ion conductivity unchanged. In addition, La forms a crystalline phase with low reactivity with lithium ions in the lithium silicate phase, reducing the sites that can react with lithium ions in the lithium silicate phase. As a result, the irreversible capacity is reduced and the initial charge and discharge efficiency is improved.

[0040] From the viewpoint of electrolyte resistance and structural stability, the element M is preferably at least one selected from Zr, Ti, P, Al and B. The element M may also form a compound. The compound may be, for example, a silicate of the element M or an oxide of the element M, depending on the type of the element M.

[0041] The content of the element M is, for example, 20 mol % or less, 15 mol % or less, 10 mol % or less, or 5 mol % or less, relative to the total amount of elements other than O contained in the lithium silicate phase.

[0042] The contents of B, Na, K and Al contained in the lithium silicate phase can be determined by quantitative analysis in accordance with JIS R3105 (1995) (analysis method of borosilicate glass), and the Ca content can be determined by quantitative analysis in accordance with JIS R3101 (1995) (analysis method of soda-lime glass).

[0043] The lithium silicate phase may further contain trace amounts of other elements such as iron (Fe), chromium (Cr), nickel (Ni), manganese (Mn), copper (Cu), and molybdenum (Mo).

[0044] The elements contained in the composite particles can be determined by the following method. First, a sample of the lithium silicate phase or the silicate composite particles containing the lithium silicate phase is completely dissolved in a heated acid solution (a mixed acid of hydrofluoric acid, nitric acid, and sulfuric acid), and the carbon in the solution residue is removed by filtration. Thereafter, the resulting filtrate is analyzed by inductively coupled plasma atomic emission spectrometry (ICP-AES) to measure the spectral intensities of the respective elements. Next, a standard curve is prepared using a commercially available standard solution of the element, and the content of each element contained in the lithium silicate phase is calculated.

[0045] In the silicate composite particles, there are a lithium silicate phase, a silica phase, and a silicon phase. However, they can be quantitatively analyzed separately by using Si-NMR. The Si content obtained by ICP-AES as described above is the sum of the Si amounts in the silicon phase, the lithium silicate phase, and the silica phase. On the other hand, the Si amount in the silicon phase can be quantitatively analyzed separately by using Si-NMR. Thus, by subtracting the Si amount in the silicon phase and the Si amount in the silica phase from the Si content obtained by ICP-AES, the Si amount in the lithium silicate phase can be quantitatively analyzed. It should be noted that as the standard substance necessary for the quantitative analysis, a mixture containing a silicate phase and a silicon phase with a known Si content in a specified ratio may be used.

[0046] Hereinafter, the measurement conditions of the desired Si-NMR are given.

[0047] <Si-NMR Measurement Conditions>

[0048] Measuring apparatus: Solid nuclear magnetic resonance spectrometer (INOVA-400) manufactured by Varian

[0049] Probe: Varian 7mm CPMAS-2

[0050] MAS: 4.2 kHz

[0051] MAS speed: 4 kHz

[0052] Pulse: DD (45° pulse + signal acquisition time 1H decoupling)

[0053] Repetition time: 1200 sec to 3000 sec

[0054] Observation width: 100 kHz

[0055] Observation center: Around -100 ppm

[0056] Signal acquisition time: 0.05 sec

[0057] Number of accumulations: 560

[0058] Sample amount: 207.6 mg

[0059] In order to increase the capacity and improve the cycle characteristics, the content of the silicon phase (silicon particles) in the silicate composite particles is, for example, 30% by mass or more and 80% by mass or less. By setting the content of the silicon phase to 30% by mass or more, the proportion of the lithium silicate phase becomes smaller, and the initial charge and discharge efficiency is easy to improve. In addition, the diffusibility of lithium ions is good, and it is easy to obtain excellent load characteristics. By setting the content of the silicon phase to 80% by mass or less, it is easy to reduce the degree of expansion and contraction of the silicate composite particles during charge and discharge, and it is easy to improve the cycle characteristics. The content of the silicon phase in the silicate composite particles is preferably 40% by mass or more, and more preferably 50% by mass or more.

[0060] The average particle size of the silicate composite particles is, for example, not less than 1 μm and not more than 25 μm, or not less than 4 μm and not more than 15 μm. In the above particle size range, it is easy to relieve the stress caused by the volume change of the composite material accompanying charging and discharging, and it is easy to obtain good cycle characteristics. The surface area of ​​the composite material particles also becomes appropriate, and the capacity reduction caused by the side reaction with the non-aqueous electrolyte is also suppressed. Here, the so-called average particle size means the particle size (volume average particle size) at which the volume cumulative value reaches 50% in the particle size distribution measured by the laser diffraction scattering method. The measuring device can be, for example, "LA-750" manufactured by HORIBA Co., Ltd.

