Molded articles comprising poly (aryl ether sulfone) (PAES) polymers and methods of manufacture using melt processing

Through the poly(aryl ether sulfone) polymer based on naphthalene glycol monomer, the problems of high melt viscosity and safety of glycol monomers in high temperature melt processing are solved, and low estrogen activity and high mechanical properties are achieved Performance molded products are suitable for a variety of applications, improving processing performance and safety.

CN118900871APending Publication Date: 2024-11-05SOLVAY SPECIALTY POLYMERS USA LLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380027421.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-18
Filing Date
2023-01-18
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Existing poly(aryl ether sulfone) polymers have high melt viscosity problems in high temperature melt processing, limiting their fluidity and molding properties in injection molding and other applications of thin-walled parts, while some Diol monomers such as BPA and BPS are subject to safety concerns due to potential endocrine interference and are difficult to replace.

Method used

Poly(aryl ether sulfone) polymer prepared based on naphthalene glycol monomer is used to form molded products with low estrogen activity and good mechanical characteristics through high temperature melt processing, and naphthalene glycol monomer and dihalodiphenyl The condensation reaction of sulfone forms a PAES polymer with high glass transition temperature and high elastic modulus.

Benefits of technology

Achieving polymers with low melt viscosity and high mechanical properties at high temperatures are suitable for a variety of applications, including food, beverage, medical and aerospace, while reducing the potential risks to human health.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005041751170000022
    Figure BDA0005041751170000022
  • Figure BDA0005041751170000023
    Figure BDA0005041751170000023
  • Figure BDA0005041751170000025
    Figure BDA0005041751170000025
Patent Text Reader

Abstract

The present invention relates to a shaped article comprising at least one poly (aryl ether sulfone) (PAES) polymer made from at least one naphthalene glycol monomer and at least one dihalodiphenyl sulfone monomer; a method of making such an article and the use of the article in biomedical, food, beverage applications, automotive, aerospace, electrical, electronic, industrial product applications and / or in composites.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to U.S. Provisional Patent Application No. 63 / 300667, filed on January 19, 2022, and European Patent Application No. 22162978.5, filed on March 18, 2022, the entire contents of which are incorporated herein by reference for all purposes. Technical Field

[0003] The present invention relates to a shaped article comprising at least one poly(aryl ether sulfone) (PAES) polymer derived from at least one naphthalene diol monomer. The present invention also relates to a method for making such a shaped article using melt processing and the use of the shaped article in various applications such as medical applications, food and beverage applications, aerospace applications and / or composite materials. Background Art

[0004] Poly(aryl ether sulfone) polymers (PAES) are a general term used to describe any polymer containing at least one sulfone group (-SO2-), at least one ether group (-O-), and at least one arylene group. PAES polymers have been used to manufacture products in different application areas, such as the medical market, due to their excellent mechanical and thermal properties coupled with outstanding hydrolytic stability.

[0005] PAES is typically made by polycondensation using dihalodiphenyl sulfone (sulfone monomer) and at least one aromatic diol monomer such as bisphenol A (BPA), diphenol (BP), or dihydroxydiphenyl sulfone (DHDPS), also known as bisphenol S (BPS).

[0006] A commercially important group of PAES includes polysulfone polymers referred to herein as polysulfones, or PSUs for short. PSU polymers contain repeating units derived from the condensation of BPA and dihalosulfone monomers such as 4,4'-dichlorodiphenyl sulfone (DCDPS). Such PSU polymers are commercially available from Solvay Specialty Polymers USALLC under the trademark Commercially available. The structure of the repeating unit of this PSU polymer is shown below:

[0007]

[0008] The PSU polymer has a high glass transition temperature (eg, about 185° C.), and exhibits high strength and toughness.

[0009] Another important group of PAES includes polyethersulfone polymers, referred to as PES. PES polymers are derived from the condensation of BPS and dihalosulfone monomers (such as DCDPS). Such PES polymers are purchased from Solvay Specialty Polymers LLC in the United States under the trademark Commercially available. The structure of the repeating unit of this PES polymer is shown below:

[0010]

[0011] Another important group of PAES includes poly(biphenyl ether sulfone) polymers, or PPSU for short. PPSU is made by reacting 4,4'-biphenol (BP) and a dihalosulfone monomer (such as DCDPS) and is notably available from Solvay Specialty Polymers LLC in the United States under the trade name Commercially available. The structure of the repeating unit of this PPSU polymer is shown below:

[0012]

[0013] It is generally accepted in the art that the mechanical properties of PPSU depend on its molecular weight, and that the higher the molecular weight, the higher the mechanical properties. However, a consequence of a high molecular weight of PPSU is that it exhibits a high melt viscosity, which then makes PPSU less attractive for certain markets. For example, for injection molding of thin-walled parts, it is still desirable to have a PPSU with a low melt viscosity so that the molding operation can be performed with improved flow and molding properties. Due to its high viscosity, PPSU is usually processed at temperatures between 360°C and 400°C, which is well above its Tg of 220°C.

[0014] PAES is a highly thermally stable polymer with excellent toughness and impact strength. PAES is used in a variety of different applications, such as in composites, injection molded articles and film applications.

[0015] For applications including those requiring contact with water, food, beverages, drugs and / or blood, it is important that polymeric materials are safe for both humans and the environment. Polymeric materials in contact with food and drugs must meet specific requirements set by, for example, the US Food and Drug Administration (FDA), the European Food Safety Agency (European Food Safety Agency) and the Environmental Protection Agency (EPA).

[0016] However, diol monomers such as BPA and BPS are chemicals of concern regarding potential endocrine disruption in medical or food contact applications. Since the 1960s, PSU and PES polymers based on BPA and BPS, respectively, have been frequently used to manufacture articles, including plastic bottles and food and beverage cans, and further used to prepare membranes for use in contact with biological fluids such as blood. In recent years, concerns have been raised regarding the safety of BPA and BPS.

[0017] To overcome this concern, several publications, such as WO 2019 / 048652A1 and WO 2021 / 110954A1, both from Solvay Specialty Polymers, USA, disclose the use of alternative diols such as isosorbide and tetramethylbisphenol F (TMBPF) to make PAES, as these diols appear to have less endocrine disrupting potential.

[0018] However, these diol monomers are based on cycloaliphatic units in the case of isosorbide and / or have benzylic protons as in the case of tetramethylbisphenol F (TMBPF), both of which are heat sensitive materials with the result that end-use applications and polymer processing become limited to solution processing at low temperatures.

[0019] US2014 / 0113093A1 (Solvay Specialty Polymers, USA) also describes PAES polymers derived from specific aromatic diols, which have weak binding affinity to estrogen receptors and are very suitable for the food and pharmaceutical industries, advantageously with lower risks to human health. The present invention further relates to compositions containing such polymers, and articles made from such polymers.

[0020] None of these documents describes the use of naphthalene diol to make PAES polymers and then articles made therefrom.

