Optical laminate for OLED display device
By stacking the adhesive layer with light scattering characteristics in the OLED display device and adjusting its distance from the color filter, combining the low polarization optical element and hard coating layer, the color shift of the OLED display device when observing the tilt direction is solved. and the problem of inequality of interference improves visual recognition and reduces power consumption and cost.
Patent Information
- Application Number
- CN202380023845.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-02-22
- Filing Date
- 2023-02-27
- Publication Date
- 2024-11-01
AI Technical Summary
When observing the tilt direction, there are problems of color shift and interference unevenness. When using the polarizing plate, the interference in the two-dimensional structure of the color filter affects visual identification. sex.
The adhesive layer with light scattering characteristics is laminated on the visual recognition side of the OLED display device, and the distance between it and the color filter is adjusted to avoid image blurring. Optical components with a polarization degree of less than 95% are used, combined with a hard coating layer and Other optical components to improve visual recognition.
It effectively suppresses color shift and interference inequality, improves visual recognition, avoids image blur, and reduces power consumption and cost.
Smart Images

Figure CN118891972A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an optical laminate for an OLED display device, and more particularly to an optical laminate for use in an OLED display device that does not use a polarizing plate. Background Art
[0002] Compared with liquid crystal display devices, OLED (organic light emitting diode) display devices have advantages in display performance such as high visual recognition, low viewing angle dependence, and fast response speed. In addition, OLED display devices do not use backlight sources, so they are conducive to thinning and can also be used as flexibly bent or foldable devices.
[0003] An OLED display device generally has an OLED element in which an anode, an OLED layer including a light-emitting layer, and a cathode are stacked in sequence. The electrodes (anode or cathode) of the OLED element use transparent conductive materials with high refractive index such as ITO, metal materials with high reflectivity, etc., so there are problems such as external light being reflected by the electrodes, resulting in reduced contrast and reflection caused by internal reflection, which sometimes deteriorates the display performance of the OLED display device.
[0004] In order to suppress the adverse effects caused by external light reflection, a scheme of configuring a polarizing plate and a circular polarizing plate such as a λ / 4 plate on the visual recognition side of an OLED display device has been proposed (for example, Patent Document 1). Such a circular polarizing plate also has the function of blocking ultraviolet rays contained in external light and preventing the degradation of OLED elements caused by ultraviolet rays. In addition, the mechanical properties of the circular polarizing plate itself also have the function of absorbing external impacts and preventing damage to the OLED display device.
[0005] However, when a circular polarizing plate is used, the light utilization efficiency (i.e., light collection rate) deteriorates and the brightness decreases due to the absorption of the polarizing plate. When the luminous intensity of the OLED element is increased in order to obtain the desired brightness, the power consumption increases and the life of the OLED element is shortened. In addition, when the polarizing plate includes an adhesive layer for pasting, the thickness can reach about 0.15 mm, which is not conducive to the thinning of the OLED display device. In addition, since the circular polarizing plate is expensive, there is also the problem of increased manufacturing cost.
[0006] As an alternative to the circular polarizing plate, the following method has been proposed: for an OLED element, a color filter is arranged on its visual identification side, and the color filter of the same color as the luminous color of the OLED layer is aligned with the OLED element, thereby preventing external light reflection and improving the luminous brightness of the OLED element (for example, Patent Document 2).
[0007] As one form of OLED display device, an OLED display device having a microcavity (also called multiple reflection interference, optical resonator or microresonator) structure is known. According to the OLED display device having a microcavity structure, the spectrum of light extracted to the outside becomes steep and has high intensity, so that the brightness and color purity can be improved (for example, Patent Document 3).
[0008] In an OLED display device, various optical element layers such as an adhesive layer, a base material such as plastic or thin glass, and a hard coat layer are stacked to provide functions such as surface protection and flexibility on the visual recognition side of the OLED element.
[0009] Prior art literature
[0010] Patent Literature
[0011] Patent Document 1: Japanese Patent Application Publication No. 2003-332068
[0012] Patent Document 2: Japanese Patent Application Publication No. 2018-112715
[0013] Patent Document 3: Japanese Patent Application Publication No. 2015-207377 Summary of the invention
[0014] Problems to be solved by the invention
[0015] As an alternative to the circular polarizing plate, a color filter is arranged on the visual recognition side of the OLED element and the color filter of the same color as the luminous color of the OLED layer is positioned facing the OLED element, thereby preventing external light reflection and improving the luminous intensity of the OLED element. However, due to the regular two-dimensional structure of the color filter, interference unevenness (interference mura) of the reflected light is sometimes generated, thereby impairing the visual recognition of the OLED display device.
[0016] In addition, the OLED display device with a microcavity structure has a problem of strong viewing angle dependence (narrow viewing angle). More specifically, the OLED display device with a microcavity structure has a situation where the brightness drops sharply or the hue changes significantly depending on the viewing angle. As a result, when the image is viewed from an oblique direction during image display, a color shift sometimes occurs in which the color appears to be different from the color originally intended to be displayed.
[0017] These interference unevenness and color shift may be reduced by stacking a light scattering layer on the viewing side of the OLED element. However, in this case, a problem of image blurring may occur in which the displayed image appears blurred due to light scattering.
[0018] Therefore, an object of the present invention is to provide an optical laminate for use in an OLED display device that does not use a polarizing plate and that is less likely to cause image blurring even if a light scattering layer is laminated to suppress color shift and interference unevenness when viewed from an oblique direction.
[0019] Means used to solve problems
[0020] The present inventors have conducted intensive research to achieve the above-mentioned purpose, and as a result, have found that, in an OLED display device that does not use a polarizing plate, by stacking an optical laminate including an adhesive layer having light scattering properties on the visual recognition side of the OLED element and adjusting the distance between the color filter and the adhesive layer, it is possible to provide an OLED display device that is less likely to produce color shift and interference unevenness when observed from an oblique direction, and that suppresses image blurring caused by light scattering and has excellent visual recognition, thereby completing the present invention.
[0021] That is, the present invention provides an optical laminate for an OLED display device, wherein the optical laminate for an OLED display device is used for an OLED display device in which only an optical element with a polarization degree of 95% or less is laminated on a visual recognition side of an OLED element, the OLED display device is provided with a color filter on the visual recognition side of the OLED element, only the optical element is laminated on the visual recognition side of the color filter, the optical element has at least an adhesive layer, at least one layer of the adhesive layer has a light scattering property, and the distance between the adhesive layer with the light scattering property and the color filter is 700 μm or less.
[0022] Preferably, when the distance between the light-scattering adhesive layer and the color filter is d [μm] and the haze value of the light-scattering adhesive layer is H [%], the value of d×H is 70000 or less and H is 20 or more.
[0023] Preferably, when the thickness of the pressure-sensitive adhesive layer having light scattering properties is T [μm] and the haze value of the pressure-sensitive adhesive layer having light scattering properties is H [%], the value of T×H is 400 or more.
[0024] Preferably, the pressure-sensitive adhesive layer having light scattering properties includes light scattering fine particles dispersed in the pressure-sensitive adhesive layer, and the volume average particle size of the light scattering fine particles is 1 μm to 5 μm.
[0025] Preferably, the optical laminate for an OLED display device further includes a hard coating layer having a thickness of 2 μm to 20 μm as the optical element.
[0026] It is preferred that the water contact angle of the hard coat layer be 100° or more.
[0027] It is preferred that the water contact angle of the hard coating layer after a steel wool test is 95° or more.
[0028] Effects of the Invention
[0029] The OLED display device in which the optical laminate for an OLED display device of the present invention is laminated on the viewing side of the OLED element does not easily cause image blurring even if a light scattering layer is laminated to suppress color shift and interference unevenness, and has excellent visibility. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 FIG. 1 is a schematic cross-sectional view showing an embodiment of an OLED display panel of the present invention.
[0031] Figure 2 This is a schematic cross-sectional view showing one embodiment of an OLED display device on which the optical laminate of the present invention is stacked.
[0032] Figure 3 This is a schematic cross-sectional view showing one embodiment of an OLED display device on which the optical laminate of the present invention is stacked.
[0033] Figure 4 This is a schematic cross-sectional view showing one embodiment of an OLED display device on which the optical laminate of the present invention is stacked.
[0034] Figure 5 This is a schematic cross-sectional view showing one embodiment of an OLED display device on which the optical laminate of the present invention is stacked.
[0035] Figure 6 This is a schematic cross-sectional view showing one embodiment of an OLED display device on which the optical laminate of the present invention is stacked.
[0036] Figure 7 This is a schematic cross-sectional view showing one embodiment of an OLED display device on which the optical laminate of the present invention is stacked.
[0037] Figure 8 This is a schematic cross-sectional view showing one embodiment of an OLED display device on which the optical laminate of the present invention is stacked.
[0038] Fig. 9 This is a schematic cross-sectional view showing one embodiment of an OLED display device on which the optical laminate of the present invention is stacked.
[0039] Fig.10 This is a schematic cross-sectional view showing one embodiment of an OLED display device on which the optical laminate of the present invention is stacked.
[0040] Fig.11This is a schematic cross-sectional view showing one embodiment of an OLED display device on which the optical laminate of the present invention is stacked.
[0041] Fig.12 This is a schematic cross-sectional view showing one embodiment of an OLED display device on which the optical laminate of the present invention is stacked.
[0042] Fig.13 This is a schematic cross-sectional view showing one embodiment of an OLED display device on which the optical laminate of the present invention is stacked.
[0043] Fig.14 This is a schematic cross-sectional view showing one embodiment of an OLED display device on which the optical laminate of the present invention is stacked.
[0044] Fig.15 This is a schematic cross-sectional view showing one embodiment of an OLED display device on which the optical laminate of the present invention is stacked.
[0045] Fig.16 This is a schematic cross-sectional view showing one embodiment of an OLED display device on which the optical laminate of the present invention is stacked.
[0046] Fig.17 This is a schematic cross-sectional view showing one embodiment of an OLED display device on which the optical laminate of the present invention is stacked. DETAILED DESCRIPTION
[0047] The present invention provides an optical laminate for use in an OLED display device in which only an optical element having a polarization degree of 95% or less is laminated on the visual recognition side of an OLED element (optical laminate for an OLED display device). The optical laminate for an OLED display device of the present invention is sometimes referred to as "the optical laminate of the present invention", the OLED display device using the optical laminate of the present invention is sometimes referred to as "the OLED display device of the present invention", and the optical element constituting the optical laminate of the present invention is sometimes referred to as "the optical element of the present invention".
[0048] In the OLED display device of the present invention, as an indispensable structure, there is an OLED display panel including an OLED element in which an anode, an OLED layer including a light-emitting layer, and a cathode are sequentially stacked, and the optical laminate of the present invention is stacked on the visual recognition side of the OLED element. The OLED display panel constituting the OLED display device of the present invention is sometimes referred to as "the OLED display panel of the present invention".
[0049] The OLED display device of the present invention has only optical elements with a polarization degree of less than 95% stacked on the visual recognition side of the OLED element in the OLED display panel. "Only optical elements with a polarization degree of less than 95% are stacked on the visual recognition side of the OLED element" means that the optical elements on the visual recognition side of the OLED element do not contain optical elements with a polarization degree greater than 95%. There is no particular restriction on "optical elements with a polarization degree greater than 95%", including polarizing plates such as linear polarizing plates, 1 / 4 phase difference plates, 1 / 2 phase difference plates, circular polarizing plates, and reflective polarizing plates. That is, the OLED display device of the present invention is an OLED display device that does not include a polarizing plate on the visual recognition side of the OLED element.
[0050] The polarization degree is determined by the following formula based on the parallel transmittance Tp and the orthogonal transmittance Tc measured using an ultraviolet-visible spectrophotometer and subjected to visibility correction.
[0051] Polarization degree (%) = {(Tp-Tc) / (Tp+Tc)}1 / 2×100
[0052] The OLED display device of the present invention does not include a polarizing plate on the visual recognition side of the OLED element, thereby suppressing the absorption of light emitted from the OLED element by the polarizing plate, improving the light collection rate to save power consumption, and achieving a longer life of the OLED element. In addition, by not using a polarizing plate, a thinner device can be achieved, and the manufacturing cost can also be reduced.
[0053] The OLED display device of the present invention is provided with a color filter on the visual recognition side of the OLED element, and only the optical element of the present invention is stacked on the visual recognition side of the above-mentioned color filter. The optical element of the present invention has at least an adhesive layer, at least one layer of the above-mentioned adhesive layer has light scattering properties, and the distance between the above-mentioned adhesive layer with light scattering properties and the above-mentioned color filter is 700μm or less. By making the distance (d) between the adhesive layer with the above-mentioned light scattering properties and the above-mentioned color filter less than 700μm, even if a light scattering layer is stacked to suppress the color shift and interference unevenness caused by the OLED display device of the present invention, it is not easy to cause image blur, and it is suitable in terms of excellent visual recognition.
[0054] In another embodiment of the OLED display device of the present invention, it is preferred that the optical element of the present embodiment has at least an adhesive layer, and at least one of the adhesive layers has light scattering properties. The adhesive layer constituting the optical laminate of the present embodiment has light scattering properties, which is suitable in terms of suppressing color shift and interference unevenness caused by the OLED display device of the present embodiment and having excellent visual recognition.
[0055] In another embodiment of the OLED display device of the present invention, the optical element of this embodiment preferably has at least an anti-reflection layer. The optical element of this embodiment is suitable because it is not easy to produce interference unevenness of the OLED display device of this embodiment due to the anti-reflection layer and has excellent visual recognition.
[0056] In another embodiment of the OLED display device of the present invention, the optical element of this embodiment preferably has at least an anti-glare layer. The optical element of this embodiment has an anti-glare layer to suppress color shift and interference unevenness caused by the OLED display device of this embodiment, and is suitable in terms of excellent visual recognition.
[0057] In another embodiment of the OLED display device of the present invention, it is preferred that the optical element of this embodiment has at least a glass layer and a resin layer, and the glass layer and the resin layer are bonded by an adhesive layer. In the optical laminate of this embodiment, the impact resistance of the OLED display device of this embodiment is improved by bonding the glass layer and the resin layer by using an adhesive layer, so it is suitable.
[0058] In another embodiment of the OLED display device of the present invention, the optical element of this embodiment preferably has at least a transparent polyimide layer and a hard coating layer. The optical element of this embodiment has a transparent polyimide layer and a hard coating layer, thereby improving the impact resistance of the OLED display device of this embodiment, and is therefore suitable.
[0059] Hereinafter, each structure will be described.
[0060] (OLED display panel)
[0061] The OLED display panel used in the OLED display device of the present invention includes an OLED element in which an anode, an OLED layer including a light-emitting layer, and a cathode are sequentially stacked as an essential structure. The optical laminate of the present invention is stacked on the viewing side of the OLED element of the OLED display panel.
[0062] Hereinafter, an embodiment of an OLED display panel constituting the OLED display device of the present invention will be described with reference to the drawings, but the present invention is not limited to this embodiment.
[0063] Figure 1 is a schematic cross-sectional view showing one embodiment of the OLED display panel of the present invention.
[0064] like Figure 1As shown, the OLED display panel 100 has: a red OLED element 12R having a transparent electrode 11a, a red OLED layer 10R emitting red light, and a back electrode 11b stacked in sequence; a green OLED element 12G having a transparent electrode 11a, a green OLED layer 10G emitting green light, and a back electrode 11b stacked in sequence; and a blue OLED element 12B having a transparent electrode 11a, a blue OLED layer 10B emitting blue light, and a back electrode 11b stacked in sequence. The OLED elements 12R, 12G, and 12B of various colors are sequentially arranged on a substrate 13. A TFT (thin film transistor) layer 14 is formed on the surface of the substrate 13 where the OLED elements are arranged, and is connected to the back electrodes 11b of the OLED elements 12R, 12G, and 12B of various colors.
[0065] exist Figure 1 In the OLED display panel 100, on the visual recognition side of each of the multiple color OLED elements 12R, 12G, and 12B ( Figure 1 A color filter 15 is disposed on the upper side (in the middle). The color filter 15 includes a red coloring layer 15R, a green coloring layer 15G, and a blue coloring layer 15B, and a black matrix layer 16 is provided between the coloring layers.
[0066] exist Figure 1 In the embodiment, the color filter 15 is arranged such that the red coloring layer 15R, the green coloring layer 15G, and the blue coloring layer 15B face the red OLED element 12R, the green OLED element 12G, and the blue OLED element 12B, respectively.
[0067] The transparent electrode 11a is either a cathode or an anode, but is usually a cathode. As a material for forming the transparent electrode 11a, a transparent conductive material such as ITO (indium tin oxide), indium oxide, IZO (indium zinc oxide), SnO2, or ZnO is used.
[0068] The back electrode 11b is used as a counter electrode of the transparent electrode 11a. The back electrode 11b is either an anode or a cathode, but is usually provided as an anode on the substrate 13. As a forming material, metals such as gold, silver, and chromium can be cited. Therefore, the back electrode 11b can reflect light.
[0069] A bonding layer 17 is provided between the substrate 13 and the color filter 15. The bonding layer 17 is light-transmissive. As the material of the bonding layer 17, a material used in a common OLED display device may be used, for example, a photocurable resin such as a photosensitive polyimide resin, or a thermosetting resin, etc.
[0070] OLED display panel 100 Figure 1In addition to the structure shown, the OLED display panel may also have structures such as a hole injection layer, a hole transport layer, an electron transport layer, a sealing layer, a touch sensor panel, etc. (not shown).
[0071] Figure 1 The OLED display panel is characterized in that a color filter 15 is disposed on each of the OLED elements 12R, 12G, and 12B of multiple colors so as to be opposite to a coloring layer 15R, a coloring layer 15G, and a coloring layer 15B of the same color. Figure 1 As shown, white external light W, for example, passes through the red coloring layer 15R, further passes through the transparent electrode 11a and the red OLED layer 10R that emits red light and is reflected at the back electrode 11b, passes through the red OLED layer 10R, the transparent electrode 11a and the red coloring layer 15R again, and then the reflected light G enters the observer's eyes.
[0072] The external light W is absorbed by the red coloring layer 15R in green and blue, so the light intensity becomes 1 / 3. In addition, the reflected light G passes through the red coloring layer 15R and the red OLED layer 10R again, so attenuation occurs. In addition, the reflected light G is red, so the red light emitted from the OLED layer 10R can be enhanced. The same is true when the external light W is incident on the green coloring layer 15G and the blue coloring layer 15B, and the green light and blue light can be enhanced respectively. Therefore, by using a color filter in the OLED display panel, even if a circular polarizing plate is not used to prevent reflection, the reflection of external light can be greatly suppressed, and the light intensity of the OLED element can be increased.
[0073] However, color filters are generally prone to interference unevenness caused by regular two-dimensional structures.
[0074] In addition, there is a problem that color filters are easily reflected at the interface, which reduces the light collection efficiency of light emitted from the OLED element.
[0075] In addition, the color filter has an insufficient ultraviolet absorption function compared to the case of using a circular polarizing plate, and the OLED element is easily degraded over time by ultraviolet rays contained in external light (that is, the weather resistance is low).
[0076] In addition, there is a problem that the color filter has an insufficient impact absorption function compared to the case of using a circular polarizing plate.
[0077] In addition, the OLED display panel 100 of the present embodiment has a microcavity structure. The light generated from the OLED layers 10R, 10G, and 10B is emitted to the outside through the transparent electrode 11a. Here, the emitted light includes two components: "direct light" emitted directly from the OLED layers 10R, 10G, and 10B toward the transparent electrode 11a and "reflected light" emitted from the OLED layers 10R, 10G, and 10B toward the back electrode 11b and reflected at the back electrode 11b and then toward the transparent electrode 11a. That is, a first optical path C1 is formed in which a part of the light emitted from the OLED layers 10R, 10G, and 10B does not travel toward the back electrode 11b side but travels toward the transparent electrode 11a side and is emitted to the outside through the transparent electrode 11a, and a second optical path C2 is formed in which the remaining part of the light emitted from the OLED layers 10R, 10G, and 10B travels toward the back electrode 11b side and is reflected by the back electrode 11b, and then passes through the OLED layers 10R, 10G, 10B and the transparent electrode 11a and is emitted to the outside. The thickness of the OLED layers 10R, 10G, and 10B is different so that the light component corresponding to each color is enhanced by the interference of the direct light and the reflected light. That is, the thickness of the OLED layers 10R, 10G, and 10B is different so that the optical path length between the back electrode (positive electrode) 11b and the transparent electrode (negative electrode) 11a is consistent with the peak wavelength of the EL spectrum of each of red, green, and blue, thereby extracting the strongest light from each color. Specifically, the thickness of the short-wavelength blue OLED layer 10B is designed to be thin, and the thickness of the long-wavelength red OLED layer 10R is designed to be thick. When the light generated in the OLED layer is repeatedly reflected between the positive electrode and the negative electrode, only the light of the wavelength that matches the optical path length is resonated and strengthened, and the light of other wavelengths that do not match the optical path length is weakened, thereby the spectrum of the light extracted to the outside becomes steep and high in intensity, and the brightness and color purity are improved.
[0078] The OLED display panel with a microcavity structure can achieve excellent effects such as improved brightness and color purity, but on the other hand, due to the steep spectrum, it may have a problem of strong viewing angle dependence (narrow viewing angle). Therefore, when the image is viewed from an oblique direction during image display, a color shift may occur in which the color appears to be different from the color originally intended to be displayed.
[0079] (Optical element of the present invention)
[0080] The optical element of the present invention is an optical element laminated on the visual recognition side of the OLED display device, and includes at least one layer selected from a binder layer, an adhesive layer, a resin layer, a glass layer, a hard coating layer, an anti-reflection layer, an anti-glare layer, an intermediate layer (compatible layer), an impact absorbing layer, an antistatic layer, etc. However, the optical element of the present invention does not include an optical element having a polarization degree greater than 95% such as a polarizing plate.
[0081] (Adhesive layer)
[0082] The adhesive layer is a layer having adhesiveness at room temperature and adhering to an adherend with light pressure, and is a layer that maintains practical adhesive strength even when the adherend affixed to the adhesive layer is peeled off.
[0083] From the viewpoint of effectively reducing the color shift and interference unevenness of the OLED display device, the adhesive layer constituting the optical element of the present invention (hereinafter sometimes referred to as "the adhesive layer of the present invention") preferably has light scattering properties (a function of scattering light). When the adhesive layer of the present invention has light scattering properties, it preferably contains light scattering particles dispersed in the adhesive layer.
[0084] In the case where the OLED display device of the present invention includes a color filter on the visual recognition side and the adhesive layer has light scattering properties, from the viewpoint of reducing the color shift and interference unevenness of the OLED display device and suppressing the image blur of the OLED display device caused by light scattering, the distance (d) between the above-mentioned adhesive layer with light scattering properties and the above-mentioned color filter is preferably 700 μm or less. From the viewpoint of suppressing the image blur of the OLED display device caused by light scattering, the distance between the adhesive layer with light scattering properties and the color filter is more preferably 600 μm or less, and further preferably 500 μm or less. It is most preferred that the adhesive layer with light scattering properties is in direct contact with the color filter.
[0085] The distance between the adhesive layer having light scattering properties and the color filter represents the distance (μm) between the surface of the adhesive layer in the color filter direction and the surface of the color filter in the adhesive layer direction. When other layers are stacked between the adhesive layer having light scattering properties and the color filter, it is equivalent to the thickness (μm) of the other layers (the total in the case of two or more layers).
[0086] The haze value (H) of the adhesive layer of the present invention is not particularly limited. From the perspective of effectively reducing the color shift and interference unevenness of the OLED display device, it is preferably 20% or more, more preferably 30% or more, further preferably 40% or more, and particularly preferably 50% or more. In addition, from the perspective of suppressing image blurring of the OLED display device and displaying a high-definition image, the haze value of the adhesive layer of the present invention is preferably 90% or less, more preferably 80% or less, and more preferably 70% or less.
[0087] The total light transmittance of the adhesive layer of the present invention is not particularly limited. From the perspective of ensuring the brightness of the OLED display device, it is preferably 60% or more, more preferably 70% or more, further preferably 80% or more, and particularly preferably 90% or more. In addition, the upper limit of the total light transmittance of the adhesive layer of the present invention is not particularly limited, and may be less than 100%, or may be 99.9% or less, or 99% or less.
[0088] The haze value and total light transmittance of the adhesive layer of the present invention can be measured by the methods specified in JIS K7136 and JIS K7361, respectively, and can be controlled by the type and thickness of the adhesive layer, and the type and amount of light scattering fine particles described below.
[0089] From the viewpoint of effectively reducing color shift and interference unevenness of an OLED display device, the thickness (T) of the adhesive layer of the present invention is preferably 10 μm to 100 μm, more preferably 15 μm to 90 μm, and even more preferably 20 μm to 80 μm.
[0090] The light scattering particles have an appropriate refractive index difference with the adhesive in the adhesive layer, and the light scattering characteristics are given to the adhesive layer. When the adhesive layer contains light scattering particles, it is satisfactory to give the scattering performance of light. As light scattering particles, inorganic particles, polymer particles, etc. can be listed. As the material of inorganic particles, for example, silicon dioxide, calcium carbonate, aluminum hydroxide, magnesium hydroxide, clay, talc and titanium dioxide can be listed. As the material of polymer particles, for example, silicone resin, acrylic resin, methacrylic resin (such as polymethyl methacrylate), polystyrene resin, polyurethane resin, melamine resin, polyethylene resin, epoxy resin, etc. can be listed. The light scattering particles are preferably polymer particles, and in particular, particles composed of silicone resin (such as Tospearl series manufactured by Maitu High-Tech Materials Japan Co., Ltd.) have excellent dispersibility and stability to the adhesive layer and an appropriate refractive index difference with the adhesive layer, and an adhesive layer with excellent scattering performance showing uniform haze in the plane can be obtained, which is suitable in reducing the color shift and interference unevenness of the OLED display device. The shape of the light scattering fine particles may be, for example, a perfect sphere, a flat shape, or an irregular shape. The light scattering fine particles may be used alone or in combination of two or more.
[0091] From the viewpoint of giving appropriate light scattering properties to the adhesive layer, the volume average particle size of the light scattering particles is preferably 0.1 μm or more, more preferably 0.15 μm or more, further preferably 0.2 μm or more, further preferably 0.25 μm or more, and particularly preferably 1 μm or more. In addition, from the viewpoint of preventing the haze value from becoming too high and displaying a high-definition image, the volume average particle size of the light scattering particles is preferably 12 μm or less, more preferably 10 μm or less, further preferably 8 μm or less, and particularly preferably 5 μm or less. The volume average particle size can be measured, for example, using a Coulter counter.
[0092] The refractive index (n3) of the light scattering fine particles is preferably 1.2 to 5, more preferably 1.25 to 4.5, and may be 1.3 to 4 or 1.35 to 3.
[0093] From the perspective of effectively reducing the color shift and interference unevenness of the OLED display device, the absolute value of the refractive index difference between the light scattering particles and the adhesive in the adhesive layer (the adhesive layer from which the light scattering particles are removed) is preferably 0.001 or more, more preferably 0.01 or more, further preferably 0.02 or more, particularly preferably 0.03 or more, and may be 0.04 or more or 0.05 or more. In addition, from the perspective of preventing the haze value from becoming too high, suppressing image blur, and displaying a high-definition image, the absolute value of the refractive index difference between the light scattering particles and the adhesive is preferably 5 or less, more preferably 4 or less, and further preferably 3 or less.