[0061] In silicate composite particles, from the viewpoint of suppressing the cracking of the silicon phase itself accompanying charging and discharging, the average particle size of the silicon phase is preferably less than 500nm, more preferably less than 200nm, and further preferably less than 50nm before the first charge. After the first charge, the average particle size of the silicon phase is preferably less than 400nm, more preferably less than 100nm. By miniaturizing the silicon phase, the volume change during charging and discharging becomes smaller, and the structural stability of the composite particles is further improved. In addition, the expansion and contraction of the silicon phase is homogenized, and particle cracks are suppressed, thereby improving the cycle characteristics. The average particle size of the silicon phase is measured using a cross-sectional image of the composite material obtained using SEM. Specifically, the average particle size of the silicon phase can be obtained by averaging the maximum diameters of any 100 silicon phases.

[0062] The silicon phase dispersed in the lithium silicate phase has a particle-like phase of a silicon (Si) single substance, and is composed of a single or multiple crystallites. The crystallite size of the silicon phase is preferably less than 30nm. When the crystallite size of the silicon phase is less than 30nm, the stress generated by the volume change of the silicon phase is easily dispersed in the composite particles, and the cracks and cracks of the composite particles are suppressed. In addition, the volume change caused by the expansion and contraction of the silicon phase accompanying charging and discharging can be reduced, and the cycle characteristics are further improved. For example, due to the formation of gaps around the silicon phase during the contraction of the silicon phase, the contact points with the surrounding are reduced, and the isolation of the silicon phase caused by this is suppressed, and the reduction in charge and discharge efficiency caused by the isolation of the silicon phase is suppressed. The lower limit of the crystallite size of the silicon phase is not particularly limited, for example, it is 5nm. If the crystallite size of the silicon phase is greater than 5nm, the surface area of ​​the silicon phase can be controlled to be smaller, so it is not easy to produce the degradation of the silicon phase accompanied by the generation of irreversible capacity.

[0063] The crystallite size of the silicon phase can be calculated using the Scherrer equation from the half-value width of the diffraction peak attributable to the Si (111) plane in the X-ray diffraction (XRD) spectrum of the silicon phase.

[0064] At least a portion of the surface of the silicate composite particles may be covered with a conductive material. Since the lithium silicate phase lacks electronic conductivity, the conductivity of the silicate composite particles is also likely to decrease. However, by forming a conductive layer by covering the surface of the composite particles with a conductive material, the conductivity of the silicate composite particles can be improved. A carbon material is preferably used as the conductive material. The carbon material preferably includes at least one selected from a carbon compound and a carbonaceous material.

[0065] The thickness of the conductive layer is preferably thin enough not to substantially affect the average particle size of the silicate composite particles. The thickness of the conductive layer is preferably 1 to 200 nm, more preferably 5 to 100 nm, in consideration of ensuring conductivity and diffusibility of lithium ions. The thickness of the conductive layer can be measured by cross-sectional observation of the silicate composite particles using a SEM or TEM (transmission electron microscope).

[0066] As carbon compounds, for example, compounds containing carbon and hydrogen, compounds containing carbon, hydrogen and oxygen can be mentioned. As carbonaceous materials, low-crystalline amorphous carbon, high-crystalline graphite, etc. can be used. As amorphous carbon, carbon black, coal, coke, charcoal, activated carbon, etc. can be mentioned. As graphite, natural graphite, artificial graphite, graphitized mesophase carbon particles, etc. can be mentioned. Among them, amorphous carbon is preferred from the perspective of low hardness and large buffering effect on the silicon phase whose volume changes due to charge and discharge. Amorphous carbon can be easily graphitized carbon (soft carbon) or difficult to graphitize carbon (hard carbon). As carbon black, acetylene black, Ketjen black, etc. can be mentioned.

[0067] Silicate composite particles can be taken out from the battery using the following method. First, disassemble the battery and take out the negative electrode, wash the negative electrode with anhydrous ethyl methyl carbonate or dimethyl carbonate, and remove the electrolyte. Then, peel off the negative electrode mixture from the copper foil and crush it in a mortar to obtain a sample powder. Then, dry the sample powder in a dry atmosphere for 1 hour, and immerse it in 6M hydrochloric acid boiled over a low heat for 10 minutes to remove alkali metals such as Na and Li that may be contained in the binder, etc. Then, wash the sample powder with ion exchange water, filter and separate it, and dry it at 200°C for 1 hour. Thereafter, heat it to 900°C in an oxygen atmosphere to remove the carbon component, thereby isolating only the silicate composite particles.