[0021] Generally speaking, the type and quality of articles that can be formed from a polymer depends on the processability of the polymer. Melt processing of polymers involves heating the polymer at high temperatures; the high temperature is usually much higher than the glass transition temperature to form a molten polymer before manufacturing the article. The thermochemical stability of the polymer at this elevated temperature is an important factor in determining the suitability of such a polymer for the intended shaping (e.g., molding) of the article. Therefore, compared with PAES polymers with lower melt processability that degrade or crosslink at elevated temperatures used in melt processing, amorphous PAES polymers with increased melt processability can be used in a large number of application environments using melt processing techniques.

[0022] Amorphous polymer materials such as PAES with improved thermal properties combined with very good mechanical properties offer opportunities for high temperature injection molding applications that have traditionally been limited to filled semi-crystalline polymers. For example, applications for such PAES polymers include opportunities in metal replacement and high performance thermosetting resins in a wide range of engineering applications. This includes automotive, aerospace, electrical, electronic and industrial product applications, the manufacture of composite materials or use in composite materials.

[0023] There is still a continuing need for shaped articles made of polymeric materials, especially polyethersulfones obtained from diol monomers (M), which have a weak binding affinity for estrogen receptors and whereby the polymeric materials are particularly heat-resistant, melt-processable, while exhibiting good mechanical properties. The use of such amorphous PAES materials with low estrogenic activity compared to PAES made from BPA and BPS provides opportunities for the manufacture of articles intended to come into contact with food, beverages, drugs, biological fluids (such as blood) and / or water, for example for the manufacture of parts for biomedical devices (such as tubing used in medical applications), for the manufacture of articles intended to come into contact with food (such as baby bottles). Summary of the invention

[0024] The applicant has now discovered that certain PAES polymer materials based on naphthalene diol monomers can solve the above-mentioned problems.

[0025] The invention is set out in the accompanying set of claims.

[0026] Specifically, the first aspect of the present disclosure relates to a shaped article as defined in any one of claims 1 to 13. The shaped article comprises a PAES polymer, the polymer comprising at least 80 mol.% of a repeating unit (R) having formula (I) based on the total moles of repeating units in the PAES polymer. PAES ):

[0027]

[0028] in:

[0029] -E is selected from formula (IIa) and / or formula (IIb)

[0030] - each R' is independently at each position an alkyl group having 1 to 5 carbon atoms; and

[0031] - j' is 0 or an integer from 1 to 10, preferably j'=0.

[0032] In some embodiments, the PAES in the shaped article is obtained from the condensation of at least one naphthalene diol monomer and a dihalodiphenyl sulfone.

[0033] Non-limiting examples of shaped articles according to the invention are notably food and / or beverage containers (such as milk bottles), tubes (such as biomedical tubes), catheters, fittings, housings, coatings and / or composites.

[0034] The second aspect of the present invention is a method for preparing the shaped article as defined in any one of claims 14 to 16. The method comprises using the PAES polymer described herein. In some embodiments, the method for preparing the shaped article according to the present invention may comprise melt processing a composition comprising the naphthalene diol-based PAES described herein to form the article.

[0035] A third aspect of the present disclosure relates to the use of a shaped article as defined in claim 17 suitable for biomedical applications (such as biomedical tubing), coatings and / or toughened thermoplastic composites.

[0036] More precise information and details on these topics are now provided below. DETAILED DESCRIPTION

[0037] In this application:

[0038] - even any description related to a specific embodiment is applicable to and interchangeable with other embodiments of the present disclosure;

[0039] - When an element or component is said to be included in and / or selected from a list of listed elements or components, it should be understood that in the relevant embodiments explicitly considered herein, the element or component may also be any of these listed independent elements or components, or may also be selected from a group consisting of any two or more of the explicitly listed elements or components; any element or component listed in the list of elements or components may be omitted from this list; and

[0040] - Any recitation of numerical ranges by endpoints herein includes all numbers subsumed within the recited range as well as the endpoints of that range and equivalents thereof.

[0041] As used herein, and unless otherwise expressly stated, "substantially free" of a component in a substance (e.g., a reaction mixture, a monomer mixture, a polymer, a molded article, ...) means that the concentration of the component is no more than 1 wt.% or no more than 0.5 wt.% based on the total weight of such substance. In addition, such a specific component may be in a free state or in a combined state in the substance.

[0042] As used herein, and unless otherwise expressly stated, "free" of a component in a substance (e.g., a reaction mixture, a monomer mixture, a polymer, a molded article, ...) means that the concentration of the component is no more than 0.1 wt.% or no more than 0.05 wt.% based on the total weight of such substance. In addition, such a specific component may be in a free state and / or in a state of association with the substance.

[0043] When "substantially free" or "free of" is used in the context of a 'bound' compound (e.g., BPA monomer) of a polymer or article that is "substantially free" or "free of" a bound compound (BPA), the term "bound" is intended to be understood as the polymer or article containing less than the aforementioned amount of repeating units derived from such bound compound (BPA). For example, when bound BPA is present, a polymer that is substantially free of bound BPA contains no more than 1 wt.% of BPA-derived repeating units.

[0044] For the purposes of the present invention, the expression "substantially all" in combination with the stated amount of repeating units in the polymer is intended here to mean that small amounts, generally less than 1 mol %, preferably less than 0.5 mol %, of other repeating units may be tolerated, for example as a result of lower purity of the monomers used.

[0045] The expression "polymer" is used herein to designate homopolymers containing substantially all identical repeating units, as well as copolymers comprising at least 50 mol.%, for example at least about 60 mol.%, at least about 65 mol.%, at least about 70 mol.%, at least about 75 mol.%, at least about 80 mol.%, at least about 85 mol.%, at least about 90 mol.%, at least about 95 mol.%, or at least about 98 mol.% of identical repeating units.

[0046] The terms "estrogenic activity" or "estrogen agonist activity" refer to the ability of a substance to mimic hormone-like activity by interacting with endogenous estrogen receptors, typically endogenous human estrogen receptors.

[0047] The applicant has discovered that certain PAES polymer materials based on naphthalene diol monomers have at least one of the following properties:

[0048] - High elastic modulus at high temperatures (as measured by ASTM D5279 at 190°C 190 ≥400MPa, preferably ≥600MPa, more preferably ≥800MPa); and / or

[0049] - Suitable melt stability represented by VR40, wherein VR40 is the ratio of the melt viscosity at 40 minutes ("MV40") to the melt viscosity at 5 minutes ("MV5"), the melt viscosity being measured using ASTM D3835: VR40 = MV40 / MV5 (e.g., VR40 measured at 380°C of 0.95 to 1.05 or VR40 measured at 410°C of ≤ 2, preferably ≤ 1.9); and / or

[0050] - A glass transition temperature Tg of -200°C to 250°C or 205°C to 240°C, wherein Tg is measured via differential scanning calorimetry (DSC).

[0051] The applicant has further discovered that certain PAES polymer materials based on naphthalene diol monomers, particularly 2,7-NDO monomers, are characterized by having a low thermal loss of elastic modulus (% loss) of at most 15%, preferably at most 13%, more preferably at most 11%, wherein % loss = (E 50 -E 190 ) / E 50 , the E 50 is the elastic modulus of the polymer material measured at 50°C, and E 190 is the elastic modulus of the polymer material, both are measured using ASTM D5279.

