Dispersing agent, preparation method and application thereof, and nanometer silicon particle dispersion liquid

Through the design and preparation of block polyether dispersants, the problem of easy foaming and poor dispersion effect of nano-silicon particle dispersants is solved, and a stable nano-silicon particle dispersion liquid is achieved, which significantly improves the dispersion performance and stability.

CN118894764APending Publication Date: 2024-11-05CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310501017.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-05
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

In the prior art, nano-silicon particle dispersant is prone to foaming and has poor dispersion effect, which fails to effectively solve the problems of silicon surface properties and dispersant screening, resulting in unsatisfactory dispersion and stability effects.

Method used

Provide a block polyether dispersant, through the sequential polymerization of ethylene oxide and propylene oxide, to form a molecular structure with steric hindrance effect, reduce surface tension, improve defoaming effect, and promote polymerization reaction through catalysts, prepare Dispersants with low surface energy and low foaming are produced.

Benefits of technology

The stable dispersion of nano-silicon particles was achieved, and the dispersion liquid did not accumulate within 1-6 months, which significantly improved the stability and dispersion performance of the dispersant, reduced the surface tension, and enhanced the wetting effect on nano-silicon particles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118894764A_ABST
    Figure CN118894764A_ABST
Patent Text Reader

Abstract

The invention relates to the field of dispersants, and discloses a dispersant, a preparation method and application thereof, and a nanometer silicon particle dispersion liquid, the dispersant has a structure represented by a formula (1): # imgabs0 #, the ratio of m to n is 0.3-3: 1, and the weight-average molecular weight of the dispersant does not exceed 2000 g / mol; r has a structure as shown in a formula (2), R1 is alkylene of C1-C10, and R2, R3 and R4 are respectively and independently selected from alkyl of C1-C3. The dispersing agent provided by the invention is easy to defoam and is also beneficial to dispersion of nano silicon, and the prepared nano silicon particle dispersion liquid is good in stability and can be stably stored for 1-6 months without aggregation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of dispersants, and in particular to a dispersant and a preparation method and application thereof, and a nano silicon particle dispersion. Background Art

[0002] Elemental silicon has high theoretical specific capacity, good safety performance, abundant reserves and high cost performance. Therefore, it has received extensive attention and research from academia and industry in recent years and is considered to be the first choice for the next generation of ideal negative electrode materials. However, the huge volume change of silicon during the charging and discharging process also brings about problems such as material pulverization, conductive network fragmentation, rapid battery capacity decay and even battery failure. Studies have shown that nano-scaling of silicon can alleviate the volume expansion effect, shorten the ion diffusion distance, improve the electrochemical cycle performance of silicon-based negative electrodes, and improve the cycle life and stability of batteries.

[0003] Nanoparticles usually have high surface energy and are easy to spontaneously agglomerate to form large particles, thereby reducing energy and returning to a low-energy stable state. Agglomerated nanoparticles are not easy to disperse evenly in the solvent, making it difficult for the material to perform as expected. Generally, surfactants are added to nanoparticles during synthesis to improve the stability of the nanoparticle dispersion system. Common nanoparticle stabilizers mainly include carboxylic acids, polyethers, and amides. These surfactants generally disperse nanoparticles together through the synergistic effect of chelation-steric hindrance.

[0004] CN110289400A discloses the use of ball milling to grind micron silicon particles into nano silicon particles, and adds hexadecyl trimethyl ammonium bromide ion dispersant during the grinding process, so that the dispersant is adsorbed on the surface of the nano silicon particles to improve the dispersibility of the silicon grinding liquid. CN1544335A discloses adding different anionic dispersants to titanium dioxide dispersion liquid, and all of them have achieved certain dispersing effects. However, the above methods all directly use common dispersants on the market, and fail to further study the surface properties of the solute to be dispersed and the screening of the dispersant, resulting in much foaming, and the dispersion and stabilization effects achieved are not very ideal.

[0005] The existing technology still lacks dispersants that can efficiently disperse nano-silicon particles. Therefore, it is crucial to prepare stable nano-silicon dispersions by obtaining low surface energy and low foaming dispersants through structural design under the premise of comprehensively considering the surface properties of the dispersion medium and the solvent system in which it is located. Summary of the invention

[0006] The purpose of the present invention is to overcome the problems of the prior art that the dispersant is easy to foam and has a poor dispersing effect on nano silicon particles, and to provide a dispersant and its preparation method and application, a nano silicon particle dispersion liquid, which has a good wetting effect on the silicon surface, is easy to defoam, and is conducive to the dispersion of nano silicon particles.

[0007] In order to achieve the above object, the first aspect of the present invention provides a dispersant having a structure shown in formula (1):

[0008]

[0009] wherein the ratio of m to n is 0.3-3:1; the weight average molecular weight of the dispersant does not exceed 2000 g / mol;

[0010] R has a structure as shown in formula (2),

[0011]

[0012] Wherein, R1 is a C1-C10 alkylene group, and R2, R3, and R4 are each independently selected from a C1-C3 alkyl group.

[0013] Preferably, R is selected from -CH2CH2CH(CH3)CH2C(CH3)2CH3, -C(CH3)2C(CH3)2CH3, -CH2CH(CH3)2CH3, -CH2CH2C(CH3)2CH3, -C(CH2CH3)(CH2CH2CH3)CH3 or -C(CH3)2CH2CH3; preferably -CH2CH2CH(CH3)CH2C(CH3)2CH3 or -C(CH3)2C(CH3)2CH3.