[0068] The cross-sectional observation of silicate composite particles can be performed, for example, using the following method. First, the battery is disassembled, the negative electrode is taken out, and the cross-sectional view of the negative electrode mixture layer is obtained by cross-sectional polishing (CP). The cross-sectional view of the negative electrode mixture layer is observed using a scanning electron microscope (SEM). From the cross-sectional image of the reflected electron image of the negative electrode mixture layer, 10 silicate composite particles with a maximum diameter of 5 μm or more are randomly selected, and each particle is subjected to element mapping analysis based on energy dispersive X-ray (EDX). The area containing the element to be targeted is calculated using image analysis software. The observation magnification is preferably 2000 to 20000 times. The measured values ​​of the area containing the specified element contained in the 10 particles are averaged. The content of the target element is calculated based on the obtained average value. The composition of the lithium silicate phase is calculated based on the content of the element.

[0069] It should be noted that, during the charge and discharge process, a film is formed on the surface of the silicate composite particles due to the decomposition of the electrolyte, etc. In addition, as described later, sometimes the silicate composite particles also have a conductive layer covering the surface of the composite particles. Thus, the range of the inner side of 1 μm relative to the peripheral edge of the cross section of the composite particles is subjected to EDX-based mapping analysis so that the thin film and conductive layer are not included in the measurement range. Using EDX-based mapping analysis, the distribution state of the carbon material inside the silicate composite particles can also be confirmed. Since it is difficult to distinguish the decomposition products of the electrolyte at the end of the cycle, it is preferred to measure the sample before or at the beginning of the cycle.

[0070] Desirable measurement conditions for cross-sectional SEM-EDX analysis are given below.

[0071] <SEM-EDX measurement conditions>

[0072] Processing equipment: JEOL, SM-09010 (Cross Section Polisher)

[0073] Processing conditions: Acceleration voltage 6kV

[0074] Current value: 140μA

[0075] Vacuum degree: 1×10 -3 ~2×10 -3 Pa

[0076] Measuring device: Electron microscope SU-70 manufactured by HITACHI

[0077] Accelerating voltage during analysis: 10kV

[0078] Field: Free Mode

[0079] Probe current mode: Medium

[0080] Probe current range: High

[0081] Anode Ap.: 3

[0082] OBJ Ap.:2

[0083] Analysis area: 1μm square

[0084] Analysis software: EDAX Genesis

[0085] CPS: 20500

[0086] Lsec: 50

[0087] Time constant: 3.2

[0088] In addition, the quantification of each element in the silicate composite particles contained in the negative electrode active material layer in the discharged state can be achieved not only by SEM-EDX analysis, but also by Auger electron spectroscopy (AES), laser ablation ICP mass spectrometry (LA-ICP-MS), X-ray photoelectron spectroscopy (XPS), etc.

[0089] [Method for producing negative electrode active material for secondary battery]

[0090] Next, an example of a method for producing silicate composite particles will be described in detail.

[0091] The method for producing a negative electrode active material for a secondary battery includes, for example, a step (i) of obtaining lithium silicate and a step (ii) of compositeing the lithium silicate with raw silicon to obtain composite particles in which a silicon phase and a silicon oxide phase are dispersed in a lithium silicate phase.

[0092] Process (i)

[0093] The raw material of lithium silicate uses a raw material mixture containing a Si-containing raw material and a Li raw material in a specified ratio. The raw material mixture may contain the above-mentioned element M. The mixture obtained by mixing the above-mentioned raw materials in a specified amount is dissolved, and the molten metal is passed through a metal roller to flake, thereby producing lithium silicate. Thereafter, the flake silicate is crystallized by heat treatment in an atmospheric atmosphere at a temperature above the glass transition temperature and below the melting point. It should be noted that the flake silicate can also be used without crystallization. In addition, instead of dissolving the mixture obtained by mixing the specified amount, the silicate can be manufactured by solid phase reaction by sintering at a temperature below the melting point. The heat treatment is carried out, for example, in an oxidizing atmosphere. The heat treatment temperature is preferably above 400°C and below 1200°C, and more preferably above 800°C and below 1100°C.

[0094] Silicon oxide can be used as Si raw material. For example, lithium carbonate, lithium oxide, lithium hydroxide, lithium hydride, etc. can be used as Li raw material. They can be used alone or in combination of two or more. The raw material of element M can include oxides, hydroxides, carbonate compounds, hydrides, nitrates, sulfates, etc. of each element.

[0095] In lithium silicate, Si raw material which has not reacted with Li raw material may remain.

[0096] Step (ii)

[0097] Then, raw material silicon is mixed with lithium silicate to form a composite. For example, composite particles are produced through the following steps (a) to (c).

[0098] Process (a)

[0099] First, raw silicon powder and lithium silicate powder are mixed at a mass ratio of, for example, 20:80 to 95:5. Raw silicon may be coarse silicon particles having an average particle size of about several μm to several tens of μm.

[0100] Process (b)

[0101] Then, the mixture of raw silicon and lithium silicate is crushed while applying shear force to the mixture, and the mixture is crushed and composited while being micronized. For example, raw silicon and lithium silicate are mixed in a predetermined mass ratio, and a crushing device such as a ball mill is used to stir the mixture while micronizing the mixture. At this time, an organic solvent can be added to the mixture for wet crushing. A predetermined amount of organic solvent can be added to the crushing container at one time at the beginning of the crushing, or a predetermined amount of organic solvent can be added to the crushing container in multiple times and intermittently during the crushing process. The organic solvent plays a role in preventing the crushed object from adhering to the inner wall of the crushing container.