[0094] The refractive index (n2) of the binder is preferably 1.40 to 1.60, more preferably 1.42 to 1.55, and even more preferably 1.43 to 1.50. The refractive index of the binder can be adjusted by the type and content of the aromatic ring-containing monomer, high refractive index organic material, and high refractive index inorganic material described below.
[0095] From the viewpoint of imparting appropriate light scattering properties to the adhesive layer, the content of light scattering particles in the adhesive layer is preferably 0.01 parts by weight or more, more preferably 0.05 parts by weight or more, further preferably 0.1 parts by weight or more, and particularly preferably 0.15 parts by weight or more, relative to 100 parts by weight of the adhesive constituting the adhesive layer. In addition, from the viewpoint of preventing the haze value from becoming too high, suppressing image blur, and displaying a high-definition image, the content of light scattering particles is preferably 80 parts by weight or less, more preferably 70 parts by weight or less, relative to 100 parts by weight of the adhesive constituting the adhesive layer.
[0096] The adhesive layer of the present invention is not particularly limited, but preferably has a high refractive index from the viewpoint of preventing interface reflection and improving the light collection rate of light emitted from the OLED element. From the viewpoint of preventing interface reflection and improving the light collection rate of light emitted from the OLED element, the refractive index of the adhesive layer of the present invention is preferably 1.57 or more, more preferably 1.575 or more, further preferably 1.580 or more, particularly preferably 1.585 or more, further preferably 1.590 or more, and can be 1.595 or more.
[0097] The refractive index of the adhesive layer of the present invention can be adjusted by the types and contents of the aromatic ring-containing monomer, the high-refractive-index organic material, and the high-refractive-index inorganic material described below.
[0098] The change ratio of the refractive index of the adhesive layer of the present invention before and after humidification is not particularly limited, but from the viewpoint of preventing interface reflection even in a high temperature and high humidity environment and stably improving the light collection rate of light emitted from the OLED element, the change ratio of the refractive index of the adhesive layer of the present invention before and after humidification is preferably 0.05 or less, preferably 0.04 or less, further preferably 0.02 or less, and particularly preferably 0.01 or less.
[0099] The change ratio of the refractive index of the adhesive layer of the present invention before and after humidification can be calculated by the following formula by storing the adhesive layer of the present invention in a humidified environment at a temperature of 85° C. and a relative humidity of 85% for 120 hours.
[0100] Change ratio of refractive index before and after humidification = |initial refractive index - refractive index after humidification| / (initial refractive index)
[0101] The refractive index change ratio before and after humidification can be adjusted by the types and contents of the aromatic ring-containing monomer, high refractive index organic material, and high refractive index inorganic material described below, and the type, monomer composition, crosslinking degree, and thickness of the adhesive constituting the adhesive layer.
[0102] As the adhesive constituting the adhesive layer of the present invention, there is no particular limitation, and for example, acrylic adhesives, rubber adhesives, vinyl alkyl ether adhesives, polysiloxane adhesives, polyester adhesives, polyamide adhesives, polyurethane adhesives, fluorine-containing adhesives, epoxy adhesives, etc. can be cited. Among them, as the adhesive constituting the adhesive layer, acrylic adhesives are preferred from the viewpoints of transparency, adhesion, weather resistance, cost, and ease of design of the adhesive. That is, the adhesive layer of the present invention is preferably an acrylic adhesive layer consisting of an acrylic adhesive. The above-mentioned adhesives can be used alone or in combination of two or more.
[0103] The acrylic adhesive layer contains an acrylic polymer as a base polymer. The acrylic polymer is a polymer containing an acrylic monomer (a monomer having a (meth)acryloyl group in the molecule) as a monomer component constituting the polymer. The acrylic polymer is preferably a polymer containing an alkyl (meth)acrylate as a monomer component constituting the polymer. It should be noted that the acrylic polymer can be used alone or in combination of two or more.
[0104] The adhesive composition forming the adhesive layer of the present invention may be in any form. For example, the adhesive composition may be an emulsion type, a solvent type (solution type), an active energy ray curable type, a hot melt type (hot melt type), etc. Among them, from the aspect of productivity, easy to obtain an adhesive layer with excellent optical properties and appearance, a solvent type or active energy ray curable adhesive composition is preferred.
[0105] That is, the pressure-sensitive adhesive layer of the present invention is an acrylic pressure-sensitive adhesive layer containing an acrylic polymer as a base polymer, and is preferably formed from a solvent-based or active energy ray-curable acrylic pressure-sensitive adhesive composition.
[0106] Examples of the active energy rays include ionizing radiation such as α rays, β rays, γ rays, neutron rays, electron beams, and ultraviolet rays, and ultraviolet rays are particularly preferred. That is, the active energy ray-curable adhesive composition is preferably an ultraviolet-curable adhesive composition.
[0107] As the adhesive composition (acrylic adhesive composition) forming the acrylic adhesive layer, for example, there can be mentioned: an acrylic adhesive composition having an acrylic polymer as an essential component, or an acrylic adhesive composition having a mixture of monomers (monomers) constituting acrylic polymers (sometimes referred to as a "monomer mixture") or a partial polymer thereof as an essential component. As the former, for example, so-called solvent-based acrylic adhesive compositions can be listed. In addition, as the latter, for example, so-called active energy ray-curable acrylic adhesive compositions can be listed. The above-mentioned "monomer mixture" refers to a mixture containing monomer components constituting a polymer. In addition, the above-mentioned "partial polymer" is sometimes also referred to as a "prepolymer", which refers to a composition formed by partial polymerization of one or more monomer components among the monomer components in the above-mentioned monomer mixture.
[0108] The acrylic polymer is a polymer composed (formed) of an acrylic monomer as an essential monomer component (monomer component). The acrylic polymer is preferably a polymer composed (formed) of an alkyl (meth)acrylate as an essential monomer component. That is, the acrylic polymer preferably contains an alkyl (meth)acrylate as a structural unit. In this specification, "(meth)acrylic acid" means "acrylic acid" and / or "methacrylic acid" (either or both of "acrylic acid" and "methacrylic acid"), and the same applies to others. It should be noted that the acrylic polymer is composed of one or more monomer components.
[0109] As the (meth)acrylic acid alkyl ester which is an essential monomer component, preferably, there can be mentioned an (meth)acrylic acid alkyl ester having a linear or branched alkyl group. The (meth)acrylic acid alkyl ester can be used alone or in combination of two or more.
[0110] The (meth)acrylic acid alkyl ester having a linear or branched alkyl group is not particularly limited, and examples thereof include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, propyl ...tert-butyl (meth)acrylate, tert-butyl (meth)acrylate, tert-butyl (meth)acrylate, tert-butyl (meth)acrylate, tert-butyl (meth)acrylate, tert-butyl (meth)acrylate, tert-butyl (meth)acrylate, tert-butyl (meth)acrylate, tert-butyl ( Alkyl (meth)acrylates having a linear or branched alkyl group having 1 to 20 carbon atoms, such as isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate (stearyl (meth)acrylate), isostearyl (meth)acrylate, nonadecyl (meth)acrylate, eicosyl (meth)acrylate. Among them, the alkyl (meth)acrylate having a linear or branched alkyl group is preferably an alkyl (meth)acrylate having a linear or branched alkyl group having 4 to 18 carbon atoms, and more preferably 2-ethylhexyl acrylate (2EHA) and isostearyl acrylate (ISTA). In addition, the above-mentioned alkyl (meth)acrylates having a linear or branched alkyl group can be used alone or in combination of two or more.
[0111] The proportion of the alkyl (meth)acrylate in all monomer components (100 wt %) constituting the acrylic polymer is not particularly limited, but is preferably 50 wt % or more (e.g., 50 to 100 wt %), more preferably 53 to 90 wt %, and further preferably 55 to 85 wt %.
[0112] The acrylic polymer may contain a copolymerizable monomer together with the (meth) alkyl ester as a monomer component constituting the polymer. That is, the acrylic polymer may contain a copolymerizable monomer as a structural unit. It should be noted that the copolymerizable monomer may be used alone or in combination of two or more.
[0113] The copolymerizable monomer is not particularly limited, but preferably includes a monomer having an aromatic ring in the molecule from the viewpoint of obtaining a high refractive index adhesive layer, suppressing interface reflection with the OLED display panel, and improving the light collection efficiency of light from the OLED element. That is, the acrylic polymer preferably contains a monomer having an aromatic ring in the molecule as a constituent unit.
[0114] The monomer having an aromatic ring in the molecule is a monomer (monomer) having at least one aromatic ring in the molecule (in one molecule). In the present specification, the "monomer having an aromatic ring in the molecule" may be referred to as an "aromatic ring-containing monomer".
[0115] As the aromatic ring-containing monomer, a compound containing at least one aromatic ring and at least one ethylenically unsaturated group in one molecule is used. As the aromatic ring-containing monomer, one type of the compound may be used alone or two or more types may be used in combination.
[0116] Examples of the ethylenically unsaturated group include (meth)acryloyl, vinyl, (meth)allyl, etc. From the viewpoint of polymerization reactivity, (meth)acryloyl is preferred, and from the viewpoint of flexibility and adhesiveness, acryloyl is more preferred. From the viewpoint of suppressing the decrease in the flexibility of the adhesive, as the aromatic ring-containing monomer, a compound having 1 ethylenically unsaturated group contained in one molecule (i.e., a monofunctional monomer) is preferably used.
[0117] The number of aromatic rings contained in one molecule of the compound used as the aromatic ring-containing monomer may be 1 or may be 2 or more. The upper limit of the number of aromatic rings contained in the aromatic ring-containing monomer is not particularly limited, and may be, for example, 16 or less. From the viewpoint of the ease of preparation of the acrylic polymer and the transparency of the adhesive, the number of the aromatic rings may be, for example, 12 or less, preferably 8 or less, more preferably 6 or less, 5 or less, 4 or less, 3 or less, or 2 or less.
[0118] The aromatic ring possessed by the compound used as the aromatic ring-containing monomer may be, for example, a benzene ring (which may be a benzene ring constituting a part of a biphenyl structure or a fluorene structure); a carbon ring such as a condensed ring of a naphthalene ring, an indene ring, an azulene ring, an anthracene ring, or a phenanthrene ring; and may be, for example, a pyridine ring, a pyrimidine ring, a pyridazine ring, a pyrazine ring, a triazine ring, a pyrrole ring, a pyrazole ring, an imidazole ring, a triazole ring, Azole ring, iso The heteroatoms included as ring atoms in the heterocyclic rings may be one or more selected from the group consisting of nitrogen, sulfur and oxygen. The heteroatoms constituting the heterocyclic rings may be one or both of nitrogen and sulfur. The aromatic ring-containing monomer may have a structure in which one or more carbon rings are fused with one or more heterocyclic rings, such as a dinaphthothiophene structure.
[0119] The above-mentioned aromatic ring (preferably a carbon ring) may have one or more substituents on the ring-constituting atoms, or may not have substituents. In the case of having a substituent, examples of the substituent include: alkyl, alkoxy, aryloxy, hydroxyl, halogen atoms (fluorine atoms, chlorine atoms, bromine atoms, etc.), hydroxyalkyl, hydroxyalkoxy, glycidoxy, etc., but are not limited to these groups. In the substituent containing carbon atoms, the number of carbon atoms contained in the substituent is preferably 1 to 4, more preferably 1 to 3, for example, 1 or 2. The above-mentioned aromatic ring may be an aromatic ring that has no substituent on the ring-constituting atoms, or has one or more substituents selected from alkyl, alkoxy and halogen atoms (such as bromine atoms). It should be noted that the aromatic ring possessed by the aromatic ring-containing monomer has a substituent on its ring-constituting atom means that the aromatic ring has a substituent other than a substituent having an ethylenically unsaturated group.
[0120] The aromatic ring and the ethylenically unsaturated group may be directly bonded or bonded via a linking group. The above-mentioned linking group may be, for example, a group containing one or more structures selected from alkylene, oxyalkylene, poly(oxyalkylene) groups, phenyl, alkylphenyl, alkoxyphenyl, a group in which one or more hydrogen atoms in these groups are substituted with hydroxyl groups (e.g., hydroxyalkylene), oxy (-O-group), thiol (-S-group), etc. An aromatic ring-containing monomer having a structure in which the aromatic ring and the ethylenically unsaturated group are directly bonded or bonded via a linking group selected from alkylene, oxyalkylene and poly(oxyalkylene) groups may be preferably used. The number of carbon atoms in the above-mentioned alkylene and the above-mentioned oxyalkylene is preferably 1 to 4, more preferably 1 to 3, for example, 1 or 2. The number of repetitions of the oxyalkylene unit in the above-mentioned poly(oxyalkylene) group may be, for example, 2 to 3.
[0121] Examples of compounds that can be preferably used as aromatic ring-containing monomers include aromatic ring-containing (meth)acrylates and aromatic ring-containing vinyl compounds. Aromatic ring-containing (meth)acrylates and aromatic ring-containing vinyl compounds can be used alone or in combination of two or more. One or two or more aromatic ring-containing (meth)acrylates can be used in combination with one or two or more aromatic ring-containing vinyl compounds.
[0122] In the case where the acrylic polymer contains the aromatic ring-containing monomer as the monomer component constituting the polymer, the ratio of the aromatic ring-containing monomer in all the monomer components (100% by weight) constituting the acrylic polymer is not particularly limited, preferably more than 30% by weight, more preferably more than 50% by weight, further preferably more than 60% by weight, and can be more than 70% by weight. When the above ratio is more than 30% by weight, it is preferred to have a tendency to easily obtain a higher refractive index. From the viewpoint of easily obtaining a higher refractive index, the content of the aromatic ring-containing monomer can be, for example, greater than 70% by weight, can be more than 75% by weight, can be more than 80% by weight, can be more than 85% by weight, can be more than 90% by weight, and can also be more than 95% by weight. In addition, from the aspect of obtaining an adhesive layer with appropriate softness, the aspect of obtaining an adhesive layer with excellent transparency, the upper limit of the ratio of the aromatic ring-containing monomer is preferably less than 99% by weight, more preferably less than 98% by weight, further preferably less than 97% by weight, and can be less than 96% by weight. In addition, the content of the aromatic ring-containing monomer may be 93% by weight or less, 90% by weight or less, 80% by weight or less, or 75% by weight or less. In some embodiments that place more emphasis on adhesive properties and / or optical properties, the content of the aromatic ring-containing monomer may be 70% by weight or less, 60% by weight or less, or 45% by weight or less.
[0123] As an aromatic ring-containing monomer, from the viewpoint of easily obtaining a high refractive index effect, a monomer having two or more aromatic rings (preferably a carbon ring) in one molecule can be preferably used. As an example of a monomer having two or more aromatic rings in one molecule (hereinafter, also referred to as "a monomer containing multiple aromatic rings"), a monomer having a structure in which two or more non-condensed aromatic rings are bonded via a connecting group, a monomer having a structure in which two or more non-condensed aromatic rings are directly (i.e., not via other atoms) chemically bonded, a monomer having a condensed aromatic ring structure, a monomer having a fluorene structure, a monomer having a dinaphthothiophene structure, a monomer having a dibenzothiophene structure, etc. can be cited. Multiple aromatic ring-containing monomers can be used alone or in combination of two or more.
[0124] The above-mentioned linking group can be, for example, an oxy group (-O-), a thiol group (-S-), an oxyalkylene group (e.g., -O-(CH2)n - alkyl, where n is 1 to 3, preferably 1), sulfanyl (e.g. -S-(CH2) n -alkyl, where n is 1 to 3, preferably 1), straight chain alkylene (i.e. -(CH2) n - group, where n is 1 to 6, preferably 1 to 3), a group obtained by partially or completely halogenating the alkylene in the above-mentioned oxyalkylene, the above-mentioned sulfenylene and the above-mentioned linear alkylene, etc. From the viewpoint of the flexibility of the adhesive, preferred examples of the above-mentioned linking group include oxy, sulfenyl, oxyalkylene and linear alkylene. Specific examples of monomers having a structure in which two or more non-condensed aromatic rings are bonded via a linking group include phenoxybenzyl (meth)acrylate (e.g., m-phenoxybenzyl (meth)acrylate), phenylthiobenzyl (meth)acrylate, benzylbenzyl (meth)acrylate, etc.
[0125] The monomer having a structure in which two or more non-condensed aromatic rings are directly chemically bonded may be, for example, a (meth)acrylate containing a biphenyl structure, a (meth)acrylate containing a triphenyl structure, a vinyl-containing biphenyl, etc. Specific examples include o-phenylphenol (meth)acrylate, biphenyl methyl (meth)acrylate, etc.
[0126] Examples of the monomer having a condensed aromatic ring structure include naphthalene ring-containing (meth)acrylates, anthracene ring-containing (meth)acrylates, vinyl-containing naphthalene, vinyl-containing anthracene, etc. Specific examples include 1-naphthylmethyl (meth)acrylate (also known as 1-naphthylmethyl (meth)acrylate), hydroxyethylated β-naphthol acrylate, 2-naphthylethyl (meth)acrylate, 2-naphthyloxyethyl acrylate, and 2-(4-methoxy-1-naphthyloxy)ethyl (meth)acrylate.
[0127] Specific examples of the above-mentioned monomer having a fluorene structure include 9,9-bis(4-hydroxyphenyl)fluorene(meth)acrylate, 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene(meth)acrylate, etc. It should be noted that the monomer having a fluorene structure includes a structural portion in which two benzene rings are directly chemically bonded, and is therefore included in the concept of the above-mentioned monomer having a structure in which two or more non-condensed aromatic rings are directly chemically bonded.
[0128] Examples of the monomer having a dinaphthothiophene structure include dinaphthothiophene containing a (meth)acryloyl group, dinaphthothiophene containing a vinyl group, and dinaphthothiophene containing a (meth)allyl group. Specific examples include (meth)acryloyloxymethyl dinaphthothiophene (for example, CH2CH(R) is bonded to the 5-position or 6-position of the dinaphthothiophene ring). 1 )C(O)OCH2-. Here, R 1is a hydrogen atom or a methyl group. ), (meth)acryloyloxyethyl dinaphthothiophene (for example, CH2CH(R) is bonded to the 5-position or 6-position of the dinaphthothiophene ring) 1 )C(O)OCH(CH3)- or CH2CH(R 1 )C(O)OCH2CH2-. Here, R 1 is a hydrogen atom or a methyl group. ), vinyl dinaphthothiophene (for example, a compound having a structure in which a vinyl group is bonded to the 5-position or 6-position of the naphthothiophene ring), (methyl)allyloxy dinaphthothiophene, etc. It should be noted that the monomer having a dinaphthothiophene structure is also included in the concept of the monomer having the above-mentioned fused aromatic ring structure because it includes a naphthalene structure and has a structure in which a thiophene ring is fused to two naphthalene structures.
[0129] Examples of the monomer having a dibenzothiophene structure include (meth)acryloyl-containing dibenzothiophene and vinyl-containing dibenzothiophene. It should be noted that the monomer having a dibenzothiophene structure is included in the concept of the monomer having a fused aromatic ring structure because it has a structure in which a thiophene ring is fused to two benzene rings.
[0130] It should be noted that neither the dinaphthothiophene structure nor the dibenzothiophene structure belongs to a structure in which two or more non-condensed aromatic rings are directly chemically bonded.
[0131] As the aromatic ring-containing monomer, a monomer having one aromatic ring (preferably a carbocyclic ring) in one molecule can be used. A monomer having one aromatic ring in one molecule can, for example, contribute to the improvement of the flexibility of the adhesive, the adjustment of the adhesive properties, the improvement of the transparency, etc. From the viewpoint of increasing the refractive index of the adhesive, a monomer having one aromatic ring in one molecule is preferably used in combination with a monomer containing multiple aromatic rings.
[0132] Examples of monomers having one aromatic ring in one molecule include: (meth)acrylates containing carbon aromatic rings, such as benzyl (meth)acrylate, methoxybenzyl (meth)acrylate, phenyl (meth)acrylate, ethoxylated phenol (meth)acrylate, phenoxypropyl (meth)acrylate, phenoxybutyl (meth)acrylate, tolyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, and benzyl (meth)acrylate chloride; (meth)acrylate 2-(4,6-dibromo-2-sec-butylphenoxy)ethyl; (meth)acrylate 2-(4,6-dibromo-2-isobutylphenoxy)ethyl; 6-(4,6-dibromo-2-sec-butylphenoxy)hexyl (meth)acrylate; (meth)acrylates containing bromine-substituted aromatic rings, such as 6-(4,6-dibromo-2-isopropylphenoxy)hexyl (meth)acrylate, 2,6-dibromo-4-nonylphenyl acrylate, and 2,6-dibromo-4-dodecylphenyl acrylate; vinyl compounds containing carbon aromatic rings, such as styrene, α-methylstyrene, vinyltoluene, and tert-butylstyrene; N-vinylpyridine, N-vinylpyrimidine, N-vinylpyrazine, N-vinylpyrrole, N-vinylimidazole, N-vinyl Compounds such as azoles having a vinyl substituent on a heteroaromatic ring; etc.
[0133] As the aromatic ring-containing monomer, a monomer having a structure in which an oxyethylene chain exists between the ethylenically unsaturated group and the aromatic ring in the various aromatic ring-containing monomers described above can be used. The monomer having an oxyethylene chain between the ethylenically unsaturated group and the aromatic ring can be understood as an ethoxylate of the original monomer. The number of repetitions of the oxyethylene unit (-CH2CH2O-) in the above-mentioned oxyethylene chain is typically 1 to 4, preferably 1 to 3, more preferably 1 to 2, for example 1. Specific examples of ethoxylated aromatic ring-containing monomers include: ethoxylated o-phenylphenol (meth) acrylate, ethoxylated nonylphenol (meth) acrylate, ethoxylated cresol (meth) acrylate, phenoxyethyl (meth) acrylate, phenoxydiethylene glycol di(meth) acrylate, etc.
[0134] The content of the monomer containing multiple aromatic rings in the aromatic ring-containing monomer is not particularly limited, for example, it can be more than 5% by weight, can be more than 25% by weight, can be more than 40% by weight. From the viewpoint of easily realizing an adhesive with a higher refractive index, the content of the monomer containing multiple aromatic rings in the aromatic ring-containing monomer can be, for example, more than 50% by weight, preferably more than 70% by weight, can be more than 85% by weight, can be more than 90% by weight, can be more than 95% by weight. The aromatic ring-containing monomer can be substantially 100% by weight of a monomer containing multiple aromatic rings. That is, as an aromatic ring-containing monomer, only one or more monomers containing multiple aromatic rings can be used. In addition, for example, considering the balance between high refractive index and adhesive properties and / or optical properties, the content of the monomer containing multiple aromatic rings in the aromatic ring-containing monomer can be less than 100% by weight, can be less than 98% by weight, can be less than 90% by weight, can be less than 80% by weight, can be less than 65% by weight. Considering the adhesive properties and / or optical properties, the content of the monomer containing multiple aromatic rings in the aromatic ring-containing monomer may be 70% by weight or less, 50% by weight or less, 25% by weight or less, or 10% by weight or less. It is also possible to implement the method in which the content of the monomer containing multiple aromatic rings in the aromatic ring-containing monomer is less than 5% by weight. It is also possible not to use the monomer containing multiple aromatic rings.
[0135] In the case where the acrylic polymer contains the monomer containing multiple aromatic rings as a monomer component constituting the polymer, the proportion of the monomer containing multiple aromatic rings in the total monomer components (100% by weight) constituting the acrylic polymer is not particularly limited, and is preferably 3% by weight or more, more preferably 10% by weight or more, and further preferably 25% by weight or more. When the above proportion is 3% by weight or more, there is a tendency to easily obtain a higher refractive index, which is satisfactory. In addition, from the viewpoint of easily obtaining a higher refractive index, the content of the monomer containing multiple aromatic rings can be, for example, greater than 35% by weight, can be 50% by weight or more, can be 70% by weight or more, can be 75% by weight or more, can be 85% by weight or more, can be 90% by weight or more, and can be 95% by weight or more. In addition, from the viewpoint of balancing high refractive index and adhesive properties and / or optical properties, the upper limit of the ratio of the above-mentioned monomer containing multiple aromatic rings is preferably 99% by weight or less, more preferably 98% by weight or less, further preferably 96% by weight or less, and can be 93% by weight or less, 90% by weight or less, 85% by weight or less, 80% by weight or less, or 75% by weight or less. In addition, from the viewpoint of adhesive properties and / or optical properties, the content of the above-mentioned monomer containing multiple aromatic rings can be 70% by weight or less, 50% by weight or less, 25% by weight or less, 15% by weight or less, or 5% by weight or less.
[0136] The copolymerizable monomer is not particularly limited, but preferably includes monomers having nitrogen atoms in the molecule and monomers having hydroxyl groups in the molecule from the viewpoints of suppressing cloudiness in a high humidity environment, improving durability, compatibility with various additives such as ultraviolet absorbers, and transparency. That is, the acrylic polymer preferably contains a monomer having a nitrogen atom in the molecule as a constituent unit. In addition, the acrylic polymer preferably contains a monomer having a hydroxyl group in the molecule as a constituent unit.
[0137] The monomer having a nitrogen atom in the molecule is a monomer (monomer) having at least one nitrogen atom in the molecule (in one molecule). In this specification, the "monomer having a nitrogen atom in the molecule" is sometimes referred to as a "nitrogen atom-containing monomer". There are no particular restrictions on the nitrogen atom-containing monomer, and preferably, cyclic nitrogen-containing monomers, (meth)acrylamides, etc. can be cited. It should be noted that the nitrogen atom-containing monomer can be used alone or in combination of two or more.
[0138] The cyclic nitrogen-containing monomer is not particularly limited as long as it has a polymerizable functional group having an unsaturated double bond such as a (meth)acryloyl group or a vinyl group and has a cyclic nitrogen structure. The cyclic nitrogen structure preferably has a nitrogen atom in the cyclic structure.
[0139] Examples of the cyclic nitrogen-containing monomer include N-vinyl cyclic amides (lactam-based vinyl monomers) and vinyl-based monomers having a nitrogen-containing heterocyclic ring.
[0140] Examples of the N-vinyl cyclic amide include N-vinyl cyclic amides represented by the following formula (1).
[0141]
[0142] (In formula (1), R 1 represents a divalent organic group. )
[0143] In the above formula (1), R 1 It is a divalent organic group, preferably a divalent saturated hydrocarbon group or an unsaturated hydrocarbon group, and more preferably a divalent saturated hydrocarbon group (for example, an alkylene group having 3 to 5 carbon atoms).
[0144] Examples of the N-vinyl cyclic amide represented by the formula (1) include N-vinyl-2-pyrrolidone, N-vinyl-2-piperidone, N-vinyl-3-morpholinone, N-vinyl-2-caprolactam, N-vinyl-1,3- Oxazine-2-one and N-vinyl-3,5-morpholinedione.
[0145] Examples of the vinyl monomer having a nitrogen-containing heterocyclic ring include acrylic monomers having a nitrogen-containing heterocyclic ring such as a morpholine ring, a piperidine ring, a pyrrolidine ring, and a piperazine ring.