[0052] The incorporation of these naphthalene moieties does not impair the thermal processing and thermomechanical properties of the final polymers, which will be suitable for high temperature polymer recovery such as in melt extrusion or molding.

[0053] These naphthalene groups do not impair the solubility of the resulting polymers, with the result that these polymers are both solution-processable and melt-processable. This broadly increases the application range and processability compared to PAES polymers based on alternative diols such as isosorbide or tetramethylbisphenol F (TMBPF).

[0054] The presence of these naphthalene rings can also provide additional performance benefits (such as increased thermomechanical properties) and increase stiffness at higher temperatures compared to, for example, 4,4'-biphenol, because the naphthalene rings fused to each other do not reduce stiffness at higher temperatures. Such performance attributes may be advantageous in applications such as composites, injection molded articles, coatings, etc.

[0055] The applicant has found that the present invention allows to obtain shaped articles at least in part from PAES polymers, which have good viscosity stability and high elastic modulus at high temperatures (such as 190° C.), are notably melt-processable, and are most useful for molding, especially injection molding. The thermomechanical properties of PAES polymers are similar to those of commercially available PES polymers. These PAES polymers can then be used to prepare shaped articles to be used in food, beverage, medical, automotive, aerospace, electrical, electronic and industrial product applications and / or in composite materials via melt processing.

[0056] The applicants have further discovered that certain naphthalene diol monomers with low estrogenic activity (compared to the commonly used diols BPA, BPS and / or BP) can be used to successfully prepare PAES polymers with an appropriate combination of thermal and mechanical properties to prepare shaped articles. Since PAES polymers incorporating such monomers are also expected to exhibit reduced estrogenic activity, shaped articles containing them will pose a lower risk to human health than shaped articles containing PAES derived from BPA, BPS and / or BP, and should therefore be suitable for use in food, beverage and / or biomedical applications where the polymer surface will come into contact with, for example, food, beverage, biological fluids and / or drugs.

[0057] Molded products

[0058] The shaped article is preferably selected from the group consisting of a tube, a conduit, a food or beverage container (such as a baby bottle), a fitting, a housing, a coating, a composite material or a part thereof, and any combination thereof.

[0059] In some embodiments, the shaped article comprises a PAES polymer containing at least 80 mol.% of a repeating unit (R) having formula (I) based on the total moles of repeating units in the PAES polymer. PAES ),in:

[0060] -E is selected from formula (IIa) and / or formula (IIb)

[0061] - each R1 is independently at each position an alkyl group having 1 to 5 carbon atoms, and

[0062] -j is 0 or an integer from 1 to 10.

[0063] The repeating unit (R) of formula (I) PAES ) in which E can be selected from the group consisting of:

[0064]

[0065] and any combination thereof.

[0066] The repeating unit (R) of formula (I) PAES ) is preferably selected from the group consisting of:

[0067] and any combination thereof.

[0068] The repeating unit (R) of formula (I) PAES ) may not include the following structures:

[0069]

[0070] j' in formula (I) is preferably 0.

[0071] The PAES polymer in the shaped article can be a homopolymer or a copolymer. If it is a copolymer, it can be a random copolymer, an alternating copolymer or a block copolymer.

[0072] The PAES polymer in the shaped article comprises at least 90 mol.%, at least 95 mol.%, or at least 99 mol.%, based on the total moles of repeating units in the PAES polymer, of repeating units (R PAES Preferably, the PAES polymer in the shaped article comprises substantially all repeating units (R PAES ).

[0073] In a preferred embodiment, the shaped article comprises a PAES polymer containing at least 80 mol.% of a repeating unit (R) selected from the group consisting of formula (Ia), (Ib), (Ic) and any combination thereof, based on the total moles of repeating units in the PAES polymer. PAES ):

[0074]

[0075] In a more preferred embodiment, the shaped article comprises a PAES polymer containing at least about 85 mol%, at least about 90 mol%, at least about 95 mol%, or at least about 98 mol%, based on the total moles of repeating units in the PAES polymer, of repeating units (R) selected from formula (Ia), (Ib), and / or (II-c), preferably selected from formula (Ia) and / or (Ib), more preferably having formula (Ia). PAES ).

[0076] In an even more preferred embodiment, the shaped article comprises a PAES polymer containing substantially all identical repeating units (R) selected from formula (Ia), (Ib) and / or (II-c), preferably having formula (Ia) and / or (Ib), more preferably having formula (Ia). PAES ).

[0077] The PAES polymer in the molded article may be substantially free of 4,4'-dihydroxydiphenyl sulfone (BPS), 4,4'-isopropylidene diphenol (BPA) and / or 4,4'-biphenol (BP), preferably substantially free of BPA and BPS or free of BPA and BP, more preferably substantially free of all three. BPA, BPS and / or BP may be in a free state or in a bound state in the PAES polymer.

[0078] In some embodiments, the PAES polymer in the shaped article preferably does not include sulfone repeating units derived from BPA, BPS, and BP.

[0079] In some embodiments, the shaped article is preferably substantially free of BPA, BPS and / or BP (whether they are in a free state or in a bound state), preferably substantially free of BPA and BPS (whether they are in a free state or in a bound state) or substantially free of BPA and BP (whether they are in a free state or in a bound state), and more preferably substantially free of all three.

[0080] In some embodiments, shaped articles comprising PAES obtained from certain specific naphthalene diol monomers are expected to have low endocrine disrupting potential and should exhibit lower estrogenic activity compared to shaped articles comprising PAES obtained from BPA, BPS and / or BP.

[0081] More specifically, the shaped article comprises a PAES obtained from a naphthalene diol monomer having an EC for estrogen receptor alpha (ERα) of at least 30,000 nM. 50 Response value.

[0082] In a preferred embodiment, the shaped article comprises PAES obtained from a naphthalene diol monomer selected from the group consisting of 1,5-naphthalene diol isomers, 2,3-naphthalene diol isomers and 2,7-naphthalene diol isomers, more preferably selected from the group consisting of 1,5-naphthalene diol isomers and 2,7-naphthalene diol isomers.

[0083] The shaped article may contain a PAES described herein in an amount of at least 1 wt.%, such as at least 5 wt.%, at least 10 wt.%, at least 15 wt.%, at least 20 wt.%, at least 25 wt.%, or at least 30 wt.%, based on the total weight of the shaped article.

[0084] The shaped article may contain the PAES described herein in an amount greater than 50 wt.%, e.g., greater than 55 wt.%, greater than 60 wt.%, greater than 65 wt.%, greater than 70 wt.%, greater than 75 wt.%, greater than 80 wt.%, greater than 85 wt.%, greater than 90 wt.%, greater than 95 wt.%, or greater than 99 wt.%, based on the total weight of the shaped article.

