Optical laminate, image display panel, and image display device
By using organic cationic conductive agents and specific crosslinking agents in the optical laminate, the color difference is controlled, and the problem of image quality reduction and yellowing under high-photo backlights is solved, thereby achieving efficient anti-static and durability improvement.
Patent Information
- Application Number
- CN202380029121.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-14
- Filing Date
- 2023-04-12
- Publication Date
- 2024-11-05
AI Technical Summary
When using an optical laminated body containing an adhesive sheet containing a conductive agent and a high-photo backlight, the image quality is likely to be reduced, especially in a high-temperature environment, which may affect the display effect.
Adhesive sheets containing organic cationic conductive agents, and the color difference of the optical laminate|Δb*| is less than 0.60 through a specific optical laminate structure and material combination, and combines isocyanate crosslinking agents and peroxides. The crosslinking agent forms a heat-resistant and anti-static optical laminate.
It effectively suppresses the yellowing of the image under high-light irradiation and heating, improves the durability and anti-static performance of the image display panel, and ensures the image quality stability in the environment of high-light backlight.
Smart Images

Figure CN118901030A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an optical laminate, an image display panel and an image display device. Background Art
[0002] In recent years, image display devices represented by liquid crystal display devices have been rapidly popularized. The above-mentioned various image display devices, for example, have a laminated structure of an image display unit such as a liquid crystal unit, an optical laminate including an optical film such as a polarizing film, and an adhesive sheet. The adhesive sheet is mainly used for bonding the optical films contained in the optical laminate, and bonding the image display unit and the optical laminate.
[0003] For image display devices, static electricity is generated during their manufacture (for example, when an optical laminate is attached to an image display unit via an adhesive sheet) or during use (for example, when a user touches the image display device). If the image display device is charged due to the static electricity, problems such as poor display may occur. In an environment where static electricity is particularly likely to be generated, such as the interior of a vehicle where other electronic devices are present around, when the image display device is used, in order to fully prevent poor display caused by the charging of the image display device, it may be considered to add a conductive agent to the adhesive composition. Patent document 1 discloses an adhesive composition comprising a (meth) acrylic polymer having a specific composition and a conductive agent.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2018-123330 Summary of the invention
[0007] Problems to be solved by the invention
[0008] Depending on the type of image display device, a lighting system including a backlight can be combined. In recent years, there has been a demand for increasing the luminance of the irradiated light from the backlight in order to achieve high quality of displayed images and optimization in various usage environments. However, it has been found that when an optical laminate using an adhesive sheet containing a conductive agent is combined with a high-luminance backlight, a decrease in image quality occurs that has not been observed in the conventional combination with the backlight.
[0009] An object of the present invention is to provide an optical laminate including a polarizing film and a pressure-sensitive adhesive sheet, which is suitable for use in an image display panel assuming a combination with a high-intensity backlight despite having a pressure-sensitive adhesive sheet containing a conductive agent.
[0010] Solutions to the problem
[0011] The present invention provides an optical laminate comprising a polarizing film and an adhesive sheet.
[0012] The adhesive sheet contains an organic cationic conductive agent.
[0013] The optical laminate has a |Δb of less than 0.60 * |,
[0014] Among them, the above |Δb * | is the chromaticity difference Δb determined by the following evaluation method * The absolute value of
[0015] <Evaluation Method>
[0016] (1) The optical laminate is cut into a rectangle of 220 mm×110 mm with the absorption axis of the polarizing film as the long side, and a glass plate is laminated with the polarizing film and the adhesive sheet sandwiched therebetween to form a test sample;
[0017] (2) placing the test sample formed above on a surface light source, irradiating the entire test sample with white light having a luminous intensity of 15,000 candela through the surface light source, and performing a heating test at 95° C. and for 500 hours;
[0018] (3) The test sample after the heating test was irradiated with white light of 15,000 candela through the surface light source, and the L values of the transmitted light of the white light at the center and the end of the test sample were measured. * a * b * Chroma b in color system * 0 and b * 1, and according to the formula: Δb * =b * 1-b * 0 to find the above Δb * .
[0019] From another aspect, the present invention provides an image display panel including the above-mentioned optical layered body.
[0020] From another aspect, the present invention provides an image display device including the above-mentioned image display panel.
[0021] Effects of the Invention
[0022] According to the present invention, there is provided an optical laminate including a polarizing film and a pressure-sensitive adhesive sheet, which is suitable for use in an image display panel assuming a combination with a high-intensity backlight despite having a pressure-sensitive adhesive sheet containing a conductive agent. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1This is a cross-sectional view schematically showing an example of the optical layered body of the present invention.