[0146] The vinyl monomer having a nitrogen-containing heterocyclic ring is not particularly limited, and examples thereof include (meth)acryloylmorpholine, N-vinylpiperazine, N-vinylpyrrole, N-vinylimidazole, N-vinylpyrazine, N-vinylmorpholine, N-vinylpyrazole, vinylpyridine, vinylpyrimidine, vinyl Azoles, vinyl isocyanates oxazole, vinylthiazole, vinylisothiazole, vinylpyridazine, (meth)acryloylpyrrolidone, (meth)acryloylpyrrolidine, (meth)acryloylpiperidine and the like.
[0147] As the vinyl monomer having a nitrogen-containing heterocyclic ring, among them, an acrylic monomer having a nitrogen-containing heterocyclic ring is preferred, and (meth)acryloylmorpholine, (meth)acryloylpyrrolidine, and (meth)acryloylpiperidine are more preferred.
[0148] Examples of the (meth)acrylamides include (meth)acrylamide, N-alkyl (meth)acrylamide, N,N-dialkyl (meth)acrylamide, etc. Examples of the N-alkyl (meth)acrylamide include N-ethyl (meth)acrylamide, N-isopropyl (meth)acrylamide, N-n-butyl (meth)acrylamide, and N-octyl (meth)acrylamide. In addition, the N-alkyl (meth)acrylamide also includes (meth)acrylamide having an amino group, such as dimethylaminoethyl (meth)acrylamide, diethylaminoethyl (meth)acrylamide, and dimethylaminopropyl (meth)acrylamide. Examples of the N,N-dialkyl(meth)acrylamide include N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-dipropyl(meth)acrylamide, N,N-diisopropyl(meth)acrylamide, N,N-di(n-butyl)(meth)acrylamide, and N,N-di(tert-butyl)(meth)acrylamide.
[0149] In addition, the (meth)acrylamides include, for example, various N-hydroxyalkyl (meth)acrylamides. Examples of the N-hydroxyalkyl (meth)acrylamides include N-methylol (meth)acrylamide, N-(2-hydroxyethyl) (meth)acrylamide, N-(2-hydroxypropyl) (meth)acrylamide, N-(1-hydroxypropyl) (meth)acrylamide, N-(3-hydroxypropyl) (meth)acrylamide, N-(2-hydroxybutyl) (meth)acrylamide, N-(3-hydroxybutyl) (meth)acrylamide, N-(4-hydroxybutyl) (meth)acrylamide, and N-methyl-N-2-hydroxyethyl (meth)acrylamide.
[0150] The (meth)acrylamides include, for example, various N-alkoxyalkyl (meth)acrylamides. Examples of the N-alkoxyalkyl (meth)acrylamides include N-methoxymethyl (meth)acrylamide and N-butoxymethyl (meth)acrylamide.
[0151] In addition, examples of nitrogen-containing monomers other than the cyclic nitrogen-containing monomers and the (meth)acrylamides include amino-containing monomers, cyano-containing monomers, imide-containing monomers, isocyanate-containing monomers, etc. Examples of the amino-containing monomers include aminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, dimethylaminopropyl (meth)acrylate, and tert-butylaminoethyl (meth)acrylate. Examples of the cyano-containing monomers include acrylonitrile, methacrylonitrile, etc. Examples of the imide group-containing monomer include maleimide monomers (e.g., N-cyclohexylmaleimide, N-isopropylmaleimide, N-laurylmaleimide, N-phenylmaleimide, etc.), itaconimide monomers (e.g., N-methylitaconimide, N-ethylitaconimide, N-butylitaconimide, N-octylitaconimide, N-2-ethylhexylitaconimide, N-laurylitaconimide, N-cyclohexylitaconimide, etc.), succinimide monomers (e.g., N-(meth)acryloyloxymethylenesuccinimide, N-(meth)acryloyl-6-oxyhexamethylenesuccinimide, N-(meth)acryloyl-8-oxyoctamethylenesuccinimide, etc.), etc. Examples of the isocyanate group-containing monomer include 2-(meth)acryloyloxyethyl isocyanate.
[0152] Among them, as the nitrogen atom-containing monomer, a cyclic nitrogen-containing monomer is preferred, and N-vinyl cyclic amide is more preferred. More specifically, N-vinyl-2-pyrrolidone (NVP) is particularly preferred.
[0153] When the acrylic polymer contains the nitrogen-containing monomer as a monomer component constituting the polymer, the proportion of the nitrogen-containing monomer in all monomer components (100% by weight) constituting the acrylic polymer is not particularly limited, and is preferably 1% by weight or more, more preferably 3% by weight or more, and further preferably 5% by weight or more. When the above proportion is 1% by weight or more, the suppression of white turbidity and the durability under a high humidity environment can be further improved, which is satisfactory. In addition, from the viewpoint of obtaining an adhesive layer with moderate softness and the viewpoint of obtaining an adhesive layer with excellent transparency, the upper limit of the proportion of the nitrogen-containing monomer is preferably 30% by weight or less, more preferably 25% by weight or less, and further preferably 20% by weight or less.
[0154] The above-mentioned monomer having a hydroxyl group in the molecule is a monomer having at least one hydroxyl group (hydroxyl group) in the molecule (in one molecule), preferably a monomer having a polymerizable functional group having an unsaturated double bond such as a (meth)acryloyl group or a vinyl group and having a hydroxyl group. Among them, the monomer having a hydroxyl group in the molecule does not include the above-mentioned nitrogen atom-containing monomer. That is, in this specification, a monomer having both a nitrogen atom and a hydroxyl group in the molecule is included in the above-mentioned "nitrogen atom-containing monomer". In this specification, the above-mentioned "monomer having a hydroxyl group in the molecule" is sometimes referred to as a "hydroxyl-containing monomer". It should be noted that the hydroxyl-containing monomer can be used alone or in combination of two or more.
[0155] Examples of the hydroxyl-containing monomer include hydroxyl-containing (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, hydroxyoctyl (meth)acrylate, hydroxydecyl (meth)acrylate, hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl) (meth)acrylate; vinyl alcohol; allyl alcohol, and the like.
[0156] Among them, as the hydroxyl group-containing monomer, hydroxyl group-containing (meth)acrylate is preferred, and 2-hydroxyethyl acrylate (HEA) and 4-hydroxybutyl acrylate (4HBA) are more preferred.
[0157] When the acrylic polymer contains the hydroxyl-containing monomer as a monomer component constituting the polymer, the proportion of the hydroxyl-containing monomer in all monomer components (100% by weight) constituting the acrylic polymer is not particularly limited, but is preferably 0.5% by weight or more, more preferably 0.8% by weight or more, and further preferably 1% by weight or more from the viewpoint of suppressing cloudiness in a high-humidity environment and improving durability. In addition, from the viewpoint of obtaining an adhesive layer with moderate flexibility and an adhesive layer with excellent transparency, the upper limit of the proportion of the hydroxyl-containing monomer is preferably 30% by weight or less, more preferably 25% by weight or less, and further preferably 15% by weight or less.
[0158] The total ratio of the nitrogen-atom-containing monomer and the hydroxyl-containing monomer in all monomer components (100% by weight) constituting the acrylic polymer is not particularly limited, but is preferably 1% by weight or more, more preferably 5% by weight or more, and further preferably 10% by weight or more from the viewpoint of suppressing cloudiness under high humidity and improving durability. In addition, from the viewpoint of obtaining an adhesive layer with appropriate flexibility and an adhesive layer with excellent transparency, the upper limit of the total ratio is preferably 50% by weight or less, more preferably 40% by weight or less, and further preferably 35% by weight or less.
[0159] As copolymerizable monomers other than nitrogen-containing monomers and hydroxyl-containing monomers, alicyclic structure-containing monomers can also be cited. The above-mentioned alicyclic structure-containing monomers are not particularly limited as long as they have a polymerizable functional group having an unsaturated double bond such as a (meth)acryloyl group or a vinyl group and have an alicyclic structure. For example, (meth)acrylic acid alkyl esters having a cycloalkyl group are included in the above-mentioned alicyclic structure-containing monomers. It should be noted that the alicyclic structure-containing monomers can be used alone or in combination of two or more.
[0160] The alicyclic structure in the alicyclic structure-containing monomer is a cyclic hydrocarbon structure, and preferably has 5 or more carbon atoms, more preferably 6 to 24 carbon atoms, further preferably 6 to 15 carbon atoms, and particularly preferably 6 to 10 carbon atoms.
[0161] Examples of the above-mentioned alicyclic structure-containing monomers include: cyclopropyl (meth)acrylate, cyclobutyl (meth)acrylate, cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, cycloheptyl (meth)acrylate, cyclooctyl (meth)acrylate, isobornyl (meth)acrylate, tetrahydrodicyclopentadienyl (meth)acrylate, HPMPA represented by the following formula (2), TMA-2 represented by the following formula (3), HCPA represented by the following formula (4), and other acrylic monomers. It should be noted that in the following formula (4), there is no particular limitation on the bonding position of the cyclohexyl ring connected by a line to the structural formula in the brackets. Among them, isobornyl (meth)acrylate is preferred.
[0162]
[0163]
[0164]
[0165] When the acrylic polymer contains the alicyclic structure-containing monomer as a monomer component constituting the polymer, the proportion of the alicyclic structure-containing monomer in the total monomer components (100% by weight) constituting the acrylic polymer is not particularly limited, but is preferably 10% by weight or more from the viewpoint of improving durability. In addition, from the viewpoint of obtaining an adhesive layer having moderate flexibility, the upper limit of the proportion of the alicyclic structure-containing monomer is preferably 50% by weight or less, more preferably 40% by weight or less, and further preferably 30% by weight or less.
[0166] In addition, as copolymerizable monomers, for example, multifunctional monomers can be cited. As multifunctional monomers, for example, hexanediol di(meth)acrylate, butanediol di(meth)acrylate, (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, trimethylolpropane tri(meth)acrylate, tetramethylolmethane tri(meth)acrylate, allyl (meth)acrylate, vinyl (meth)acrylate, divinylbenzene, epoxy acrylate, polyester acrylate and urethane acrylate. It should be noted that the multifunctional monomers can be used alone or in combination of two or more.
[0167] In the case where the acrylic polymer contains the multifunctional monomer as a monomer component constituting the polymer, the proportion of the multifunctional monomer in all monomer components (100 wt %) constituting the acrylic polymer is not particularly limited, and is preferably 0.5 wt % or less (e.g., greater than 0 wt % and less than or equal to 0.5 wt %), and more preferably 0.2 wt % or less (e.g., greater than 0 wt % and less than or equal to 0.2 wt %).
[0168] In addition, as the copolymerizable monomer, alkoxyalkyl (meth)acrylate can be cited. As the alkoxyalkyl (meth)acrylate, there is no particular limitation, for example, 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, methoxytriethylene glycol (meth)acrylate, 3-methoxypropyl (meth)acrylate, 3-ethoxypropyl (meth)acrylate, 4-methoxybutyl (meth)acrylate, 4-ethoxybutyl (meth)acrylate, etc. can be cited. Among them, the alkoxyalkyl (meth)acrylate is preferably an alkoxyalkyl acrylate, more preferably 2-methoxyethyl acrylate (MEA). It should be noted that the alkoxyalkyl (meth)acrylate can be used alone or in combination of two or more.
[0169] When the acrylic polymer contains the alkoxyalkyl (meth)acrylate as a monomer component constituting the polymer, the ratio of the alkyl (meth)acrylate to the alkoxyalkyl (meth)acrylate is not particularly limited, but is preferably 100: greater than 0 to 25:75 or less, and more preferably 100: greater than 0 to 50:50 or less in terms of [former:latter] (weight ratio).
[0170] In addition, as the copolymerizable monomers, for example, carboxyl-containing monomers, epoxy-containing monomers, sulfonic acid-containing monomers, phosphoric acid-containing monomers, (meth)acrylates having aromatic hydrocarbon groups, vinyl esters, aromatic vinyl compounds, olefins or dienes, vinyl ethers, vinyl chloride, etc. can be cited. As the above-mentioned carboxyl-containing monomers, for example, (meth)acrylic acid, itaconic acid, maleic acid, fumaric acid, crotonic acid, isocrotonic acid, etc. can be cited. In addition, the above-mentioned carboxyl-containing monomers also include acid anhydride-containing monomers such as maleic anhydride and itaconic anhydride. As the above-mentioned epoxy-containing monomers, for example, (meth)acrylate glycidyl and (meth)acrylate methyl glycidyl can be cited. As the above-mentioned sulfonic acid-containing monomers, for example, sodium vinyl sulfonate can be cited. As the above-mentioned (meth)acrylates having aromatic hydrocarbon groups, for example, phenyl (meth)acrylate, phenoxyethyl (meth)acrylate, benzyl (meth)acrylate, etc. can be cited. As the above-mentioned vinyl esters, for example, vinyl acetate and vinyl propionate can be cited. Examples of the aromatic vinyl compounds include styrene and vinyltoluene. Examples of the olefins or dienes include ethylene, propylene, butadiene, isoprene and isobutylene. Examples of the vinyl ethers include vinyl alkyl ethers.
[0171] In the case where the adherend of the adhesive layer includes wiring of metal or metal oxide such as a touch panel, from the viewpoint of obtaining an acrylic adhesive layer with excellent corrosion resistance, the acrylic polymer preferably does not contain or substantially does not contain an acidic group-containing monomer as a monomer component constituting the polymer, and particularly preferably does not contain or substantially does not contain a carboxyl group-containing monomer. As the acidic group-containing monomer, for example, carboxyl group-containing monomers, sulfonic acid group-containing monomers, phosphoric acid group-containing monomers, etc. can be cited. Specifically, the ratio of the acidic group-containing monomer in all monomer components (100% by weight) constituting the acrylic polymer is 0.05% by weight or less (preferably 0.01% by weight or less), which can be called substantially free of acidic group-containing monomers.
[0172] The content of the base polymer (especially acrylic polymer) in the adhesive layer of the present invention is not particularly limited, and is preferably 50 wt % or more (e.g., 50 wt % to 100 wt %), more preferably 80 wt % or more (e.g., 80 wt % to 100 wt %), and further preferably 90 wt % or more (e.g., 90 wt % to 100 wt %), relative to 100 wt % of the total weight of the adhesive layer of the present invention.
[0173] The base polymer such as the acrylic polymer contained in the adhesive layer of the present invention can be obtained by polymerizing the monomer components. There are no particular restrictions on the polymerization method, and examples thereof include solution polymerization, emulsion polymerization, bulk polymerization, and polymerization using active energy ray irradiation (active energy ray polymerization). Among them, from the perspectives of transparency and cost of the adhesive layer, solution polymerization and active energy ray polymerization are preferred.
[0174] In addition, various common solvents can be used in the polymerization of the above-mentioned monomer components. Examples of the above-mentioned solvents include esters such as ethyl acetate and n-butyl acetate; aromatic hydrocarbons such as toluene and benzene; aliphatic hydrocarbons such as n-hexane and n-heptane; alicyclic hydrocarbons such as cyclohexane and methylcyclohexane; ketones such as methyl ethyl ketone and methyl isobutyl ketone, and other organic solvents. It should be noted that the solvents can be used alone or in combination of two or more.
[0175] In the polymerization of the above-mentioned monomer components, a polymerization initiator such as a thermal polymerization initiator or a photopolymerization initiator (photoinitiator) may be used depending on the type of the polymerization reaction. The polymerization initiator may be used alone or in combination of two or more.
[0176] As the above-mentioned thermal polymerization initiator, there is no particular limitation, for example, azo polymerization initiators, peroxide polymerization initiators (such as dibenzoyl peroxide, tert-butyl permaleate, etc.), redox polymerization initiators, etc. can be listed. Among them, the azo polymerization initiators disclosed in Japanese Patent Publication No. 2002-69411 are preferred. As the above-mentioned azo polymerization initiators, 2,2'-azobisisobutyronitrile (hereinafter sometimes referred to as "AIBN"), 2,2'-azobis(-2-methylbutyronitrile) (hereinafter sometimes referred to as "AMBN"), 2,2'-azobis(2-methylpropionic acid) dimethyl ester and 4,4'-azobis(-4-cyanovaleric acid) can be listed. It should be noted that the thermal polymerization initiator can be used alone or in combination of two or more.
[0177] When the azo polymerization initiator is used in the polymerization of the acrylic polymer, the amount of the azo polymerization initiator used is not particularly limited. For example, the amount of the azo polymerization initiator used is preferably 0.05 parts by weight or more, more preferably 0.1 parts by weight or more, relative to 100 parts by weight of all monomer components constituting the acrylic polymer. In addition, the amount of the azo polymerization initiator used is preferably 0.5 parts by weight or less, more preferably 0.3 parts by weight or less.
[0178] As the above-mentioned photopolymerization initiator, there is no particular limitation, and examples thereof include benzoin ether photopolymerization initiators, acetophenone photopolymerization initiators, α-ketol photopolymerization initiators, aromatic sulfonyl chloride photopolymerization initiators, photoactive oxime photopolymerization initiators, benzoin photopolymerization initiators, benzyl photopolymerization initiators, benzophenone photopolymerization initiators, ketal photopolymerization initiators, thioxanthone photopolymerization initiators, etc. In addition, acylphosphine oxide photopolymerization initiators and titanocene photopolymerization initiators can be listed. As the above-mentioned benzoin ether photopolymerization initiators, for example, benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, benzoin isopropyl ether, benzoin isobutyl ether, 2,2-dimethoxy-1,2-diphenylethane-one, anisole methyl ether, etc. can be listed. Examples of the acetophenone-based photopolymerization initiator include 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxycyclohexylphenyl ketone, 4-phenoxydichloroacetophenone, and 4-(tert-butyl)dichloroacetophenone. Examples of the α-ketoalcohol-based photopolymerization initiator include 2-methyl-2-hydroxypropiophenone and 1-[4-(2-hydroxyethyl)phenyl]-2-methylpropane-1-one. Examples of the aromatic sulfonyl chloride-based photopolymerization initiator include 2-naphthalenesulfonyl chloride and the like. Examples of the photoactive oxime-based photopolymerization initiator include 1-phenyl-1,2-propanedione-2-(O-ethoxycarbonyl)-oxime. Examples of the benzoin-based photopolymerization initiator include benzoin and the like. Examples of the benzyl-based photopolymerization initiator include benzyl. As the above-mentioned benzophenone-based photopolymerization initiator, for example, benzophenone, benzoylbenzoic acid, 3,3'-dimethyl-4-methoxybenzophenone, poly(vinylbenzophenone) and α-hydroxycyclohexylphenyl ketone can be listed. As the above-mentioned ketal-based photopolymerization initiator, for example, benzildimethylketal can be listed. As the above-mentioned thioxanthone-based photopolymerization initiator, for example, thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-diisopropylthioxanthone and dodecylthioxanthone can be listed. As the above-mentioned acylphosphine oxide-based photopolymerization initiator, for example, 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, etc. As the above-mentioned titanocene-based photopolymerization initiator, for example, bis(η 5 -2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl)titanium, etc. In addition, the photopolymerization initiator can be used alone or in combination of two or more.
[0179] When the photopolymerization initiator is used in the polymerization of the acrylic polymer, the amount of the photopolymerization initiator used is not particularly limited. For example, it is preferably 0.01 parts by weight or more, more preferably 0.1 parts by weight or more, relative to 100 parts by weight of all monomer components constituting the acrylic polymer. In addition, it is preferably 3 parts by weight or less, more preferably 1.5 parts by weight or less.
[0180] The adhesive layer of the present invention is not particularly limited, but may contain a high refractive index organic material. When the adhesive layer of the present invention contains a high refractive index organic material, it is satisfactory from the viewpoint of being able to obtain a high refractive index adhesive layer, being able to suppress interface reflection with the OLED display panel, and being able to increase the light collection rate of light from the OLED element. It should be noted that the high refractive index organic material can be used alone or in combination of two or more.
[0181] High refractive index organic material is an organic material (Organic material) with high refractive index (high refractive index). By using such high refractive index organic material and acrylic polymer in combination, it is possible to realize an adhesive that suitably takes into account refractive index and bonding properties (peel strength, flexibility, etc.) and / or optical properties (total light transmittance, haze value, etc.). The organic material used as high refractive index organic material can be a polymer or a non-polymer. In addition, it can have a polymerizable functional group or not.
[0182] The refractive index of the high refractive index organic material can be set to an appropriate range according to the relative relationship with the refractive index of the acrylic polymer, and is therefore not limited to a specific range. The refractive index of the high refractive index organic material is, for example, greater than 1.50, greater than 1.55 or greater than 1.57, and is preferably higher than the refractive index of the acrylic polymer. From the viewpoint of the high refractive index of the adhesive, it is advantageous for the refractive index of the high refractive index organic material to be greater than 1.58, preferably greater than 1.60, more preferably greater than 1.63, greater than 1.65, greater than 1.70, and greater than 1.75. According to the high refractive index organic material with a higher refractive index, the target refractive index can be achieved even with a smaller amount of the high refractive index organic material. This is preferred from the viewpoint of suppressing the reduction of the adhesive properties and the optical properties. The upper limit of the refractive index of the high refractive index organic material is not particularly limited. From the perspectives of compatibility in the adhesive, high refractive indexization and the ease of taking into account the flexibility of the adhesive, the upper limit of the refractive index of the high refractive index organic material is, for example, below 3.000, below 2.500, below 2.000, below 1.950, below 1.900, or below 1.850. In addition, the high refractive index organic material can also be used as a plasticizer that gives the flexibility of the adhesive layer.
[0183] The refractive index of the high refractive index organic material and the adhesive layer is measured using an Abbe refractometer at a wavelength of 589 nm and a temperature of 25° C. If a nominal value of the refractive index at 25° C. is provided by a manufacturer or the like, the nominal value may be used.
[0184] The refractive index n of high refractive index organic materials b Refractive index n of acrylic polymer a The difference, that is, n b -n a (hereinafter also referred to as "Δn A ”) is set to be greater than 0. Δn A For example, it may be 0.02 or more, 0.05 or more, 0.07 or more, 0.10 or more, 0.15 or more, 0.20 or more, or 0.25 or more. A In order to make it larger, the acrylic polymer and the high refractive index organic material are selected, and the refractive index improvement effect brought about by the use of the high refractive index organic material tends to be higher. In addition, from the perspective of compatibility of the high refractive index organic material in the adhesive layer, Δn A For example, it may be 0.70 or less, may be 0.60 or less, may be 0.50 or less, may be 0.40 or less, or may be 0.35 or less.
[0185] The refractive index n of high refractive index organic materials b The refractive index n of the adhesive layer containing the high refractive index organic material is T The difference, that is, n b -n T (hereinafter also referred to as "Δn B ”) can be set to be greater than 0. In some embodiments, Δn B For example, it may be 0.02 or more, 0.05 or more, 0.07 or more, 0.10 or more, 0.15 or more, 0.20 or more, or 0.25 or more. B In some embodiments, the composition of the adhesive layer and the high refractive index organic material are selected, and the refractive index improvement effect brought about by the use of the high refractive index organic material tends to be higher. In addition, from the perspective of compatibility within the adhesive layer, transparency of the adhesive layer, etc., in some embodiments, Δn B For example, it may be 0.70 or less, may be 0.60 or less, may be 0.50 or less, may be 0.40 or less, or may be 0.35 or less.
[0186] The molecular weight of the organic material used as the high refractive index organic material is not particularly limited and can be selected according to the purpose. From the viewpoint of balanced consideration of the effect of high refractive index and other characteristics (for example, optical characteristics such as flexibility and haze suitable for adhesives), it is appropriate that the molecular weight of the high refractive index organic material is approximately less than 10000, preferably less than 5000, more preferably less than 3000 (for example, less than 1000), can be less than 800, can be less than 600, can be less than 500, can be less than 400. From the viewpoint of improving the compatibility in the adhesive layer, the molecular weight of the high refractive index organic material is not too large and can become advantageous. In addition, the molecular weight of the high refractive index organic material can be, for example, more than 130, or more than 150. From the viewpoint of the high refractive index of the high refractive index organic material, the molecular weight of the high refractive index organic material is preferably more than 170, more preferably more than 200, can be more than 230, can be more than 250, can be more than 270, can be more than 500, can be more than 1000, can be more than 2000. As the high refractive index organic material, a polymer having a molecular weight of about 1000 to about 10000 (eg, 1000 or more and less than 5000) can be used.
[0187] As the molecular weight of high refractive index organic material, for non-polymer or low polymerization degree (such as about 2 polymers to about 5 polymers), the molecular weight calculated based on the chemical structure or the measured value using matrix-assisted laser desorption ionization time-of-flight mass spectrometry (MALDI-TOF-MS) can be used. In the case where the high refractive index organic material is a higher polymer of polymerization degree, the weight average molecular weight (Mw) based on GPC carried out under appropriate conditions can be used. In the case where the nominal value of molecular weight is provided by manufacturers, the nominal value can be adopted.
[0188] Examples of organic materials that can be selected as the high refractive index organic material include organic compounds having an aromatic ring, organic compounds having a heterocyclic ring (which may be an aromatic ring or a non-aromatic heterocyclic ring), etc., but are not limited to these substances.
[0189] The aromatic ring contained in the organic compound having an aromatic ring (hereinafter also referred to as "aromatic ring-containing compound") used as the high refractive index organic material can be selected from the same aromatic rings as those contained in the compound used as the aromatic ring-containing monomer.
[0190] The above aromatic ring may have one or more substituents on the ring-constituting atoms, or may not have substituents. In the case of having substituents, examples of the substituents include alkyl, alkoxy, aryloxy, hydroxyl, halogen atoms (fluorine atoms, chlorine atoms, bromine atoms, etc.), hydroxyalkyl, hydroxyalkoxy, glycidoxy, etc., but are not limited to these groups. In the substituent containing carbon atoms, the number of carbon atoms contained in the substituent is, for example, 1 to 10, advantageously 1 to 6, preferably 1 to 4, more preferably 1 to 3, for example, 1 or 2. The above aromatic ring may be an aromatic ring that has no substituents on the ring-constituting atoms, or has one or more substituents selected from alkyl, alkoxy and halogen atoms (for example, bromine atoms).
[0191] Examples of aromatic ring-containing compounds that can be used as high refractive index organic materials include: compounds that can be used as aromatic ring-containing monomers; oligomers containing compounds that can be used as aromatic ring-containing monomers as monomer units; compounds having a structure in which a group having an ethylenically unsaturated group (a substituent bonded to a ring-constituting atom) or a portion of the group that constitutes an ethylenically unsaturated group is removed from a compound that can be used as an aromatic ring-containing monomer and replaced with a hydrogen atom or a group that does not have an ethylenically unsaturated group (e.g., a hydroxyl group, an amino group, a halogen atom, an alkyl group, an alkoxy group, a hydroxyalkyl group, a hydroxyalkoxy group, a glycidoxy group, etc.), etc., but are not limited to these. Non-limiting specific examples of aromatic ring-containing compounds that can be used as high refractive index organic materials include: benzyl acrylate, m-phenoxybenzyl acrylate, 2-(o-phenylphenoxy)ethyl acrylate, phenoxyethyl acrylate, phenoxydiethylene glycol acrylate, phenoxypolyethylene glycol acrylate, 2-hydroxy-3-phenoxypropyl acrylate, the above-mentioned monomers having a fluorene structure, monomers having a dinaphthothiophene structure, monomers having a dibenzothiophene structure, and other aromatic ring-containing monomers; 3-phenoxybenzyl alcohol, dinaphthothiophene and its derivatives (for example, compounds having a structure in which one or two or more substituents selected from hydroxyl, carbinol, diethanol, glycidyl, etc. are bonded to the dinaphthothiophene ring) and other aromatic ring-containing compounds that do not have an ethylenically unsaturated group, etc. In addition, the aromatic ring-containing compound may be an oligomer (preferably an oligomer having a molecular weight of about 5000 or less, more preferably about 1000 or less, such as an oligomer of about dimers to about pentamers) containing such an aromatic ring-containing monomer as a monomer unit. The oligomer may be, for example, a homopolymer of an aromatic ring-containing monomer, a copolymer of one or more aromatic ring-containing monomers, a copolymer of one or more aromatic ring-containing monomers and other monomers, etc. As the other monomers, one or more monomers without an aromatic ring may be used.