[0085] The molded article may further comprise at least one polymer different from the PAES described herein, such as another sulfone polymer such as polysulfone (PSU), polyarylethersulfone (PPSU), polyethersulfone (PES), or polyphenylene sulfide (PPS), poly(aryletherketone) (PAEK) such as poly(etheretherketone) (PEEK), poly(etherketoneketone) (PEKK), poly(etherketone) (PEK) or copolymers of PEEK and poly(diphenyletherketone) (PEEK-PEDEK copolymers), polyetherimide (PEI) and / or polycarbonate (PC). The other polymer component may also be polyvinylpyrrolidone and / or polyethylene glycol. In such cases, the shaped articles of the present invention may contain at least one polymer different from the PAES described herein in an amount of up to 50 wt.%, for example, up to 45 wt.%, up to 40 wt.%, up to 35 wt.%, up to 30 wt.%, up to 25 wt.%, up to 20 wt.%, up to 15 wt.%, up to 10 wt.%, up to 5 wt.%, up to 2 wt.% or up to 1 wt.%, based on the total weight of the shaped article.

[0086] The molded article may further comprise at least one additional ingredient, such as a solvent, a filler, a lubricant, a light stabilizer, a UV stabilizer, a heat stabilizer, a plasticizer, an impact modifier / toughener, a nucleating agent, an antioxidant, a mold release agent, an antistatic agent, a flame retardant, an antifogging agent, a matting agent, a pigment, a dye and / or an optical brightener.

[0087] In such cases, the shaped article may contain more than 0 wt % and up to 20 wt % (based on the total weight of the polymer composition) of one or more optional additional ingredients (excluding fillers).

[0088] In some embodiments, the shaped articles may contain greater than 5 wt % and up to 70 wt % (based on the total weight of the polymer composition) of one or more optional fillers.

[0089] Method for producing PAES

[0090] The PAES in the shaped article is preferably prepared by the following reaction mixture (R G ) to obtain:

[0091] - at least one aromatic dihydroxy monomer (a), comprising at least 80 mol.% of naphthalene diol monomers (a1) having formula (IIIa) and / or (IIIb), based on the total moles of monomers (a):

[0092] and / or

[0093] at least one aromatic dihalogen sulfone monomer (b), comprising at least 50 mol % of a monomer (b1) having the formula (IV), based on the total moles of monomer (b):

[0094]

[0095] - at least one carbonate component;

[0096] - in a solvent;

[0097] in:

[0098] - each R' is independently at each position an alkyl group having 1 to 5 carbon atoms;

[0099] - j' is an integer from 0 to 10, preferably j'=0; and

[0100] -X is a halogen atom, preferably F or Cl, more preferably Cl.

[0101] The at least one aromatic dihydroxy monomer (a) comprises at least about 85 mol.%, at least about 90 mol.%, at least about 95 mol.%, or at least about 98 mol.% of monomer (a1) based on the total moles of monomer (a). According to a preferred embodiment, the aromatic dihydroxy monomer (a) consists essentially of monomer (a1).

[0102] In a preferred embodiment, the naphthalene diol monomer (a1) is preferably a naphthalene diol isomer having an estrogen agonist activity lower than bisphenol A (BPA). In some embodiments, the naphthalene diol monomer (a1) is preferably a naphthalene diol isomer having an estrogen agonist activity lower than bisphenol S (BPS). In some embodiments, the naphthalene diol monomer (a1) is preferably a naphthalene diol isomer having an estrogen agonist activity lower than 4,4'-biphenol (BP).

[0103] The naphthalene diol monomer (a1) preferably has an EC for estrogen receptor α (ERα) of at least 30,000 nM. 50 Response value.

[0104] Monomer (a1) preferably comprises a naphthalene diol isomer selected from the group consisting of isomers having formulae (5a) to (5j):

[0105]

[0106] Monomer (a1) may, for example, contain at least 80 wt.%, at least 90 wt.%, at least 95 wt.% or at least 99 wt.% of naphthalene diol isomers selected from the group consisting of isomers having formulae (5a) to (5j), based on the total weight of monomer (a).

[0107] The naphthalene diol monomer (a1) is more preferably selected from the group consisting of 1,5-naphthalene diol isomers having the formula (5d), 2,3-naphthalene diol isomers having the formula (5h) and 2,7-naphthalene diol isomers having the formula (5d), and is even more preferably selected from the group consisting of 1,5-naphthalene diol isomers and 2,7-naphthalene diol isomers.

[0108] In some embodiments, the naphthalene diol monomer (a1) does not include the 2,6-naphthalene diol isomer having the formula (5i).

[0109] The at least one aromatic dihalogen sulfone monomer (b) comprises at least about 60 mol.%, at least about 65 mol.%, at least about 70 mol.%, at least about 75 mol.%, at least about 80 mol.%, at least about 85 mol.%, at least about 90 mol.%, at least about 95 mol.% or at least about 98 mol.% of monomer (b1) based on the total moles of monomer (b). According to a preferred embodiment, the aromatic dihalogen sulfone monomer (b) is substantially composed of monomer (b1).

[0110] Monomer (b) preferably comprises at least 50 mol.% of 4,4'-dichlorodiphenyl sulfone (DCPDS) and / or 4,4'-difluorodiphenyl sulfone (DFPDS) as monomer (b1) based on the total moles of aromatic dihalogen sulfone monomer (b). Monomer (b) more preferably comprises at least about 60 mol.%, at least about 65 mol.%, at least about 70 mol.%, at least about 75 mol.%, at least about 80 mol.%, at least about 85 mol.%, at least about 90 mol.%, at least about 95 mol.% or at least about 98 mol.% of DCPDS and / or DFDPS as monomer (b1) based on the total moles of monomer (b).

[0111] In a specific embodiment, the reaction mixture (R G ) is substantially free of BPA, BPS and / or BP, preferably substantially free of BPA and BPS, and more preferably substantially free of all three.

[0112] The molar ratio of monomers (a) to (b) may vary between 0.9 and 1.1. For example, the molar ratio of (a) to (b) may vary from 1.01 to 1.05.

[0113] The solvent used to prepare the PAES described herein can be selected from the group consisting of dimethyl sulfoxide (DMSO), dimethyl sulfone (DMS), diphenyl sulfone (DPS), 1,3-dimethyl-2-imidazolidinone (DMI), diethyl sulfoxide, diethyl sulfone, diisopropyl sulfone, tetrahydrothiophene-1,1-dioxide, tetrahydrothiophene-1-monoxide, N-methylpyrrolidone (NMP), N-butylpyrrolidone (NBP), N-ethyl-2-pyrrolidone, N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAC), tetrahydrofuran (THF), toluene, benzene, monochlorobenzene, dichlorobenzene, anisole, chloroform, dichloromethane (DCM), sulfolane, and mixtures thereof.