[0014] A second aspect of the present invention provides a method for preparing a dispersant, comprising the following steps:

[0015] (1) contacting an initiator and ethylene oxide in the presence of a catalyst under first polymerization reaction conditions to carry out a first polymerization reaction;

[0016] Wherein, the molar ratio of ethylene oxide to initiator is 30-200:1, and the molar ratio of ethylene oxide to propylene oxide is 0.3-3:1;

[0017] (2) subjecting the product obtained from the first polymerization reaction to a second polymerization reaction with propylene oxide under second polymerization reaction conditions;

[0018] The initiator has a structure shown in formula (3),

[0019]

[0020] Wherein, R1 is a C1-C10 alkylene group, and R2, R3, and R4 are each independently selected from a C1-C3 alkyl group.

[0021] The third aspect of the present invention provides use of the dispersant described in the first aspect or the dispersant prepared by the preparation method described in the second aspect in dispersing nano-silicon particles.

[0022] A fourth aspect of the present invention provides a nano-silicon particle dispersion, the nano-silicon particle dispersion comprising a dispersion and nano-silicon particles;

[0023] The dispersion comprises a solvent and the dispersant described in the first aspect or the dispersant prepared by the preparation method described in the second aspect.

[0024] Preferably, the mass ratio of the nano silicon particles to the dispersion is 1:10-100.

[0025] Through the above technical solution, the beneficial effects obtained by the present invention are as follows:

[0026] The dispersant provided by the present invention has a branched alkyl group at one end of the molecular chain and a propylene oxide structural unit as an end cap. The steric hindrance effect is achieved through the synergistic effect of the end capping. The molar ratio of ethylene oxide to propylene oxide structural units in the molecule, the molecular weight and the polymer structure are further regulated to make the dispersant easy to defoam and also conducive to the dispersion of nano silicon.

[0027] The preparation method of the dispersant provided by the invention uses a branched alcohol with a large steric hindrance effect as an initiator, and obtains a block polyether dispersant with the above structure by sequentially polymerizing ethylene oxide and propylene oxide. The process conditions are simple and large-scale production is easy.

[0028] The nano silicon particle dispersion provided by the invention has good stability and can be stably stored for 1 to 6 months without aggregation. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 is the hydrogen nuclear magnetic resonance spectrum of dispersant A1 in Example 1;

[0030] Figure 2 is the carbon NMR spectrum of dispersant A1 in Example 1;

[0031] Figure 3 is the NMR HMBC two-dimensional carbon-hydrogen correlation spectrum of the dispersant A1 in Example 1;

[0032] Figure 4 is the mass spectrometry total particle flow diagram of dispersant A1 in Example 1;

[0033] Figure 5 is a static surface tension diagram of an aqueous solution of dispersant A1 with a mass fraction of 0.1% in Example 1;

[0034] Figure 6 This is a dynamic surface tension diagram of an aqueous solution of dispersant A1 with a mass fraction of 0.1% in Example 1. DETAILED DESCRIPTION

[0035] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0036] The first aspect of the present invention provides a dispersant having a structure shown in formula (1):

[0037]

[0038] wherein the ratio of m to n is 0.3-3:1; the weight average molecular weight of the dispersant does not exceed 2000 g / mol;

[0039] R has a structure as shown in formula (2),

[0040]

[0041] Wherein, R1 is a C1-C10 alkylene group, and R2, R3, and R4 are each independently selected from a C1-C3 alkyl group.

[0042] In the dispersant provided by the present invention, RO- is the starting terminal group brought into the polymer structure by the polyether initiator, which connects the ethylene oxide block and the propylene oxide block in sequence, and the other end of the polymer main chain is capped with the propylene oxide block and the terminal is a hydroxyl group. Through the synergistic effect of the capping groups at both ends of the copolymer main chain, the defoaming effect can be improved while reducing the surface tension.

[0043] In the present invention, the structure of the copolymer can be confirmed by nuclear magnetic resonance analysis. In the nuclear magnetic resonance HMBC two-dimensional carbon-hydrogen correlation spectrum of the dispersant, there are three carbon signals related to the hydrogen of the terminal hydroxyl group, that is, there are three spatially adjacent carbons near the hydroxyl group, proving that the terminal hydroxyl group comes from the propylene oxide block.

[0044] According to the present invention, R1 is a C1-C10 alkylene group, wherein the alkylene group may be a linear or branched alkylene group, preferably, R1 is selected from -(CH2) x1 -、-CH2-CH(CH3)-(CH2) x2 -、-CH2-C(CH3)2-(CH2) x3 -、-CH(CH3)-(CH2) x4 -、-C(CH3)2-(CH2) x5 -、-C(CH3)(CH2CH3)-(CH2) x6-or-C(CH3)(C3H7)-(CH2) x7 -, wherein x1-x7 are each independently selected from 0, 1, 2, 3 or 4;

[0045] In the present invention, R2, R3, and R4 are each independently selected from C1-C3 alkyl groups, wherein the alkyl group may be a straight chain or branched chain alkyl group, including but not limited to methyl, ethyl, n-propyl, or isopropyl, and more preferably, R2, R3, and R4 are all methyl groups. The above preferred structural composition is conducive to accelerating the disappearance of the foam.

[0046] According to the present invention, preferably, R is selected from -CH2CH2CH(CH3)CH2C(CH3)2CH3, -C(CH3)2C(CH3)2CH3, -CH2CH(CH3)2CH3, -CH2CH2C(CH3)2CH3, -C(CH2CH3)(CH2CH2CH3)CH3 or -C(CH3)2CH2CH3; preferably -CH2CH2CH(CH3)CH2C(CH3)2CH3 or -C(CH3)2C(CH3)2CH3.