[0192] In some embodiments, as a high refractive index organic material, from the viewpoint of easily obtaining a high refractive index effect, an organic compound having two or more aromatic rings in one molecule (hereinafter also referred to as a "compound containing multiple aromatic rings") can be preferably used. The compound containing multiple aromatic rings may or may not have a polymerizable functional group such as an ethylenically unsaturated group. In addition, the compound containing multiple aromatic rings may be a polymer or a non-polymer. In addition, the above-mentioned polymer may be an oligomer (preferably an oligomer having a molecular weight of about 5000 or less, more preferably about 1000 or less, such as an oligomer of about 2 to about 5 polymers) containing a monomer containing multiple aromatic rings as a monomer unit. The above-mentioned oligomer may be, for example: a homopolymer of a monomer containing multiple aromatic rings; a copolymer of one or more monomers containing multiple aromatic rings; a copolymer of one or more monomers containing multiple aromatic rings and other monomers, etc. The above-mentioned other monomers may be an aromatic ring-containing monomer that does not belong to the monomer containing multiple aromatic rings, or a monomer without an aromatic ring, or a combination thereof.
[0193] As non-limiting examples of compounds containing multiple aromatic rings, there can be cited compounds having a structure in which two or more non-condensed aromatic rings are bonded via a linking group, compounds having a structure in which two or more non-condensed aromatic rings are directly (i.e., not via other atoms) chemically bonded, compounds having a condensed aromatic ring structure, compounds having a fluorene structure, compounds having a dinaphthothiophene structure, compounds having a dibenzothiophene structure, etc. Compounds containing multiple aromatic rings can be used alone or in combination of two or more.
[0194] Specific examples of the above-mentioned compounds having a fluorene structure include, in addition to the above-mentioned monomers having a fluorene structure and oligomers as homopolymers or copolymers of the monomers, 9,9-bis(4-hydroxyphenyl)fluorene (refractive index: 1.68), 9,9-bis(4-aminophenyl)fluorene (refractive index: 1.73), 9,9-bis(4-hydroxy-3-methylphenyl)fluorene (refractive index: 1.68), 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene (refractive index: 1.65), and 9,9-bisphenylfluorene and its derivatives.
[0195] Specific examples of the above-mentioned compounds having a dinaphthothiophene structure include, in addition to the above-mentioned monomers having a dinaphthothiophene structure and oligomers as homopolymers or copolymers of the monomers, dinaphthothiophene (refractive index: 1.808); hydroxyalkyl dinaphthothiophenes such as 6-hydroxymethyl dinaphthothiophene (refractive index: 1.766); dihydroxy dinaphthothiophenes such as 2,12-dihydroxy dinaphthothiophene (refractive index: 1.750); dihydroxyalkoxy dinaphthothiophenes such as 2,12-dihydroxyethoxy dinaphthothiophene (refractive index: 1.677); diglycidoxy dinaphthothiophenes such as 2,12-dielyloxy dinaphthothiophene (refractive index 1.723); dinaphthothiophenes having two or more ethylenically unsaturated groups such as 2,12-diallyloxy dinaphthothiophene (abbreviation: 2,12-DAODNT, refractive index 1.729) and the like and their derivatives.
[0196] As specific examples of the above-mentioned compounds having a dibenzothiophene structure, in addition to the above-mentioned monomers having a dibenzothiophene structure and oligomers as homopolymers or copolymers of the monomers, dibenzothiophene (refractive index: 1.607), 4-dimethyldibenzothiophene (refractive index: 1.617), 4,6-dimethyldibenzothiophene (refractive index: 1.617), etc. can also be listed.
[0197] Examples of organic compounds having heterocyclic rings (hereinafter also referred to as heterocyclic organic compounds) that can be selected as high refractive index organic materials include thioepoxide compounds, compounds having triazine rings, and the like. Examples of thioepoxide compounds include bis(2,3-epithiopropyl)disulfide and its polymer (refractive index 1.74) described in Japanese Patent Gazette No. 3712653. Examples of compounds having triazine rings include compounds having at least one (e.g., 3 to 40, preferably 5 to 20) triazine rings in one molecule. It should be noted that the triazine ring has aromaticity, and therefore compounds having a triazine ring are also included in the concept of the above-mentioned aromatic ring-containing compounds. In addition, compounds having multiple triazine rings are also included in the concept of the above-mentioned compounds containing multiple aromatic rings.
[0198] As the high refractive index organic material, a compound without ethylenically unsaturated groups can be preferably used. Thus, the deterioration of the adhesive composition caused by heat and light (the reduction of leveling caused by the progress of gelation and the increase of viscosity) can be suppressed, thereby improving storage stability. It is also preferred to use a high refractive index organic material without ethylenically unsaturated groups from the viewpoint of suppressing the dimensional change, deformation (warping, undulation, etc.), generation of optical distortion, etc. caused by the reaction of ethylenically unsaturated groups in an adhesive film having an adhesive layer containing the high refractive index organic material, a laminate containing the adhesive film, etc.
[0199] In the method of using oligomer as high refractive index organic material, the oligomer can be obtained by polymerizing the corresponding monomer components using a known method. In the case of manufacturing the above-mentioned oligomer by free radical polymerization, the polymerization initiator, chain transfer agent, emulsifier, etc. used in the free radical polymerization can be appropriately added to the above-mentioned monomer components for polymerization. The polymerization initiator, chain transfer agent, emulsifier, etc. used in the above-mentioned free radical polymerization are not particularly limited and can be appropriately selected for use. It should be noted that the weight average molecular weight of the oligomer can be controlled by the amount of the polymerization initiator and chain transfer agent used and the reaction conditions, and its amount can be appropriately adjusted according to their types.
[0200] As the chain transfer agent, for example, lauryl mercaptan, glycidyl mercaptan, thioglycolic acid, 2-mercaptoethanol, α-thioglycerol, thioglycolic acid, 2-ethylhexyl thioglycolate and 2,3-dimercapto-1-propanol can be listed. The chain transfer agent can be used alone or in combination of two or more. The amount of the chain transfer agent used can be set according to the composition of the monomer components used in the synthesis of the oligomer, the type of the chain transfer agent, etc., in order to obtain the desired weight average molecular weight of the oligomer. In some embodiments, it is appropriate to set the amount of the chain transfer agent to about 15 parts by weight or less relative to 100 parts by weight of the total amount of the monomers used in the synthesis of the oligomer, which can be 10 parts by weight or less, or about 5 parts by weight or less. The lower limit of the amount of the chain transfer agent used is not particularly limited relative to 100 parts by weight of the total amount of the monomers used in the synthesis of the oligomer, for example, it can be 0.01 parts by weight or more, 0.1 parts by weight or more, 0.5 parts by weight or more, or 1 part by weight or more.
[0201] Relative to 100 parts by weight of acrylic polymer, the usage amount of high refractive index organic material (their total amount when using multiple compounds) is not particularly limited as long as it is greater than 0 parts by weight, and can be set according to the purpose. Relative to 100 parts by weight of acrylic polymer, the usage amount of high refractive index organic material can be set to below 80 parts by weight, for example, from the viewpoint of balanced consideration of the high refractive index of adhesive and the reduction of suppression of bonding characteristics and optical characteristics, it is advantageous to be below 60 parts by weight, preferably below 45 parts by weight. From the viewpoint of more emphasis on bonding characteristics and optical characteristics, relative to 100 parts by weight of acrylic polymer, the usage amount of high refractive index organic material can be, for example, below 30 parts by weight, can be below 20 parts by weight, can be below 15 parts by weight, can also be below 10 parts by weight. In addition, from the viewpoint of high refractive index of adhesive, relative to 100 parts by weight of acrylic polymer, the usage amount of high refractive index organic material can be, for example, above 1 part by weight, is advantageous to be above 3 parts by weight, is preferably above 5 parts by weight, can be above 7 parts by weight, can be above 10 parts by weight, can be above 15 parts by weight, can be above 20 parts by weight.
[0202] The adhesive layer of the present invention is not particularly limited, but preferably contains an ultraviolet absorber (UVA). When the adhesive layer of the present invention contains an ultraviolet absorber, it is possible to suppress the degradation of the OLED element caused by ultraviolet rays contained in the external light, and an OLED display device with excellent weather resistance can be obtained even without using a polarizing plate. In addition, it is possible to suppress the degradation of the above-mentioned high refractive index component caused by ultraviolet rays and maintain a high light-collecting rate. It should be noted that the ultraviolet absorber can be used alone or in combination of two or more.
[0203] The ultraviolet absorber is not particularly limited, and examples thereof include benzotriazole ultraviolet absorbers, hydroxyphenyltriazine ultraviolet absorbers, benzophenone ultraviolet absorbers, salicylate ultraviolet absorbers, cyanoacrylate ultraviolet absorbers, and hydroxybenzophenone ultraviolet absorbers.
[0204] Examples of the benzotriazole ultraviolet absorber (benzotriazole-based compound) include 2-(2-hydroxy-5-tert-butylphenyl)-2H-benzotriazole (trade name "TINUVIN PS", manufactured by BASF), an ester compound of phenylpropionic acid and 3-(2H-benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxy (C7-9 side chain and linear alkyl) (trade name "TINUVIN384-2", manufactured by BASF), a mixture of octyl 3-[3-tert-butyl-4-hydroxy-5-(5-chloro-2H-benzotriazol-2-yl)phenyl]propionate and 2-ethylhexyl 3-[3-tert-butyl-4-hydroxy-5-(5-chloro-2H-benzotriazol-2-yl)phenyl]propionate (trade name "TINUVIN109", manufactured by BASF), 2-(2H-benzotriazol-2-yl)- 4,6-bis(1-methyl-1-phenylethyl)phenol (trade name "TINUVIN900", manufactured by BASF), 2-(2H-benzotriazol-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol (trade name "TINUVIN928", manufactured by BASF), 3-(3-(2H-benzotriazol-2-yl)-5-tert-butyl-4-hydroxyphenyl)propionic acid methyl ester / polyethylene glycol 300 reaction product (trade name "TINUVIN1130", manufactured by BASF), 2-(2H-benzotriazol-2-yl)-p-cresol (trade name "TINUVIN P", manufactured by BASF), 2-(2H-benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol (trade name "TINUVIN234", manufactured by BASF), 2-[5-chloro-2H-benzotriazol-2-yl]-4-methyl-6-(tert-butyl)phenol (trade name "TINUVIN326", manufactured by BASF), 2-(2H-benzotriazol-2-yl)-4,6-di-tert-amylphenol (trade name "TINUVIN328", manufactured by BASF), 2-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol (trade name "TINUVIN IN329", manufactured by BASF), 2,2'-methylenebis[6-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol] (trade name "TINUVIN360", manufactured by BASF), reaction product of methyl 3-(3-(2H-benzotriazol-2-yl)-5-tert-butyl-4-hydroxyphenyl)propionate and polyethylene glycol 300 (trade name "TINUVIN213", manufactured by BASF), 2-(2H-benzotriazol-2-yl)-6-dodecyl-4-methylphenol (trade name "TINUVIN571", manufactured by BASF), 2-[2-hydroxy-3-(3,4,5,6-tetrahydrophthalimidomethyl)-5-methylphenyl]benzotriazole (trade name "Sumisorb 250", manufactured by Sumitomo Chemical Co., Ltd.), 2,2'-methylenebis[6-(2H-benzotriazol-2-yl)-4-tert-octylphenol] (trade name "ADK STAB LA-31", manufactured by ADEKA Corporation), etc.
[0205] Examples of the hydroxyphenyltriazine ultraviolet absorber (hydroxyphenyltriazine compound) include a reaction product of 2-(4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine-2-yl)-5-hydroxyphenyl and [(C10-C16 (mainly C12-C13) alkoxy)methyl]ethylene oxide (trade name "TINUVIN 400", manufactured by BASF), 2-[4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine-2-yl]-[3-(dodecyloxy)-2-hydroxypropoxy]phenol), a reaction product of 2-(2,4-dihydroxyphenyl)-4,6-bis-(2,4-dimethylphenyl)-1,3,5-triazine and glycidic acid (2-ethylhexyl) ester (trade name "TINUVIN 405", manufactured by BASF), 2,4 -bis(2-hydroxy-4-butoxyphenyl)-6-(2,4-dibutoxyphenyl)-1,3,5-triazine (trade name "TINUVIN 460", manufactured by BASF), 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-[(hexyl)oxy]-phenol (trade name "TINUVIN 1577", manufactured by BASF), 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-[2-(2-ethylhexanoyloxy)ethoxy]-phenol (trade name "ADKSTABLA-46", manufactured by ADEKA Corporation), 2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine (trade name "TINUVIN 479", manufactured by BASF), etc. In addition, a compound represented by the following formula (5) (trade name "TINUVIN 477", manufactured by BASF Corporation) can be mentioned.
[0206]
[0207] Examples of the benzophenone-based ultraviolet absorbers (benzophenone-based compounds) and hydroxybenzophenone-based ultraviolet absorbers (hydroxybenzophenone-based compounds) include 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxybenzophenone-5-sulfonic acid (anhydride and trihydrate salt), 2-hydroxy-4-octyloxybenzophenone, 4-dodecyloxy-2-hydroxybenzophenone, 4-benzyloxy-2-hydroxybenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone (trade name "KEMISORB111", manufactured by Chemipro Chemicals Co., Ltd.), 2,2',4,4'-tetrahydroxybenzophenone (trade name "SEESORB106", manufactured by Shipro Chemicals Co., Ltd.), and 2,2'-dihydroxy-4,4'-dimethoxybenzophenone.
[0208] Examples of the salicylate ultraviolet absorber (salicylate compound) include phenyl 2-acryloxybenzoate, phenyl 2-acryloxy-3-methylbenzoate, phenyl 2-acryloxy-4-methylbenzoate, phenyl 2-acryloxy-5-methylbenzoate, phenyl 2-acryloxy-3-methoxybenzoate, phenyl 2-hydroxybenzoate, phenyl 2-hydroxy-3-methylbenzoate, phenyl 2-hydroxy-4-methylbenzoate, phenyl 2-hydroxy-5-methylbenzoate, phenyl 2-hydroxy-3-methoxybenzoate, phenyl 2-hydroxybenzoate, phenyl 2-hydroxy-3-methylbenzoate, phenyl 2-hydroxy-4-methylbenzoate, phenyl 2-hydroxy-5-methylbenzoate, phenyl 2-hydroxy-3-methoxybenzoate, and phenyl 2,4-di-tert-butylphenyl 3,5-di-tert-butyl-4-hydroxybenzoate (trade name "TINUVIN 120", manufactured by BASF).
[0209] Examples of the cyanoacrylate ultraviolet absorber (cyanoacrylate compound) include 2-cyanoacrylate alkyl esters, 2-cyanoacrylate cycloalkyl esters, 2-cyanoacrylate alkoxyalkyl esters, 2-cyanoacrylate alkenyl esters, and 2-cyanoacrylate alkynyl esters.
[0210] As the above-mentioned ultraviolet absorber, from the viewpoint of having high ultraviolet absorbency, having excellent optical properties, the viewpoint of easy availability of a highly transparent adhesive layer, and having excellent light stability, it is preferred to select at least one ultraviolet absorber from the group consisting of benzotriazole ultraviolet absorbers, benzophenone ultraviolet absorbers, and hydroxyphenyltriazine ultraviolet absorbers, and more preferably benzotriazole ultraviolet absorbers and benzophenone ultraviolet absorbers. It is particularly preferred that a benzotriazole ultraviolet absorber having a group having 6 or more carbon atoms and a phenyl group as a substituent is bonded to a nitrogen atom constituting a benzotriazole ring. In addition, from the viewpoint of preventing the reduction of the appearance caused by the precipitation of the ultraviolet absorber, it is preferred to use a liquid ultraviolet absorber or two or more ultraviolet absorbers.
[0211] In addition, from the viewpoint of obtaining higher ultraviolet absorbency, the absorbance A of the ultraviolet absorber determined below is preferably 0.5 or less.
[0212] Absorbance A: Absorbance measured by irradiating a 0.08% toluene solution of the above-mentioned ultraviolet absorber with light of wavelength 400nm
[0213] In the case where the adhesive layer of the present invention contains an ultraviolet absorber, the content of the ultraviolet absorber in the adhesive layer of the present invention (especially the acrylic adhesive layer) is not particularly limited. From the perspective of suppressing the degradation of the OLED element caused by ultraviolet rays contained in external light and obtaining an OLED display device with excellent weather resistance even without using a polarizing plate, the content of the ultraviolet absorber is preferably 0.01 parts by weight or more, more preferably 0.05 parts by weight or more, and further preferably 0.1 parts by weight or more relative to 100 parts by weight of the acrylic polymer. In addition, from the perspective of suppressing the occurrence of yellowing of the adhesive accompanied by the addition of the ultraviolet absorber and obtaining excellent optical properties, high transparency and excellent appearance characteristics, the upper limit of the content of the ultraviolet absorber is preferably 20 parts by weight or less, more preferably 10 parts by weight or less, and further preferably 8 parts by weight or less relative to 100 parts by weight of the acrylic polymer.
[0214] A pigment compound having a maximum absorption wavelength in the wavelength range of 380nm to 430nm may be contained to replace the above-mentioned ultraviolet absorber, or a pigment compound having a maximum absorption wavelength in the wavelength range of 380nm to 430nm may be used together with the above-mentioned ultraviolet absorber. The pigment compound can suppress the degradation of the OLED element and the degradation of the high refractive index component caused by ultraviolet light.
[0215] The above-mentioned pigment compound can be used alone or in a mixture of two or more. When only the above-mentioned pigment compound is used, the content of the above-mentioned pigment compound as a whole is preferably 0.1 to 20 parts by weight, preferably 0.1 to 10 parts by weight, preferably 0.1 to 5 parts by weight, and more preferably 0.5 to 3 parts by weight, relative to 100 parts by weight of the base polymer (e.g., acrylic polymer). By making the addition amount of the pigment compound within the above-mentioned range, the light in the region that does not affect the light emission of the OLED element can be fully absorbed, and by using the adhesive layer formed by the adhesive composition, the degradation of the OLED element and the degradation of the high refractive index component can be suppressed, so it is satisfactory.
[0216] Any of the above-mentioned ultraviolet absorbers and pigment compounds can be used, and it is preferred to use the above-mentioned ultraviolet absorbers and pigment compounds in combination. Although the ultraviolet absorber can absorb light of a wavelength of 380nm, the light of the wavelength region (380nm to 430nm) on the wavelength side shorter than the luminous region of the OLED element (the wavelength side longer than 430nm) is not fully absorbed, and sometimes deterioration occurs due to the transmitted light. The above-mentioned pigment compound can inhibit the transmission of the light of the wavelength (380nm to 430nm) on the wavelength side shorter than the luminous region of the OLED element (the wavelength side longer than 430nm), and by using the above-mentioned ultraviolet absorber and pigment compound in combination, the transmittance of visible light in the luminous region of the above-mentioned OLED element can be fully ensured.
[0217] In the present invention, by using such a pigment compound and the above-mentioned ultraviolet absorber in combination, the light in the region (wavelength 380nm to 430nm) that does not affect the luminescence of the OLED element can be fully absorbed, and the luminescent region (wavelength side longer than 430nm) of the OLED element can be fully transmitted, and as a result, the degradation of the OLED element caused by external light and the degradation of the high refractive index component can be suppressed at the same time. In the case of using the ultraviolet absorber and the pigment compound in combination, the ultraviolet absorber is preferably 0.1 to 10 parts by weight, preferably 0.1 to 5 parts by weight, and more preferably 0.5 to 3 parts by weight relative to 100 parts by weight of the base polymer (e.g., acrylic polymer). The above-mentioned pigment compound is preferably about 0.1 to about 10 parts by weight, more preferably about 0.1 to about 5 parts by weight, and more preferably 0.5 to 3 parts by weight relative to 100 parts by weight of the base polymer (e.g., acrylic polymer).
[0218] Pigment compound is not particularly limited as long as the maximum absorption wavelength of absorption spectrum is present in the compound of the wavelength region of 380nm~430nm.It should be noted that the maximum absorption wavelength refers to the absorption maximum wavelength of the maximum absorbance when there are multiple absorption maxima in the spectral absorption spectrum of the wavelength region of 300nm~460nm.
[0219] The maximum absorption wavelength of the absorption spectrum of the pigment compound is more preferably present in the wavelength region of 380 nm to 420 nm. In addition, the pigment compound is not particularly limited as long as it has the above wavelength characteristics, and preferably a material having no fluorescence or phosphorescence properties (photoluminescence) that does not hinder the display of the OLED element.
[0220] Examples of the organic pigment compound include azomethine compounds, indole compounds, cinnamic acid compounds, pyrimidine compounds, porphyrin compounds, and cyanine compounds.
[0221] As the organic pigment compound, commercially available organic pigment compounds can be preferably used. Specifically, as the indole compound, BONASORB Examples of the cinnamic acid compound include SOM-5-0106 (trade name, maximum absorption wavelength in absorption spectrum: 416 nm, manufactured by Orient Chemical Industry Co., Ltd.), and examples of the porphyrin compound include FDB-001 (trade name, maximum absorption wavelength in absorption spectrum: 420 nm, manufactured by Yamada Chemical Industry Co., Ltd.). Examples of the cyanine compound include a merocyanine compound (trade name: FDB-009, maximum absorption wavelength in absorption spectrum: 394 nm, manufactured by Yamada Chemical Industry Co., Ltd.) and a polymethine compound (trade name: DAA-247, maximum absorption wavelength in absorption spectrum: 389 nm, manufactured by Yamada Chemical Industry Co., Ltd.). Among them, the above-mentioned cyanine compounds are preferred from the viewpoint of suppression of crosslinking hindrance and optical reliability, and the polymethine compound is particularly preferred.
[0222] The adhesive layer of the present invention may contain a light stabilizer. When the adhesive layer of the present invention contains a light stabilizer, it is particularly preferred to contain the light stabilizer together with the above-mentioned ultraviolet absorber. The light stabilizer can capture free radicals generated by photooxidation, thereby improving the tolerance of the adhesive layer to light (especially ultraviolet rays). It should be noted that the light stabilizer can be used alone or in combination of two or more.
[0223] The above-mentioned light stabilizer is not particularly limited, and examples thereof include phenolic light stabilizers (phenolic compounds), phosphorus-containing light stabilizers (phosphorus-containing compounds), thioether light stabilizers (thioether compounds), amine light stabilizers (amine compounds) (especially hindered amine stabilizers (hindered amine compounds)), etc.
[0224] Examples of the phenolic light stabilizer (phenolic compound) include 2,6-di-tert-butyl-4-methylphenol, 4-hydroxymethyl-2,6-di-tert-butylphenol, 2,6-di-tert-butyl-4-ethylphenol, butylated hydroxyanisole, 3-(4-hydroxy-3,5-di-tert-butylphenyl) propionate, (4-hydroxy-3-methyl-5-tert-butyl) benzylmalonate distearyl ester, tocopherol, 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 2,2'-methylenebis(4-ethyl-6-tert-butylphenol), 4,4'-methylenebis(2,6-di-tert-butylphenol), 4,4'-butylenebis(6-tert-butyl-m-cresol), 4,4'-thiobis(6-tert-butyl-m-cresol), styrenated phenol, N,N'-hexamethylenebis(3,5-di-tert-butyl-4-hydroxyhydrocinnamic acid), bis(3, 5-di-tert-butyl-4-hydroxybenzylphosphonic acid ethyl ester) calcium, 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyloxymethyl]methane, 1,6-hexanediol-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 2,2'-methylenebis(4-methyl-6-cyclohexylphenol), 2,2'-methylenebis[ 6-(1-methylcyclohexyl)-p-cresol], 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)isocyanuric acid, 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanuric acid, triethylene glycol-bis[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate], 2,2'-oxalamidebis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 6-(4-hydroxy-3,5-di-tert-butylanilino)-2,4-dioctylthio-1,3,5 -triazine, bis[2-tert-butyl-4-methyl-6-(2-hydroxy-3-tert-butyl-5-methylbenzyl)phenyl]terephthalate, 3,9-bis{2-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl}-2,4,8,10-tetraoxaspiro[5.5]undecane, 3,9-bis{2-[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyloxy]-1,1-dimethylethyl}-2,4,8,10-tetraoxaspiro[5.5]undecane, and the like.
[0225] Examples of the phosphorus-containing light stabilizer (phosphorus-containing compound) include trisnonylphenyl phosphite, tris(2,4-di-tert-butylphenyl)phosphite, tris[2-tert-butyl-4-(3-tert-butyl-4-hydroxy-5-methylphenylthio)-5-methylphenyl]phosphite, tridecylphosphite, octyldiphenylphosphite, di(decyl)monophenylphosphite, di(tridecyl)pentaerythritol diphosphite, distearylpentaerythritol diphosphite, di(nonylphenyl)pentaerythritol diphosphite, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, bis(2, 4,6-tri-tert-butylphenyl) pentaerythritol diphosphite; tetra(tridecyl) isopropylidene diphenol diphosphite, tetra(tridecyl)-4,4'-n-butylene bis(2-tert-butyl-5-methylphenol) diphosphite, hexa(tridecyl)-1,1,3-tri(2-methyl-4-hydroxy-5-tert-butylphenyl) butane triphosphate, tetra(2,4-di-tert-butylphenyl) biphenylene diphosphite, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, tris(2-[(2,4,8,10-tetra-tert-butyldibenzo[d,f][1,3,2]dioxaphosphacycloheptane-6-yl)oxy]ethyl)amine, etc.
[0226] Examples of thioether light stabilizers (thioether compounds) include dialkyl thiodipropionate compounds such as dilauryl thiodipropionate, dimyristyl thiodipropionate, and distearyl thiodipropionate; and β-alkylmercaptopropionate compounds of polyhydric alcohols such as tetrakis[methylene(3-dodecylthio)propionate]methane.