[0024] Figure 2 This is a cross-sectional view schematically showing an example of the optical layered body of the present invention.
[0025] Figure 3 This is a cross-sectional view schematically showing an example of the optical layered body of the present invention.
[0026] Figure 4 This is a cross-sectional view schematically showing an example of the optical layered body of the present invention.
[0027] Figure 5 This is a cross-sectional view schematically showing an example of the image display panel of the present invention.
[0028] Figure 6 This is a cross-sectional view schematically showing an example of the image display panel of the present invention.
[0029] Figure 7 This is a cross-sectional view schematically showing an example of the image display panel of the present invention. DETAILED DESCRIPTION
[0030] The optical layered body according to the first aspect of the present invention comprises a polarizing film and a pressure-sensitive adhesive sheet.
[0031] The adhesive sheet contains an organic cationic conductive agent.
[0032] The optical laminate has a |Δb of less than 0.60 * |.
[0033] Among them, the above |Δb * | is the chromaticity difference Δb determined by the following evaluation method * The absolute value of .
[0034] <Evaluation Method>
[0035] (1) The optical laminated body obtained by cutting out a rectangle of 220 mm×110 mm with the absorption axis of the polarizing film as the long side was laminated on glass plates so as to sandwich the pressure-sensitive adhesive sheet together with the polarizing film to prepare a test sample.
[0036] (2) The test sample formed as above was placed on a surface light source, and the surface light source was used to irradiate the entire test sample with white light having a luminous intensity of 15,000 candela, while a heating test at 95° C. and for 500 hours was performed.
[0037] (3) The test sample after the heating test was irradiated with white light of 15,000 candela through the surface light source, and the L values of the transmitted light of the white light at the center and the end of the test sample were measured.* a * b * Chroma b in color system * 0 and b * 1, and according to the formula: Δb * =b * 1-b * 0 to find the above Δb * .
[0038] In the second aspect of the present invention, for example, in the optical laminate of the first aspect, the pressure-sensitive adhesive sheet has 9×10 11 Surface resistivity below Ω / □.
[0039] In a third aspect of the present invention, for example, in the optical layered body of the first or second aspect, the pressure-sensitive adhesive sheet is a sheet formed of a pressure-sensitive adhesive composition containing a (meth)acrylic polymer as a main component.
[0040] In a fourth aspect of the present invention, for example, in the optical layered body of the third aspect, the (meth)acrylic polymer has a structural unit derived from a hydroxyl group-containing monomer at a content of 1% by weight or less.
[0041] In a fifth aspect of the present invention, for example, in the optical layered body of the third or fourth aspect, the (meth)acrylic polymer has a structural unit derived from a carboxyl group-containing monomer at a content of 3% by weight or more.
[0042] In a sixth aspect of the present invention, for example, in the optical layered body according to any one of the first to fifth aspects, the pressure-sensitive adhesive sheet is a sheet formed of a pressure-sensitive adhesive composition containing an isocyanate-based crosslinking agent.
[0043] In a seventh aspect of the present invention, for example, in the optical layered body according to the sixth aspect, the isocyanate-based crosslinking agent is a non-aromatic ring-based crosslinking agent.
[0044] In an eighth aspect of the present invention, for example, in the optical layered body of the sixth or seventh aspect, the pressure-sensitive adhesive composition further contains a peroxide-based crosslinking agent.
[0045] An image display panel according to a ninth aspect of the present invention includes the optical layered body according to any one of the first to eighth aspects.
[0046] An image display device according to a tenth aspect of the present invention includes the image display panel according to the ninth aspect.
[0047] In the eleventh aspect of the present invention, for example, the image display device according to the tenth aspect further comprises an illumination system including a backlight, wherein the luminous intensity of light irradiated by the backlight to the image display panel is 15000 candela or more.
[0048] Hereinafter, the present invention will be described in detail, but the present invention is not limited to the following embodiments and can be implemented with arbitrary modifications within the scope of the present invention.
[0049] [Optical laminate]
[0050] An example of the optical layered body of the present embodiment is shown in Figure 1 . Figure 1 The optical laminate 10 (10A) includes an adhesive sheet 1 and a polarizing film 2. The polarizing film 2 generally includes a polarizer. The adhesive sheet 1 and the polarizing film 2 are laminated together. The optical laminate 10A can be bonded to an object (e.g., an image display panel) via the adhesive sheet 1. The optical laminate 10A can be used as an optical film with an adhesive sheet, more specifically, as a polarizing film with an adhesive sheet.