[0047] In the present invention, preferably, the ratio of m to n is 0.5-2:1.

[0048] Preferably, m is 1-14, preferably 3-9; n is 1-14, preferably 3-9. Within the above preferred degree of polymerization range, it is beneficial to reduce surface tension and easier to defoam.

[0049] In the present invention, the degree of polymerization is obtained by nuclear magnetic resonance analysis.

[0050] According to the present invention, in order to improve the dispersing effect of the dispersant, the weight average molecular weight of the dispersant is no more than 2000g / mol, preferably 450-1500g / mol, for example, it can be 450g / mol, 500g / mol, 550g / mol, 600g / mol, 650g / mol, 700g / mol, 750g / mol, 800g / mol, 850g / mol, 900g / mol, 950g / mol, 1000g / mol, 1100g / mol, 1200g / mol, 1300g / mol, 1400g / mol, 1500g / mol or a value between two points. Within the above preferred molecular weight range, it is beneficial to reduce the viscosity of the dispersant and improve the dispersibility.

[0051] In the present invention, the molecular weight is obtained by gas chromatography-mass spectrometry analysis.

[0052] In the present invention, the effect of reducing the surface tension of the dispersant can be determined by the surface tension of the aqueous solution of the dispersant. Preferably, the dispersant is mixed with water to obtain an aqueous solution of the dispersant, the mass concentration of the dispersant is 0.1%, and the static surface tension of the aqueous solution of the dispersant is 23-40mN / m, preferably 25-30mN / m.

[0053] Preferably, the dispersant is mixed with water to obtain an aqueous solution of the dispersant, the mass concentration of the dispersant is 0.1%, and the dynamic surface tension of the aqueous solution of the dispersant is 25-42 mN / m, preferably 25-30 mN / m.

[0054] In the present invention, the static surface tension is obtained by testing with a static surface tension meter, and the dynamic surface tension is obtained by testing with a dynamic surface tension meter.

[0055] In the present invention, the wettability of the dispersant for silicon nanoparticles can be determined by the contact angle of the dispersant dispersed on the solid silicon wafer. Preferably, the contact angle of the dispersant on the solid silicon wafer is less than 80°, preferably 20-50°. Wherein, the solid silicon wafer is a commercial single crystal silicon wafer, and the contact angle is tested by a contact angle meter.

[0056] A second aspect of the present invention provides a method for preparing a dispersant, comprising the following steps:

[0057] (1) contacting an initiator and ethylene oxide in the presence of a catalyst under first polymerization reaction conditions to carry out a first polymerization reaction;

[0058] (2) subjecting the product obtained from the first polymerization reaction to a second polymerization reaction with propylene oxide under second polymerization reaction conditions;

[0059] Wherein, the molar ratio of ethylene oxide to initiator is 30-200:1, and the molar ratio of ethylene oxide to propylene oxide is 0.3-3:1;

[0060] The initiator has a structure shown in formula (3),

[0061]

[0062] Wherein, R1 is a C1-C10 alkylene group, and R2, R3, and R4 are each independently selected from a C1-C3 alkyl group.

[0063] The preparation method provided by the present invention obtains a block polyether dispersant by sequentially polymerizing ethylene oxide and propylene oxide. The obtained dispersant has the characteristics of low surface energy, low foaming and low toxicity, and has a good promoting effect on the wetting of nano silicon particles and dispersion medium.

[0064] It should be noted that in the preparation method of the present invention, step (1) and step (2) are carried out in sequence, and the order of the first polymerization reaction and the second polymerization reaction has a significant effect on the product structure and performance. In the first polymerization reaction, ethylene oxide can be ring-opened and polymerized with an initiator to obtain a first block copolymer containing an ethylene oxide block, and then the first block copolymer is subjected to a second polymerization reaction with propylene oxide. The obtained dispersant has a block polyether structure as shown in formula (1).

[0065] According to the present invention, R1 is a C1-C10 alkylene group, wherein the alkylene group may be a linear or branched alkylene group, preferably selected from -(CH2) x1 -、-CH2-CH(CH3)-(CH2) x2 -、-CH2-C(CH3)2-(CH2) x3 -、-CH(CH3)-(CH2) x4 -、-C(CH3)2-(CH2) x5 -、-C(CH3)(CH2CH3)-(CH2) x6 -or-C(CH3)(C3H7)-(CH2) x7 -, wherein x1-x7 are each independently selected from 0, 1, 2, 3 or 4.

[0066] In the present invention, R2, R3, and R4 are each independently selected from a C1-C3 alkyl group, wherein the alkyl group may be a linear or branched alkyl group, including but not limited to a methyl group, an ethyl group, a n-propyl group, or an isopropyl group. More preferably, R2, R3, and R4 are methyl groups.

[0067] According to the present invention, the above preferred structural composition of the dispersant is conducive to reducing surface tension and accelerating the disappearance of foam.

[0068] According to the present invention, preferably, the initiator is selected from at least one of 3,5,5-trimethyl-1-hexanol, 2,3,3-trimethyl-2-butanol, 2,2-dimethyl-1-propanol, 3,3-dimethyl-1-butanol, 2,3-dimethyl-3-pentanol, and 2-methyl-2-butanol, preferably 3,5,5-trimethyl-1-hexanol and / or 2,3,3-trimethyl-2-butanol.