[0102] As the organic solvent, alcohol, ether, fatty acid, alkane, cycloalkane, silicate, metal alkoxide or the like can be used.

[0103] It should be noted that the raw silicon and lithium silicate can be micronized separately and then mixed. In addition, it is also possible not to use a pulverizing device, but to produce silicon nanoparticles and lithium silicate nanoparticles and mix them. In the production of nanoparticles, a known method such as a gas phase method (such as a plasma method) or a liquid phase method (such as a liquid phase reduction method) can be used.

[0104] Process (c)

[0105] Then, the mixture is heated and pressurized, for example, in an inert gas atmosphere (e.g., an atmosphere such as argon or nitrogen), to be sintered. Pressurization can be performed simultaneously (or in parallel) with heating, or after heating. Pressurization can be performed as long as the high temperature state brought about by heating is maintained. During sintering, a sintering device such as a hot press capable of pressurizing in an inert atmosphere can be used. During sintering, the silicate softens and flows in a manner that fills the gaps between the silicon particles. As a result, a dense, blocky sintered body with a lithium silicate phase as a sea portion and a silicon oxide phase and a silicon phase as an island portion can be obtained.

[0106] The heating temperature is preferably 600° C. or higher and 1000° C. or lower. When the heating temperature is within the above range, it is easy to disperse a micro silicon phase in a silicate phase with low crystallinity. In addition, since the raw silicate is stable in the above temperature range and basically does not react with silicon, even if a capacity reduction occurs, it is slight.

[0107] The obtained sintered body is pulverized to obtain silicate composite particles. By appropriately selecting pulverization conditions, silicate composite particles having a predetermined average particle size can be obtained.

[0108] Process (iii)

[0109] Then, at least a portion of the surface of the composite particles can be covered with a conductive material to form a conductive layer. The conductive material is preferably electrochemically stable, and a conductive carbon material is preferably used. As a method for covering the surface of the composite particles with a conductive carbon material, there can be exemplified a CVD method using hydrocarbon gases such as acetylene and methane as raw materials, a method of mixing coal tar, petroleum asphalt, phenolic resin, etc. with composite particles and heating them to carbonize them, etc. In addition, carbon black can also be attached to the surface of the composite particles. The covering of the conductive carbon material can be carried out, for example, by heating a mixture of a material from which particles have been removed and a conductive carbon material, for example, in an inert atmosphere (for example, an atmosphere of argon, nitrogen, etc.) at 700°C to 950°C.

[0110] Step (iv)

[0111] A step of washing the composite particles (including the case where the composite particles have a conductive layer on the surface) with an acid may be performed. For example, by washing the composite particles with an acidic aqueous solution, a trace amount of alkaline components that may be generated when the raw silicon and lithium silicate are combined and exist on the surface of the composite particles can be dissolved and removed. As the acidic aqueous solution, an aqueous solution of an inorganic acid such as hydrochloric acid, hydrofluoric acid, sulfuric acid, nitric acid, phosphoric acid, carbonic acid, or an aqueous solution of an organic acid such as citric acid, acetic acid, or the like can be used.

[0112] Figure 1 , a cross section of a silicate composite particle 20 is schematically shown as an example of a negative electrode active material.

[0113] The mother particle 25 includes a lithium silicate phase 21, silicon (simple Si) particles 22 dispersed in the lithium silicate phase 21, and a silicon oxide phase 24 dispersed in the lithium silicate phase 21. The surface of the mother particle 25 is covered with a conductive layer 26, and the silicate composite particle 20 is formed.

[0114] The silicate composite particles 20 have, for example, a sea-island structure, and in any cross section, fine silicon phases 22 and silicon oxide phases 24 are dispersed roughly uniformly without being localized in a matrix of a lithium silicate phase 21. The SiO2 content in the mother particle 25 measured by Si-NMR is, for example, preferably 30% by mass or less, and more preferably less than 7% by mass.

[0115] The mother particle 25 may contain other components in addition to the lithium silicate phase 21, the silicon phase 22, and the silicon oxide phase 24. For example, from the viewpoint of improving the strength of the mother particle 25, a reinforcing material such as an oxide such as ZrO2 or a carbide may be contained up to less than 10 wt% relative to the mother particle 25.

[0116] [Secondary battery]

[0117] The secondary battery of the embodiment of the present invention comprises a positive electrode, a negative electrode, an electrolyte, and a separator interposed between the positive electrode and the negative electrode. The negative electrode comprises a current collector and a negative electrode active material layer containing the negative electrode active material for the secondary battery. The secondary battery may be a non-aqueous electrolyte secondary battery.