[0051] The pressure-sensitive adhesive sheet 1 contains an organic cationic conductive agent. In addition, the optical laminate 10 has a |Δb of less than 0.60. * |. Among them, |Δb * | is the chromaticity difference determined by the following evaluation method, more specifically, the chromaticity b observed when white light is transmitted between the center and the end of the optical layered body 10 * The difference (chromaticity difference Δb * ) is the absolute value of . Chroma b * It is through L * a * b * b determined by the color system (CIELAB color system) * .
[0052] <Evaluation method>(Δb * )
[0053] (1) For an optical laminate 10 obtained by cutting out a rectangle having a size of 220 mm × 110 mm with the absorption axis of the polarizing film 2 as the long side, a glass plate is laminated in a manner of sandwiching an adhesive sheet 1 together with the polarizing film 2 to form a test sample. The glass plate can be selected as an alkali-free glass plate that does not substantially contain an alkali component (alkali metal oxide). The weight ratio of the alkali component in the alkali-free glass is, for example, less than 1000 ppm, or less than 500 ppm. The thickness of the glass plate is, for example, about 0.5 to 1 mm. In the optical laminate 10 in which the adhesive sheet 1 is exposed, the adhesive sheet 1 can be bonded to the glass plate. In this case, reflection of light at the interface between the optical laminate 10 and the glass plate can be suppressed.
[0054] (2) While the formed test sample is placed on a surface light source, a heating test is performed at 95°C and for 500 hours while irradiating the entire test sample with white light having a luminosity of 15,000 candela through the surface light source. The test sample can be placed in a manner such that the glass plate is in contact with the surface light source. The surface light source can be, for example, a backlight that can be used for an image display device such as a liquid crystal display device. The irradiated white light is usually set to be light equivalent to the CIE standard light source D65 (color temperature 6500K). The heating test can be performed, for example, by placing the surface light source and the test sample in a heating furnace that can be maintained at a given temperature.
[0055] (3) The test sample after the heating test was irradiated with white light of 15000 candela through the surface light source, and the chromaticity b of the transmitted light of the white light observed at the center and end of the test sample was measured respectively. * (For the central part, b * 0, for the end b * 1). According to the formula: Δb * =b * 1-b * 0Calculate the chromaticity difference Δb * The center is defined as a circular area with a diameter of 30 mm centered at a position 110 mm in the long side direction and 55 mm in the short side direction from the corner of the rectangular test sample. The end is defined as a circular area with a diameter of 30 mm centered at a position 30 mm in each direction of the long side and the short side from the corner of the test sample. There are four end portions for one test sample. b * 1 can be determined as the average value of the measured values at each end. The irradiated white light is as described above. b * In the determination of L * a * b * Chroma b of the color system * The measurement is usually carried out at room temperature (25°C ± 5°C).
[0056] The inventors of the present invention have found out through research that when the adhesive sheet 1 contains an inorganic cationic conductive agent (typically a conductive agent containing cations of alkali metals), there is a tendency for the above-mentioned image quality to be visually recognizable only when combined with a high-intensity backlight; the quality reduction is typically observed as yellowing at the periphery of the image; and the above-mentioned tendency becomes particularly strong in the case of a high-temperature environment such as the interior of a vehicle after summer. As the cause of yellowing, the following mechanism can be inferred: the various components contained in the adhesive sheet 1 will be denatured due to free radicals generated by inorganic cations, heat and light, and oxygen diffused from the end face to the inside of the adhesive sheet 1. It should be noted that in the denaturation, free radicals generated starting from free radicals generated by inorganic cations and other components (for example, various additives such as polymerization initiators, crosslinking agents and antioxidants, and polymers having chemical structures in which free radicals such as polar groups and polymerization groups can play a role) will also play a role. According to further research, organic cationic conductive agents are suitable for inhibiting the generation of free radicals and inhibiting the yellowing of the above-mentioned periphery. Furthermore, in the optical laminate 10, the chromaticity b after irradiation with high-intensity light and heating is between the center and the end portions. * Therefore, the optical laminate 10 is preferably used for an image display panel that is assumed to be combined with a high-intensity backlight, although it includes a pressure-sensitive adhesive sheet containing a conductive agent.
[0057] |Δb of the optical laminate 10 * | may be 0.58 or less, 0.55 or less, 0.53 or less, 0.50 or less, 0.48 or less, 0.45 or less, 0.43 or less, 0.40 or less, 0.38 or less, 0.35 or less, 0.33 or less, 0.30 or less, 0.28 or less, 0.25 or less, and may further be 0.23 or less. |Δb * The lower limit of | is, for example, 0.05 or more, and may be 0.10 or more.