[0069] According to the present invention, preferably, the molar ratio of ethylene oxide to the initiator is 50-150:1, for example, it can be 50:1, 60:1, 70:1, 80:1, 90:1, 100:1, 110:1, 120:1, 130:1, 140:1, 150:1, etc. Typical but non-limiting ratios. The molar ratio of ethylene oxide to the initiator is within the above preferred range, which is conducive to obtaining ethylene oxide with a moderate degree of polymerization and improving the dispersing effect of the dispersant.

[0070] Preferably, the molar ratio of ethylene oxide to propylene oxide is 0.5-2: 1. It is understood that the amount of each component is sufficient to obtain a dispersant having the required structural unit composition.

[0071] In the present invention, the catalyst has a wide range of choices, as long as it can catalyze the ring-opening polymerization of ethylene oxide and propylene oxide, and can be selected from conventional alkali metal or alkaline earth metal catalysts in the art, which are well known to those skilled in the art. Preferably, the catalyst is selected from at least one of potassium hydroxide, sodium hydroxide, barium hydroxide and calcium acetate, preferably potassium hydroxide and / or sodium hydroxide. The use of the above preferred catalyst is conducive to reducing production costs.

[0072] Preferably, the amount of catalyst used is 2-6 wt %, preferably 2.5-4 wt %, based on the total amount of ethylene oxide and propylene oxide used.

[0073] In the present invention, preferably, the first polymerization reaction conditions include: reaction temperature of 110-160°C, preferably 120-150°C; reaction pressure of 0-0.4 MPa, preferably 0.2-0.4 MPa; reaction time of 10-60 min, preferably 30-40 min.

[0074] Preferably, the second polymerization reaction conditions include: reaction temperature of 110-160° C., preferably 130-150° C.; reaction pressure of 0-0.4 MPa, preferably 0.2-0.4 MPa; reaction time of 10-60 min, preferably 20-30 min.

[0075] In the present invention, it can be understood that during the first polymerization or the second polymerization reaction, as the reaction proceeds, the pressure in the reaction system gradually decreases, and due to the exothermic reaction, the temperature in the reaction system increases, as long as the pressure and temperature during the reaction meet the above-mentioned pressure and temperature ranges.

[0076] In the present invention, the first polymerization reaction and the second polymerization reaction can be carried out in conventional operation modes and reactors in the art, and the present invention has no special limitation on this. Preferably, the first polymerization reaction and the second polymerization reaction are carried out in a high temperature and high pressure reactor.

[0077] According to the present invention, preferably, the first polymerization reaction method includes: firstly putting the catalyst and the initiator into the reactor, deoxygenating and evacuating, then adjusting to the first polymerization reaction conditions, and then adding ethylene oxide to carry out the first polymerization reaction.

[0078] Preferably, the deoxygenation operation can be performed in a conventional manner in the art, for example, introducing an inert gas into the reactor for replacement. Preferably, the inert gas is nitrogen.

[0079] In the present invention, the deoxygenation and vacuuming steps can be optionally repeated. Preferably, the deoxygenation and vacuuming steps are repeated at least twice.

[0080] Preferably, the first polymerization reaction and the second polymerization reaction are each independently carried out under stirring conditions, and the stirring rate is each independently 1500-3000 rpm, preferably 1800-2500 rpm.

[0081] Preferably, the preparation method further comprises: removing impurities, neutralizing, adsorbing and filtering the product of the second polymerization reaction in sequence to obtain the dispersant. The removal of impurities, neutralization, adsorption and filtration can be performed by conventional operations in the art, and the present invention has no special requirements for this. For example, unreacted monomers and small molecules in the system can be removed by vacuuming.

[0082] The third aspect of the present invention provides use of the dispersant described in the first aspect or the dispersant prepared by the preparation method described in the second aspect in dispersing nano-silicon particles.

[0083] A fourth aspect of the present invention provides a nano-silicon particle dispersion, the nano-silicon particle dispersion comprising a dispersion and nano-silicon particles;

[0084] The dispersion comprises a solvent and the dispersant described in the first aspect or the dispersant prepared by the preparation method described in the second aspect.

[0085] Preferably, in the dispersion, the concentration of the dispersant is 0.05-0.2 wt %.

[0086] Preferably, the solvent is water.

[0087] Preferably, the particle size of the nano-silicon particles is 200-3000 nm, preferably 300-800 nm.

[0088] The nano silicon particles can be silicon powder, and the diameter of the silicon powder is the particle size of the nano silicon particles.

[0089] Preferably, the mass ratio of the nano silicon particles to the dispersion is 1:10-100, preferably 1:20-80.

[0090] The present invention will be described in detail below through examples.

[0091] The static surface tension is obtained by testing with a static surface tension meter, and the dynamic surface tension is obtained by testing with a dynamic surface tension meter.

[0092] The molecular weight of the dispersant was tested by gas chromatography-mass spectrometry. Test conditions: HP-5MS column, column temperature 50(5)-10-300(20), injection volume 1μL, split ratio 50:1, injection port temperature 300℃, carrier gas flow rate 1mL / min, and the mass spectrometry total particle flow of the standard sample was collected as a reference.

[0093] Example 1

[0094] (1) Add 1g of 3,5,5-trimethyl-1-hexanol and 2g of potassium hydroxide to a high-temperature and high-pressure reactor, and seal the reactor. Before heating, purge and replace with nitrogen, then evacuate, and purge and replace with nitrogen and then evacuate at least twice. Start stirring and heat to 125°C, add 40g of ethylene oxide for the first polymerization reaction (the molar ratio of ethylene oxide to initiator is about 130:1), control the reaction temperature to 140-150°C, control the reaction pressure to 0.3-0.4MPa, continue stirring for 40min, and reduce the pressure to 0MPa.