[0118] Hereinafter, the negative electrode, the positive electrode, the electrolyte, and the separator included in the secondary battery according to the embodiment of the present invention will be described in detail.

[0119] [negative electrode]

[0120] The negative electrode, for example, comprises a negative electrode current collector and a negative electrode mixture layer formed on the surface of the negative electrode current collector and containing a negative electrode active material. The negative electrode mixture layer can be formed by applying a negative electrode slurry in which a negative electrode mixture is dispersed in a dispersion medium to the surface of the negative electrode current collector and drying it. The dried coating film can be rolled as needed. The negative electrode mixture layer can be formed on one surface of the negative electrode current collector or on both surfaces.

[0121] The negative electrode mixture may contain the negative electrode active material for a secondary battery containing the silicate composite particles as an essential component as the negative electrode active material, and may contain a binder, a conductive agent, a thickener, etc. as optional components. The silicon phase in the silicate composite particles can absorb a large amount of lithium ions, thus contributing to the high capacity of the negative electrode.

[0122] The negative electrode active material may further include other active material materials that electrochemically absorb and release lithium ions. As other active material materials, carbon-based active materials are preferred. Since the volume of silicate composite particles expands and contracts with charging and discharging, if the ratio of silicate composite particles in the negative electrode active material increases, it is easy to produce poor contact between the negative electrode active material and the negative electrode collector with charging and discharging. On the other hand, by using silicate composite particles and carbon-based active materials together, it is possible to achieve excellent cycle characteristics while giving the negative electrode a high capacity of the silicon phase. The proportion of silicate composite particles in the total of silicate composite particles and carbon-based active materials is preferably 0.5 to 15% by mass, and more preferably 1 to 5% by mass. As a result, it is easy to take into account both high capacity and improved cycle characteristics.

[0123] As carbon-based active materials, for example, graphite, easily graphitized carbon (soft carbon), and difficultly graphitized carbon (hard carbon) can be exemplified. Among them, graphite having excellent charge and discharge stability and low irreversible capacity is preferred. The so-called graphite refers to a material having a graphite-type crystal structure, such as natural graphite, artificial graphite, and graphitized mesophase carbon particles. One carbon-based active material can be used alone, or two or more can be used in combination.

[0124] A nonporous conductive substrate (metal foil, etc.) or a porous conductive substrate (net, mesh, punched sheet, etc.) is used as the negative electrode collector. Examples of the material of the negative electrode collector include stainless steel, nickel, nickel alloy, copper, copper alloy, etc. The thickness of the negative electrode collector is not particularly limited, but is preferably 1 to 50 μm, more preferably 5 to 20 μm, from the perspective of balancing the strength and lightness of the negative electrode.

[0125] As binders, fluororesins, polyolefin resins, polyamide resins, polyimide resins, vinyl resins, styrene-butadiene copolymer rubber (SBR), polyacrylic acid and its derivatives can be exemplified. They can be used alone or in combination of two or more. As conductive agents, carbon black, conductive fibers, fluorinated carbon, organic conductive materials can be exemplified. They can be used alone or in combination of two or more. As thickeners, carboxymethyl cellulose (CMC), polyvinyl alcohol can be cited. They can be used alone or in combination of two or more.

[0126] Examples of the dispersion medium include water, alcohol, ether, N-methyl-2-pyrrolidone (NMP), and mixed solvents thereof.

[0127] [positive electrode]

[0128] The positive electrode, for example, comprises a positive electrode current collector and a positive electrode mixture layer formed on the surface of the positive electrode current collector. The positive electrode mixture layer can be formed by applying a positive electrode slurry in which a positive electrode mixture is dispersed in a dispersion medium to the surface of the positive electrode current collector and drying it. The dried coating can be rolled as needed. The positive electrode mixture layer can be formed on one surface of the positive electrode current collector or on both surfaces.

[0129] The positive electrode mixture contains a positive electrode active material as an essential component, and may contain a binder, a conductive agent, etc. as optional components.

[0130] A lithium composite metal oxide can be used as the positive electrode active material. Examples of the lithium composite metal oxide include Li a CoO2、Li a NiO2、Li a MnO2、Li a Co b Ni 1-b O2、Li a Co b M 1-b O c , Li a Ni 1-b M b O c , Li a Mn2O4、Li a Mn 2- b M bO4, LiMePO4, Li2MePO4F. Here, M is at least one selected from Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb and B. Me contains at least a transition element (for example, contains at least one selected from Mn, Fe, Co, Ni). Here, 0≤a≤1.2, 0≤b≤0.9, 2.0≤c≤2.3. It should be noted that the value a representing the molar ratio of lithium increases or decreases due to charge and discharge.