[0114] The condensation described herein can be carried out in the presence of a carbonate component selected from the group of alkali metal bicarbonates (e.g., sodium bicarbonate (NaHCO3) and potassium bicarbonate (KHCO3)) or from the group of alkali metal carbonates (e.g., potassium carbonate (K2CO3) and sodium carbonate (Na2CO3)). Preferably, the condensation is carried out in the presence of potassium carbonate (K2CO3), sodium carbonate (Na2CO3) or a blend of the two. According to an embodiment, the condensation is carried out in the presence of a low-particle alkali metal carbonate (e.g., comprising anhydrous K2CO3) having a volume average particle size of less than about 100 μm, for example, less than 45 μm, less than 30 μm or less than 20 μm. According to a preferred embodiment, the condensation is carried out in the presence of a carbonate component having a volume average particle size of less than about 100 μm, for example, less than 45 μm, less than 30 μm or less than 20 μm, comprising not less than 50 wt.% of K2CO3 based on the total weight of the base components in the reaction mixture. The volume average particle size of the carbonate used can be determined, for example, using a Mastersizer 2000 from Malvern on a suspension of the particles in chlorobenzene / sulfolane (60 / 40 v / v).

[0115] The molar ratio of carbonate component: dihydroxy monomer (a) may be 1.0 to 1.2, such as 1.01 to 1.15 or 1.02 to 1.1. The molar ratio of carbonate component: dihydroxy monomer (a) is preferably 1.05 or higher, such as 1.06 or 1.08.

[0116] According to the condensation reaction, the reaction mixture (R G ) are usually reacted simultaneously. The condensation is preferably carried out in one stage. This means that the deprotonation of monomer (a) and the condensation reaction between monomers (a) and (b) occur in a single reaction stage without isolation of intermediate products.

[0117] According to the embodiment of PAES polymer manufacturing, condensation is carried out in a mixture of a polar aprotic solvent and a solvent that forms an azeotropic mixture with water. The solvent that forms an azeotropic mixture with water includes aromatic hydrocarbons, such as benzene, toluene, xylene, ethylbenzene, monochlorobenzene, etc. It is preferably toluene or monochlorobenzene. The solvent and polar aprotic solvent that form an azeotropic mixture are typically used in a weight ratio of about 1:20 to about 1:1 or about 1:10 to about 1:1, preferably about 1:5 to about 1:1. Water is continuously removed from the reaction mass as an azeotropic mixture with a solvent that forms an azeotropic mixture, so that a substantially anhydrous condition is maintained during polymerization. After removing the water formed in the reaction, the solvent (e.g., monochlorobenzene) that forms an azeotropic mixture is typically removed from the reaction mixture by distillation, so that PAES is dissolved in a polar aprotic solvent.

[0118] Preferably, the reaction mixture (R G ) does not include any material that forms an azeotropic mixture with water.

[0119] In some embodiments, the process results in a conversion (C) of at least 95%.

[0120] The temperature of the condensation reaction mixture is maintained at about 150°C to about 350°C, preferably about 210°C to about 300°C, for about 1 to 15 hours.

[0121] In this temperature range, the reaction mixture is polycondensed until the desired degree of condensation is reached. Depending on the nature of the starting monomers and the selected reaction conditions, the polycondensation time may be 0.1 to 10 hours, preferably 0.2 to 6 hours, 0.2 to 4 hours or 0.5 to 2 hours.

[0122] Before or after the isolation of the PAES, the inorganic components (eg sodium chloride or potassium chloride or excess base) can be removed by suitable methods such as dissolution and filtration, sieving or extraction.

[0123] According to an embodiment, the amount of PAES at the end of the condensation is at least 30 wt.%, such as at least 35 wt.% or at least 37 wt.% or at least 40 wt.%, based on the total weight of PAES and polar aprotic solvent.

[0124] At the end of the reaction, the PAES polymer is separated from the other components (salt, base, ...) to obtain a PAES solution. Filtration can be used, for example, to separate the PAES polymer from the other components. PAES can be recovered from the solvent, for example, by coagulation in a bath containing a non-solvent such as water and / or a C1-C5 alcohol (preferably methanol), or by devolatilization of the solvent.

[0125] PAES polymers as described herein can be characterized by their weight average molecular weight (Mw). The feature of PAES as described herein is advantageously that the range of its weight average molecular weight (Mw) is between 30,000 g / mol and 150,000 g / mol, or between 40,000 g / mol and 130,000 g / mol, or between 45,000 g / mol and 120,000 g / mol, or between 70,000 g / mol and 110,000 g / mol, or between 70,000 g / mol and 110,000 g / mol. The weight average molecular weight (Mw) of PAES is determined by gel permeation chromatography (GPC) using dichloromethane as mobile phase and calibrated using polystyrene standards.

[0126] Method for producing a shaped article

[0127] The method for making a shaped article according to the present invention may include melt processing a polymer composition comprising a naphthalene diol-based PAES as described herein to form the article. In some embodiments, melt processing includes heating the polymer composition. In a preferred embodiment, melt processing is performed so that the polymer composition is at a temperature of 300° C. to 420° C.

[0128] Suitable melt processing may include extrusion molding, injection molding, blow molding, pultrusion, thermoforming, rotational molding, overmolding, melt and / or powder coating, and / or compression molding of the polymer composition comprising the PAES polymer described herein; injection molding is the preferred molding method when the intention is to produce a shaped article.

[0129] The polymer composition comprising the PAES polymer may further comprise one or more optional additional ingredients, such as one or more polymers different from the naphthalene diol-based PAES described herein, solvents, fillers, lubricants, light stabilizers, UV stabilizers, heat stabilizers, plasticizers, impact modifiers / tougheners, nucleating agents, antioxidants, mold release agents, antistatic agents, flame retardants, antifogging agents, matting agents, pigments, dyes and / or optical brighteners.

[0130] A large amount of selected fillers can be optionally added to the polymer composition. They can be selected from fibrous fillers and particulate fillers. Fibrous fillers are considered to be three-dimensional materials with length, width and thickness in this article, wherein the average length is significantly greater than both width and thickness. Optional fillers can be selected from mineral fillers (such as talc, mica, kaolin, calcium carbonate, calcium silicate, magnesium carbonate), carbon fiber, synthetic polymer fiber, aromatic polyamide fiber, aluminum fiber, titanium fiber, magnesium fiber, boron carbide fiber, rock wool fiber, steel fiber, wollastonite, glass ball (for example, hollow glass microsphere) and / or glass fiber.

[0131] The polymer composition comprising the PAES polymer may comprise greater than 0 wt % and up to 20 wt % (based on the total weight of the polymer composition) of one or more optional additional ingredients (excluding fillers).

[0132] The polymer composition comprising the PAES polymer may comprise more than 5 wt % and up to 70 wt % (based on the total weight of the polymer composition) of one or more optional additional fillers.

[0133] The polymer composition comprising the PAES polymer is preferably provided by melt blending the PAES based on naphthalene diol and one or more optional additional ingredients as described herein before or during the melt processing step. In some cases, the PAES based on naphthalene diol and other optional one or more ingredients (together or added separately) can be fed into a melt mixer, such as a single screw extruder or twin screw extruder, agitator, single screw or twin screw kneader, or Banbury mixer.