[0095] (2) The temperature of the high-temperature and high-pressure reactor was raised to 125°C, 40 g of propylene oxide was added to carry out the second polymerization reaction (the molar ratio of ethylene oxide to propylene oxide was 1.32:1), the reaction temperature was controlled to be 140-150°C, and the reaction pressure was controlled to be 0.3-0.4 MPa. Stirring was carried out for 30 minutes to reduce the pressure to 0 MPa.

[0096] (3) Turn on the vacuum pump and keep it for 20 minutes to remove the unreacted monomers and small molecules in the system. After the temperature of the reactor drops below 50°C, the potassium hydroxide is removed by neutralization, adsorption and filtration to obtain dispersant A1.

[0097] The obtained dispersant A1 was analyzed by NMR carbon spectrum and NMR hydrogen spectrum to determine that it is a block polyether dispersant with the following structural composition. The NMR hydrogen spectrum of dispersant A1 is as follows: Figure 1 As shown, the carbon NMR spectrum of dispersant A1 is as follows Figure 2 As shown;

[0098] like Figure 3 In the NMR HMBC two-dimensional carbon-hydrogen correlation spectrum shown, it can be seen that there are three carbon signals related to the hydrogen of the terminal hydroxyl group, proving that the terminal hydroxyl group comes from the propylene oxide block.

[0099]

[0100] Wherein, m=3, n=3, m:n=1, and the mass spectrum total particle flow diagram of dispersant A1 is as follows: Figure 4 As shown, the molecular weight of the dispersant was measured to be 480 g / mol.

[0101] The dispersant is mixed with water to obtain an aqueous solution of the dispersant, wherein the mass concentration of the dispersant is 0.1% and the static surface tension of the aqueous solution of the dispersant is Figure 5 , its value is 28.93mN / m; dynamic surface tension see Figure 6 , its value is 35.06mN / m.

[0102] The contact angle of the dispersant on the commercial single crystal silicon wafer was tested by a contact angle meter. The contact angle of dispersant A1 on the solid silicon wafer was 25.5°.

[0103] The above dispersant A1 was mixed with water to obtain a dispersion with a mass concentration of 0.1%. Silicon powder with a diameter of 500 nm was mixed with the dispersion at a mass ratio of 1:20. The mixture was stirred at a speed of 1000 rpm for 30 minutes. The obtained silicon dispersion was completely defoamed after 5 minutes and did not aggregate after being stationary for 3 months.

[0104] Example 2

[0105] (1) Add 1g of 2,3,3-trimethyl-2-butanol and 2g of potassium hydroxide to a high-temperature and high-pressure reactor, and seal the reactor. Before heating, purge and replace with nitrogen, then evacuate, and purge and replace with nitrogen and then evacuate at least twice. Start stirring and heat to 125°C, add 40g of ethylene oxide for the first polymerization reaction (the molar ratio of ethylene oxide to initiator is about 105:1), control the reaction temperature to 130-140°C, control the reaction pressure to below 0.3-0.4MPa, and continue stirring for 30min after the pressure drops to 0MPa.

[0106] (2) The high temperature and high pressure reactor was heated to 125°C, 60 g of propylene oxide was added to carry out the second polymerization reaction (the molar ratio of ethylene oxide to propylene oxide was 0.88:1), the reaction temperature was controlled to be 140-150°C, and the reaction pressure was controlled to be 0.3-0.4 MPa. Stirring was continued for 20 min until the pressure dropped to 0 MPa.

[0107] (3) Turn on the vacuum pump and keep it for 20 minutes to remove the unreacted monomers and small molecules in the system. After the temperature of the reactor drops to below 50°C, potassium hydroxide is removed by neutralization, adsorption, and filtration to obtain dispersant A2, the structure of which is shown in formula (1), wherein R is -C(CH3)2C(CH3)2CH3, m:n=0.5:1, m=3, n=6, and M=596 g / mol.

[0108] The dispersant is mixed with water to obtain an aqueous solution of the dispersant, wherein the mass concentration of the dispersant is 0.1%, and the static surface tension of the aqueous solution of the dispersant is 29.56 mN / m; and the dynamic surface tension is 38.62 mN / m.

[0109] The contact angle of the dispersant on the commercial single crystal silicon wafer was tested by a contact angle meter. The contact angle of dispersant A2 on the solid silicon wafer was 31.9°.

[0110] The above dispersant A2 was mixed with water to obtain a dispersion with a mass concentration of 0.1%. Silicon powder with a diameter of 500 nm was mixed with the dispersion at a mass ratio of 1:20. The mixture was stirred at a speed of 1000 rpm for 30 minutes. The obtained silicon dispersion was completely defoamed after 8 minutes and did not aggregate after being stationary for 2 months.

[0111] Example 3

[0112] (1) Add 1g of 2,3,3-trimethyl-2-butanol and 2g of potassium hydroxide to a high-temperature and high-pressure reactor, and seal the reactor. Before heating, first purge and replace with nitrogen, then evacuate, and purge and replace with nitrogen and then evacuate at least twice. Start stirring and heat to 125°C, add 80g of ethylene oxide for the first polymerization reaction (the molar ratio of ethylene oxide to initiator is about 211:1), control the reaction temperature to 120-130°C, control the reaction pressure to 0.3-0.4MPa, continue stirring for 40min, and reduce the pressure to 0MPa.