[0131] Among them, Li a Ni b Me 1-b A lithium nickel composite oxide represented by O2 (Me is at least one selected from Mn, Co and Al, 0<a≤1.2, 0.3≤b≤1.). From the viewpoint of high capacity, it is more preferable to satisfy 0.85≤b≤1. From the viewpoint of crystal structure stability, Li2O3 containing Co and Al as Me is further preferred. a Ni b Co c Al d O2 (0<a≤1.2, 0.85≤b<1, 0<.<0.15, 0<d≤0.1, b+c+d×1).

[0132] As the binder and the conductive agent, the same substances as those exemplified for the negative electrode can be used. As the conductive agent, graphite such as natural graphite and artificial graphite can be used.

[0133] The shape and thickness of the positive electrode current collector can be selected from the shape and range corresponding to the negative electrode current collector. Examples of the material of the positive electrode current collector include stainless steel, aluminum, aluminum alloy, titanium, and the like.

[0134] [Electrolytes]

[0135] The electrolyte includes a solvent and a lithium salt dissolved in the solvent. The concentration of the lithium salt in the electrolyte is, for example, 0.5 to 2 mol / L. The electrolyte may contain a known additive.

[0136] The solvent uses an aqueous solvent or a non-aqueous solvent. As the non-aqueous solvent, for example, cyclic carbonates, chain carbonates, cyclic carboxylates, etc. can be used. As cyclic carbonates, propylene carbonate (PC), ethylene carbonate (EC), etc. can be mentioned. As chain carbonates, diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), etc. can be mentioned. As cyclic carboxylates, γ-butyrolactone (GBL), γ-valerolactone (GVL), etc. can be mentioned. The non-aqueous solvent can be used alone or in combination of two or more.

[0137] As the lithium salt, for example, a lithium salt containing chloric acid (LiClO4, LiAlCl4, LiB 10 Cl 10 etc.), lithium salts of fluorinated acids (LiPF6, LiBF4, LiSbF6, LiAsF6, LiCF3SO3, LiCF3CO2, etc.), lithium salts of fluorinated acid imides (LiN(CF3SO2)2, LiN(CF3SO2)(C4F9SO2), LiN(C2F5SO2)2, etc.), lithium halides (LiCl, LiBr, LiI, etc.), etc. The lithium salts may be used alone or in combination of two or more.

[0138] [Spacer]

[0139] It is usually desirable to sandwich a separator between the positive electrode and the negative electrode. For the separator, the ion permeability is high and it has appropriate mechanical strength and insulation. As the separator, a microporous film, a woven fabric, a non-woven fabric, etc. can be used. As the material of the separator, for example, polyolefins such as polypropylene and polyethylene can be used.

[0140] As an example of the structure of a secondary battery, a structure in which an electrode group and an electrolyte are contained in an outer package and a positive electrode and a negative electrode are wound with a separator. Alternatively, an electrode group of other forms such as a stacked electrode group in which a positive electrode and a negative electrode are stacked with a separator can be used instead of a wound electrode group. The secondary battery can be, for example, in any form such as a cylindrical, square, coin-shaped, button-shaped, laminated, etc.

[0141] Figure 2 This is a schematic perspective view showing a partially cutaway view of a rectangular secondary battery according to an embodiment of the present invention.

[0142] The battery comprises a square-bottomed battery case 4, an electrode group 1 and an electrolyte (not shown) contained in the battery case 4, and a sealing plate 5 for sealing the opening of the battery case 4. The electrode group 1 comprises a long strip-shaped negative electrode, a long strip-shaped positive electrode, and a separator sandwiched therebetween. The negative electrode, the positive electrode, and the separator are wound around a flat winding core, and the winding core is pulled out to form the electrode group 1. The sealing plate 5 comprises a liquid injection port blocked by a sealing plug 8 and a negative terminal 6 insulated from the sealing plate 5 by a gasket 7.

[0143] One end of a negative electrode lead 3 is attached to the negative electrode current collector of the negative electrode by welding or the like. One end of a positive electrode lead 2 is attached to the positive electrode current collector of the positive electrode by welding or the like. The other end of the negative electrode lead 3 is electrically connected to the negative electrode terminal 6. The other end of the positive electrode lead 2 is electrically connected to the sealing plate 5. A resin frame is arranged on the upper part of the electrode group 1 to isolate the electrode group 1 from the sealing plate 5 and to isolate the negative electrode lead 3 from the battery case 4.

[0144] Hereinafter, the secondary battery of the present invention will be specifically described based on Examples and Comparative Examples; however, the present invention is not limited to the following Examples.

[0145] <Example 1>

[0146] [Preparation of silicate composite particles]

[0147] Lithium carbonate and silicon dioxide were mixed to form a molar ratio of Li2CO3:SiO2=34:66, and the mixture was melted at 1100°C for 5 hours in an inert gas atmosphere, and the melt was passed through a metal roller to form a thin sheet, and heat-treated at 750°C for 5 hours in air to obtain a lithium silicate composite oxide existing as a mixed phase of amorphous and crystalline. The obtained lithium silicate composite oxide was crushed to an average particle size of 10 μm.