[0058] (Adhesive Sheet)
[0059] For example, the adhesive sheet 1 has 9×10 11 The surface resistivity of the adhesive sheet 1 can be 5×10 11 Ω / □ or less, 3×10 11 Ω / □ or less, 2×10 11 Ω / □ or less, 1×10 11 Ω / □ or less, 9×10 10 Ω / □ or less, 5×10 10 Ω / □ or less, 3×10 10 Ω / □ or less, 1×10 10 Ω / □ or less, 9×10 9Ω / □ or less, 5×10 9 Ω / □ or less, 3×10 9 Ω / □ or less, and can be further 1×10 9 Ω / □ or less. The lower limit of the surface resistivity is, for example, 1×10 6 Ω / □ or more, or 1×10 7 Ω / □ or more. The optical layered body 10 having the surface resistivity of the pressure-sensitive adhesive sheet 1 within the above range is suitable for use in an environment where static electricity is easily generated, such as the interior of a vehicle.
[0060] <Polymer>
[0061] Adhesive sheet 1 is, for example, a sheet formed by an adhesive composition containing a polymer as a main component. Examples of polymers are (meth) acrylic polymers, urethane polymers, silicone polymers and rubber polymers. But the polymer is not limited to the above examples. The polymer is preferably a (meth) acrylic polymer. In other words, adhesive sheet 1 can be a sheet formed by an adhesive composition (I) containing a (meth) acrylic polymer (A) as a main component. The main component refers to the component with the largest content in the composition. The content of the main component is, for example, 50% by weight or more, and can be 60% by weight or more, 70% by weight or more, 75% by weight or more, and further can be 80% by weight or more. In this specification, a (meth) acrylic polymer refers to a polymer having a structural unit derived from a (meth) acrylic monomer, such as a (meth) acrylic ester. The content of the structural unit derived from the (meth)acrylic monomer in the (meth)acrylic polymer is, for example, 40% by weight or more, 50% by weight or more, 60% by weight or more, 70% by weight or more, 80% by weight or more, 85% by weight or more, 90% by weight or more, and further 95% by weight or more. The (meth)acrylic polymer may also be composed only of structural units derived from (meth)acrylic monomers. (Meth)acrylic acid refers to acrylic acid and methacrylic acid. (Meth)acrylate refers to acrylic acid ester and methacrylate ester.
[0062] The (meth)acrylic polymer (A) may have one or two or more structural units derived from the following monomer (A1).
[0063] An example of the monomer (A1) is a (meth)acrylic monomer having an alkyl group having 1 to 30 carbon atoms in a side chain. The alkyl group may be linear or branched. Examples of the (meth)acrylic monomer having an alkyl group in the side chain are methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, n-hexyl (meth)acrylate, isohexyl (meth)acrylate, isoheptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, n-decyl (meth)acrylate, isodecyl (meth)acrylate, n-dodecyl (meth)acrylate (lauryl (meth)acrylate), n-tridecyl (meth)acrylate, n-tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, and octadecyl (meth)acrylate. The content of the structural unit derived from the (meth)acrylic monomer having an alkyl group with 1 to 30 carbon atoms in the side chain of the (meth)acrylic polymer (A) is, for example, 60% by weight or more, 65% by weight or more, 70% by weight or more, 72% by weight or more, 75% by weight or more, 77% by weight or more, 78% by weight or more, and further 79% by weight or less. The upper limit of the content is, for example, 99% by weight or less, 97% by weight or less, 95% by weight or less, 92% by weight or less, 90% by weight or less, 87% by weight or less, 85% by weight or less, and further 82% by weight or less.
[0064] Other examples of monomer (A1) are hydroxyl-containing monomers. Hydroxyl-containing monomers can be hydroxyl-containing (meth) acrylic acid monomers. Examples of hydroxyl-containing monomers are (meth) 2-hydroxyethyl acrylate, (meth) 3-hydroxypropyl acrylate, (meth) 4-hydroxybutyl acrylate, (meth) 6-hydroxyhexyl acrylate, (meth) 8-hydroxyoctyl acrylate, (meth) 10-hydroxydecyl acrylate and (meth) 12-hydroxylauryl acrylate and (meth) 12-hydroxyalkyl acrylates, and acrylate (4-hydroxymethylcyclohexyl) methyl ester. From the viewpoint of improving the durability of the adhesive sheet 1, preferably (meth) 2-hydroxyethyl acrylate, (meth) 4-hydroxybutyl acrylate, more preferably (meth) 4-hydroxybutyl acrylate. (Meth) acrylic polymer (A) can have a structural unit derived from a hydroxyl-containing monomer at a content of less than 1% by weight. The content may be less than 1 wt%, less than 0.9 wt%, less than 0.8 wt%, less than 0.7 wt%, less than 0.6 wt%, less than 0.5 wt%, less than 0.5 wt%, less than 0.4 wt%, less than 0.4 wt%, less than 0.3 wt%, less than 0.3 wt%, less than 0.2 wt%, less than 0.2 wt%, less than 0.15 wt%, less than 0.1 wt%, less than 0.1 wt%, and further may be less than 0.09 wt%. The lower limit of the content is, for example, greater than 0.01 wt%, may be greater than 0.02 wt%, greater than 0.03 wt%, greater than 0.04 wt%, and further may be greater than 0.05 wt%. The content of the structural unit derived from the hydroxyl-containing monomer in the above range can contribute to the improvement of the durability of the adhesive sheet 1, and can particularly contribute to |Δb * |reduction.