[0113] (2) The high temperature and high pressure reactor was heated to 125°C, 40 g of propylene oxide was added to carry out the second polymerization reaction (the molar ratio of ethylene oxide to propylene oxide was 2.64:1), the reaction temperature was controlled to be 140-150°C, and the reaction pressure was controlled to be 0.3-0.4 MPa. After the pressure dropped, stirring was continued for 20 minutes to reduce the pressure to 0 MPa.

[0114] (3) Turn on the vacuum pump and keep it for 20 minutes to remove the unreacted monomers and small molecules in the system. After the temperature of the reactor drops below 50°C, potassium hydroxide is removed by neutralization, adsorption, and filtration to obtain dispersant A3, the structure of which is shown in formula (1), wherein R is -C(CH3)2C(CH3)2CH3, m:n=2:1, m=8, n=4, and M=728 g / mol;

[0115] The dispersant is mixed with water to obtain an aqueous solution of the dispersant, wherein the mass concentration of the dispersant is 0.1%, and the static surface tension of the aqueous solution of the dispersant is 28.23 mN / m; and the dynamic surface tension is 36.45 mN / m.

[0116] The contact angle of the dispersant on the commercial single crystal silicon wafer was tested by a contact angle meter. The contact angle of dispersant A3 on the solid silicon wafer was 40.2°.

[0117] The above dispersant A3 was mixed with water to obtain a dispersion with a mass concentration of 0.1%. Silicon powder with a diameter of 500 nm was mixed with the dispersion at a mass ratio of 1:20. The mixture was stirred at a speed of 1000 rpm for 30 minutes. The obtained silicon dispersion was completely defoamed after 7 minutes and did not aggregate after being stationary for 2.5 months.

[0118] Example 4

[0119] According to the method of Example 1, except that the amount of ethylene oxide added is 200 g, and the amount of propylene oxide added is 220 g (the molar ratio of ethylene oxide to propylene oxide is 1.2:1), dispersant A4 is prepared, and the structure is shown in formula (1), wherein R is -CH2CH2CH(CH3)CH2C(CH3)2CH3, m:n=0.93:1, m=13, n=14, and M=1528 g / mol.

[0120] The dispersant is mixed with water to obtain an aqueous solution of the dispersant, wherein the mass concentration of the dispersant is 0.1%, and the static surface tension of the aqueous solution of the dispersant is 32.52 mN / m; and the dynamic surface tension is 41.21 mN / m.

[0121] The contact angle of the dispersant on the commercial single crystal silicon wafer was tested by a contact angle meter. The contact angle of dispersant A4 on the solid silicon wafer was 45.1°.

[0122] The above dispersant A4 was mixed with water to obtain a dispersion with a mass concentration of 0.1%. Silicon powder with a diameter of 500 nm was mixed with the dispersion at a mass ratio of 1:20. The mixture was stirred at a speed of 1000 rpm for 30 minutes. The obtained silicon dispersion was completely defoamed after 15 minutes and did not aggregate after being stationary for 1 month.

[0123] Example 5

[0124] The method of Example 1 is followed, except that the amount of 3,5,5-trimethyl-1-hexanol used is 6.5 g, and the molar ratio of ethylene oxide to the initiator is about 20:1.

[0125] Dispersant A5 was obtained, the structure of which is shown in formula (1), wherein R is -CH2CH2CH(CH3)CH2C(CH3)2CH3, m:n=0.6:1, m=2, n=3, and M=400 g / mol.

[0126] The dispersant is mixed with water to obtain an aqueous solution of the dispersant, wherein the mass concentration of the dispersant is 0.1%, and the static surface tension of the aqueous solution of the dispersant is 35.21 mN / m; and the dynamic surface tension is 45.56 mN / m.

[0127] The contact angle of the dispersant on the commercial single crystal silicon wafer was tested by a contact angle meter. The contact angle of dispersant A4 on the solid silicon wafer was 47.5°.

[0128] The above dispersant A4 was mixed with water to obtain a dispersion with a mass concentration of 0.1%. Silicon powder with a diameter of 500 nm was mixed with the dispersion at a mass ratio of 1:20. The mixture was stirred at a speed of 1000 rpm for 30 minutes. The obtained silicon dispersion was completely defoamed after 20 minutes and did not aggregate after being stationary for 1 month.

[0129] Comparative Example 1

[0130] The method of Example 1 is different in that the order of adding materials is to first add propylene oxide for the first polymerization, and then add ethylene oxide for the second polymerization, to obtain dispersant DA1. The structure of DA1 is shown in the following formula, that is, the other end of the polymer main chain is capped with an ethylene oxide block:

[0131]

[0132] The dispersant is mixed with water to obtain an aqueous solution of the dispersant, wherein the mass concentration of the dispersant is 0.1%, and the static surface tension of the aqueous solution of the dispersant is 42.54 mN / m; and the dynamic surface tension is 52.85 mN / m.

[0133] The contact angle of the dispersant on the commercial single crystal silicon wafer was tested by a contact angle meter. The contact angle of the dispersant DA1 on the solid silicon wafer was 78.5°.

[0134] The above dispersant DA1 was mixed with water to obtain a dispersion with a mass concentration of 0.1%. Silicon powder with a diameter of 500 nm was mixed with the dispersion at a mass ratio of 1:20. The mixture was stirred at a speed of 1000 rpm for 30 minutes. The obtained silicon dispersion was completely defoamed after 20 minutes and did not aggregate after being stationary for 0.5 month.