[0134] If the polymer composition comprising the PAES polymer further contains a fibrous filler in an elongated physical shape (e.g., 'continuous' fibers having a length of about 50 mm or more, as distinct from chopped or milled fibers having a shorter length), then a reinforced shaped article can be prepared using draw extrusion molding, pultrusion for forming long fiber pellets, or pultrusion for forming unidirectional composite tapes. Pultrusion pulls the polymer composition through a die, as opposed to extrusion, which pushes the polymer composition through a die. Pultrusion is particularly useful for making composite materials.

[0135] Shaped articles comprising the polymer (PAES) can undergo post-manufacturing operations such as ultrasonic welding, adhesive bonding and laser marking as well as heat staking, threading and machining.

[0136] Uses of molded products

[0137] Another aspect of the present disclosure relates to the use of shaped articles in food, beverage, medical, automotive, aerospace, electrical, electronic and industrial product applications and / or in composite materials.

[0138] As non-limiting examples, the shaped articles may be used in biomedical applications such as biomedical tubing, food and beverage applications such as baby bottles or other food containers, coatings, and / or tough thermoplastic composites.

[0139] Should the disclosure of any patents, patent applications, and publications incorporated herein by reference conflict with the description of the present application to the extent that a term may be unclear, the present description shall take precedence.

[0140] Exemplary embodiments will now be described in the following non-limiting examples.

[0141] Examples

[0142] raw materials

[0143] 4,4'-Dichlorodiphenyl sulfone (DCDPS), available from Solvay Speciality Polymers

[0144] 1,5-Naphthalene diol (1,5-NDO), available from Sigma-Aldrich

[0145] 2,7-Naphthalenediol (2,7-NDO), available from Sigma-Aldrich

[0146] 2,3-Naphthalene diol (2,3-NDO), available from Sigma-Aldrich

[0147] K2CO3 (potassium carbonate), available from Armand Products

[0148] Sulfolane, available from Chevron Phillips

[0149] Chlorobenzene, available from Sigma-Aldrich

[0150] DMSO, available from Sigma-Aldrich

[0151] NaOH, available from Sigma-Aldrich

[0152] PSU P3500, available from Solvay Specialty Polymers

[0153] PPSU R5100, available from Solvay Specialty Polymers

[0154] PES 300MP, available from Solvay Specialty Polymers

[0155] Polyetherimide (PEI) 1010, available from Saudi Basic Industries Corporation (SABIC)

[0156] Test Method

[0157] GPC-Molecular weight (Mn, Mw)

[0158] Use dichloromethane as mobile phase to measure the molecular weight (Mn, Mw) of polysulfone based on naphthalene diol by gel permeation chromatography (GPC). Use two 5 μ mixed D columns with guard columns from Agilent Technologies (Agilent Technologies) to separate. Use the ultraviolet detector of 254nm to obtain chromatogram. Select the flow velocity of 1.5ml / min of 0.2w / v% solution in mobile phase and the injection volume of 20 μL. Use 12 kinds of narrow molecular weight polystyrene standards (peak molecular weight range: 371,000 to 580g / mol) to calibrate. Report the molecular weight average (Mn, Mw) defined as follows:

[0159]

[0160] Where Wi is the weight of a molecule with molecular weight Mi.

[0161] PDI

[0162] The sulfone polymers based on naphthalene diol are also characterized by their respective polydispersity index (hereinafter "PDI" or "PDI index"), sometimes also referred to as the multimolecularity index. The polydispersity or multimolecularity corresponds to the molecular weight distribution of the various macromolecules within the polymer. The PDI is calculated from the ratio Mw / Mn, with the number average molecular weight Mn and the weight average molecular weight Mw being determined as described in detail above.

[0163] Thermogravimetric analysis (TGA)

[0164] TGA experiments were performed using a TA Instrument TGA Q500. TGA measurements were obtained by heating the sample from 20°C to 800°C at a heating rate of 10°C / min under nitrogen.

[0165] 1 H NMR

[0166] Measured using a 400 MHz Bruker spectrometer with TCE or DMSO as the deuterated solvent 1 H NMR spectroscopy. All spectra are referenced to residual protons in the solvent.

[0167] Differential Scanning Calorimetry (DSC)

[0168] DSC was used to determine the glass transition temperature (Tg) and melting point (Tm) (if present). The DSC experiment was performed using the Q100 of TA Instruments. The DSC curve was recorded by heating, cooling, reheating and then recooling the sample at a heating and cooling rate of 20°C / min between 25°C and 320°C. All DSC measurements were taken under nitrogen purge. Unless otherwise noted, the Tg value reported was provided using the second heating curve.

[0169] Elastic modulus

[0170] The elastic modulus 'E' (or tensile modulus) was measured using the TA Instruments ARES-G2 rotational rheometer according to ASTM D5279-Dynamic Mechanical Properties in Torsion at two different temperatures: 50°C ('E 50 ') and 190℃('E 190 '). A temperature ramp from 10°C to 200°C at 5°C / min with a frequency of 10 Hz and a strain of 0.05% was used. Sample specimens in the form of 500 micron thick sheets were manufactured using a compression molding process.

[0171] VR40

[0172] Melt stability was measured using a Dynisco LCR 7000 capillary rheometer using ASTM D3835. A measuring temperature of 380°C or 410°C and a melt time of 300 seconds were used. The shear rate was 46.4 1 / s and a die ratio of L / D of 20 was used. Melt stability VR40 was calculated by the ratio of the viscosity measured at 40 minutes (2400 seconds) to the viscosity measured at 10 minutes (600 seconds) at a given temperature.

[0173] Example 1: Synthesis of 2,7-naphthalenediol-based polysulfone (P1) using weak base reaction conditions (K2CO3) and DCDPS

[0174]

[0175] Scheme 1 - Preparation of 2,7-NDO-based polysulfone (P1)

[0176] 2,7-NDO based polysulfone (P1) was prepared according to Scheme 1.

[0177] The polymerization took place in a (1-L) glass reactor vessel equipped with an overhead stirrer, nitrogen inlet, and overhead distillation apparatus. Monomers: 4,4'-dichlorodiphenyl sulfone (200.49 g) and 2,7-naphthalene diol (112.12 g) were first added to the vessel followed by potassium carbonate (105.43 g) and sulfolane (611.6 g). The reaction mixture was heated from room temperature to 210°C using a heating ramp of 150°C / min. The temperature of the reaction mixture was maintained for 45 minutes to 1 hour depending on the viscosity of the solution. The reaction was terminated by the addition of methyl chloride and sulfolane, thereby stopping the heating. The reaction mixture was filtered, coagulated in methanol and dried at 110°C.

[0178] Characterization of 2,7-NDO-based sulfone polymer (P1)

[0179] Table 1

[0180] <![CDATA[M w (g / mol)]]> 82000 <![CDATA[M n (g / mol)]]> 26981 <![CDATA[M w / M n =PDI]]> 3.04 DSC-2nd heating-Tg(℃) 209 <![CDATA[TGA - Initial T 分解 (°C)]]> 542

[0181] Example 2: Synthesis of 2,7-naphthalene diol-based sulfone polymer (P2) using strong base reaction conditions (NaOH) and DCDPS

[0182]

[0183] Scheme 2 - Preparation of 2,7-NDO-based sulfone polymer (P2)

[0184] According to Scheme 2, a 2,7-NDO based sulfone polymer (P2) was prepared.