[0065] Other examples of monomer (A1) are carboxyl-containing monomers. Carboxyl-containing monomers can be carboxyl-containing (meth) acrylic monomers. Examples of carboxyl-containing monomers are (meth) acrylic acid, (meth) carboxylethyl acrylate, (meth) carboxylpentyl acrylate, itaconic acid, maleic acid, fumaric acid and crotonic acid. From the viewpoint of improving the durability of the adhesive sheet 1, it is preferably (meth) acrylic acid. (Meth) acrylic polymer (A) can have a structural unit derived from a carboxyl-containing monomer at a content of more than 0.5 weight %. The content can be more than 0.7 weight %, more than 1 weight %, more than 1.2 weight %, more than 1.5 weight %, more than 1.7 weight %, more than 2 weight %, more than 2.2 weight %, more than 2.5 weight %, more than 2.7 weight %, more than 3 weight %, more than 3.2 weight %, and further can be more than 3.4 weight %. The upper limit of the content is, for example, less than 10 weight %, can be less than 8 weight %, less than 7 weight %, less than 6 weight %, and further can be less than 5 weight %. The content of the structural unit derived from the carboxyl group-containing monomer within the above range, particularly 3 wt % or more, can contribute to the improvement of the durability of the pressure-sensitive adhesive sheet 1 and particularly contribute to the improvement of |Δb * |reduction.
[0066] Monomer (A1) may be an aromatic ring-containing monomer, an amino group-containing monomer, or an amide group-containing monomer. The aromatic ring-containing monomer may be an aromatic ring-containing (meth)acrylic monomer. Examples of aromatic ring-containing monomers are phenyl (meth)acrylate, phenoxyethyl (meth)acrylate, benzyl (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, ethylene oxide-modified nonylphenol (meth)acrylate, hydroxyethylated β-naphthol (meth)acrylate, and biphenyl (meth)acrylate. Examples of amino group-containing monomers are N,N-dimethylaminoethyl (meth)acrylate and N,N-dimethylaminopropyl (meth)acrylate. Examples of the amide group-containing monomer include acrylamide monomers such as (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-isopropylacrylamide, N-methyl(meth)acrylamide, N-butyl(meth)acrylamide, N-hexyl(meth)acrylamide, N-methylol(meth)acrylamide, N-methylol-N-propyl(meth)acrylamide, aminomethyl(meth)acrylamide, aminoethyl(meth)acrylamide, mercaptomethyl(meth)acrylamide, and mercaptoethyl(meth)acrylamide; N-acryloyl heterocyclic monomers such as N-(meth)acryloylmorpholine, N-(meth)acryloylpiperidine, and N-(meth)acryloylpyrrolidine; and N-vinyl-containing lactam monomers such as N-vinylpyrrolidone and N-vinyl-ε-caprolactam. The (meth)acrylic polymer (A) may not have a structural unit derived from an amino group-containing monomer.
[0067] The content of the structural unit derived from the aromatic ring-containing monomer in the (meth)acrylic polymer (A) is, for example, 20% by weight or less, 19% by weight or less, 18% by weight or less, 17% by weight or less, or 16% by weight or less. The lower limit of the content is, for example, 0% by weight or more, 2% by weight or more, 5% by weight or more, 7% by weight or more, 10% by weight or more, 12% by weight or more, or 15% by weight or more.
[0068] The content of the structural unit derived from the amide group-containing monomer in the (meth)acrylic polymer (A) is, for example, 10% by weight or less, 8% by weight or less, 5% by weight or less, 3% by weight or less, 2% by weight or less, 1.5% by weight or less, and further 1% by weight or less. The lower limit of the content is, for example, 0% by weight or more, 0.2% by weight or more, 0.5% by weight or more, and further 0.7% by weight or more.