[0135] Comparative Example 2

[0136] The method in Example 1 is followed, except that methyl chloride is added to the product obtained in step (2) at 60° C. for methyl end-capping. After the reaction is continued until the pressure is stable, heating is stopped, phosphoric acid solution is used for neutralization, the mixture is filtered, and dehydrated to obtain a product with methyl ends, namely, dispersant DA2, the structure of which is shown in the following formula:

[0137]

[0138] The dispersant is mixed with water to obtain an aqueous solution of the dispersant, wherein the mass concentration of the dispersant is 0.1%, and the static surface tension of the aqueous solution of the dispersant is 48.24 mN / m; and the dynamic surface tension is 43.58 mN / m.

[0139] The contact angle of the dispersant on the commercial single crystal silicon wafer was tested by a contact angle meter. The contact angle of the dispersant DA2 on the solid silicon wafer was 65.8°.

[0140] The above dispersant DA2 was mixed with water to obtain a dispersion with a mass concentration of 0.1%. Silicon powder with a diameter of 500 nm was mixed with the dispersion at a mass ratio of 1:20. The mixture was stirred at a speed of 1000 rpm for 30 minutes. The obtained silicon dispersion was completely defoamed after 30 minutes and did not aggregate after being stationary for 1 month.

[0141] Comparative Example 3

[0142] The method of Example 1 was followed, except that an equal amount of 1-pentanol was used to replace 3,5,5-trimethyl-1-hexanol. Dispersant DA3 was obtained, the structure of which is shown in formula (1), wherein R is -CH2CH2CH2CH2CH3, m:n=2:1, m=8, n=4, and M=670 g / mol.

[0143] The dispersant is mixed with water to obtain an aqueous solution of the dispersant, wherein the mass concentration of the dispersant is 0.1%, and the static surface tension of the aqueous solution of the dispersant is 43.56 mN / m; and the dynamic surface tension is 54.52 mN / m.

[0144] The contact angle of the dispersant on the commercial single crystal silicon wafer was tested by a contact angle meter. The contact angle of dispersant DA3 on the solid silicon wafer was 76.3°.

[0145] The above dispersant DA3 was mixed with water to obtain a dispersion with a mass concentration of 0.1%. Silicon powder with a diameter of 500 nm was mixed with the dispersion at a mass ratio of 1:20. The mixture was stirred at a speed of 1000 rpm for 30 minutes. The obtained silicon dispersion was completely defoamed after 80 minutes and did not aggregate after being stationary for 0.2 months.

[0146] Comparative Example 4

[0147] The method in Example 1 was followed, except that 200 g of ethylene oxide was added for the first polymerization reaction, and the molar ratio of ethylene oxide to the initiator was about 650:1. 200 g of propylene oxide was added for the second polymerization reaction (the molar ratio of ethylene oxide to propylene oxide was 1.32:1); a dispersant DA4 was obtained, the structure of which is shown in formula (1), wherein R is -CH2CH2CH(CH3)CH2C(CH3)2CH3, m:n=0.9:1, m=20, n=22, and M=2300 g / mol.

[0148] The dispersant is mixed with water to obtain an aqueous solution of the dispersant, wherein the mass concentration of the dispersant is 0.1%, and the static surface tension of the aqueous solution of the dispersant is 50.65 mN / m; and the dynamic surface tension is 54.56 mN / m.

[0149] The contact angle of the dispersant on the commercial single crystal silicon wafer was tested by a contact angle meter. The contact angle of dispersant A4 on the solid silicon wafer was 80.2°.

[0150] The above dispersant A4 was mixed with water to obtain a dispersion with a mass concentration of 0.1%. Silicon powder with a diameter of 500 nm was mixed with the dispersion at a mass ratio of 1:20. The mixture was stirred at a speed of 1000 rpm for 30 minutes. The obtained silicon dispersion was completely defoamed after 5 minutes and did not aggregate after standing for 1 hour.

[0151] It can be seen from the above examples and comparative examples that the dispersant provided by the present invention is easy to defoam and is also conducive to the dispersion of nano-silicon. It can be seen from the comparison of Example 1, Example 4 and Comparative Example 4 that too high a weight average molecular weight is not conducive to the defoaming and dispersing performance of the dispersant; it can be seen from the comparison of Example 1 and Comparative Examples 2-3 that the defoaming effect can be improved while reducing the surface tension through the synergistic effect of the specific end-capping groups at both ends of the copolymer main chain. It can be seen from the comparison of Example 1 and Comparative Example 1 that the dispersant with a specific connection sequence of ethylene oxide blocks and propylene oxide blocks has a small contact angle with the solid silicon wafer, low surface tension and good dispersibility.

[0152] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A dispersant, characterized in that: The dispersant has a structure shown in formula (1): wherein the ratio of m to n is 0.3-3:1; the weight average molecular weight of the dispersant does not exceed 2000 g / mol; R has a structure as shown in formula (2), Wherein, R1 is a C1-C10 alkylene group, and R2, R3, and R4 are each independently selected from a C1-C3 alkyl group.