[0185] Polymerization occurs in a (1-L) glass reactor vessel equipped with an overhead stirrer, nitrogen inlet and Vigreux fractionation column (a modified barrette water separator with a water-cooled condenser). First, 2,7-naphthalene diol (93.62 g), DMSO (54.4 g) and monochlorobenzene (319 g) are added to the vessel, then a stoichiometric amount of NaOH in the form of a 50% aqueous solution is slowly added to the mixture and purged with nitrogen at room temperature for half an hour. The reaction is dehydrated using monochlorobenzene azeotropically until the internal reaction temperature reaches about 150°C, after which DCDPS (169.43 g) is introduced as a hot solution in monochlorobenzene (129 g) at a temperature of about 120°C. The reaction temperature is increased to 170°C and the reaction is continued until a high molecular weight polymer is formed. The reaction mixture is quenched with monochlorobenzene (400 g) and cooled to 120°C.

[0186] The reaction was terminated by slowly introducing methyl chloride gas for 20 minutes (about 20-22 g). After the addition of methyl chloride, 2.7 g of caustic aqueous solution (25 wt% NaOH) was added, and the mixture was stirred for 15 minutes, followed by the addition of methyl chloride (15-20 g). The reaction mixture was cooled to 90°C by adding 200 g of monochlorobenzene. Dilute oxalic acid DMSO solution (1.7 g in 193 g DMSO) was added to the reaction mixture until a pH of 4 (as measured by pH test paper) was obtained. The reaction mixture was filtered, condensed in methanol, washed twice with methanol and dried at 110°C.

[0187] Characterization of 2,7-NDO-based sulfone polymer (P2)

[0188] Table 2

[0189] Mw(g / mol) 48239 Mn(g / mol) 18542 Mw / Mn=PDI 2.6

[0190] Example 3: Synthesis of 1,5-naphthalene diol sulfone polymer (P3) using weak base reaction conditions (K2CO3) and DCDPS

[0191]

[0192] Scheme 3 - Preparation of 1,5-NDO-based sulfone polymer (P3)

[0193] According to Scheme 3, a 1,5-NDO based sulfone polymer (P3) was prepared.

[0194] The polymerization was carried out in a glass reactor vessel (1-L) equipped with an overhead stirrer, a nitrogen inlet and an overhead distillation apparatus. The monomers 4,4'-dichlorodiphenyl sulfone (200.99 g), 1,5 dihydroxynaphthalene (112.11 g) were first added to the vessel, followed by potassium carbonate (145.15 g) and sulfolane (395.35 g). The reaction mixture was heated from room temperature to 210°C using a heating ramp of 150°C / min. The temperature of the reaction mixture was maintained for 45 minutes to 1 hour, depending on the viscosity of the solution. The reaction was terminated by addition of methyl chloride and sulfolane, thereby stopping the heating. The reaction mixture was filtered, condensed in methanol and dried at 110°C.

[0195] Characterization of 1,5-NDO-based sulfone polymer (P3)

[0196] Table 3

[0197] Mw(g / mol) 102983 Mn(g / mol) 22172 Mw / Mn=PDI 4.64

[0198] Example 4: Synthesis of 2,3-naphthalenediol-based polysulfone (P4) using weak base reaction conditions (K2CO3) and DCDPS

[0199]

[0200] Scheme 4 - Preparation of 2,3-NDO-based polysulfone (P4)

[0201] 2,3-NDO based polysulfone (P4) was prepared according to Scheme 4.

[0202] Polymerization occurs in a 1-L glass reactor vessel equipped with an overhead stirrer, nitrogen inlet and overhead distillation apparatus. First, DCDPS (201.04 g) and 2,3-naphthalene diol (112.1 g) are added to the vessel, followed by potassium carbonate (145.1 g) and sulfolane (393 g). The reaction mixture is heated from room temperature to 210 ° C using a heating ramp of 150 ° C / min. Depending on the viscosity of the solution, the temperature of the reaction mixture is maintained for 45 minutes to 1 hour. The reaction is terminated by addition of methyl chloride and sulfolane, thereby stopping heating. The reaction mixture is filtered, condensed in methanol and dried at 110 ° C.

[0203] Characterization of 2,3-NDO-based sulfone polymer (P4)

[0204] Table 4

[0205] Mw(g / mol) 83310 Mn(g / mol) 7083 Mw / Mn=PDI 11.7 (Tg℃)DSC 202.4

[0206] Example 5: Melt Stability Evaluation

[0207] VR40 measurements were performed at 380°C and 410°C for the 2,7-NDO based sulfone polymer (P1) prepared in Example 1 and are reported in Table 5.

[0208] At a VR40 of about 1 at 380°C, the melt viscosity of polymer (P1) did not change measurably within 35 minutes (40 minutes - 5 minutes). Thus, polymer P1 with a VR40 closer to 1 has increased melt viscosity stability relative to other polymers with a VR40 further away from 1.

[0209] The VR40 value measured at 410°C was 1.9.

[0210] The results showed that the material could be hot processed.

[0211] Table 5

[0212] VR40(410℃) 1.9 VR40(380℃) 0.98

[0213] Example 6: Elastic modulus and Tg

[0214] For the 2,7-NDO-based sulfone polymer (P1) prepared in Example 1 and for the 1,5-NDO-based sulfone polymer (P3) prepared in Example 3, elastic modulus measurements were performed at 50°C and 190°C.

[0215] For comparison, a commercially available amorphous sulfone polymer, PSU sold by Solvay Specialty Polymers P3500、PPSU R5100 and PES 300MP, and commercially available amorphous polyetherimide polymers sold by Saudi Basic Industries Corporation Elastic modulus of 1010 at 50°C and 190°C.

[0216] At 50℃(E 50 ) and 190℃(E 190 ) and the loss percentage of elastic modulus ("loss %") = (E 50 -E 190 ) / E 50 ) and Tg (measured by DSC) are reported in Table 6.

[0217] Table 6

[0218]

[0219] The results in Table 6 show that the 2,7-NDO based polymer (P1) outperforms the PSU, PPSU and 1,5-NDO based polymers (P3). Compared with PES, the 2,7-NDO based polymer (P1) has very similar thermomechanical properties. When the temperature increases from 50°C to 190°C, the 2,7-NDO based polymer (P1) has an 11% loss in elastic modulus, while PES had a 9% loss. The other tested polymers had losses ranging from 18% to 71%. Because the 2,7-NDO based polymer (P1) is made from diol monomers, unlike the 2,7-NDO based polymer (P2) made from bisphenol S (BPS), Since 2,7-NDO-based polymers (P1) have much lower estrogenic activity than PES (see the results in Example 7), articles comprising or made from 2,7-NDO-based polymers (P1) have advantages over 2,7-NDO-based polymers in applications where endocrine activity or toxicity may be a problem. Advantages of PES.