[0069] Monomer (A1) may be a multifunctional monomer. Examples of multifunctional monomers include hexanediol di(meth)acrylate (1,6-hexanediol di(meth)acrylate), butanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tetramethylolmethane tri(meth)acrylate, allyl (meth)acrylate, vinyl (meth)acrylate, epoxy acrylate, polyester acrylate, and urethane acrylate; and divinylbenzene. Multifunctional acrylates are preferably 1,6-hexanediol diacrylate and dipentaerythritol hexa(meth)acrylate. The (meth)acrylic polymer (A) may not have a structural unit derived from a multifunctional monomer.
[0070] The total content of the structural units derived from the amino group-containing monomer and the multifunctional monomer in the (meth)acrylic polymer (A) is preferably 5% by weight or less, more preferably 3% by weight or less, and further preferably 1% by weight or less. When the polymer (A) has such structural units, the total content is, for example, 0.01% by weight or more, 0.1% by weight or more, and further 0.5% by weight or more.
[0071] Examples of other monomers (A1) are (meth)acrylate alkoxyalkyl ester monomers such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate; nitrile-containing (meth)acrylates such as (meth)acrylonitrile; epoxy-containing monomers such as glycidyl (meth)acrylate and methylglycidyl (meth)acrylate; sulfonic acid group-containing monomers such as sodium vinyl sulfonate; phosphoric acid group-containing monomers; (meth)acrylates having alicyclic hydrocarbon groups such as cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate and isobornyl (meth)acrylate; vinyl esters such as vinyl acetate and vinyl propionate; aromatic vinyl compounds such as styrene and vinyltoluene; olefins such as ethylene, propylene, butadiene, isoprene and isobutylene, or dienes; vinyl ethers such as vinyl alkyl ether; and vinyl chloride.
[0072] The total content of the structural units derived from the other monomers (A1) in the polymer (A) is, for example, 10 wt% or less, 5 wt% or less, 3 wt% or less, further 1 wt% or less, and preferably 0 wt% (containing no such structural units).
[0073] The polymer (A) can be formed by polymerizing one or more of the above-mentioned monomers using a known method. Monomers and partial polymers of monomers can also be polymerized. The polymerization can be implemented by, for example, solution polymerization, emulsion polymerization, bulk polymerization, thermal polymerization, and active energy ray polymerization. From the viewpoint of being able to form an adhesive sheet with excellent optical transparency, solution polymerization and active energy ray polymerization are preferred. It is preferred to avoid contact between the monomer and / or partial polymer and oxygen and implement polymerization. For this purpose, polymerization in an inactive gas atmosphere such as nitrogen or polymerization in a state where oxygen is blocked by a resin film or the like can be adopted. The polymer (A) to be formed can be any form of a random copolymer, a block copolymer, a graft copolymer, etc.
[0074] The polymerization system for forming the polymer (A) may contain one or more polymerization initiators. The type of polymerization initiator may be selected according to the polymerization reaction, and may be, for example, a thermal polymerization initiator or a photopolymerization initiator.
[0075] The solvent used in the solution polymerization is, for example, esters such as ethyl acetate and n-butyl acetate; aromatic hydrocarbons such as toluene and benzene; aliphatic hydrocarbons such as n-hexane and n-heptane; alicyclic hydrocarbons such as cyclohexane and methylcyclohexane; ketones such as methyl ethyl ketone and methyl isobutyl ketone, but the solvent is not limited to the above examples. The solvent may be a mixed solvent of two or more solvents.
[0076] The polymerization initiator used in the solution polymerization is, for example, an azo polymerization initiator, a peroxide polymerization initiator, and a redox polymerization initiator. Peroxide polymerization initiators are, for example, dibenzoyl peroxide and tert-butyl permaleate. Among them, the azo polymerization initiator disclosed in Japanese Patent Publication No. 2002-69411 is preferred. The azo polymerization initiator is, for example, 2,2'-azobisisobutyronitrile (AIBN), 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2-methylpropionic acid) dimethyl ester, 4,4'-azobis(4-cyanovaleric acid), but the polymerization initiator is not limited to the above examples. The amount of the azo polymerization initiator used is, for example, 0.05 to 0.5 parts by weight, or 0.1 to 0.3 parts by weight relative to 100 parts by weight of the total amount of the monomers.