[0227] Examples of the amine light stabilizer (amine compound) include a polymer of dimethyl succinate and 4-hydroxy-2,2,6,6-tetramethyl-1-piperidinol (trade name "TINUVIN 622", manufactured by BASF), a 1:1 reaction product of a polymer of dimethyl succinate and 4-hydroxy-2,2,6,6-tetramethyl-1-piperidinol and N,N',N",N"'-tetrakis-(4,6-bis-(butyl-(N-methyl-2,2,6,6-tetramethylpiperidin-4-yl)amino)-triazine-2-yl)-4,7-diazadecane-1,10-diamine (trade name "TINUVIN 119", manufactured by BASF), dibutylamine·1,3-triazine·N,N'-tetrakis-(4,6-bis-(butyl-(N-methyl-2,2,6,6-tetramethylpiperidin-4-yl)amino)-triazine-2-yl)-4,7-diazadecane-1,10-diamine. -condensation product of bis(2,2,6,6-tetramethyl-4-piperidinyl-1,6-hexamethylenediamine and N-(2,2,6,6-tetramethyl-4-piperidinyl)butylamine (trade name "TINUVIN 2020", manufactured by BASF), poly[{6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{2,2,6,6-tetramethyl-4-piperidinyl}imino]hexamethylene{(2,2,6,6-tetramethyl-4-piperidinyl)imino} (trade name "TINUVIN 944", manufactured by BASF), bis(1,2,2,6,6-pentamethyl-4-piperidinyl) sebacate and methyl 1,2,6,6-pentamethyl-4-piperidinyl) sebacate -piperidinyl ester mixture (trade name "TINUVIN765", manufactured by BASF), bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate (trade name "TINUVIN770", manufactured by BASF), bis(2,2,6,6-tetramethyl-1-(octyloxy)-4-piperidinyl) sebacate, reaction product of 1,1-dimethylethyl hydroperoxide and octane (trade name "TINUVIN123", manufactured by BASF), bis(1,2,2,6,6-pentamethyl-4-piperidinyl)[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]butylmalonate (trade name "TINUVIN144", manufactured by BASF) ), the reaction product of cyclohexane and N-butyl peroxide 2,2,6,6-tetramethyl-4-piperidinamine-2,4,6-trichloro-1,3,5-triazine and 2-aminoethanol (trade name "TINUVIN152", manufactured by BASF), a mixture of bis(1,2,2,6,6-pentamethyl-4-piperidinyl) sebacate and methyl sebacate 1,2,2,6,6-pentamethyl-4-piperidinyl ester (trade name "TINUVIN292", manufactured by BASF), 1,2,3,4-butanetetracarboxylic acid with 1,2,2,6,6-pentamethyl-4-piperidinol and 3,9-bis(2-hydroxy-1,1-dimethylethyl)-2,4,8,10-tetraoxaspiro[5.5] Undecane mixed ester (trade name "Adekastab LA-63P", manufactured by ADEKA Corporation), etc. As the amine stabilizer, hindered amine stabilizers are particularly preferred.
[0228] When the adhesive layer of the present invention contains a light stabilizer, the content of the light stabilizer in the adhesive layer of the present invention (especially the acrylic adhesive layer) is not particularly limited. From the viewpoint of easily exhibiting light resistance, the content of the light stabilizer in the adhesive layer of the present invention (especially the acrylic adhesive layer) is preferably 0.1 parts by weight or more, and more preferably 0.2 parts by weight or more, relative to 100 parts by weight of the acrylic polymer. In addition, from the viewpoint of not easily causing coloring caused by the light stabilizer itself, easily obtaining high transparency, and from the viewpoint of optical properties, the upper limit of the above content is preferably 5 parts by weight or less, and more preferably 3 parts by weight or less, relative to 100 parts by weight of the acrylic polymer.
[0229] The formation of the adhesive layer of the present invention is not particularly limited, and a crosslinking agent may be used. For example, the acrylic polymer in the acrylic adhesive layer may be crosslinked to control the gel fraction. It should be noted that the crosslinking agent may be used alone or in combination of two or more.
[0230] The crosslinking agent is not particularly limited, and examples thereof include isocyanate crosslinking agents, epoxy crosslinking agents, melamine crosslinking agents, peroxide crosslinking agents, urea crosslinking agents, metal alkoxide crosslinking agents, metal chelate crosslinking agents, metal salt crosslinking agents, carbodiimide crosslinking agents, Oxazoline crosslinking agents, aziridine crosslinking agents, amine crosslinking agents, etc. Among them, isocyanate crosslinking agents and epoxy crosslinking agents are preferred, and isocyanate crosslinking agents are more preferred.
[0231] Examples of the isocyanate crosslinking agent (polyfunctional isocyanate compound) include lower aliphatic polyisocyanates such as 1,2-ethylene diisocyanate, 1,4-butylene diisocyanate, and 1,6-hexamethylene diisocyanate; alicyclic polyisocyanates such as cyclopentylene diisocyanate, cyclohexylene diisocyanate, isophorone diisocyanate, hydrogenated toluene diisocyanate, and hydrogenated xylene diisocyanate; and aromatic polyisocyanates such as 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 4,4′-diphenylmethane diisocyanate, and xylylene diisocyanate. In addition, examples of the isocyanate crosslinking agent include commercially available products such as trimethylolpropane / toluene diisocyanate adduct (trade name "CORONATE L", manufactured by Tosoh Corporation), trimethylolpropane / hexamethylene diisocyanate adduct (trade name "CORONATE HL", manufactured by Tosoh Corporation), and trimethylolpropane / xylylene diisocyanate adduct (trade name "TAKENATE D-110N", manufactured by Mitsui Chemicals, Inc.).
[0232] Examples of the epoxy crosslinking agent (polyfunctional epoxy compound) include N,N,N',N'-tetraglycidyl-m-xylylenediamine, diglycidyl aniline, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, 1,6-hexanediol diglycidyl ether, neopentyl glycol diglycidyl ether, ethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, sorbitol polyol, Examples of the epoxy crosslinking agent include glycidyl ether, glycerol polyglycidyl ether, pentaerythritol polyglycidyl ether, polyglycerol polyglycidyl ether, sorbitan polyglycidyl ether, trimethylolpropane polyglycidyl ether, diglycidyl adipate, diglycidyl phthalate, tris(2-hydroxyethyl)isocyanurate triglycidyl ether, resorcinol diglycidyl ether, bisphenol-S-diglycidyl ether, and epoxy resins having two or more epoxy groups in the molecule. Examples of the epoxy crosslinking agent include commercial products such as "TETRAD C" (manufactured by Mitsubishi Gas Chemical Co., Ltd.).
[0233] When a cross-linking agent is used in the formation of the adhesive layer of the present invention, the amount of the cross-linking agent used is not particularly limited. From the viewpoint of obtaining sufficient adhesive reliability, it is preferably 0.001 parts by weight or more, and more preferably 0.01 parts by weight or more, relative to 100 parts by weight of the base polymer. In addition, from the viewpoint of obtaining appropriate flexibility and improving the adhesive strength of the adhesive layer, the upper limit of the amount used is preferably 10 parts by weight or less, and more preferably 5 parts by weight or less, relative to 100 parts by weight of the base polymer.
[0234] From the viewpoint of improving the adhesive reliability under humidification conditions, especially the viewpoint of improving the adhesive reliability to glass, the adhesive layer (especially the acrylic adhesive layer) of the present invention may contain a silane coupling agent. It should be noted that the silane coupling agent may be used alone or in combination of two or more. When the above-mentioned adhesive layer contains a silane coupling agent, it is possible to improve the adhesiveness under humidification conditions, especially the adhesiveness to glass.
[0235] The silane coupling agent is not particularly limited, and examples thereof include γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, γ-aminopropyltrimethoxysilane, N-phenyl-aminopropyltrimethoxysilane, etc. In addition, commercial products such as trade name "KBM-403" (manufactured by Shin-Etsu Chemical Co., Ltd.) can also be cited as silane coupling agents. Among them, γ-glycidoxypropyltrimethoxysilane is preferred as the silane coupling agent.
[0236] When the adhesive layer of the present invention contains a silane coupling agent, the content of the silane coupling agent in the adhesive layer of the present invention (particularly the acrylic adhesive layer) is not particularly limited, but is preferably 0.01 parts by weight or more, more preferably 0.02 parts by weight or more, relative to 100 parts by weight of the base polymer. In addition, the upper limit of the content of the silane coupling agent is preferably 10 parts by weight or less, more preferably 1 part by weight or less, relative to 100 parts by weight of the base polymer.
[0237] The adhesive layer of the present invention may further contain additives such as a crosslinking accelerator, a tackifying resin (rosin derivatives, polyterpene resins, petroleum resins, oil-soluble phenolic resins, etc.), an anti-aging agent, a filler, a colorant (pigment, dye, etc.), an antioxidant, a chain transfer agent, a plasticizer, a softener, a surfactant, an antistatic agent, etc., as required, within the range that does not impair the effects of the present invention. It should be noted that such additives may be used alone or in combination of two or more.
[0238] The method for preparing the adhesive layer (especially the acrylic adhesive layer) of the present invention is not particularly limited, and examples thereof include: applying (coating) the adhesive composition on a substrate (including a resin layer or a glass layer described later) or a release liner, and drying and curing the obtained adhesive composition layer; applying (coating) the adhesive composition on a substrate (including a resin layer or a glass layer described later) or a release liner, and curing the obtained adhesive composition layer by irradiating active energy rays. In addition, heating and drying may be further performed as required.
[0239] Examples of the active energy rays include ionizing radiation such as α rays, β rays, γ rays, neutron rays, electron beams, and ultraviolet rays, and ultraviolet rays are particularly preferred. The irradiation energy, irradiation time, and irradiation method of the active energy rays are not particularly limited.
[0240] The above-mentioned adhesive composition can be prepared by a known or customary method. For example, a solvent-based acrylic adhesive composition can be prepared by mixing an additive (such as a UV absorber, etc.) into a solution containing the above-mentioned acrylic polymer as required. For example, an active energy ray-curable acrylic adhesive composition can be prepared by mixing an additive (such as a UV absorber, etc.) into a mixture of the above-mentioned acrylic monomers or a partial polymer thereof as required.
[0241] It should be noted that the coating (application) of the above-mentioned adhesive composition can utilize a known coating method. For example, a coating machine such as a gravure roll coater, a reverse roll coater, a lick coater, a dip roll coater, a bar coater, a knife coater, a spray coater, a comma coater, a direct coater, etc. can be used.
[0242] In particular, when the adhesive layer is formed by an active energy ray-curable adhesive composition, the active energy ray-curable adhesive composition preferably contains a photopolymerization initiator. It should be noted that when the active energy ray-curable adhesive composition contains an ultraviolet absorber, as a photopolymerization initiator, it is preferred to contain at least a photopolymerization initiator having light absorption characteristics in a wide wavelength range. For example, it is preferred to contain at least a photopolymerization initiator having light absorption characteristics for visible light in addition to ultraviolet light. This is because: there is a concern that the curing caused by active energy rays is hindered by the action of the ultraviolet absorber, and when a photopolymerization initiator having light absorption characteristics in a wide wavelength range is contained, the adhesive composition is easy to obtain high photocurability.
[0243] (Adhesive layer)
[0244] The adhesive layer is a layer that can bond substances by being sandwiched between adherends. When the adherends attached with the adhesive layer are peeled off, the adhesive layer does not have practical adhesive strength.
[0245] As the adhesive forming the adhesive layer constituting the optical element of the present invention (hereinafter, sometimes referred to as "the adhesive layer of the present invention"), various adhesives can be applied, for example, isocyanate adhesives, polyvinyl alcohol adhesives, gelatin adhesives, vinyl latex, water-based polyesters, etc. These adhesives are usually used as adhesives containing aqueous solutions (water-based adhesives) and contain 0.5 wt % to 60 wt % of solid content. Among them, polyvinyl alcohol adhesives are preferred, and polyvinyl alcohol adhesives containing acetoacetyl groups are more preferred.
[0246] The water-based adhesive may contain a crosslinking agent. As the crosslinking agent, a compound having at least two functional groups reactive with the polymer or other components constituting the adhesive in one molecule is generally used, for example: alkylenediamines; isocyanates; epoxies; aldehydes; amino-formaldehydes such as methylol urea and methylol melamine, etc. The amount of the crosslinking agent in the adhesive is generally about 10 to 60 parts by weight relative to 100 parts by weight of the polymer or other components constituting the adhesive.
[0247] As the above-mentioned adhesive, in addition to the above-mentioned, active energy ray curing adhesives such as ultraviolet curing adhesives and electron beam curing adhesives can also be listed. As the above-mentioned active energy ray curing adhesive, for example, (meth)acrylate adhesives can be listed. As the curable component in the above-mentioned (meth)acrylate adhesive, for example, compounds having a (meth)acryloyl group and compounds having a vinyl group can be listed. (As compounds having a meth)acryloyl group, for example, (meth)acrylic acid alkyl esters such as (meth)acrylic acid chain alkyl esters, (meth)acrylic acid alicyclic alkyl esters, and (meth)acrylic acid polycyclic alkyl esters having 1 to 20 carbon atoms can be listed; (meth)acrylic acid esters containing hydroxyl groups; (meth)acrylic acid esters containing epoxy groups such as glycidyl (meth)acrylate. (Meth) acrylate adhesives may include nitrogen-containing monomers such as hydroxyethyl (meth) acrylamide, N-hydroxymethyl (meth) acrylamide, N-methoxymethyl (meth) acrylamide, N-ethoxymethyl (meth) acrylamide, (meth) acrylamide, (meth) acrylamide, (meth) acrylamide, and (meth) acryl morpholine. (Meth) acrylate adhesives may include polyfunctional monomers such as tripropylene glycol diacrylate, 1,9-nonanediol diacrylate, tricyclodecane dimethanol diacrylate, cyclic trimethylolpropane formal acrylate, dioxanediol diacrylate, and EO-modified diglycerol tetraacrylate as crosslinking components. In addition, as a cationic polymerization curing adhesive, compounds having epoxy groups and oxetane groups may also be used. The compound having an epoxy group is not particularly limited as long as it has at least two epoxy groups in the molecule, and various commonly known curable epoxy compounds may be used.
[0248] The adhesive may contain appropriate additives as required. Examples of the additives include coupling agents such as silane coupling agents and titanium coupling agents, adhesion promoters such as ethylene oxide, ultraviolet absorbers, anti-deterioration agents, dyes, processing aids, ion capture agents, antioxidants, tackifiers, fillers, plasticizers, leveling agents, foaming inhibitors, antistatic agents, heat stabilizers, hydrolysis stabilizers, and the like.
[0249] The coating of the above-mentioned adhesive can be performed on either one of the two adherends to be bonded, or on both. After lamination, a drying process can be implemented to form the adhesive layer of the present invention consisting of a coated dried layer. After the above-mentioned drying process, ultraviolet rays or electron beams can be irradiated as needed. The thickness of the adhesive layer of the present invention is not particularly limited. When using a water-based adhesive, etc., it is preferably about 30nm to about 5000nm, and more preferably about 100nm to about 1000nm. When using an ultraviolet curing adhesive, an electron beam curing adhesive, etc., it is preferably about 0.1 to about 100μm, and more preferably about 0.5 to about 10μm.
[0250] When the indentation elastic modulus of the adhesive layer of the present invention is set to Ea, the indentation elastic modulus Ea is preferably 1 GPa or more, more preferably 2 GPa or more, and further preferably 3 GPa or more. When the indentation elastic modulus Ea is 1 GPa or more, the impact resistance is further improved. The indentation elastic modulus Ea is, for example, 50 GPa or less, and can be 30 GPa or less, or 10 GPa or less.
[0251] The indentation elastic modulus Ea can be measured by a nanoindentation method. The nanoindentation method is measured under the conditions of a spherical indenter (curvature radius 10 μm), a temperature of 25° C., and an indentation depth of 100 nm.
[0252] (Resin layer)
[0253] The resin layer constituting the optical element of the present invention (hereinafter sometimes referred to as "resin layer of the present invention") is not particularly limited, and examples thereof include plastic films. Examples of raw materials for the plastic films include polyester resins such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), cyclic olefin polymers (COP) (e.g., trade name "ARTON" (manufactured by JSR (Strain)), trade name "ZEONOR" (manufactured by ZEON (Strain) in Japan), acrylic resins such as polymethyl methacrylate (PMMA), polycarbonate (PC), triacetyl cellulose (TAC), polysulfone, polyarylate, polyether ether ketone (PEEK), polyimide (PI), transparent poly Plastic materials such as polyimide (CPI), polyvinyl chloride, polyvinyl acetate, polyethylene, polypropylene, ethylene-propylene copolymer, etc., preferably polyester resins such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN) that are excellent in dimensional stability and not easy to shrink, cyclic olefin polymers (COP), polycarbonate (PC), polyetheretherketone (PEEK), transparent polyimide (CPI), more preferably polyethylene terephthalate (PET), transparent polyimide (CPI), and particularly preferably transparent polyimide (CPI) with excellent impact resistance. It should be noted that these plastic materials can be used alone or in combination of two or more. The release liner that is peeled off when the optical element of the present invention is used (when pasted) is not included in the "resin layer".
[0254] The resin layer of the present invention is preferably transparent. The total light transmittance of the resin layer of the present invention in the visible light wavelength region (based on JIS K7361-1) is not particularly limited, but is preferably 85% or more, and more preferably 88% or more. In addition, the haze of the resin layer of the present invention (based on JIS K7136) is not particularly limited, but is preferably 1.5% or less, and more preferably 1.0% or less.
[0255] The refractive index difference between the adhesive (adhesive layer from which light scattering particles are removed) and the resin layer in the present invention (absolute value of "refractive index of adhesive" - "refractive index of resin layer") is not particularly limited. From the viewpoint of improving the anti-reflectivity of the interface and being able to increase the light collection efficiency of the light from the OLED element, it is preferably less than 2, preferably less than 1, further preferably less than 0.5, and particularly preferably less than 0.3.
[0256] The thickness of the resin layer of the present invention is not particularly limited, and is preferably 10 μm to 80 μm, for example. It should be noted that the resin layer of the present invention may have any form of a single layer or a multilayer. In addition, the surface of the resin layer of the present invention may be appropriately subjected to a known and conventional surface treatment such as a physical treatment such as a corona discharge treatment or a plasma treatment, or a chemical treatment such as a primer treatment.
[0257] The resin layer of the present invention is not particularly limited, and preferably contains an ultraviolet absorber (UVA) and a pigment compound whose maximum absorption wavelength of the absorption spectrum exists in the wavelength region of 380nm to 430nm. When the resin layer of the present invention contains an ultraviolet absorber and the above-mentioned pigment compound, the degradation of the OLED element caused by the ultraviolet rays contained in the external light can be suppressed, and an OLED display device with excellent weather resistance can be obtained even without using a polarizing plate. In addition, the degradation of the high refractive index component of the adhesive layer caused by ultraviolet rays can be suppressed, and a high light-collecting rate can be maintained. In particular, by the resin layer of the present invention containing an ultraviolet absorber and the above-mentioned pigment compound, the content of the ultraviolet absorber and the above-mentioned pigment compound in the adhesive layer of the present invention can be reduced, and the precipitation and seepage of the ultraviolet absorber and the above-mentioned pigment compound in the adhesive layer of the present invention can be suppressed, which is satisfactory.
[0258] As the ultraviolet absorber (UVA) and the pigment compound contained in the resin layer of the present invention, the same ultraviolet absorber and the pigment compound as those contained in the adhesive layer of the present invention can be used. It should be noted that the ultraviolet absorber and the pigment compound can be used alone or in combination of two or more.
[0259] In the case where the resin layer of the present invention contains an ultraviolet absorber and the above-mentioned pigment compound, the content of each of the above-mentioned ultraviolet absorber and the above-mentioned pigment compound in the resin layer of the present invention is not particularly limited. From the perspective of suppressing the degradation of the OLED element caused by ultraviolet rays contained in the external light and obtaining an OLED display device with excellent weather resistance even without using a polarizing plate, the content of each of the above-mentioned ultraviolet absorber and the above-mentioned pigment compound in the resin layer is preferably 0.01 parts by weight or more, more preferably 0.05 parts by weight or more, and further preferably 0.1 parts by weight or more, relative to 100 parts by weight of the resin layer. In addition, from the perspective of suppressing the occurrence of yellowing of the adhesive accompanied by the addition of the ultraviolet absorber and obtaining excellent optical properties, high transparency and excellent appearance characteristics, the upper limit of the content of the above-mentioned ultraviolet absorber and the above-mentioned pigment compound is preferably 10 parts by weight or less, more preferably 9 parts by weight or less, and further preferably 8 parts by weight or less, relative to 100 parts by weight of the resin layer.
[0260] When both the resin layer and the adhesive layer of the present invention contain an ultraviolet absorber and the above-mentioned pigment compound, the total amount thereof may be adjusted to fall within the above-mentioned range.
[0261] The moisture permeability of the resin layer of the present invention is not particularly limited. For example, from the viewpoint of suppressing the separation and precipitation of additives such as the high refractive index organic material in the above-mentioned adhesive layer, it is preferably high to a certain extent (high moisture permeability), and more preferably 40 g / m 2·24 hours or more, more preferably 100g / m 2 ·24 hours or more, particularly preferably 200g / m 2 24 hours or more. The upper limit of the moisture permeability of the resin layer of the present invention is not particularly limited, but from the viewpoint of suppressing humidification expansion, it can be 1200 g / m 2 · 24 hours or less. The resin layer of the present invention has a high moisture permeability, so that the reliability of light transmission tends to be improved.
[0262] The moisture permeability of the resin layer of the present invention can be measured in accordance with JIS Z0208 at a temperature of 40° C. and a relative humidity of 92%, and can be adjusted by the type and thickness of the resin constituting the resin layer of the present invention.
[0263] (Glass layer)
[0264] The glass layer constituting the optical element of the present invention (hereinafter sometimes referred to as "the glass layer of the present invention") is not particularly limited, and an appropriate glass layer can be used according to the purpose. According to the classification based on the composition, the glass layer of the present invention can be, for example, soda-lime glass, boric acid glass, aluminosilicate glass, quartz glass, etc. In addition, according to the classification based on the alkali component, alkali-free glass and low-alkali glass can be listed. The content of the alkali metal component (such as Na2O, K2O, Li2O) of the above-mentioned glass is preferably 15% by weight or less, and more preferably 10% by weight or less.
[0265] When considering the surface hardness, air tightness, and corrosion resistance of the glass, the thickness of the glass layer of the present invention is preferably 20 μm or more. In addition, the glass layer of the present invention preferably has flexibility and bendability like a film, and in order to suppress image ghosting and project a clear image, the thickness is preferably 60 μm or less. The thickness of the glass layer of the present invention is more preferably 30 μm or more and 55 μm or less, and particularly preferably 40 μm or more and 50 μm or less.
[0266] The light transmittance of the glass layer of the present invention at a wavelength of 550 nm is preferably 85% or more. The refractive index of the glass layer of the present invention at a wavelength of 550 nm is preferably 1.4 to 1.65. The density of the glass layer of the present invention is preferably 2.3 g / cm 3 ~3.0g / cm 3 , more preferably 2.3 g / cm 3 ~2.7g / cm 3 .
[0267] The forming method of the glass layer of the present invention is not particularly limited, and an appropriate method can be adopted according to the purpose. Representatively, the glass layer of the present invention can be produced by melting a mixture of main raw materials including silica, aluminum oxide, etc., defoaming agents such as sodium sulfate and antimony oxide, and reducing agents such as carbon at a temperature of about 1400°C to about 1600°C, forming it into a thin plate, and then cooling it. As the forming method of the glass layer of the present invention, for example, a slit down-draw method, a fusion method, a float method, etc. can be cited. In order to thin the glass layer formed into a plate by these methods or to improve the smoothness, chemical polishing can be performed using a solvent such as hydrofluoric acid as needed.
[0268] (Hard Coating)
[0269] The hard coating layer (hereinafter, sometimes referred to as "the hard coating layer of the present invention") constituting the optical element of the present invention can be formed by any appropriate resin as long as it has sufficient surface hardness, excellent mechanical strength and excellent light transmittance. As specific examples of resins, thermosetting resins, thermoplastic resins, ultraviolet curing resins, electron beam curing resins, and two-liquid mixed resins can be cited. Ultraviolet curing resins are preferred. This is because the hard coating layer can be formed with simple operation and high efficiency.
[0270] Specific examples of ultraviolet curable resins include polyester, acrylic, urethane, amide, silicone, and epoxy ultraviolet curable resins. Ultraviolet curable resins include ultraviolet curable monomers, oligomers, and polymers. Preferred ultraviolet curable resins include resin compositions containing monomer components or oligomer components of acrylics having preferably 2 or more, more preferably 3 to 6 ultraviolet polymerizable functional groups. Typically, a photopolymerization initiator is added to the ultraviolet curable resin.
[0271] The hard coating of the present invention can be formed by any appropriate method. For example, the hard coating of the present invention can be formed by applying a hard coating forming resin composition on a substrate (including the above-mentioned resin layer and glass layer) and drying it, and irradiating the dried coating film with ultraviolet rays to cure it.
[0272] The thickness of the hard coat layer of the present invention is, for example, 2 μm to 20 μm, preferably 4 μm to 15 μm, and more preferably 4 μm to 10 μm.
[0273] From the viewpoint of antifouling properties, the water contact angle of the hard coat layer of the present invention is preferably 95° or more, more preferably 100° or more, and even more preferably 105° or more.
[0274] The water contact angle of the hard coat layer of the present invention is measured according to JIS R3257 and can be adjusted according to the type of resin constituting the hard coat layer, curing conditions, etc. The water contact angle of the hard coat layer of the present invention after the steel wool test described below is preferably within the above range.
[0275] <Steel Wool Test>
[0276] Steel wool "Product No. #0000" manufactured by TRUSCO was cut into 1 cm squares and rubbed against the surface of the hard coating layer 1000 times back and forth under the conditions of a load of 1 kg and a moving speed of 100 mm / sec.
[0277] From the viewpoint of excellent surface hardness and scratch resistance, the Vickers hardness of the hard coating layer of the present invention is preferably 80 or more, more preferably 90 or more, and even more preferably 100 or more.
[0278] The Vickers hardness of the hard coat layer of the present invention is measured in accordance with JIS Z2244 and can be adjusted by the type of resin constituting the hard coat layer, curing conditions, and the like.
[0279] From the viewpoint of antifouling properties, the surface element ratio of carbon element on the surface of the hard coating layer of the present invention is 50 atomic % or less, preferably 45 atomic % or less, and the surface element ratio of fluorine element on the surface of the hard coating layer is 30 atomic % or more.
[0280] The nitrogen element ratio in the surface of the hard coat layer is, for example, less than 1.5 atomic %, preferably 1.3 atomic % or less, for example, 0 atomic % or more.
[0281] The surface element ratio of fluorine, carbon and nitrogen on the surface of the hard coat layer of the present invention can be measured by X-ray photoelectron spectroscopy and can be adjusted by the type of resin constituting the hard coat layer, curing conditions and the like.
[0282] (Anti-reflection layer)
[0283] The antireflection layer constituting the optical element of the present invention (hereinafter sometimes referred to as "the antireflection layer of the present invention") is preferably composed of an inorganic substance. As the above-mentioned inorganic substance, the inorganic substances exemplified and explained as materials constituting the high refractive index layer, the low refractive index layer and the medium refractive index layer described later can be cited.
[0284] The antireflection layer of the present invention may be any suitable structure, for example: (i) a single layer of a low refractive index layer having an optical film thickness of 120 nm to 140 nm and a refractive index of 1.35 to 1.55; (ii) a laminate having a medium refractive index layer, a high refractive index layer and a low refractive index layer in sequence; (iii) a laminate having a plurality of layers alternating high refractive index layers and low refractive index layers.
[0285] Examples of materials that can form the low refractive index layer include silicon oxide (SiO2) and magnesium fluoride (MgF2). The refractive index of the low refractive index layer is typically about 1.35 to 1.55.