[0220] Example 7: EC for Estrogen Receptor α (ERα) 50 (nM) Response value determination

[0221] Response value "EC 50 ” is achieved by using The cell-based nuclear receptor assay uses β-lactamase reporter gene technology, which is notably described in US5,955,604 and US2014 / 113093A1, both of which are incorporated herein by reference in their entirety.

[0222] Monomers (see Table 7) were dissolved in 100% biological grade DMSO at concentrations ranging from 7 to 250,000 nM (nanomolar). TM 293 cells to measure EC 50 .EC 50 The higher the value, the weaker the estrogen agonist activity of the tested monomer.

[0223] ER-α-UAS-bla GripTite TM The cells contain the ligand binding domain (LBD) of the human estrogen receptor α (ERα) stably integrated in UAS-bla GripTite TM Cell lines fused to the DNA binding domain of the GAL4 plasmid. UAS-bla GripTite TM The cells stably express a β-lactamase reporter gene under the transcriptional control of an upstream activation sequence (UAS). When an estrogen agonist binds to the LBD of a GAL4(DBD)-ERα(LBD) fusion protein, the protein binds to the UAS, resulting in the expression of β-lactamase.

[0224] The results in Table 7 show that the three naphthalene diol isomers tested (1,5-NDO, 2,3-NDO, 2,7-NDO) have much lower estrogenic activity on ERα cells than BPA, BPS and BP. Their respective EC 50 The value is at least 30000 nM, that is, at least 10 times higher than BP and at least 100 times higher than BPA.

[0225] Table 7

[0226] Diol Monomer <![CDATA[EC 50 (nM)]]> BPA 263 BPS 791 BP 2920 1,5-NDO >79100 2,7-NDO 32000 2,3-NDO >79100

Claims

1. A shaped article comprising at least one poly(aryl ether sulfone) (PAES) polymer, wherein the PAES comprises at least 80 mol.% of repeating units (R) having formula (I), based on the total moles of repeating units in the PAES polymer. PAES ): in: -E is selected from formula (IIa) and / or formula (IIb) - each R' is independently at each position an alkyl group having 1 to 5 carbon atoms; and - j' is 0 or an integer from 1 to 10, preferably j'=0.

2. The molded product according to claim 1, wherein The PAES polymer comprises at least 90 mol.% of repeating units (R PAES ), said mol. % is based on the total moles of repeating units in the PAES polymer.

3. The shaped article according to claim 1 or 2, which is substantially free of 4,4'-dihydroxydiphenyl sulfone (BPS), 4,4'-isopropylidene diphenol (BPA) and / or 4,4'-biphenol (BP).

4. A shaped article as claimed in any one of the preceding claims, wherein These repeating units (R PAES ) wherein E is selected from the group consisting of: and any combination thereof.

5. The shaped article according to any one of claims 1 to 4, wherein These repeating units (R PAES ) is selected from the group consisting of formula (Ia), (Ib), (Ic) and any combination thereof:

6. The molded article according to claim 6, wherein These repeating units (R PAES ) has a formula selected from formula (Ia) and / or (II-b), preferably has formula (Ia).

7. The shaped article according to any one of claims 1 to 5, which is obtained by reacting the following reaction mixture (R G ) to obtain: - at least one aromatic dihydroxy monomer (a), comprising at least 50 mol.%, based on the total moles of monomers (a), of at least one naphthalene diol monomer (a1) having the formula (IIIa) and / or (IIIb): and / or at least one aromatic dihalogen sulfone monomer (b), comprising at least 50 mol % of a monomer (b1) having the formula (IV), based on the total moles of monomer (b): - at least one carbonate component; - in a solvent; in: - each R' is independently at each position an alkyl group having 1 to 5 carbon atoms; - j' is an integer from 0 to 10, preferably j'=0; and -X is a halogen atom, preferably F or Cl, more preferably Cl.

8. The molded article according to claim 7, wherein The naphthalene diol monomer (a1) has an EC of at least 30,000 nM for estrogen receptor α (ERα). 50 Response value.

9. The molded product according to claim 7 or 8, wherein The monomer (b) contains at least 50 mol% of 4,4'-dichlorodiphenyl sulfone (DCPDS) and / or 4,4'-difluorodiphenyl sulfone (DFPDS) as monomer (b1), based on the total moles of the aromatic dihalogen sulfone monomer (b).

10. The shaped article according to any one of claims 7 to 9, wherein The monomer (a) does not include at least one of 4,4'-dihydroxydiphenyl sulfone (BPS), 4,4'-isopropylidene diphenol (BPA) and / or 4,4'-biphenol (BP).

11. The shaped article according to any one of claims 1 to 10, wherein The PAES polymer has at least one of the following properties: - High elastic modulus at high temperatures (as measured by ASTM D5279 at 190°C 190 ≥400MPa, preferably ≥600MPa, more preferably ≥800MPa); and / or - Suitable melt stability represented by VR40, wherein VR40 is the ratio of the melt viscosity at 40 minutes ("MV40") to the melt viscosity at 5 minutes ("MV5"), the melt viscosity being measured using ASTM D3835: VR40 = MV40 / MV5 (e.g., VR40 measured at 380°C of 0.95 to 1.05 or VR40 measured at 410°C of ≤ 2, preferably ≤ 1.9); and / or - A glass transition temperature Tg of -200°C to 250°C or 205°C to 240°C, wherein Tg is measured via differential scanning calorimetry (DSC).

12. The shaped article according to any one of claims 1 to 11, wherein The PAES polymer has a low thermal loss of elastic modulus (loss %) of at most 15%, preferably at most 13%, more preferably at most 11%, Where loss% = (E 50 -E 190 ) / E 50 , the E 50 is the elastic modulus of the polymer material measured at 50°C, and E 190 is the elastic modulus of the polymer material, both measured using ASTM D5279.

13. The shaped article according to any one of claims 1 to 12, selected from the group consisting of a tube, a food or beverage container such as a milk bottle, a catheter, a fitting, a housing, a coating, a composite material or any part thereof.

14. A method for making a shaped article as claimed in any one of claims 1 to 13, comprising melt processing a polymer composition comprising the PAES polymer to form the article, wherein the melt processing comprises heating the polymer composition.

15. The method of claim 14, wherein: The melt processing includes extrusion molding, injection molding, blow molding, pultrusion, thermoforming, rotational molding, overmolding, melt and / or powder coating and / or compression molding of the polymer composition, preferably includes injection molding.

16. The method according to any one of claims 14 to 15, wherein: The polymer composition further comprises at least one additional ingredient selected from the group consisting of: one or more polymers different from the PAES polymer, solvents, fillers, lubricants, light stabilizers, UV stabilizers, heat stabilizers, plasticizers, impact modifiers / tougheners, nucleating agents, antioxidants, mold release agents, antistatic agents, flame retardants, antifogging agents, matting agents, pigments, dyes, and optical brighteners.

17. Use of the shaped article according to any one of claims 1 to 13 in biomedical applications, food and / or beverage applications, automotive applications, aerospace applications, electrical and / or electronic applications, industrial product applications and / or in composite materials.