[0077] The active energy rays used in the active energy ray polymerization are, for example, ionizing rays such as α rays, β rays, γ rays, neutron rays, electron rays, and ultraviolet rays. The active energy rays are preferably ultraviolet rays. Polymerization using ultraviolet irradiation is also called photopolymerization. The polymerization system of active energy ray polymerization typically includes a photopolymerization initiator. The polymerization conditions of the active energy polymerization are not limited as long as the polymer (A) can be formed.
[0078] Photopolymerization initiators include, for example, benzoin ether photopolymerization initiators, acetophenone photopolymerization initiators, α-ketol photopolymerization initiators, aromatic sulfonyl chloride photopolymerization initiators, photoactive oxime photopolymerization initiators, benzoin photopolymerization initiators, benzyl photopolymerization initiators, benzophenone photopolymerization initiators, ketal photopolymerization initiators, and thioxanthone photopolymerization initiators, but the photopolymerization initiators are not limited to the above examples.
[0079] Examples of benzoin ether photopolymerization initiators include benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, benzoin isopropyl ether, benzoin isobutyl ether, 2,2-dimethoxy-1,2-diphenylethane-1-one, and anisole methyl ether. Examples of acetophenone photopolymerization initiators include 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxycyclohexyl phenyl ketone, 4-phenoxydichloroacetophenone, and 4-(tert-butyl)dichloroacetophenone. Examples of α-ketoalcohol photopolymerization initiators include 2-methyl-2-hydroxypropiophenone and 1-[4-(2-hydroxyethyl)phenyl]-2-methylpropane-1-one. Examples of aromatic sulfonyl chloride photopolymerization initiators include 2-naphthalenesulfonyl chloride. An example of a photoactive oxime photopolymerization initiator is 1-phenyl-1,1-propanedione-2-(O-ethoxycarbonyl oxime). An example of a benzoin photopolymerization initiator is benzoin. An example of a benzyl photopolymerization initiator is benzyl. An example of a benzophenone photopolymerization initiator is benzophenone, benzoylbenzoic acid, 3,3'-dimethyl-4-methoxybenzophenone, polyvinylbenzophenone, α-hydroxycyclohexylphenylketone. An example of a ketal photopolymerization initiator is benzyldimethylketal. An example of a thioxanthone photopolymerization initiator is thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-diisopropylthioxanthone, and dodecylthioxanthone.
[0080] The amount of the photopolymerization initiator used is, for example, 0.01 to 1 part by weight, or 0.05 to 0.5 part by weight, relative to 100 parts by weight of the total amount of the monomers.
[0081] The weight average molecular weight (Mw) of polymer (A) is, for example, 1 million to 3 million, preferably 1.8 million to 3 million. By making the weight average molecular weight of polymer (A) 1 million to 3 million, there is a tendency to suppress cracks in the adhesive sheet and to suppress the increase in viscosity and the occurrence of gelation. The weight average molecular weight (Mw) of the polymer in this specification is a value (in terms of polystyrene) obtained by measurement based on GPC (gel permeation chromatography).
[0082] The glass transition temperature (Tg) of the polymer (A) is, for example, -50°C or less, preferably -52°C or less, and more preferably -55°C or less. The lower limit of the Tg of the polymer (A) is, for example, -75°C. The Tg of the polymer (A) is a value obtained by calculating the Tg of each monomer constituting a structural unit of the polymer (A) when a homopolymer is prepared, and averaging these Tgs in consideration of the content of the structural unit.
[0083] The content of the polymer (A) in the adhesive composition (I) is, for example, 50% by weight or more, 60% by weight or more, 70% by weight or more, 75% by weight or more, 80% by weight or more, 85% by weight or more, 90% by weight or more, 92% by weight or more, 95% by weight or more, and further 97% by weight or more. The upper limit of the content is, for example, 99% by weight or less, 98% by weight or less, 97% by weight or less, 95% by weight or less, 92% by weight or less, and further 90% by weight or less.
[0084] <Conductive agent>
[0085] The adhesive sheet 1 contains an organic cationic conductive agent. The adhesive sheet 1 may be a sheet formed of an adhesive composition (I) containing a (meth)acrylic polymer (A) as a main component and further containing an organic cationic conductive agent. The adhesive sheet 1 may contain one or more organic cationic conductive agents.
[0086] An example of an organic cationic conductive agent is an organic cationic salt. Generally, the cationic portion (cationic component) of the organic cationic salt has an organic structure. The anionic portion (anionic component) of the organic cationic salt may have an organic structure or an inorganic structure. The organic cationic salt may be an ionic solid having a melting point of 40° C. or above.