[0286] The material of the low refractive index layer can be a cured product of a curable fluorine-containing resin. The curable fluorine-containing resin, for example, has a structural unit derived from a fluorine-containing monomer and a structural unit derived from a crosslinkable monomer. As specific examples of fluorine-containing monomers, for example, fluoroolefins (vinyl fluoride, vinylidene fluoride, tetrafluoroethylene, hexafluoroethylene, hexafluoropropylene, perfluoro-2,2-dimethyl-1,3-dioxole, etc.), (meth)acrylate derivatives with partially or completely fluorinated alkyl groups (Viscoat 6FM (manufactured by Osaka Organic Chemical Co., Ltd.), M-2020 (manufactured by Daikin Co., Ltd.), etc.), and completely or partially fluorinated vinyl ethers. As crosslinkable monomers, for example, (meth)acrylate monomers having crosslinkable functional groups in the molecule such as glycidyl methacrylate; (meth)acrylate monomers having functional groups such as carboxyl, hydroxyl, amino, and sulfonic acid groups ((meth)acrylic acid, (meth)hydroxymethyl acrylate, (meth)hydroxyalkyl acrylate, (meth)allyl acrylate, etc.). The fluorine-containing resin may have a structural unit derived from other monomers (eg, olefin-based monomers, (meth)acrylate-based monomers, styrene-based monomers) other than the above-mentioned compounds.
[0287] Examples of materials that can form the high refractive index layer include titanium oxide (TiO2), niobium oxide (Nb2O3 or Nb2O5), tin-doped indium oxide (ITO), antimony-doped tin oxide (ATO), and ZrO2-TiO2. The refractive index of the high refractive index layer is typically about 1.60 to about 2.40.
[0288] As materials capable of forming the medium refractive index layer, for example, titanium oxide (TiO2), a mixture of a material capable of forming a low refractive index layer and a material capable of forming a high refractive index layer (for example, a mixture of titanium oxide and silicon oxide) can be cited. The refractive index of the medium refractive index layer is representatively about 1.50 to about 1.85. The thickness of the low refractive index layer, the medium refractive index layer, and the high refractive index layer can be set in a manner to achieve an appropriate optical film thickness corresponding to the layer structure of the anti-reflection layer, the desired anti-reflection performance, etc.
[0289] The anti-reflection layer of the present invention can be formed by a dry process (e.g., sputtering), can be formed by a wet process (e.g., coating), or can be formed by combining a dry process and a wet process. As specific examples of dry processes, PVD (physical vapor deposition) methods and CVD (chemical vapor deposition) methods can be cited. As PVD methods, vacuum evaporation methods, reactive evaporation methods, ion beam assisted methods, sputtering methods, and ion plating methods can be cited. As CVD methods, plasma CVD methods can be cited.
[0290] As a specific example of a wet process, for example, a coating liquid for forming an anti-reflection layer can be applied to form a coating film, and the coating film is cured to form an anti-reflection layer. As a method for coating, for example, a coating method such as a jet coating method, a die coating method, a spin coating method, a spray coating method, a gravure coating method, a roller coating method, a rod coating method, etc. can be used. Preferably, the coating film is dried before the above-mentioned curing. The above-mentioned drying can be, for example, natural drying, air drying by blowing, heating drying, or a method obtained by combining them. The curing means of the coating film is not particularly limited, and ultraviolet curing is preferred.
[0291] The thickness of the anti-reflection layer of the present invention is, for example, about 20 nm to about 300 nm.
[0292] From the viewpoint of antifouling properties, the water contact angle of the antireflection layer of the present invention is preferably 90° or more, more preferably 95° or more, further preferably 100° or more, particularly preferably 105° or more.
[0293] The water contact angle of anti-reflection layer of the present invention is measured according to JIS R3257, and can be regulated according to the kind of the composition that constitutes anti-reflection layer etc. In addition, the water contact angle after the preferred following eraser abrasion test of anti-reflection layer of the present invention is in the above-mentioned scope.By stacking the anti-reflection layer in these scopes with the water contact angle after the eraser abrasion test on the visual recognition side, particularly the outermost surface of OLED display device, even after OLED display device is rubbed by hand or cloth, also can keep excellent antifouling property.
[0294] <Eraser wear test>
[0295] An eraser for evaluating wear resistance manufactured by Minoan, Model 4004005007, was cut into 7 mm pieces and rubbed against the surface of the hard coating layer 6000 times in a reciprocating motion under the conditions of a load of 1 kg and a moving speed of 32 mm / sec.
[0296] (Anti-glare layer)
[0297] As the antiglare layer constituting the optical element of the present invention (hereinafter sometimes referred to as "the antiglare layer of the present invention"), any known antiglare layer can be adopted without limitation, and is generally formed as a layer in which inorganic or organic particles as an antiglare agent are dispersed in a resin.
[0298] The anti-glare layer of the present invention is not particularly limited, and is formed, for example, by using an anti-glare layer-forming material comprising a resin, particles, and a thixotropy-imparting agent, and by agglomerating the particles and the thixotropy-imparting agent, a convex portion is formed on the surface of the anti-glare layer of the present invention. According to this configuration, the anti-glare layer has excellent display characteristics that take into account both anti-glare properties and prevention of white blur, and although the anti-glare layer is formed by agglomeration of particles, the generation of protrusions on the surface of the anti-glare layer that become appearance defects can be prevented, thereby improving the yield rate of the product.
[0299] Examples of the resin include thermosetting resins and ionizing radiation curable resins that are cured by ultraviolet rays or light. As the resin, commercially available thermosetting resins, ultraviolet curable resins, and the like may also be used.
[0300] As the above-mentioned thermosetting resin and ultraviolet curing resin, for example, curable compounds having at least one of acrylate and methacrylate groups cured by heat, light (ultraviolet rays, etc.) or electron beams, for example, oligomers or prepolymers such as acrylate and methacrylate of multifunctional compounds such as silicone resins, polyester resins, polyether resins, epoxy resins, urethane resins, alkyd resins, spiroacetal resins, polybutadiene resins, polythiol polyene resins, and polyols can be used. They can be used alone or in combination of two or more.
[0301] The above-mentioned resin, for example, can also use a reactive diluent having at least one group of an acrylate group and a methacrylate group. The above-mentioned reactive diluent, for example, can use the reactive diluent recorded in Japanese Patent Publication No. 2008-88309, for example, including monofunctional acrylate, monofunctional methacrylate, multifunctional acrylate, multifunctional methacrylate, etc. As the above-mentioned reactive diluent, preferred acrylates with more than three functions and methacrylates with more than three functions are used. This is because the hardness of the anti-glare layer of the present invention can be made excellent. As the above-mentioned reactive diluent, for example, butanediol glycerol ether diacrylate, acrylate of isocyanuric acid, methacrylate of isocyanuric acid, etc. can also be cited. They can be used alone or in combination of two or more.
[0302] As the resin, a urethane acrylate resin is preferably included, and a copolymer of a curable urethane acrylate resin and a multifunctional acrylate (for example, pentaerythritol triacrylate) is more preferred.
[0303] The main function of the particles used to form the anti-glare layer of the present invention is to give the anti-glare property by making the surface of the anti-glare layer to be formed into a concave-convex shape, and to control the haze value of the anti-glare layer. The haze value of the anti-glare layer can be designed by controlling the refractive index difference between the above-mentioned particles and the above-mentioned resin. As the above-mentioned particles, for example, there are inorganic particles and organic particles. The above-mentioned inorganic particles are not particularly limited, and for example, silicon oxide particles, titanium oxide particles, aluminum oxide particles, zinc oxide particles, tin oxide particles, zirconium oxide particles, calcium carbonate particles, barium sulfate particles, talc particles, kaolin particles, calcium sulfate particles, etc. In addition, the above-mentioned organic particles are not particularly limited, and for example, polymethyl methacrylate resin powder (PMMA particles), silicone resin powder, polystyrene resin powder, polycarbonate resin powder, acrylic styrene resin powder, benzoguanamine resin powder, melamine resin powder, polyolefin resin powder, polyester resin powder, polyamide resin powder, polyimide resin powder, polyvinyl fluoride resin powder, etc. can be listed. These inorganic particles and organic particles can be used alone or in combination of two or more.
[0304] The weight average particle size (D) of the above-mentioned particles is preferably in the range of 2.5μm to 10μm. By making the weight average particle size of the above-mentioned particles in the above-mentioned range, for example, the anti-glare property can be made more excellent, and white blur can be prevented. The weight average particle size of the particles is more preferably in the range of 3μm to 7μm. It should be noted that the weight average particle size of the above-mentioned particles can be measured by, for example, the Coulter counting method. For example, a particle size distribution measuring device using the pore resistance method (trade name: Coulter counter, manufactured by Beckman Coulter) is used to measure the resistance of the electrolyte equivalent to the volume of the particles when the particles pass through the above-mentioned holes, thereby measuring the number and volume of the above-mentioned particles, and calculating the weight average particle size.
[0305] The shape of the particles is not particularly limited, and may be, for example, roughly spherical beads or irregularly shaped particles such as powders. Roughly spherical particles are preferred, roughly spherical particles with an aspect ratio of less than 1.5 are more preferred, and spherical particles are most preferred.
[0306] The ratio of the particles in the anti-glare layer of the present invention is preferably in the range of 0.2 to 12 parts by weight, more preferably in the range of 0.5 to 12 parts by weight, and further preferably in the range of 1 to 7 parts by weight relative to 100 parts by weight of the resin. By setting the above range, for example, the anti-glare property is more excellent and white blur can be prevented.
[0307] The anti-glare layer of the present invention may contain a thixotropy imparting agent. By containing the thixotropy imparting agent, the agglomeration state of the particles can be easily controlled. As the thixotropy imparting agent used to form the anti-glare layer of the present invention, for example, organic clay, oxidized polyolefin, modified urea, etc. can be cited.
[0308] In order to improve the affinity with the resin, the organoclay is preferably an organically treated clay. Examples of the organoclay include layered organoclay. The organoclay may be prepared by itself or a commercial product may be used. Examples of the commercially available products include Lucentite SAN, Lucentite STN, Lucentite SEN, Lucentite SPN, Somasif ME-100, Somasif MAE, Somasif MTE, Somasif MEE, and Somasif MPE (trade names, all manufactured by Co-op Chemical Co., Ltd.); ESBEN, ESBEN C, ESBEN E, ESBEN W, ESBEN P, ESBEN WX, ESBEN N-400, ESBEN NX, ESBEN NX80, ESBEN NO12S, ESBEN NEZ, ESBEN NO12, ESBEN NE, ESBEN NZ, ESBEN NZ70, ORGANITE, ORGANITE D, and ORGANITE T (trade names, all manufactured by HOJUN Co., Ltd.); KUNIPIA F, KUNIPIA G, and KUNIPIA G4 (trade names, all manufactured by KUNIMINE Industries Co., Ltd.); TIXOGEL VZ, Kraton HT, Kraton 40 (trade names, all manufactured by Rockwood Additives), etc.
[0309] The oxidized polyolefin may be prepared by itself or a commercial product may be used. Examples of the commercial product include Disparlon 4200-20 (trade name, manufactured by Kusumoto Chemicals Co., Ltd.) and Flownon SA300 (trade name, manufactured by Kyoeisha Chemical Co., Ltd.).
[0310] The modified urea is a reaction product of an isocyanate monomer or an adduct thereof with an organic amine. The modified urea can be prepared by itself or a commercial product can be used. Examples of the commercial product include BYK410 (manufactured by BYK-Chemie).
[0311] The thixotropy-imparting agent may be used alone or in combination of two or more.
[0312] The height of the roughness average line of the anti-glare layer of the present invention from the above-mentioned convex portion is preferably less than 0.4 times the thickness of the anti-glare layer. It is more preferably in the range of greater than or equal to 0.01 times and less than 0.4 times, and further preferably in the range of greater than or equal to 0.01 times and less than 0.3 times. If within this range, it is possible to appropriately prevent the formation of protrusions that become appearance defects on the convex portion. The anti-glare layer of the present invention can be less prone to appearance defects by having convex portions of such a height. Here, the height from the average line can be measured, for example, by the method described in Japanese Patent Gazette No. 2017-138620.
[0313] The ratio of the thixotropy-imparting agent in the anti-glare layer of the present invention is preferably in the range of 0.1 to 5 parts by weight, more preferably in the range of 0.2 to 4 parts by weight, based on 100 parts by weight of the resin.
[0314] The thickness (d') of the anti-glare layer of the present invention is not particularly limited, and is preferably in the range of 2μm to 12μm. By setting the thickness (d') of the anti-glare layer to the above range, for example, the optical laminate of the present invention can be prevented from curling, and problems of reduced productivity such as poor transportability can be avoided. In addition, when the thickness (d') is in the above range, as described above, the weight-average particle size (D) of the particles is preferably in the range of 2.5μm to 10μm. By combining the thickness (d') of the anti-glare layer of the present invention and the weight-average particle size (D) of the particles as the above combination, the anti-glare property can be made more excellent. The thickness (d') of the anti-glare layer of the present invention is more preferably in the range of 2μm to 10μm, and further preferably in the range of 3μm to 8μm.
[0315] The relationship between the thickness (d') of the anti-glare layer of the present invention and the weight average particle size (D) of the particles is preferably in the range of 0.3≤D / d'≤0.9. By being in such a relationship, the anti-glare property can be made better, white blur can be prevented, and an anti-glare layer without appearance defects can be made.
[0316] The haze value (H') of the anti-glare layer of the present invention is not particularly limited. From the perspective of effectively reducing the color shift and interference unevenness of the OLED display device, it is preferably 5% or more, more preferably 10% or more, further preferably 15% or more, and particularly preferably 20% or more. In addition, from the perspective of suppressing image blurring of the OLED display device and displaying a high-definition image, the haze value of the anti-glare layer of the present invention is preferably 80% or less, more preferably 70% or less, further preferably 60% or less, and particularly preferably 50% or less.
[0317] The haze value of the antiglare layer of the present invention can be measured by the method specified in JIS K7136, and can be designed by controlling the type and thickness of the antiglare layer and the refractive index difference between the particles and the resin.
[0318] The anti-glare layer of the present invention forms convex portions on the surface of the anti-glare layer of the present invention by agglomerating the above-mentioned particles and the above-mentioned thixotropy imparting agent. In the agglomerated portion forming the above-mentioned convex portions, the above-mentioned particles are present in the surface direction of the anti-glare layer of the present invention in a state of multiple aggregations. Thus, the convex portions become a gentle shape. The anti-glare layer of the present invention can prevent white blurring while maintaining anti-glare properties by having convex portions of such a shape, and thus can be less likely to produce appearance defects.
[0319] The surface shape of the anti-glare layer of the present invention can be arbitrarily designed by controlling the coagulation state of the particles contained in the anti-glare layer forming material. The coagulation state of the above-mentioned particles can be controlled, for example, by the material of the above-mentioned particles (for example, the chemical modification state of the particle surface, the affinity to the solvent, the resin, etc.), the type and combination of the resin (binder) or the solvent. Here, the coagulation state of the particles can be controlled by the thixotropy imparting agent contained in the anti-glare layer forming material of the present invention. As a result, the coagulation state of the above-mentioned particles can be made as described above, and the above-mentioned convex portion can be made into a gentle shape.
[0320] In the anti-glare layer of the present invention, it is preferred that the number of appearance defects having a maximum diameter of 200 μm or more is 1 m2 per 1 m2 of the anti-glare layer. 2 More preferably, there is no such appearance defect.
[0321] In the concavo-convex shape of the anti-glare layer surface of the present invention, the average tilt angle θa (°) is preferably in the range of 0.1 to 5.0, more preferably in the range of 0.3 to 4.5, further preferably in the range of 1.0 to 4.0, and particularly preferably in the range of 1.6 to 4.0. Here, the average tilt angle θa is a value defined by the following mathematical formula (1). The above average tilt angle θa is, for example, a value measured by the method described in Japanese Patent Application Laid-Open No. 2017-138620.
[0322]
[0323] In the mathematical formula (1), Δa is a value obtained by dividing the sum of the differences (height h) between the apex of adjacent peaks and the lowest points of troughs (h1+h2+h3···+hn) by the reference length L of the roughness curve specified in JIS B0601 (1994 edition), as shown in the following mathematical formula (2). The roughness curve is a curve obtained by removing surface undulation components longer than a specified wavelength from a profile curve using a phase difference compensation type high-pass filter. In addition, the profile curve refers to a contour that appears at the cut when the target surface is cut by a plane at right angles to the target surface.
[0324]
[0325] When θa is within the above range, the anti-glare property is more excellent and white blurring can be prevented.
[0326] When forming the antiglare layer of the present invention, the prepared antiglare layer-forming material (coating solution) preferably exhibits thixotropy, and the Ti value specified below is preferably in the range of 1.3 to 3.5, and more preferably in the range of 1.3 to 2.8.
[0327]
[0328] Here, β1 is the viscosity measured at a shear rate of 20 (1 / s) using Rheo stress 6000 manufactured by HAAKE, and β2 is the viscosity measured at a shear rate of 200 (1 / s) using Rheo stress 6000 manufactured by HAAKE.
[0329] When the Ti value is less than 1.3, appearance defects are likely to occur, and the anti-glare property and white blur properties are deteriorated. On the other hand, when the Ti value is greater than 3.5, the particles are unlikely to aggregate and are likely to be in a dispersed state.
[0330] The method for producing the anti-glare layer of the present invention is not particularly limited, and the anti-glare layer can be produced by any method, for example, by preparing an anti-glare layer-forming material (coating solution) containing the above-mentioned resin, the above-mentioned particles, the above-mentioned thixotropy imparting agent and a solvent, applying the above-mentioned anti-glare layer-forming material (coating solution) to form a coating film, and curing the above-mentioned coating film to form an anti-glare layer. A transfer method using a mold, a method of imparting a concave-convex shape by a suitable method such as sandblasting or an embossing roller, etc. can also be used together.
[0331] The above-mentioned solvent is not particularly limited, and various solvents can be used, and one can be used alone or two or more can be used in combination. According to the composition of the resin, the type and content of the particles and the thixotropy imparting agent, there are optimal solvent types and solvent ratios. As solvents, there are no particular restrictions, for example, they can be listed: alcohols such as methanol, ethanol, isopropanol, butanol, 2-methoxyethanol; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone; esters such as methyl acetate, ethyl acetate, butyl acetate; ethers such as diisopropyl ether and propylene glycol monomethyl ether; glycols such as ethylene glycol and propylene glycol; cellosolves such as ethyl cellosolve and butyl cellosolve; aliphatic hydrocarbons such as hexane, heptane, octane; aromatic hydrocarbons such as benzene, toluene, xylene, etc.
[0332] By appropriately selecting the above-mentioned solvent, the thixotropy of the anti-glare layer forming material (coating solution) using the thixotropy imparting agent can be well demonstrated. For example, when using an organoclay, toluene and xylene can be suitably used alone or in combination, for example, when using an oxidized polyolefin, methyl ethyl ketone, ethyl acetate, propylene glycol monomethyl ether can be suitably used alone or in combination, for example, when using modified urea, butyl acetate and methyl isobutyl ketone can be suitably used alone or in combination.
[0333] Various leveling agents can be added to the anti-glare layer forming material. As the above-mentioned leveling agent, in order to prevent uneven coating (uniformization of the coating surface), for example, a fluorine-containing or silicone-based leveling agent can be used. The leveling agent can be appropriately selected according to the situation that the surface of the anti-glare layer of the present invention requires antifouling properties, or the situation that an anti-reflection layer or a layer containing an interlayer filler is formed on the anti-glare layer. For example, by including the above-mentioned thixotropy imparting agent, the coating liquid can be made to exhibit thixotropy, so uneven coating is not easy to occur. Therefore, for example, there is an advantage of expanding the selection range of the above-mentioned leveling agent.
[0334] The amount of the leveling agent blended is, for example, 5 parts by weight or less, and preferably within a range of 0.01 to 5 parts by weight, relative to 100 parts by weight of the resin.
[0335] The anti-glare layer forming material may be added with pigments, fillers, dispersants, plasticizers, ultraviolet absorbers, surfactants, antifouling agents, antioxidants, etc. as needed within a range that does not impair performance. These additives may be used alone or in combination of two or more.
[0336] As the anti-glare layer forming material, a conventionally known photopolymerization initiator described in, for example, JP-A-2008-88309 can be used.
[0337] As a method for applying the anti-glare layer forming material, for example, a coating method such as a jet coating method, a die coating method, a spin coating method, a spray coating method, a gravure coating method, a roll coating method, a bar coating method, etc. can be used.
[0338] The anti-glare layer forming material is applied to form a coating film, and the coating film is cured. Preferably, the coating film is dried before the curing. The drying may be, for example, natural drying, air drying by blowing air, heating drying, or a combination of these methods.
[0339] The curing method of the coating of the anti-glare layer forming material is not particularly limited, but ultraviolet curing is preferred. The irradiation amount of the energy ray source is preferably 50 mJ / cm in terms of cumulative exposure at an ultraviolet wavelength of 365 nm. 2 ~500mJ / cm 2 If the irradiation dose is 50mJ / cm 2 If the irradiation dose is 500 mJ / cm 2 The following can prevent the formed anti-glare layer from being colored.
[0340] The anti-glare layer of the present invention can be formed by the above operation. It should be noted that the anti-glare layer can also be formed by a manufacturing method other than the above method. The hardness of the anti-glare layer of the present invention is also affected by the thickness of the layer in terms of pencil hardness, but preferably has a hardness of 2H or more.
[0341] The anti-glare layer of the present invention may have a multilayer structure in which two or more layers are stacked.
[0342] The anti-reflection layer can also be configured on the anti-glare layer of the present invention. For example, as one of the main reasons for reducing the visual recognition of the OLED display device, the reflection of light at the interface between air and the anti-glare layer can be cited. The anti-reflection layer reduces its surface reflection. It should be noted that the anti-glare layer and the anti-reflection layer of the present invention can be a multilayer structure formed by stacking two or more layers.
[0343] (Middle layer)
[0344] The intermediate layer constituting the optical element of the present invention (hereinafter sometimes referred to as "intermediate layer of the present invention") is formed between the above-mentioned resin layer and the above-mentioned hard coating layer, anti-reflection layer or anti-glare layer. By forming this intermediate layer, the adhesion between the resin layer and the above-mentioned hard coating layer, anti-reflection layer or anti-glare layer is improved.
[0345] The mechanism for forming the intermediate layer (also referred to as a permeation layer or a compatibility layer) of the present invention is not particularly limited. For example, in the formation of the above-mentioned hard coating layer, anti-reflection layer or anti-glare layer, the intermediate layer is formed in the process of coating, penetrating and drying the coating liquid for forming the hard coating layer, the coating liquid for forming the anti-reflection layer or the coating liquid for forming the anti-glare layer on the resin layer. In the above-mentioned drying process, for example, the coating liquid for forming the hard coating layer, the coating liquid for forming the anti-reflection layer or the coating liquid for forming the anti-glare layer is infiltrated into the resin layer to form the above-mentioned intermediate layer containing the resin from the resin layer and the resin from the hard coating layer, the anti-reflection layer or the anti-glare layer. The resin contained in the above-mentioned intermediate layer is not particularly limited. For example, it can be a resin obtained by simply mixing (compatibility) the resin contained in the resin layer and the resin contained in the hard coating layer, the anti-reflection layer or the anti-glare layer. In addition, for the resin contained in the above-mentioned intermediate layer, for example, at least one of the resin contained in the resin layer and the resin contained in the hard coating layer, the anti-reflection layer or the anti-glare layer can undergo a chemical change by heating, light irradiation, etc.
[0346] The thickness ratio R of the intermediate layer defined by the following mathematical formula (3) is not particularly limited, and is, for example, 0.10 to 0.80, and may be, for example, 0.15 or more, 0.20 or more, 0.25 or more, 0.30 or more, 0.40 or more, or 0.45 or more, and may be, for example, 0.75 or less, 0.70 or less, 0.65 or less, 0.60 or less, 0.50 or less, 0.40 or less, 0.45 or less, or 0.30 or less. The thickness ratio R of the intermediate layer may be, for example, 0.15 to 0.75, 0.20 to 0.70, 0.25 to 0.65, 0.30 to 0.60, 0.40 to 0.50, 0.45 to 0.50, 0.15 to 0.45, 0.15 to 0.40, 0.15 to 0.30, or 0.20 to 0.30. The intermediate layer can be confirmed by, for example, observing a cross section of the optical element with a transmission electron microscope (TEM), and the thickness can be measured.
[0347] R=[DC / (DC+DB)](3)
[0348] In the above mathematical formula (3), DB is the thickness [μm] of the hard coat layer, the antireflection layer or the antiglare layer, and DC is the thickness [μm] of the above intermediate layer.
[0349] When an intermediate layer is formed between the resin layer and the hard coating layer, the anti-reflection layer or the anti-glare layer, the shear strength between the resin layer and the hard coating layer, the anti-reflection layer or the anti-glare layer is preferably 20 MPa or more, more preferably 50 MPa or more, from the viewpoint of excellent adhesion.
[0350] The shear breaking strength can be determined by the SAICAS method and can be adjusted by the type of resin layer, the composition of the coating solution for forming a hard coat layer, the coating solution for forming an antireflection layer, the coating solution for forming an antiglare layer, the film forming method, and the like.
[0351] (Shock absorbing layer)
[0352] The impact absorbing layer constituting the optical element of the present invention (hereinafter sometimes referred to as "the impact absorbing layer of the present invention") can be composed of any appropriate resin layer capable of achieving the desired impact absorption rate. The resin layer can be composed of a resin film or an adhesive. The impact absorbing layer typically includes an epoxy resin, a urethane resin or an acrylic resin. These resins can be used alone or in combination.
[0353] The thickness of the impact absorbing layer of the present invention is preferably 30 to 200 μm, more preferably 30 to 150 μm, and further preferably 40 to 120 μm. When the thickness of the impact absorbing layer of the present invention is within such a range, an optical layered body having excellent impact resistance can be realized.
[0354] The storage modulus G' of the impact absorbing layer of the present invention at 25°C is preferably 0.1 GPa or less, more preferably 0.01 MPa to 0.1 GPa. If the storage modulus of the impact absorbing layer of the present invention is within such a range, it has the advantage of being able to absorb impact and prevent the optical laminate from breaking. In addition, a synergistic effect with the effect of the thickness described above can also be exerted.
[0355] (Antistatic layer)
[0356] The antistatic layer constituting the optical element of the present invention (hereinafter sometimes referred to as "the antistatic layer of the present invention") is not particularly limited, and may be formed by coating a conductive coating liquid containing a conductive polymer. Specific coating methods include roller coating, rod coating, gravure coating, and the like.
[0357] As the conductive polymer, for example, a conductive polymer in which a polyanion is doped in a π-conjugated conductive polymer can be cited. As the π-conjugated conductive polymer, chain conductive polymers such as polythiophene, polypyrrole, polyaniline, and polyacetylene can be cited. As the polyanion, polystyrene sulfonic acid, polyisoprene sulfonic acid, polyvinyl sulfonic acid, polyallyl sulfonic acid, polyethyl acrylate sulfonic acid, polymethacrylic acid, and the like can be cited.
[0358] The thickness of the antistatic layer is preferably 1 nm to 1000 nm, and more preferably 5 nm to 900 nm. The antistatic layer may be a single layer or may be two or more layers.
