Preparation method of export LA steel rail steel

Through specific element composition and cold-controlled treatment technology, the problems of insufficient complexity and performance of low alloy rail steel preparation in the existing technology are solved, and the preparation of low alloy rail steel that meets the American standard standards with fewer alloy types is realized, improving the preparation of low alloy rail steel with the addition of fewer alloy types. The competitiveness and economic benefits of rail steel.

CN118895413AInactive Publication Date: 2024-11-05BAOTOU IRON & STEEL (GROUP) CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411031770.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-05
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The prior art is difficult to prepare low-alloy rail steels that meet the American standard low alloy standard strength when fewer alloy types are added, and the preparation method is complex, which cannot effectively improve the competitiveness and economic benefits of rail steels.

Method used

Steel ingots composed of specific elements are rolled and controlled, and nano-scale pearlite microstructure is formed through heating, insulation, rolling and multiple cooling treatments, which meet the requirements of hardness, yield strength, tensile strength and elongation.

Benefits of technology

When fewer alloy types are added, pearlite tissue with an average sheet spacing below 0.25 μm is obtained by a simple preparation method, with a hardness value of 310-325 HBW, a yield strength of 550-590MPa, a tensile strength of 1050-1100MPa, and an elongation rate 10-11%, meets the US standard standards and improves the competitiveness and economic benefits of rail steel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895413A_ABST
    Figure CN118895413A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of exported LA steel rail steel, the exported LA steel rail steel is pearlitic steel rail steel, and the pearlitic steel rail steel comprises the following element components in percentage by mass: 0.73-0.81% of C, 0.38-0.45% of S , 0.95-1.05% of Mn, 0.30-0.35% of Cr, less than or equal to 0.02% of P and less than or equal to 0.02% of S. The balance is iron and inevitable impurities; a steel ingot with the same components as the pearlite rail steel is sequentially subjected to rolling and controlled cooling, and the pearlite rail steel is obtained; and rolling process parameters and air cooling process parameters are limited. According to the preparation method of the exported LA steel rail steel, on the premise that a small number of alloy types are added, a pearlite structure with the average lamellar spacing smaller than 0.20 [mu] m can be obtained through the simple preparation method. And the performance requirements of American standards on low-alloy standard strength steel rails are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgical materials, and in particular relates to a method for preparing LA rail steel for export. Background Art

[0002] With the increasing international cooperation, the demand for bulk raw materials such as coal, oil, and iron ore in various countries around the world has increased year by year, and freight railways will usher in a new round of rapid development. After thousands of years of development, the European and American railway freight system has become the most mature and developed freight system in the world. As an important load-bearing component of the freight system, rails have always been highly valued by the railway department. North America is a developed region for heavy-duty railways and ranks among the world's top in heavy-duty transportation technology. It has a complete and developed railway network, and large-scale lines have been completed around 2000. By 2009, the total operating mileage of heavy-duty railways in North America reached 224,000 kilometers. Australia is a country with relatively developed railway transportation, with a railway operating line of 43,000 km. The railway system has a high status in the national economy, with a freight turnover of 150 billion t·km. Railways account for more than 35% of the total domestic transportation volume. 80% of Australia's iron ore, 70% of coal and 20% of grain are exported by rail transportation. The heavy-duty train operated by BHP Billiton Iron Ore Company of Australia on the Newman Mountain-Port Hedland railway line set the world record for the longest and heaviest train. In addition, other countries with ore resources are also planning to build heavy-duty railways, and the market for low-alloy rails will also expand accordingly. The LA rail in the AREMA standard belongs to the American standard low-alloy rail. By developing a rail head tread hardness of more than 310HB and R p0.2 ≥74ks i(510MPa), R m Low alloy medium strength rails with a strength of ≥142.5ksi (980MPa) and an elongation of not less than 10% can enhance the market competitiveness of Baosteel products, fill the gap in rail varieties, increase economic benefits, and meet the demand for rails exported to America. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing LA rail steel for export, which can obtain pearlite structure with an average interlamellar spacing of less than 0.25 μm by a relatively simple preparation method under the premise of adding fewer alloy types, and meet the performance requirements of the American standard for low-alloy standard strength rails.

[0004] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0005] The invention discloses a method for preparing LA rail steel for export, which is pearlite rail steel. The pearlite rail steel comprises the following element components by mass percentage: C: 0.73-0.81%, Si: 0.38-0.50%, Mn: 0.95-1.05%, Cr: 0.30-0.35%, P≤0.02%, S≤0.02%. The balance is iron and unavoidable impurities;

[0006] Rolling and controlled cooling a steel ingot having the same composition as the pearlite rail steel in sequence to obtain the pearlite rail steel;

[0007] Heat the ingot to 1150±10℃ and keep it warm for 2-3 hours; the starting rolling temperature is 1050±10℃, the final rolling temperature is 930±10℃, and the rolling is performed for 11 times to form a 20mm thick slab;

[0008] The controlled cooling includes first-stage cooling, first-stage air cooling, second-stage cooling and second-stage air cooling; the final rolling temperature of the rolling is 850-950°C; after cooling, the rolled steel ingot is cooled to 490-510°C at a cooling rate of 5-7°C / s; the first-stage air cooling is started at 560-580°C, and the air cooling is ≤50s; the second-stage cooling is to cool the steel ingot after the first-stage air cooling to 280-350°C at a cooling rate of 7-8°C / s; the second-stage air cooling is started at 280-350°C and air cooled to room temperature.