2. The dispersant according to claim 1, wherein R1 is selected from -(CH2) x1 -、-CH2-CH(CH3)-(CH2) x2 -、-CH2-C(CH3)2-(CH2) x3 -、-CH(CH3)-(CH2) x4 -、-C(CH3)2-(CH2) x5 -、-C(CH3)(CH2CH3)-(CH2) x6 -or-C(CH3)(C3H7)-(CH2) x7 -, wherein x1-x7 are each independently selected from 0, 1, 2, 3 or 4; Preferably, in formula (2), R2, R3, and R4 are each independently selected from methyl, ethyl, n-propyl, or isopropyl; Preferably, R is selected from -CH2CH2CH(CH3)CH2C(CH3)2CH3, -C(CH3)2C(CH3)2CH3, -CH2CH(CH3)2CH3, -CH2CH2C(CH3)2CH3, -C(CH2CH3)(CH2CH2CH3)CH3 or -C(CH3)2CH2CH3; preferably -CH2CH2CH(CH3)CH2C(CH3)2CH3 or -C(CH3)2C(CH3)2CH3; Preferably, the ratio of m to n is 0.5-2:1; Preferably, m is 1-14, preferably 3-9; n is 1-14, preferably 3-9; Preferably, the weight average molecular weight of the dispersant is 450-1500 g / mol.

3. The dispersant according to claim 1 or 2, wherein Mixing the dispersant with water to obtain an aqueous solution of the dispersant, wherein the mass concentration of the dispersant is 0.1%, and the static surface tension of the aqueous solution of the dispersant is 23-40 mN / m, preferably 25-30 mN / m; Preferably, the dispersant is mixed with water to obtain an aqueous solution of the dispersant, the mass concentration of the dispersant is 0.1%, and the dynamic surface tension of the aqueous solution of the dispersant is 25-42 mN / m, preferably 27-40 mN / m.

4. The dispersant according to any one of claims 1 to 3, wherein The contact angle of the dispersant to the solid silicon wafer is less than 80°, preferably 20-50°.

5. A method for preparing a dispersant, characterized in that: The following steps are involved: (1) subjecting an initiator and ethylene oxide to a first polymerization reaction in the presence of a catalyst under first polymerization reaction conditions; (2) subjecting the product obtained from the first polymerization reaction to a second polymerization reaction with propylene oxide under second polymerization reaction conditions; Wherein, the molar ratio of ethylene oxide to initiator is 30-200:1, and the molar ratio of ethylene oxide to propylene oxide is 0.3-3:1; The initiator has a structure shown in formula (3), Wherein, R1 is a C1-C10 alkylene group, and R2, R3, and R4 are each independently selected from a C1-C3 alkyl group.

6. The preparation method according to claim 5, wherein: In formula (3), R1 is selected from -(CH2) x1 -、-CH2-CH(CH3)-(CH2) x2 -、-CH2-C(CH3)2-(CH2) x3 -、-CH(CH3)-(CH2) x4 -、-C(CH3)2-(CH2) x5 -、-C(CH3)(CH2CH3)-(CH2) x6 -or-C(CH3)(C3H7)-(CH2) x7 -, wherein x1-x7 are each independently selected from 0, 1, 2, 3 or 4; Preferably, in formula (3), R2, R3, and R4 are each independently selected from methyl, ethyl, n-propyl, or isopropyl; Preferably, the initiator is selected from at least one of 3,5,5-trimethyl-1-hexanol, 2,3,3-trimethyl-2-butanol, 2,2-dimethyl-1-propanol, 3,3-dimethyl-1-butanol, 2,3-dimethyl-3-pentanol, and 2-methyl-2-butanol, preferably 3,5,5-trimethyl-1-hexanol and / or 2,3,3-trimethyl-2-butanol; Preferably, the molar ratio of ethylene oxide to initiator is 50-150:1; Preferably, the molar ratio of ethylene oxide to propylene oxide is 0.5-2:

1.

7. The preparation method according to claim 5 or 6, wherein: The catalyst is selected from at least one of potassium hydroxide, sodium hydroxide, barium hydroxide and calcium acetate, preferably potassium hydroxide and / or sodium hydroxide; Preferably, the amount of catalyst used is 2-6 wt%, preferably 2.5-4 wt%, based on the total amount of ethylene oxide and propylene oxide used.

8. The preparation method according to any one of claims 5 to 7, wherein: The first polymerization reaction conditions include: reaction temperature of 110-160°C, preferably 120-150°C; reaction pressure of 0-0.4MPa, preferably 0.2-0.4MPa; reaction time of 10-60min, preferably 30-40min; Preferably, the second polymerization reaction conditions include: reaction temperature of 110-160° C., preferably 130-150° C.; reaction pressure of 0-0.4 MPa, preferably 0.2-0.4 MPa; reaction time of 10-60 min, preferably 20-30 min.

9. The preparation method according to any one of claims 5 to 8, wherein: The first polymerization reaction and the second polymerization reaction are each independently carried out under stirring conditions, and the stirring rate is each independently 1500-3000 rpm; Preferably, the method further comprises: removing impurities, neutralizing, adsorbing and filtering the product of the second polymerization reaction in sequence to obtain the dispersant.

10. Use of the dispersant according to any one of claims 1 to 4 or the dispersant prepared by the preparation method according to any one of claims 5 to 9 in dispersing nano-silicon particles.

11. A nano silicon particle dispersion, comprising a dispersion and nano silicon particles; The dispersion comprises a solvent and a dispersant according to any one of claims 1 to 4 or a dispersant prepared by the preparation method according to any one of claims 5 to 9; Preferably, in the dispersion, the concentration of the dispersant is 0.05-0.2wt%; Preferably, the solvent is water; Preferably, the particle size of the nano silicon particles is 200-3000 nm; Preferably, the mass ratio of the nano silicon particles to the dispersion is 1:10-100.