[0359] (Optical laminate)
[0360] In the optical laminate of the present invention, a color filter is arranged on the visual recognition side of the OLED element, and when the distance (d) between the adhesive layer of the present invention and the color filter is 700 μm or less, the distance between the adhesive layer of the present invention (especially the adhesive layer with light scattering properties) and the color filter is set to d [μm], and the haze value of the adhesive layer of the present invention (especially the adhesive layer with light scattering properties) is set to H [%], the value of d × H is preferably 70000 or less, more preferably 60000 or less, and further preferably 50000 or less. When the value of d × H is 700000 or less, it is less likely to produce image blur. The value of d × H is, for example, 100 or more, and can be 1000 or more, 10000 or more, or 20000 or more. In this case, H is preferably 20 or more.
[0361] In the optical laminate of the present invention, when the thickness of the adhesive layer of the present invention (especially the adhesive layer having light scattering properties) is set to T [μm] and the haze value of the adhesive layer of the present invention (especially the adhesive layer having light scattering properties) is set to H [%], the value of T × H is preferably 400 or more, more preferably 600 or more, further preferably 800 or more, further preferably 1000 or more, and particularly preferably 1500 or more. When the value of T × H is 400 or less, it is more difficult to produce image blur. The value of T × H is, for example, 10000 or less, and can be 8000 or less, 6000 or less, or 4000 or less.
[0362] One embodiment of the optical layered body of the present invention (for example, Figure 3 and Figure 4 In the optical laminate in the OLED display device of the present invention shown in FIG. 1 , it is preferred that the adhesive layer of the present invention (particularly the adhesive layer having light scattering properties) is provided on at least one surface of the resin layer of the present invention. In this case, when the refractive index of the resin layer of the present invention is set to n1, the refractive index of the adhesive of the adhesive layer of the present invention is set to n2, and the refractive index of the light scattering fine particles of the present invention is set to n3, it is preferred that n1>n2>n3 is satisfied. In this case, white blur is further suppressed.
[0363] One embodiment of the optical layered body of the present invention (for example, Figure 3 and Figure 4 In the optical laminate in the OLED display device of the present invention shown in FIG. 1 , the refractive index (n1) of the resin layer of the present invention is preferably 1.50 to 1.80, more preferably 1.55 to 1.75, and further preferably 1.60 to 1.70. The refractive index of the above-mentioned resin layer can be adjusted by the type and content of the resin constituting the resin layer.
[0364] One embodiment of the optical layered body of the present invention (for example, Figure 3 and Figure 4 In the optical laminate in the OLED display device of the present invention shown in FIG. 1 , it is preferred to have a structure in which the adhesive layer of the present invention (particularly an adhesive layer having light scattering properties) is provided on one side of the resin layer of the present invention and the hard coating layer of the present invention is provided on the other side. In particular, in this embodiment, it is preferred to satisfy n1>n2>n3.
[0365] In one embodiment of the optical layered body of the present invention (for example, Figure 11 to Figure 13 In the optical laminate in the OLED display device of the present invention shown in FIG. 1 , in the reflectance spectrum of the OLED display device in a state where the optical laminate for the OLED display device is not laminated, when the maximum reflectance in the wavelength range of 380nm to 455nm is set to Rp1 and the reflectance of the anti-reflection layer at the wavelength under the above Rp1 is set to Rf1, [Rf1 / Rp1] is preferably 0.3 or less, more preferably 0.25 or less, further preferably 0.2 or less, further preferably 0.15 or less, and particularly preferably 0.1 or less. The smaller the above [Rf1 / Rp1], the more interference unevenness can be suppressed.
[0366] In one embodiment of the optical layered body of the present invention (for example, Figure 11 to Figure 13 In the optical laminate in the OLED display device of the present invention shown in FIG. 1 , in the reflectance spectrum of the OLED display device in a state where the optical laminate for the OLED display device is not laminated, when the maximum reflectance in the wavelength range of 460nm to 530nm is set to Rp2 and the reflectance of the anti-reflection layer at the wavelength under the above Rp2 is set to Rf2, [Rf2 / Rp2] is preferably 0.12 or less, more preferably 0.1 or less, further preferably 0.05 or less, further preferably 0.03 or less, and particularly preferably 0.01 or less. The smaller the above [Rf2 / Rp2], the more interference unevenness can be suppressed.
[0367] It should be noted that, in this specification, wavelength WL1 is, for example, 430 nm or 440 nm, and wavelength WL2 is, for example, 500 nm or 510 nm. In addition, Rp1 and Rp2 are, for example, 7% or more (for example, 7% to 20%), preferably 10% or more (for example, 10% to 18%).
[0368] The sum of [Rf1 / Rp1] and [Rf2 / Rp2] is preferably 0.42 or less, more preferably 0.4 or less, further preferably 0.3 or less, further preferably 0.2 or less, and particularly preferably 0.1 or less. The smaller the sum, the more interference unevenness can be suppressed.
[0369] One embodiment of the optical layered body of the present invention (for example, Figure 11 to Figure 13 In the optical laminate in the OLED display device of the present invention shown in FIG. 1 , it is preferred that the anti-reflection layer of the present invention has a hard coating layer of the present invention, a substrate layer, and an adhesive layer of the present invention on the side opposite to the visual recognition side, and more preferably has a structure having these layers in sequence. The substrate layer may be a resin layer of the present invention or a glass layer of the present invention.
[0370] In one embodiment of the optical layered body of the present invention (for example, Figure 8 to Figure 10 In the optical laminate in the OLED display device of the present invention shown in FIG. 1 , when the scattering efficiency of the anti-glare layer of the present invention at the wavelength WL1 showing the maximum reflectivity in the wavelength range of 380nm to 455nm in the reflectivity spectrum of the OLED display device in a state where the optical laminate for the OLED display device is not laminated is set to S1, S1 is preferably 15% or more, more preferably 20% or more, further preferably 30% or more, further preferably 40% or more, and particularly preferably 50% or more. The larger the S1, the more interference unevenness can be suppressed.
[0371] In one embodiment of the optical layered body of the present invention (for example, Figure 8 to Figure 10 In the optical laminate in the OLED display device of the present invention shown in FIG. 1 , when the scattering efficiency of the anti-glare layer of the present invention at the wavelength WL2 showing the maximum reflectivity in the wavelength range of 460nm to 530nm in the reflectivity spectrum of the OLED display device in a state where the optical laminate for the OLED display device is not laminated is set to S2, S2 is preferably 15% or more, more preferably 20% or more, further preferably 30% or more, further preferably 40% or more, and particularly preferably 50% or more. The larger the S2, the more it is possible to suppress interference unevenness.
[0372] The total of S1 and S2 is preferably 30% or more, more preferably 40% or more, further preferably 60% or more, further preferably 80% or more, and particularly preferably 100% or more. The greater the total, the more interference unevenness can be suppressed.
[0373] One embodiment of the optical layered body of the present invention (for example, Figure 8 to Figure 10 In the optical laminate in the OLED display device of the present invention shown in FIG. 1 , it is preferred that the anti-glare layer of the present invention has a substrate layer and an adhesive layer of the present invention on the side opposite to the visual recognition side, and more preferably has a structure having these layers in sequence. The substrate layer may be a resin layer of the present invention or a glass layer of the present invention.
[0374] One embodiment of the optical layered body of the present invention (for example, Fig.14 and Fig.15 The optical laminate in the OLED display device of the present invention shown in FIG. 1 preferably has a structure in which the optical element of the present invention further comprises an adhesive layer of the present invention, a substrate layer and a hard coating layer of the present invention on the visual recognition side of the glass layer of the present invention, and more preferably has a structure in which these layers are sequentially formed. The above-mentioned substrate layer may use the resin layer of the present invention or the glass layer of the present invention.
[0375] One embodiment of the optical layered body of the present invention (for example, Fig.14 and Fig.15 In the optical laminate in the OLED display device of the present invention shown in FIG. 1 , when the indentation elastic modulus of the adhesive layer of the present invention is set to Ea and the tensile storage elastic modulus of the resin layer of the present invention is set to Er, the absolute value of Ea-Er is preferably 1 GPa or less, more preferably 0.9 GPa or less, further preferably 0.7 GPa or less, and particularly preferably 0.5 GPa or less. When the above absolute value is 1 GPa or less, the impact resistance is further improved.
[0376] One embodiment of the optical layered body of the present invention (for example, Fig.14 and Fig.15 In the optical laminate in the OLED display device of the present invention shown in FIG. 1 ), the tensile storage elastic modulus Er of the resin layer of the present invention is preferably 4 GPa or more, more preferably 4.3 GPa or more, and further preferably 4.6 GPa or more. When the tensile storage elastic modulus Er is 4 GPa or more, the impact resistance is further improved. The tensile storage elastic modulus Er is, for example, 50 GPa or less, and may be 30 GPa or less, or 10 GPa or less. The tensile storage elastic modulus Er can be measured according to JIS K 7161.
[0377] One embodiment of the optical layered body of the present invention (for example, Fig.16 and Fig.17 In the optical laminate in the OLED display device of the present invention shown in FIG. 1 , it is preferred to have a structure in which an intermediate layer (compatible layer) is formed between the transparent polyimide layer and the hard coating layer of the present invention. By forming the intermediate layer, the adhesion between the transparent polyimide layer and the hard coating layer of the present invention is improved. The intermediate layer is a layer formed by the composition (coating agent) for forming the hard coating layer of the present invention penetrating into the transparent polyimide layer. That is, the intermediate layer is a portion in which the hard coating component of the present invention exists in the transparent polyimide layer.
[0378] The ratio (P1) of the shear strength of the intermediate layer to the shear strength of the hard coating layer of the present invention is preferably 0.25 or less, more preferably 0.23, and further preferably 0.21 or less. The ratio (P1) is, for example, 0.02 or more, 0.05 or more, or 0.08 or more.
[0379] One embodiment of the optical layered body of the present invention (for example, Fig.16 and Fig.17 In the optical laminate in the OLED display device of the present invention shown in FIG. 1 , the ratio (P2) of the shear fracture strength of the transparent polyimide layer to the shear fracture strength of the hard coating layer of the present invention is preferably 0.65 or more, more preferably 0.70 or more, further preferably 0.80 or more, and particularly preferably 0.90 or more. The above ratio (P2) is, for example, 1.50 or less, and can be 1.30 or less, or 1.10 or less.
[0380] The difference (P2-P1) between the ratio (P1) and the ratio (P2) is preferably 0.6 or more, more preferably 0.70 or more, and may be 0.80 or more. The difference (P2-P1) is, for example, 1.5 or less, 1.2 or less, or 0.9 or less.
[0381] One embodiment of the optical layered body of the present invention (for example, Fig.16 and Fig.17 In the optical laminate in the OLED display device of the present invention shown in FIG. 1 , it is preferred that the transparent polyimide layer further has an adhesive layer on the side opposite to the hard coat layer of the present invention.
[0382] (Method for producing optical layered body)
[0383] The manufacturing method of the optical laminate of the present invention is not particularly limited, and can be manufactured by sequentially stacking the adhesive layer, adhesive layer, resin layer, glass layer, hard coating layer, anti-reflection layer, anti-glare layer, intermediate layer (compatible layer), impact absorbing layer, etc., which constitute the optical element of the present invention on the visual recognition side of the OLED display panel of the present invention. In addition, it can be manufactured by pre-making a laminate constituting the optical laminate of the present invention and stacking it on the visual recognition side of the OLED display panel of the present invention. In the case of pre-making a laminate constituting the optical laminate of the present invention, it can be a laminate constituting the entirety of the optical laminate of the present invention, or a laminate constituting a part of the optical laminate of the present invention can be divided and stacked on the visual recognition side of the OLED display panel of the present invention.
[0384] The layers constituting the optical element of the present invention or the laminate thereof may be protected with a release liner or a surface protective film before use.
[0385] (Release liner)
[0386] When the optical element of the present invention includes an adhesive layer, a release liner may be provided on the surface (adhesive surface) of the adhesive layer before use. The release liner may be used as a protective material for the adhesive layer and may be peeled off when attached to an adherend. It should be noted that the release liner does not constitute the optical element of the present invention and may not be provided.
[0387] As the release liner, conventional release paper etc. can be used, without particular restrictions, for example, substrates with a release treatment layer, low adhesive substrates containing fluoropolymers, low adhesive substrates containing non-polar polymers, etc. can be cited. As substrates with the above-mentioned release treatment layer, for example, plastic films, papers, etc. that have been surface-treated using release treatment agents such as silicones, long-chain alkyls, fluorine-containing types, and molybdenum sulfide can be cited. As the fluoropolymer in the above-mentioned low adhesive substrate containing fluoropolymers, for example, polytetrafluoroethylene, polychlorotrifluoroethylene, polyvinyl fluoride, polyvinylidene fluoride, tetrafluoroethylene-hexafluoropropylene copolymer, chlorofluoroethylene-vinylidene fluoride copolymer, etc. can be cited. In addition, as the above-mentioned non-polar polymer, for example, olefin resins (for example, polyethylene and polypropylene, etc.) can be cited. It should be noted that the release liner can be formed by a known or conventional method. In addition, the thickness of the release liner is not particularly limited either.
[0388] (Surface protection film)
[0389] The outermost surface (the outermost surface on the visual recognition side) of the optical laminate of the present invention may be protected by a surface protection film. The surface protection film may be attached by the consumer. It should be noted that the surface protection film does not constitute the optical element of the present invention and may not be provided.
[0390] As the above-mentioned surface protection film, a known or commonly used surface protection film can be used, without particular limitation, for example, a surface protection film having an adhesive layer on the surface of a plastic film can be used. As the above-mentioned plastic film, for example, a plastic film formed by plastic materials such as polyester (polyethylene terephthalate, polyethylene naphthalate, etc.), polyolefin (polyethylene, polypropylene, cyclic polyolefin, etc.), polystyrene, acrylic resin, polycarbonate, epoxy resin, fluorine-containing resin, silicone resin, diacetate resin, triacetate resin, polyarylate, polyvinyl chloride, polysulfone, polyethersulfone, polyether ether imide, polyimide, polyamide, etc. can be cited. As the above-mentioned adhesive layer, for example, an adhesive layer formed by one or more of the known or commonly used adhesives such as acrylic adhesives, natural rubber adhesives, synthetic rubber adhesives, ethylene-vinyl acetate copolymer adhesives, ethylene-(methyl)acrylate copolymer adhesives, styrene-isoprene block copolymer adhesives, styrene-butadiene block copolymer adhesives, etc. The adhesive layer may contain various additives (e.g., antistatic agents, slip agents, etc.). It should be noted that the plastic film and the adhesive layer may each have a single layer structure or a multilayer (multiple layers) structure. In addition, the thickness of the surface protective film is not particularly limited and can be appropriately selected.
[0391] (OLED display device of the present invention)
[0392] Hereinafter, one embodiment of an OLED display device in which the optical laminate of the present invention is stacked on the viewing side of an OLED display panel will be described with reference to the drawings, but the present invention is not limited to this embodiment. Figure 2 This is one embodiment showing the basic structure of an OLED display device in which the optical laminate of the present invention is stacked.
[0393] like Figure 2 As shown, the OLED display device 200 is on the visual recognition side ( Figure 2 The OLED display panel 100 is not particularly limited, and can be, for example, Figure 1 The OLED display panel 100 described has the same structure.
[0394] Figure 2 In the OLED display device 200, 21 to 29 are layers constituting the optical laminate 20, 21 represents an adhesive layer or an adhesive layer, 22 represents a resin layer, a glass layer or an impact absorbing layer, 23 represents a hard coating layer or an anti-glare layer, 24 represents an adhesive layer or an adhesive layer, 25 represents a resin layer, a glass layer or an impact absorbing layer, 26 represents an adhesive layer or an adhesive layer, 27 represents a resin layer, a glass layer or an impact absorbing layer, 28 represents a hard coating layer or an anti-glare layer, and 29 represents an anti-reflection layer. Figure 2 The stacked structure of the optical stack 20 shown is not limited to this embodiment, and may be Figure 2 The optical layered body 20 shown in the laminated structure may have other layers constituting the optical element of the present invention inserted between any of the layers, or may not have other layers. Figure 2 An arbitrary layer of the stacked structure of the optical stack 20 shown.
[0395] As a preferred embodiment of the present invention, Figure 2 Among them, 24 is an adhesive layer or a gluing agent layer, 25 is a resin layer, a glass layer or an impact absorbing layer, 26 is an adhesive layer or an adhesive layer, 27 is a resin layer, a glass layer or an impact absorbing layer, 28 is a hard coating layer or an anti-glare layer, 21 to 23 do not exist, and at least one of the adhesive layers 24 and 26 is an adhesive layer having light scattering properties. Figure 3 An OLED display device 300A according to this embodiment is shown. Figure 3 34A to 38A are layers constituting the optical laminate 30A, 34A is a pressure-sensitive adhesive layer or an adhesive layer, 35A is a glass layer, 36A is a pressure-sensitive adhesive layer having light scattering properties, 37A is a resin layer, and 38A is a hard coating layer. Since the pressure-sensitive adhesive layer 36A has light scattering properties, color shift and interference unevenness caused by the OLED display panel 100 can be suppressed, and the visual recognition of the OLED display device 300 is excellent.
[0396] It should be noted that in Figure 3 In the OLED display device 300A shown, an anti-reflection layer may be present on the visual recognition side of the hard coating layer 38A.
[0397] As a preferred embodiment of the present invention, Figure 2 In the figure, 21 is an adhesive layer, 22 is a resin layer, 23 is a hard coating layer, 24 is an adhesive layer, 25 is a glass layer, 26 is an adhesive layer, 27 is a resin layer, 28 is a hard coating layer, there is no anti-reflection layer 29, and at least one of the adhesive layers 21, 24, and 26 is an adhesive layer with light scattering properties. Figure 4 FIG. 3 shows an OLED display device 300B of this embodiment. Figure 4 31B to 38B are layers constituting the optical laminate 30B, 31B is an adhesive layer, 32B is a resin layer, 33B is a hard coating layer, 34B is an adhesive layer, 35B is a glass layer, 36B is an adhesive layer having light scattering properties, 37B is a resin layer, and 38B is a hard coating layer. Since the adhesive layer 36B has light scattering properties, color shift and interference unevenness caused by the OLED display panel 100 can be suppressed, and the visual recognition of the OLED display device 300B is excellent.
[0398] It should be noted that in Figure 4In the OLED display device 300B shown, an anti-reflection layer may be provided on the visual recognition side of the hard coating layer 38B.
[0399] As another preferred embodiment of the present invention, Figure 2 In the OLED display panel 100, a color filter is arranged on the visual recognition side, 26 is an adhesive layer with light scattering properties, 27 is a resin layer, 28 is a hard coating layer, 21 to 25 and 29 are not present, and the distance d (μm) between the adhesive layer 26 with light scattering properties and the color filter is 700 μm or less. Since the distance d between the adhesive layer with light scattering properties and the color filter is 700 μm or less, even if a light scattering layer is stacked to suppress color shift and interference unevenness caused by the OLED display device 300, image blur is not likely to occur, and visual recognition is excellent. Figure 5 An OLED display device 400A according to this embodiment is shown. Figure 5 46A to 48A are layers constituting the optical laminate 40A, 46A is an adhesive layer having light scattering properties, 47A is a resin layer, and 48A is a hard coating layer. 15A is disposed on the visual recognition side of the OLED display panel 400A (on the Figure 5 The adhesive layer 46A having light scattering properties is in direct contact with the color filter 15A, that is, the distance between the adhesive layer 46A having light scattering properties and the color filter 15A is 0 μm, so that the color shift and interference unevenness caused by the OLED display device 400A can be most effectively suppressed.
[0400] It should be noted that in Figure 5 In the illustrated OLED display device 400A, an anti-reflection layer may be present on the visual recognition side of the hard coating layer 48A.
[0401] As another preferred embodiment of the present invention, Figure 2 In the OLED display panel 100, a color filter is configured on the visual recognition side, 24 is an adhesive layer with light scattering properties, 25 is a glass layer, 26 is an adhesive layer or an adhesive layer, 27 is a resin layer, 28 is a hard coating layer, 21 to 23 and 29 do not exist, and the distance d (μm) between the adhesive layer 24 with scattering properties and the color filter is 700 μm or less. Since the distance d between the adhesive layer with light scattering properties and the color filter is 700 μm or less, even if a light scattering layer is stacked to suppress color shift and interference unevenness caused by the OLED display device 300, image blur is not likely to occur, and visual recognition is excellent. Figure 6 An OLED display device 400B of this embodiment is shown. Figure 644B to 48B are layers constituting the optical laminate 40B, 44B is an adhesive layer having light scattering properties, 44B is an adhesive layer having light scattering properties, 45B is a glass layer, 46B is an adhesive layer or a bonding agent layer, 47B is a resin layer, and 48B is a hard coating layer. 15B is disposed on the visual recognition side (on the Figure 6 The light scattering adhesive layer 44B is in direct contact with the color filter 15B, that is, the distance between the light scattering adhesive layer 44B and the color filter 15B is 0 μm, so that the color shift and interference unevenness caused by the OLED display device 400B can be most effectively suppressed.
[0402] It should be noted that in Figure 6 In the OLED display device 400B shown, an anti-reflection layer may be present on the visual recognition side of the hard coating layer 48B.
[0403] As another preferred embodiment of the present invention, Figure 2 In the OLED display panel 100, a color filter is arranged on the visual recognition side, 21 is an adhesive layer, 22 is a resin layer, 23 is a hard coating layer, 24 is an adhesive layer, 25 is a glass layer, 26 is an adhesive layer, 27 is a resin layer, 28 is a hard coating layer, and there is no anti-reflection layer 29. At least one of the adhesive layers 21, 24, and 26 is an adhesive layer with light scattering properties, and the distance d (μm) between the adhesive layer with light scattering properties and the color filter is 700 μm or less. Since the distance d between the adhesive layer with light scattering properties and the color filter is 700 μm or less, even if a light scattering layer is stacked to suppress color shift and interference unevenness caused by the OLED display device 300, image blur is not likely to occur, and visual recognition is excellent. From the perspective of more effectively reducing image blur in the OLED display device caused by the stacked light scattering layer, the distance between the adhesive layer with light scattering properties and the color filter is more preferably less than 600 μm, further preferably less than 500 μm, and most preferably the adhesive layer with light scattering properties is in direct contact with the color filter. Figure 7 7(a) and 7(b) respectively show OLED display devices 400C and 400D according to this embodiment. Figure 7 In (a), 41C to 48C are layers constituting the optical laminate 40C, 41C is an adhesive layer, 42C is a resin layer, 43C is a hard coating layer, 44C is an adhesive layer, 45C is a glass layer, 46C is an adhesive layer having light scattering properties, 47C is a resin layer, and 48C is a hard coating layer. 15C is disposed on the visual recognition side (on the Figure 7In the color filter (upper side in (a), the distance d (μm) between the adhesive layer 46D having light scattering properties and the color filter 15C is 700 μm or less. Figure 7 In (b), 41D to 48D are layers constituting the optical laminate 40D, 41D is an adhesive layer having light scattering properties, 42D is a resin layer, 43D is a hard coating layer, 44D is an adhesive layer, 45D is a glass layer, 46D is an adhesive layer, 47D is a resin layer, and 48D is a hard coating layer. 15D is disposed on the visual recognition side (on the Figure 7 The light scattering adhesive layer 41D is in direct contact with the color filter 15D, that is, the distance between the light scattering adhesive layer 41D and the color filter 15D is 0 μm, so that the color shift and interference unevenness caused by the OLED display device 400D can be most effectively suppressed.
[0404] It should be noted that in Figure 7 In the OLED display devices 400C and 400D shown in (a) and (b), an anti-reflection layer may be present on the visual recognition side of the hard coating layers 48C and 48D.
[0405] As another preferred embodiment of the present invention, Figure 2 In the embodiment, 26 is an adhesive layer or a bonding agent layer, 27 is a resin layer, 28 is an anti-glare layer, and 21 is not present. 25 and 29. Figure 8 An OLED display device 500A according to this embodiment is shown. Figure 8 56A to 58A are layers constituting the optical laminate 50A, 56A is a pressure-sensitive adhesive layer or an adhesive layer, 57A is a resin layer, and 58A is an anti-glare layer. Since the optical laminate 50A has the anti-glare layer 58A, the color shift and interference unevenness caused by the OLED display panel 100 can be suppressed, and the visual recognition of the OLED display device 500A is excellent.
[0406] It should be noted that in Figure 8 In the OLED display device 500A shown, an anti-reflection layer may be present on the visual recognition side of the anti-glare layer 58A.
[0407] As another preferred embodiment of the present invention, Figure 2 Among them, 24 is a binder layer or an adhesive layer, 25 is a glass layer, 26 is a binder layer or an adhesive layer, 27 is a resin layer, 28 is an anti-glare layer, and 21 to 23 and 29 do not exist. Fig. 9 An OLED display device 500B of this embodiment is shown. Fig. 954B to 58B are layers constituting the optical laminate 50B, 54B is a binder layer or an adhesive layer, 55B is a glass layer, 56B is a binder layer or an adhesive layer, 57B is a resin layer, and 58B is an anti-glare layer. Since the optical laminate 50B has the anti-glare layer 58B, the color shift and interference unevenness caused by the OLED display panel 100 can be suppressed, and the visual recognition of the OLED display device 500B is excellent.
[0408] It should be noted that in Fig. 9 In the OLED display device 500B shown, an anti-reflection layer may be present on the visual recognition side of the anti-glare layer 58B.
[0409] As another preferred embodiment of the present invention, Figure 2 21 is an adhesive layer, 22 is a resin layer, 23 is a hard coating layer, 24 is an adhesive layer, 25 is a glass layer, 26 is an adhesive layer, 27 is a resin layer, 28 is an anti-glare layer, and there is no anti-reflection layer 29. Fig.10 An OLED display device 500C of this embodiment is shown. Fig.10 51C to 58C are layers constituting the optical laminate 50C, 51C is an adhesive layer, 52C is a resin layer, 53C is a hard coating layer, 54C is an adhesive layer, 55C is a glass layer, 56C is an adhesive layer, 57C is a resin layer, and 58C is an anti-glare layer. Since the optical laminate 50C has the anti-glare layer 58C, the color shift and interference unevenness caused by the OLED display panel 100 can be suppressed, and the visual recognition of the OLED display device 500C is excellent.
[0410] It should be noted that in Fig.10 In the OLED display device 500C shown, an anti-reflection layer may be present on the visual recognition side of the anti-glare layer 58C.
[0411] As another preferred embodiment of the present invention, Figure 2 In the figure, 26 is a binder layer or an adhesive layer, 27 is a resin layer, 28 is a hard coating layer, an anti-reflection layer 29 is present, and 21 to 25 are not present. Fig.11 An OLED display device 600A of this embodiment is shown. Fig.11 61A to 69A are layers constituting the optical laminate 60A, 66 is a binder layer or an adhesive layer, 67A is a resin layer, 68A is a hard coating layer, and 69A is an anti-reflection layer. Since the optical laminate 60A has the anti-reflection layer 69A, the interference unevenness caused by the OLED display panel 100 can be suppressed, and the visual recognition of the OLED display device 600A is excellent.
[0412] exist Fig.11In the OLED display device 600A shown, 68A may be an anti-glare layer, or an anti-glare layer may be stacked between the hard coating layer 68A and the anti-reflection layer 69A. In this embodiment, the anti-reflection function is further improved by stacking the anti-glare layer 68A and the anti-reflection layer 69A.