[0148] A lithium silicate composite oxide having an average particle size of 10 μm and raw silicon (3N, average particle size of 10 μm) were mixed at a mass ratio of 70:30. The mixture was filled into a pot (SUS, volume: 500 mL) of a planetary ball mill (manufactured by FRITSCH, P-5), 24 SUS balls (diameter 20 mm) were added and the lid was closed, and the mixture was pulverized at 200 rpm in an inert atmosphere for 25 hours.

[0149] Then, the powdered mixture was taken out in an inert atmosphere, and fired at 800° C. for 4 hours in the inert atmosphere under pressure with a hot press to obtain a sintered body of the mixture.

[0150] Thereafter, the sintered body was crushed, passed through a 40 μm mesh, and then mixed with coal tar (MCP250 manufactured by JFE CHEMICAL Co., Ltd.), and the mixture was calcined at 800° C. for 5 hours in an inert atmosphere to cover the surface of the silicate composite particles with conductive carbon to form a conductive layer. The covering amount of the conductive layer was set to 5% by mass relative to the total mass of the silicate composite particles and the conductive layer. Thereafter, a sieve was used to obtain silicate composite particles having an average particle size of 5 μm with a conductive layer.

[0151] XRD analysis was performed on the silicate composite particles, and peaks derived from Si and SiO2 were measured.

[0152] [Production of negative electrode]

[0153] Silicate composite particles and graphite were mixed in a mass ratio of 5:95 and used as negative electrode active material. Negative electrode active material, sodium carboxymethyl cellulose (CMC-Na), styrene-butadiene rubber (SBR) and lithium polyacrylate were mixed in a mass ratio of 96.5:1:1.5:1, and after adding water, a mixer (manufactured by PRIMIX, TKHibismix) was used to stir and prepare negative electrode slurry. Then, the negative electrode slurry was applied to the surface of the copper foil so that every 1m 2 The mass of the negative electrode mixture was 190 g. After the coating was dried, it was rolled to form a copper foil with a density of 1.5 g / cm 3 The negative electrode of the negative electrode mixture layer.

[0154] [Production of positive electrode]

[0155] Lithium cobalt oxide, acetylene black and polyvinylidene fluoride were mixed in a mass ratio of 95:2.5:2.5, N-methyl-2-pyrrolidone (NMP) was added, and the mixture was stirred using a mixer (manufactured by PRIMIX, TKHibismix) to prepare a positive electrode slurry. Then, the positive electrode slurry was applied to the surface of the aluminum foil, and after the coating was dried, it was rolled to form a 3.6 g / cm2 film on both sides of the aluminum foil. 3 The positive electrode of the positive electrode mixture layer.

[0156] [Preparation of electrolyte]

[0157] A non-aqueous electrolyte was prepared by dissolving LiPF6 at a concentration of 1.0 mol / L in a mixed solvent containing ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 3:7.

[0158] [Manufacturing of Secondary Batteries]

[0159] The electrode group was prepared by installing a tab on each electrode so that the tab was located at the outermost part, and the positive electrode and the negative electrode were wound into a spiral shape with a separator interposed therebetween. The electrode group was inserted into an outer package made of an aluminum laminate film, vacuum dried at 105°C for 2 hours, and then injected with a non-aqueous electrolyte, and the opening of the outer package was sealed to obtain a secondary battery A1.

[0160] [Charge and discharge cycle test]

[0161] Secondary battery A1 was repeatedly charged and discharged under the following conditions.

[0162] <Charging>

[0163] The battery was charged at a constant current of 1 It (800 mA) at 25° C. until the voltage reached 4.2 V, and then charged at a constant voltage of 4.2 V until the current reached 1 / 20 It (40 mA).

[0164] <Discharge>

[0165] The battery was discharged at a constant current of 1 It (800 mA) at 25°C until the voltage reached 2.75V.

[0166] The rest period between charge and discharge was set to 10 minutes. The ratio of the discharge capacity at the 200th cycle to the discharge capacity at the 1st cycle was evaluated as the cycle retention rate.

[0167] <Examples 2, 3, Comparative Example 1>

[0168] In the preparation of silicate composite particles, the pressing pressure, heating temperature and / or heating time by the hot press were changed as follows. A negative electrode was otherwise prepared in the same manner as in Example 1, and secondary batteries A2, A3, and B1 were obtained using the prepared negative electrode.

[0169] In Example 2, the heating temperature using the hot press was changed from 800°C to 750°C.

[0170] In Example 3, the heating temperature using the hot press was changed from 800°C to 850°C.

[0171] In Comparative Example 1, the pressing pressure in the hot press was changed from 400 MPa to 180 MPa, the heating temperature was changed from 800° C. to 600° C., and the heating time was changed from 4 hours to 5 hours.