[0009] Further, the ingot was heated to 1150° C. and kept at this temperature for 2.5 hours.

[0010] Furthermore, the starting rolling temperature is 1050°C and the final rolling temperature is 930°C.

[0011] Furthermore, the average interlamellar spacing of the nano-scale pearlite microstructure is 0.23 μm.

[0012] Furthermore, the pearlite rail steel meets the following requirements: hardness value is 310-325 HBW, yield strength is 550-590 MPa, tensile strength is 1050-1100 MPa, and elongation is 10-11%.

[0013] Compared with the prior art, the beneficial technical effects of the present invention are:

[0014] The nano-level pearlite rail microstructure prepared by the present invention has an average interlamellar spacing of 0.23 μm and meets the following performance requirements: hardness value of 310-325 HBW, yield strength of 550-590 MPa, tensile strength of 1050-1100 MPa, and elongation of 10-11%. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1The distance between LA rail pieces under an optical microscope. DETAILED DESCRIPTION

[0016] The present invention will be further described below in conjunction with the embodiments.

[0017] The pearlite rail steel and the preparation method thereof provided by the present invention are described in detail below with reference to the embodiments.

[0018] Pearlite rail steel includes the following elements by mass percentage: C: 0.73-0.81%, Si: 0.38-0.50%, Mn: 0.95-1.15%, Cr: 0.30-0.45%, P≤0.02%, S≤0.02%. The balance is iron and unavoidable impurities;

[0019] Table 1 Composition and content of continuous casting finished products

[0020] C / % Si / % Mn / % P / % S / % Cr / % Solution 1 0.763 0.461 1.09 0.0130 0.0070 0.355 Solution 2 0.769 0.467 1.10 0.0130 0.0030 0.428

[0021] Table 2 Rolling process parameters

[0022] First stage cooling First stage air cooling Second stage cooling Second stage air cooling Solution 1 580℃ 40s 320℃ 8℃ / s Solution 2 560℃ 30s 290℃ 7℃ / s

[0023] The rolling results of Scheme 1 and Scheme 2 were tested in detail for various indicators such as conventional tensile properties and tread hardness in accordance with the requirements of AREMA-2020 standard strength carbon rails. The test results show that all conventional and special properties meet the standard requirements. The specific test results are shown in Tables 3 and 4.

[0024] Table 3 Test results of rail tensile properties

[0025]

[0026] Table 4 Hardness and elongation test results of rails

[0027]

[0028] The pearlite rail steel is observed under an optical microscope (eg Figure 1 shown), by Figure 1 It can be seen that the average lamellar spacing of the pearlite structure in the pearlite rail steel described in Scheme 1 is about 0.25 μm; the lamellar spacing of Scheme 2 is 0.20 μm.

[0029] The pearlite rail steel prepared by the method for preparing pearlite rail steel provided by the present invention can obtain a low-alloy medium-strength pearlite rail with a small interlamellar spacing of pearlite structure and tensile strength, yield strength, elongation and hardness meeting the requirements of American standards by using a relatively simple preparation process, under the premise of adding appropriate amounts of alloy elements.

[0030] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preparing LA rail steel for export, Features: Pearlite rail steel, which includes the following elements by mass percentage: C: 0.73-0.81%, Si: 0.38-0.45%, Mn: 0.95-1.05%, Cr: 0.30-0.35%, P≤0.02%, S≤0.02%. The balance is iron and unavoidable impurities; Rolling and controlled cooling a steel ingot having the same composition as the pearlite rail steel in sequence to obtain the pearlite rail steel; Heat the ingot to 1150±10℃ and keep it warm for 2-3 hours; the starting rolling temperature is 1050±10℃, the final rolling temperature is 930±10℃, and the rolling is performed for 11 times to form a 20mm thick slab; The controlled cooling includes first-stage cooling, first-stage air cooling, second-stage cooling and second-stage air cooling; the final rolling temperature of the rolling is 850-950°C; after cooling, the rolled steel ingot is cooled to 490-510°C at a cooling rate of 5-7°C / s; the first-stage air cooling is started at 560-580°C, and the air cooling is ≤50s; the second-stage cooling is to cool the steel ingot after the first-stage air cooling to 280-350°C at a cooling rate of 7-8°C / s; the second-stage air cooling is started at 280-350°C and air cooled to room temperature.

2. The method for preparing LA rail steel for export according to claim 1, Features: The ingot was heated to 1150°C and kept at this temperature for 2.5 hours.

3. The method for preparing LA rail steel for export according to claim 2, Features: The starting rolling temperature is 1050℃ and the final rolling temperature is 930℃.

4. The method for preparing LA rail steel for export according to claim 2, Features: The average interlamellar spacing of the nano-scale pearlite microstructure is 0.23 μm.

5. The method for preparing LA rail steel for export according to claim 2, Features: The pearlite rail steel meets the following requirements: hardness value is 310-325 HBW, yield strength is 550-590 MPa, tensile strength is 1050-1100 MPa, and elongation is 10-11%.

Citation Information

Patent Citations

  • Pearlite steel rail steel and preparation method thereof

    CN110592496A

  • Production method for eliminating abnormal structure of decarburized layer of pearlite steel rail

    CN117683985A

  • Production method for improving fatigue crack growth rate resistance of steel rail

    CN117684073A

  • Preparation method of CrV alloy-containing standard-strength steel rail steel

    CN118326139A

  • Controlled-rolled and controlled-cooled high-strength pearlitic steel rail, and production method therefor

    WO2022110812A1