[0413] As another preferred embodiment of the present invention, Figure 2 24 is a binder layer or an adhesive layer, 25 is a glass layer, 26 is a binder layer or an adhesive layer, 27 is a resin layer, 28 is a hard coating layer, an anti-reflection layer 29 is present, and 21 to 23 are not present. Fig.12 FIG. 6 shows an OLED display device 600B of this embodiment. Fig.12 61B to 69B are layers constituting the optical laminate 60B, 64B is a binder layer or an adhesive layer, 65B is a glass layer, 66B is a binder layer or an adhesive layer, 67B is a resin layer, 68B is a hard coating layer, and 69B is an anti-reflection layer. Since the optical laminate 60B has the anti-reflection layer 69B, the interference unevenness caused by the OLED display panel 100 can be suppressed, and the visual recognition of the OLED display device 600B is excellent.
[0414] exist Fig.12 In the OLED display device 600B shown, 68B may be an anti-glare layer, or an anti-glare layer may be stacked between the hard coating layer 68B and the anti-reflection layer 69B. In this embodiment, the anti-reflection function is further improved by stacking the anti-glare layer 68B and the anti-reflection layer 69B.
[0415] As another preferred embodiment of the present invention, Figure 2 In the figure, 21 is an adhesive layer, 22 is a resin layer, 23 is a hard coating layer, 24 is an adhesive layer, 25 is a glass layer, 26 is an adhesive layer, 27 is a resin layer, 28 is a hard coating layer, and an anti-reflection layer 29 is present. Fig.13 An OLED display device 600C according to this embodiment is shown. Fig.13 61C to 69C are layers constituting the optical laminate 60C, 61C is an adhesive layer, 62C is a resin layer, 63C is a hard coating layer, 64C is an adhesive layer, 65C is a glass layer, 66C is an adhesive layer, 67C is a resin layer, 68C is a hard coating layer, and 69C is an anti-reflection layer. Since the optical laminate 60C has the anti-reflection layer 69C, the interference unevenness caused by the OLED display panel 100 can be suppressed, and the visual recognition of the OLED display device 600C is excellent.
[0416] exist Fig.13In the OLED display device 600C shown, 68C may be an anti-glare layer, or an anti-glare layer may be stacked between the hard coat layer 68C and the anti-reflection layer 69C. In this embodiment, the anti-reflection function is further improved by stacking the anti-glare layer 68C and the anti-reflection layer 69C.
[0417] As another preferred embodiment of the present invention, Figure 2 In the figure, 21 is a pressure-sensitive adhesive layer or an adhesive layer, 22 is a resin layer, 23 and 24 are adhesive layers, 25 is a glass layer, and 26 to 29 are not present. Fig.14 FIG. 7 shows an OLED display device 700A according to this embodiment. Fig.14 In the figure, 71A, 72A, 74A and 75A are layers constituting the optical laminate 70A, 71A is a pressure-sensitive adhesive layer or an adhesive layer, 72A is a resin layer, 73A does not exist, 74A is an adhesive layer, and 75A is a glass layer. Fig.14 In the embodiment, the resin layer 72A and the glass layer 75A are bonded by the adhesive layer 74A, and excellent impact resistance is imparted to each of them even when the optical laminate 70A does not have a polarizing plate. In addition, the glass layer is a raw material that has excellent impact resistance but is easily broken and has low bendability. By bonding the glass layer and the resin layer with an adhesive layer, flexibility and bendability are improved, and the OLED display device 700A can be used for flexible devices and foldable devices.
[0418] As another preferred embodiment of the present invention, Figure 2 In the embodiment, 21 is an adhesive layer, 22 is a resin layer, 23 is absent, 24 is an adhesive layer, 25 is a glass layer, 26 is an adhesive layer, 27 is a resin layer, 28 is a hard coating layer, and an anti-reflection layer 29 is absent. Alternatively, Figure 2 21 is an adhesive layer, 22 is a resin layer, 23 is a hard coating layer, 24 is an adhesive layer, 25 is a glass layer, 26 is an adhesive layer, 27 is a resin layer, 28 is a hard coating layer, and there is no anti-reflection layer 29. Fig.15 (a) and Fig.15 (b) shows OLED display devices 700B and 700C of this embodiment. Fig.15 In (a), 71B, 72B, 74B to 78B are layers constituting the optical laminate 70B, 71B is a pressure-sensitive adhesive layer, 72B is a resin layer, 74B is an adhesive layer, 75B is a glass layer, 76B is a pressure-sensitive adhesive layer, 77B is a resin layer, and 78B is a hard coat layer. Fig.15 In (b), 71C to 78C are layers constituting the optical laminate 70C, 71C is an adhesive layer, 72C is a resin layer, 73C is a hard coat layer, 74C is an adhesive layer, 75C is a glass layer, 76C is an adhesive layer, 77C is a resin layer, and 78C is a hard coat layer. Fig.15In (a), the resin layer 72B and the glass layer 75B are bonded together by an adhesive layer 74B, or Fig.15 In (b), the glass layer 75C and the resin layer 77C are bonded by the adhesive layer 76C, thereby imparting excellent impact resistance even when the optical laminate 70B and 70C do not have a polarizing plate. In addition, the glass layer is a raw material that has excellent impact resistance but is easily broken and has low bendability. By bonding the glass layer and the resin layer with an adhesive layer, the flexibility and bendability are improved, and the OLED display devices 700B and 700C can be used for flexible devices and foldable devices.
[0419] It should be noted that in Fig.15 (a) and Fig.15 In the OLED display devices 700B and 700C shown in (b), an anti-reflection layer may be present on the visual recognition side of the hard coating layers 78B and 78C.
[0420] As another preferred embodiment of the present invention, Figure 2 In the figure, 21 is an adhesive layer, 22 is a resin layer, 23 is a hard coating layer, 24 to 29 are not present, and the resin layer 22 is a transparent polyimide layer. Fig.16 An OLED display device 800A according to this embodiment is shown. Fig.16 In the figure, 81A to 83A are layers constituting the optical laminate 80A, 81A is a pressure-sensitive adhesive layer or an adhesive layer, 82A is a transparent polyimide layer, and 83A is a hard coat layer. Fig.16 In the embodiment, the optical laminate 80A has a transparent polyimide layer 82A and a hard coating layer 83A, so that even if the optical laminate 80A does not have a polarizing plate, excellent impact resistance can be imparted. In addition, in the present embodiment, the optical laminate 80A does not have a glass layer. The glass layer is a raw material showing high hardness and excellent impact resistance, but has poor operability and is difficult to be used in large displays used in PCs, tablet computers, etc. By laminating a transparent polyimide layer and a hard coating layer, a high hardness equivalent to that of the glass layer can be achieved, and the operability is also excellent, so it can be used in large displays used in PCs, tablet computers, etc.
[0421] As another preferred embodiment of the present invention, Figure 2 In the figure, 21 is an adhesive layer, 22 is a resin layer, 23 is a hard coating layer, 24 is an adhesive layer, 25 and 26 do not exist, 27 is a resin layer, 28 is a hard coating layer, and there is no anti-reflection layer 29. Either or both of the resin layers 22 and 27 are transparent polyimide layers. Fig.17 FIG. 8 is an OLED display device 800B according to this embodiment. Fig.17Among them, 81B to 84B, 87B, and 88B are the layers that make up the optical laminate 80B. 81B is an adhesive layer, 82B is a transparent polyimide layer, 83B is a hard coat layer, 84B is an adhesive layer, 87B is a resin layer, and 88B is a hard coat layer. In Fig.17 Among them, since the optical laminate 80B has a transparent polyimide layer 82B and a hard coat layer 83B, excellent impact resistance can be imparted even when the optical laminate 80B does not have a polarizing plate. In addition, in the present embodiment, the optical laminate 80B does not have a glass layer. The glass layer is a raw material that exhibits high hardness and excellent impact resistance, but it has poor workability and is difficult to be used for large displays used in PCs, tablet computers, etc. By laminating a transparent polyimide layer and a hard coat layer, high hardness equivalent to that of the glass layer can be achieved, and the workability is also excellent. Therefore, it can be used for large displays used in PCs or tablet computers, etc.
[0422] In Fig.16 and Fig.17 In the illustrated embodiments, it is preferable that an intermediate layer (compatibilizing layer) (not shown) is formed between the transparent polyimide layer 82A and the hard coat layer 83A, and between the transparent polyimide layer 82B and the hard coat layer 83B. By forming an intermediate layer (compatibilizing layer) between the transparent polyimide layers 82A, 82B and the hard coat layers 83A, 83B, the adhesion between the transparent polyimide layers 82A, 82B and the hard coat layers 83A, 83B is improved. In this case, the shear fracture strength between the transparent polyimide layers 82A, 82B and the hard coat layers 83A, 83B is preferably 20 MPa or more.
[0423] Examples
[0424] Hereinafter, the present invention will be described in more detail with reference to examples, but the present invention is not limited by any of these examples.
[0425] Example 1
[0426] <OLED Display Device>
[0427] An OLED display device was prepared by peeling off the optical film laminated on the visual recognition side of a 4K OLED display (model: EPS269 Q015A) manufactured by OLED, Inc.
[0428] <Preparation of Coating Agent 1 for Hard Coat>
[0429] 100 parts by weight of a multifunctional acrylate (product name "Z-850-27ALL", manufactured by Aica Kogyo Co., Ltd.) as a base resin, 0.5 parts by weight of a leveling agent (trade name "GRANDIC PC-4100", manufactured by DIC Co., Ltd.), and 3.9 parts by weight of a photopolymerization initiator (trade name "omnirad907", manufactured by IGM Resins Italia Srl) were mixed and diluted with methyl isobutyl ketone so that the solid content concentration became 40% by weight, thereby preparing a coating agent 1 for a hard coat layer.
[0430] <Preparation of Hard Coat Layer Coating Agent 2>
[0431] 100 parts by weight of a multifunctional acrylate (product name "Z-850-16ALL", manufactured by Aica Kogyo Co., Ltd.) as a base resin, 0.15 parts by weight of a leveling agent (product name "KY-1203", manufactured by Shin-Etsu Chemical Co., Ltd.), and 3 parts by weight of a photopolymerization initiator (product name "omnirad127", manufactured by IGM Resins Italia Srl) were mixed and diluted with methyl isobutyl ketone so that the solid content concentration became 50% by weight, thereby preparing a coating agent 2 for a hard coat layer.
[0432] <Preparation of Base Film with Hard Coat Layer>
[0433] The coating agent 1 was applied to one side of a polyethylene terephthalate film (product name "DIAFOIL S100", manufactured by Mitsubishi Chemical Corporation, refractive index: 1.65) as a substrate film to form a coating layer, and the coating layer and the substrate film were heated at 120° C. for 1 minute. Then, a high-pressure mercury lamp was used to heat the film at a cumulative light intensity of 200 mJ / cm 2 The coating layer was irradiated with ultraviolet rays to form a hard coating layer 1. The thickness of the formed hard coating layer 1 was 5 μm. Next, the coating agent 2 was applied on the hard coating layer 1 to form a coating layer, and the coating layer and the substrate film were heated at 85° C. for 1 minute. Next, a high-pressure mercury lamp was used to irradiate the coating layer with a cumulative light intensity of 250 mJ / cm 2 The coating layer was irradiated with ultraviolet rays to form a hard coating layer 2. The thickness of the formed hard coating layer 2 was 5 μm. In this manner, a base film with a hard coating layer was produced.
[0434] <Preparation of Acrylic Polymer Solution>
[0435] In a four-necked flask equipped with a stirring blade, a thermometer, a nitrogen introduction tube and a condenser, 94.9 parts by weight of butyl acrylate (BA), 5 parts by weight of acrylic acid (AA), 0.1 parts by weight of 4-hydroxybutyl acrylate (4-HBA) and 0.1 parts by weight of 2,2'-azobisisobutyronitrile as a polymerization initiator (monomer concentration 50% by weight) were added together with 100 parts by weight of ethyl acetate, and nitrogen was introduced while slowly stirring to perform nitrogen replacement. Then, the liquid temperature in the flask was maintained at approximately 55° C. and a polymerization reaction was performed for 8 hours, thereby preparing a solution of an acrylic polymer having a weight average molecular weight (Mw) of 2.02 million and Mw / Mn=3.2.
[0436] <Preparation of Adhesive Composition>
[0437] With respect to 100 parts by weight of the solid content of the acrylic polymer solution, 0.6 parts by weight of an isocyanate crosslinking agent (trade name "CORONATEL", manufactured by Tosoh Corporation) and 29 parts by weight of silicone resin particles (trade name "Tospearl 145", manufactured by Momentive Advanced Materials Japan Co., Ltd., refractive index 1.43, volume average particle size 4 μm) as light scattering particles were added to prepare an adhesive composition (solid content 13.2% by weight).
[0438] <Production of Optical Laminated Body>
[0439] The pressure-sensitive adhesive composition was applied to the surface of the base film with a hard coat layer on which the hard coat layer was not laminated to form a pressure-sensitive adhesive layer in a thickness of 23 μm after drying, thereby producing an optical laminate.
[0440] <Production of OLED Display Device with Optical Laminate>
[0441] The optical layered body was laminated on the OLED display device so that the hard coat layer of the optical layered body faced the visual recognition side, thereby producing an OLED display device with an optical layered body.
[0442] Example 2
[0443] <Production of Optical Laminated Body>
[0444] An optical layered body was produced in the same manner as in Example 1 except that the amount of the silicone resin fine particles in the pressure-sensitive adhesive composition was 25.9 parts by weight.
[0445] <Production of OLED Display Device with Optical Laminate>
[0446] The optical laminate was laminated on an OLED display device in two layers with the hard coat layer of the optical laminate facing the viewing side and with a laminate of an acrylic pressure-sensitive adhesive layer and a polyethylene terephthalate film (laminate thickness: 100 μm) interposed therebetween, thereby producing an OLED display device with an optical laminate.
[0447] Example 3
[0448] An optical laminate and an OLED display device with an optical laminate were produced in the same manner as in Example 1 except that the amount of the silicone resin fine particles in the adhesive composition was 7.9 parts by weight and the adhesive layer was formed.
[0449] Example 4
[0450] The optical laminate produced in Example 1 was laminated on an OLED display device in two layers with a laminate of an acrylic pressure-sensitive adhesive layer and a polyethylene terephthalate film (laminate thickness 100 μm) interposed therebetween, so that the hard coat layer of the optical laminate was on the visual recognition side, thereby producing an OLED display device with an optical laminate.
[0451] Comparative Example 1
[0452] An optical laminate and an OLED display device with the optical laminate were produced in the same manner as in Example 1, except that the light scattering fine particles were not blended into the adhesive composition and the adhesive layer was formed.
[0453] Comparative Example 2
[0454] The optical laminate produced in Example 2 was laminated on an OLED display device with five layers of a laminate of an acrylic pressure-sensitive adhesive layer and a polyethylene terephthalate film (thickness 100 μm) interposed therebetween so that the hard coat layer of the optical laminate was on the visual recognition side, thereby producing an OLED display device with an optical laminate.
[0455] <Evaluation>
[0456] The pressure-sensitive adhesive layers, optical laminates, and OLED display devices with optical laminates obtained in Examples and Comparative Examples were evaluated as follows.
[0457] (1) Distance between color filter and optical layer (d)
[0458] The thickness of the glass stacked on the color filter of the OLED display device was measured using a scanning electron microscope (SEM) and was calculated to be 500 μm. Therefore, 500 μm was added to the thickness of the stack (a stack of an acrylic adhesive layer and a polyethylene terephthalate film (thickness 100 μm)) stacked between the optical stack and the OLED display device to calculate the distance (d) between the color filter and the optical stack.
[0459] (2) Haze value
[0460] The pressure-sensitive adhesive layers produced in Examples and Comparative Examples were measured by the method specified in JIS K7136 using a haze meter (trade name "HN-150", manufactured by Murakami Color Science Laboratory Co., Ltd.).
[0461] (3) Color shift
[0462] The OLED display device with the optical laminate obtained in the examples and comparative examples was made to display a white screen, and the chromaticity x and y at azimuth angles of 0° to 360° were measured at every 1° under the condition of a polar angle of 70° using a luminance meter (trade name "Conoscope", manufactured by AUTRONIC-MELCHERS). The chromaticity at each angle was defined as x. deg ,y deg When the chromaticity change parameter at each angle is calculated, Δx = (0.32-x deg ), Δy=(0.34-y deg ). In addition, when the sum of the chromaticity parameters Δx and Δy at the polar angle of 70° and the azimuth angle of 0° to 360° are respectively set to SUMΔx and SUMΔy, {(SUMΔx) 2 +(SUMΔy) 2} (1 / 2) As a color shift.
[0463] (4) Uneven interference
[0464] The OLED display device with an optical laminate obtained in the examples and comparative examples was set to a non-lighting state. When a three-wavelength fluorescent lamp was lit at a distance of 30 cm from the OLED display device with an optical laminate, the interference unevenness on the surface of the OLED display device with an optical laminate was visually observed and judged according to the following criteria.
[0465] ◎: No visual interference unevenness
[0466] ○: Interference unevenness is barely perceptible
[0467] ×: Interference unevenness can be clearly visually recognized
[0468] (5) Image blur
[0469] A laptop personal computer was connected to the OLED display device with an optical laminate obtained in the embodiment and the comparative example via an HDMI terminal, text with a font size of 5 was displayed on PowerPoint, and the text on the surface of the OLED display device with the optical laminate was visually observed to be blurred, and the judgment was made according to the following criteria.
[0470] ◎: No visual blur at all
[0471] 0: Almost no visual blur
[0472] △: The image is slightly blurred.
[0473] ×: The image is clearly visible but blurry
[0474]
[0475] Modifications of the invention disclosed herein will be described below.
[0476] [Supplementary Note 1] An optical laminate for an OLED display device, wherein the optical laminate for an OLED display device is used for an OLED display device in which only an optical element with a polarization degree of 95% or less is laminated on a visual recognition side of the OLED element, the OLED display device is provided with a color filter on the visual recognition side of the OLED element, only the optical element is laminated on the visual recognition side of the color filter, the optical element has at least an adhesive layer, at least one layer of the adhesive layer has a light scattering property, and the distance between the adhesive layer with the light scattering property and the color filter is 700 μm or less.
[0477] [Note 2] According to the optical laminate for an OLED display device described in Note 1, when the distance between the adhesive layer having light scattering properties and the color filter is set to d [μm] and the haze value of the adhesive layer having light scattering properties is set to H [%], the value of d×H is less than 70,000 and H is greater than 20.
[0478] [Note 3] An optical laminate for an OLED display device according to Note 1 or 2, wherein when the thickness of the adhesive layer having light scattering properties is set to T [μm] and the haze value of the adhesive layer having light scattering properties is set to H [%], the value of T×H is greater than 400.
[0479] [Note 4] An optical laminate for an OLED display device according to any one of Notes 1 to 3, wherein the adhesive layer having light scattering properties contains light scattering particles dispersed in the adhesive layer, and the volume average particle size of the light scattering particles is 1 μm to 5 μm.
[0480] [Supplementary Note 5] The optical laminate for an OLED display device according to any one of Supplementary Notes 1 to 4, further comprising a hard coating layer having a thickness of 2 μm to 20 μm as the optical element.
[0481] [Supplementary Note 6] The optical laminate for an OLED display device as described in Supplementary Note 5, wherein the water contact angle of the hard coat layer is 100° or more.
[0482] [Supplementary Note 7] The optical laminate for an OLED display device according to Supplementary Note 5 or 6, wherein the water contact angle of the hard coat layer after a steel wool test is 95° or more.
[0483] Description of symbols
[0484] 100 OLED display panel
[0485] 10R red OLED layer
[0486] 10G green OLED layer
[0487] 10B blue OLED layer
[0488] 11a Transparent electrode (cathode)
[0489] 11b Back electrode (anode)
[0490] 12R red OLED element
[0491] 12G Green OLED Component
[0492] 12B blue OLED element
[0493] 13 substrates
[0494] 14 TFT layer
[0495] 15 color filters
[0496] 15R red coloring layer
[0497] 15G green coloring layer
[0498] 15B blue coloring layer
[0499] 16 Black matrix layer
[0500] W external light
[0501] GReflected light
[0502] C1 first light path (direct light)
[0503] C2 second optical path (reflected light)
[0504] 17 Bonding layer
[0505] 200 OLED display device
[0506] 20 optical laminate
[0507] 21 Adhesive layer or adhesive layer
[0508] 22 resin layer, glass layer or impact absorbing layer
[0509] 23Hard coating or anti-glare layer
[0510] 24 Adhesive layer or adhesive layer
[0511] 25 resin layer, glass layer or impact absorbing layer
[0512] 26 Adhesive layer or adhesive layer
[0513] 27 resin layer, glass layer or impact absorbing layer
[0514] 28Hard coating or anti-glare layer
[0515] 29 Anti-reflection layer
[0516] 300A OLED display device
[0517] 30A optical laminate
[0518] 34A Adhesive layer or adhesive layer
[0519] 35A glass layer
[0520] 36A Adhesive layer having light scattering properties
[0521] 37A resin layer
[0522] 38A hard coating
[0523] 300B OLED display device
[0524] 30B optical laminate
[0525] 31B Adhesive layer
[0526] 32B resin layer
[0527] 33B hard coating
[0528] 34B adhesive layer
[0529] 35B glass layer
[0530] 36B Adhesive layer with light scattering properties
[0531] 37B resin layer
[0532] 38B hard coating
[0533] 400A OLED display device
[0534] 40A optical laminate
[0535] 46A Adhesive layer having light scattering properties
[0536] 47A resin layer
[0537] 48A hard coating
[0538] 15A color filter
[0539] 400B OLED display device
[0540] 40B optical laminate
[0541] 44B Adhesive layer with light scattering properties
[0542] 45B glass layer
[0543] 46B Adhesive layer
[0544] 47B resin layer
[0545] 48B hard coating
[0546] 15B color filter
[0547] 400C OLED display device
[0548] 40C optical laminate
[0549] 41C Adhesive layer
[0550] 42C resin layer
[0551] 43C hard coating
[0552] 44C adhesive layer
[0553] 45C glass layer
[0554] 46C Adhesive layer with light scattering properties
[0555] 47C resin layer
[0556] 48C hard coating
[0557] 15C color filter
[0558] 400D OLED display device
[0559] 40D optical laminate
[0560] 41D Adhesive layer with light scattering properties
[0561] 42D resin layer
[0562] 43D hard coating
[0563] 44D adhesive layer
[0564] 45D glass layer
[0565] 46D adhesive layer
[0566] 47D resin layer
[0567] 48D hard coating
[0568] 15D color filter
[0569] 500A OLED display device
[0570] 50A optical laminate
[0571] 56A Adhesive layer or adhesive layer
[0572] 57A resin layer
[0573] 58A anti-glare layer
[0574] 500B OLED display device
[0575] 50B optical laminate
[0576] 54B Adhesive layer or adhesive layer
[0577] 55B glass layer
[0578] 56B Adhesive layer or adhesive layer
[0579] 57B resin layer
[0580] 58B anti-glare layer
[0581] 500C OLED display device
[0582] 50C optical laminate
[0583] 51C Adhesive layer
[0584] 52C resin layer
[0585] 53C hard coating
[0586] 54C adhesive layer
[0587] 55C glass layer
[0588] 56C adhesive layer
[0589] 57C resin layer
[0590] 58C anti-glare layer
[0591] 600A OLED display device
[0592] 60A optical laminate
[0593] 66A Adhesive layer or adhesive layer
[0594] 67A resin layer
[0595] 68A hard coating
[0596] 69A anti-reflection layer
[0597] 600B OLED display device
[0598] 60B optical laminate
[0599] 64B Adhesive layer or adhesive layer
[0600] 65B glass layer
[0601] 66B Adhesive layer or adhesive layer
[0602] 67B resin layer
[0603] 68B hard coating
[0604] 69B anti-reflection layer
[0605] 600C OLED display device
[0606] 60C optical laminate
[0607] 61C Adhesive layer
[0608] 62C resin layer
[0609] 63C hard coating
[0610] 64C adhesive layer
[0611] 65C glass layer
[0612] 66C Adhesive layer
[0613] 67C resin layer
[0614] 68C hard coating
[0615] 69C anti-reflection layer
[0616] 700A OLED display device
[0617] 70A optical laminate
[0618] 71A Adhesive layer
[0619] 72A resin layer
[0620] 74A adhesive layer
[0621] 75A glass layer
[0622] 700B OLED display device
[0623] 70B optical laminate
[0624] 71B Adhesive layer
[0625] 72B resin layer
[0626] 74B adhesive layer
[0627] 75B glass layer
[0628] 76B adhesive layer
[0629] 77B resin layer
[0630] 78B hard coating
[0631] 700C OLED display device
[0632] 70C optical laminate
[0633] 71C Adhesive layer
[0634] 72C resin layer
[0635] 73C hard coating
[0636] 74C Adhesive layer
[0637] 75C glass layer
[0638] 76C adhesive layer
[0639] 77C resin layer
[0640] 78C hard coating
[0641] 800A OLED display device
[0642] 80A optical laminate
[0643] 81A Adhesive layer
[0644] 82A transparent polyimide layer
[0645] 83A hard coating
[0646] 800B OLED display device
[0647] 80B optical laminate
[0648] 81B Adhesive layer
[0649] 82B transparent polyimide layer
[0650] 83B hard coating
[0651] 84B adhesive layer
[0652] 87B resin layer
[0653] 88B hard coating
Claims
1. An optical laminate for an OLED display device, wherein: The optical laminate for an OLED display device is used for an OLED display device in which only an optical element having a polarization degree of 95% or less is laminated on the visual recognition side of an OLED element. The OLED display device is provided with a color filter on the visual recognition side of the OLED element. Only the optical element is stacked on the visual recognition side of the color filter, The optical element has at least an adhesive layer, At least one of the adhesive layers has light scattering properties, The distance between the adhesive layer having light scattering properties and the color filter is 700 μm or less.
2. The optical laminate for an OLED display device according to claim 1, wherein: When the distance between the adhesive layer having light scattering properties and the color filter is d [μm], and the haze value of the adhesive layer having light scattering properties is H [%], The value of d×H is 70,000 or less and H is 20 or more.
3. The optical laminate for an OLED display device according to claim 1 or 2, wherein: When the thickness of the pressure-sensitive adhesive layer having light scattering properties is T [μm] and the haze value of the pressure-sensitive adhesive layer having light scattering properties is H [%], The value of T×H is 400 or more.
4. The optical laminate for an OLED display device according to claim 1 or 2, wherein: The adhesive layer having light scattering properties includes light scattering fine particles dispersed in the adhesive layer, and the volume average particle size of the light scattering fine particles is 1 μm to 5 μm.
5. The optical laminate for an OLED display device according to claim 1 or 2, wherein: The optical laminate for an OLED display device further includes a hard coating layer having a thickness of 2 μm to 20 μm as the optical element.
6. The optical laminate for an OLED display device according to claim 5, wherein: The water contact angle of the hard coating layer is 100° or more.
7. The optical laminate for an OLED display device according to claim 5, wherein: The water contact angle of the hard coating layer after the steel wool test is 95° or more.
Citation Information
Patent Citations
Acrylic adhesives and its production method
JP2002069411A
Electroluminescence element
JP2003332068A
Cured coating film, Anti-reflection hard coating film using it, polarization plate and image display device
JP2008088309A
Organic electroluminescence display device
JP2015207377A
Color filter and display
JP2018112715A