[0172] Secondary battery A2 corresponds to Example 2, secondary battery A3 corresponds to Example 3, and secondary battery B1 corresponds to Comparative Example 1. The cycle retention ratios of secondary batteries A2, A3, and B1 were evaluated in the same manner.

[0173] The cycle retention rates of the secondary batteries A1 to A3 and B1 are shown in Table 1. Table 1 shows the maximum intensity I of the diffraction peak A derived from the SiO2 (011) plane of the silicon oxide phase of the silicate composite particles used in each battery. A The maximum intensity I of the diffraction peak B from the Si(111) plane of the silicon phase B Ratio I A / I B In addition, Table 1 also shows the half-value width W of the diffraction peak A. A , the half-value width W of the diffraction peak B B and the integrated intensity S of diffraction peak A A The integrated intensity S relative to the diffraction peak B B The ratio of S A / S B .

[0174] [Table 1]

[0175]

[0176] According to Table 1, I A / I B The secondary batteries A1 to A3 and I A / I B Compared with the secondary battery B1 having a cycle retention rate of less than 0.9, a high cycle retention rate can be obtained.

[0177] Figure 3 The diffraction patterns based on X-ray diffraction (XRD) of the silicate composite particles used in the secondary battery A1 of Example 1 and the silicate composite particles used in the secondary battery B1 of Comparative Example 1 are shown. In the silicate composite particles used in Example 1 and Comparative Example 1, diffraction peak A from the SiO2 (011) plane of the silicon oxide phase and diffraction peak B from the Si (111) plane of the silicon phase were observed. However, if the diffraction peak A is focused on, the diffraction peak A of Example 1 is sharper than that of Comparative Example 1, and the maximum intensity of the peak is also greater. This means that the crystallinity of the silicon oxide phase in the silicate composite particles used in Example 1 is improved compared to the silicate composite particles used in Comparative Example 1. By dispersing the silicon oxide phase with improved crystallinity in the composite particles, cracks and fissures of the composite particles can be suppressed, and the charge and discharge cycle characteristics can be improved.

[0178] Industrial Applicability

[0179] The secondary battery of the present invention is useful as a main power source for mobile communication devices, portable electronic devices, and the like.

[0180] Although the present invention has been described with respect to the present preferred embodiments, such disclosure should not be construed in a limiting sense. Upon reading the above invention, various modifications and changes will undoubtedly be apparent to those skilled in the art in the technical field of the present invention. Therefore, the scope of the appended claims should be interpreted as including all modifications and changes without departing from the true spirit and scope of the present invention.

[0181] Description of Reference Numerals

[0182] 1 electrode group, 2 positive electrode lead, 3 negative electrode lead, 4 battery casing, 5 sealing plate, 6 negative electrode terminal, 7 gasket, 8 sealing plug, 20 silicate composite particles, 21 lithium silicate phase, 22 silicon phase, 24 silicon oxide phase, 25 mother particle, 26 conductive layer.

Claims

1. A negative electrode active material for a secondary battery, It has silicate composite particles. The silicate composite particles have a lithium silicate phase, a silicon oxide phase and a silicon phase. The lithium silicate phase comprises lithium, silicon and oxygen, The silicon oxide phase comprises SiO2, The silicon oxide phase and the silicon phase are dispersed in the lithium silicate phase, In the diffraction pattern of the silicate composite particles based on X-ray diffraction (XRD), the maximum intensity I of the diffraction peak A originating from the SiO2 (011) plane of the silicon oxide phase appearing near 2θ×26° is A The maximum intensity I of the diffraction peak B originating from the Si(111) plane of the silicon phase appears near 2θ×28° B Ratio I A / I B It is 0.9 or more and 1.4 or less.

2. The negative electrode active material for a secondary battery according to claim 1, wherein In the diffraction pattern, the half value width WB of the diffraction peak B is 0.3° or more and 1.5° or less based on 2θ.

3. The negative electrode active material for a secondary battery according to claim 1 or 2, wherein In the diffraction pattern, the half-value width W of the diffraction peak A is A The 2θ standard is 0.6° or less.

4. The negative electrode active material for a secondary battery according to any one of claims 1 to 3, wherein In the diffraction pattern, the integrated intensity S of the diffraction peak A is A The integrated intensity S of the diffraction peak B B The ratio of S A / S B Below 0.

7.

5. The negative electrode active material for a secondary battery according to any one of claims 1 to 4, wherein The lithium silicate phase further comprises an element M, The element M is at least one selected from B, Al, Ca, Mg, Zr, Nb, Ta, La, V, Y, Ti, P, Bi, Zn, Sn, Pb, Sb, Co, Er, F and W.

6. A secondary battery, It comprises a positive electrode, a negative electrode, an electrolyte, and a separator interposed between the positive electrode and the negative electrode. The negative electrode comprises a current collector and a negative electrode active material layer. The negative electrode active material layer contains the negative electrode active material for a secondary battery according to any one of claims 1 to 5.