[0087] Examples of cations are organic organic Contained in Examples are nitrogen Sulfur Phosphorus Preferably nitrogen Sulfur Nitrogen Examples are ammonium cations, piperidine Cation, pyrrolidine Cation, pyridine Cation, cation having a pyrroline skeleton, cation having a pyrrole skeleton, imidazole Cation, Tetrahydropyrimidine Cations, dihydropyrimidines Cation, pyrazole Cationic, pyrazoline Cationic. Sulfur An example of a sulfonium cation is a sulfonium cation. An example is Cationic. Organic Examples of organic groups contained in are alkyl, alkoxy, alkenyl. Preferred organic Specific examples are tetraalkylammonium cations (e.g., tributylmethylammonium cations), alkylpiperidinium Cation, alkyl pyrrolidine cation.
[0088] An example of an anion is Cl - Br - ,I - 、AlCl4 - 、Al2Cl7 - 、BF4 - PF6 - 、ClO4 - 、NO3 - 、CH3COO - CF3COO - 、CH3SO3 - CF3SO3 - 、(CF3SO2)3C - 、AsF6 - 、SbF6 - 、NbF6 - 、TaF6 - 、(CN)2N - 、C4F9SO3 - 、C3F7COO - 、(CF3SO2)(CF3CO)N - , - O3S(CF2)3SO3 - , and anions represented by the following general formulae (a) to (d).
[0089] (a)(C n F 2n+1 SO2)2N - (n is an integer from 1 to 10)
[0090] (b)CF2(C m F 2m SO2)2N - (m is an integer from 1 to 10)
[0091] (c) - O3S(CF2) l SO3 - (l is an integer from 1 to 10)
[0092] (d)(C p F 2p+1 SO2)N - (C q F 2q+1 SO2) (p and q are independently integers of 1 to 10)
[0093] Specific examples of the organic cationic conductive agent include 1-ethyl-3-methylimidazolium bis(fluorosulfonyl)imide salt (EMI-FSI) and trimethylbutylammonium bis(trifluoromethanesulfonyl)imide salt.
[0094] The amount of the organic cationic conductive agent in the adhesive composition forming the adhesive sheet 1 is, for example, 0.1 parts by weight or more, 0.3 parts by weight or more, 0.5 parts by weight or more, 0.7 parts by weight or more, 0.9 parts by weight or more, 1 part by weight or more, 3 parts by weight or more, 5 parts by weight or more, and further 7 parts by weight or more, relative to 100 parts by weight of the polymer such as the (meth) acrylic polymer (A). The upper limit of the amount is, for example, 20 parts by weight or less, 15 parts by weight or less, 12 parts by weight or less, 10 parts by weight or less, 8 parts by weight or less, 5 parts by weight or less, 4 parts by weight or less, 3 parts by weight or less, 2 parts by weight or less, and further 1.5 parts by weight or less.
[0095] <Cross-linking agent>
[0096] The PSA composition forming the PSA sheet 1 (for example, the PSA composition (I) containing the (meth)acrylic polymer (A) as a main component) may further contain a crosslinking agent.
[0097] Examples of crosslinking agents are organic crosslinking agents and multifunctional metal chelates. Examples of organic crosslinking agents are isocyanate crosslinking agents, peroxide crosslinking agents, epoxy crosslinking agents and imine crosslinking agents. Organic crosslinking agents and multifunctional metal chelates can be used for any type of adhesive composition in solvent-based and active energy ray-curable types. In the case where the adhesive composition is solvent-based, the crosslinking agent is preferably an isocyanate crosslinking agent and a peroxide crosslinking agent. It is also possible to use an isocyanate crosslinking agent in combination with a peroxide crosslinking agent. The adhesive composition may include an isocyanate crosslinking agent. In other words, the adhesive sheet 1 may be a sheet formed by an adhesive composition (such as adhesive composition (I)) containing an isocyanate crosslinking agent. The adhesive composition may include a peroxide crosslinking agent. The adhesive composition may also include both an isocyanate crosslinking agent and a peroxide crosslinking agent. In other words, the adhesive sheet 1 may be a sheet formed by an adhesive composition (such as adhesive composition (I)) containing an isocyanate crosslinking agent and further containing a peroxide crosslinking agent.
[0098] Examples of isocyanate crosslinking agents include aromatic isocyanate compounds such as toluene diisocyanate, chlorophenylene diisocyanate, diphenylmethane diisocyanate, xylene diisocyanate, and polymethylene polyphenyl isocyanate; alicyclic isocyanate compounds such as cyclopentylene diisocyanate, cyclohexylene diisocyanate, hydrogenated diphenylmethane diisocyanate, and isophorone diisocyanate; and aliphatic isocyanate compounds such as butylene diisocyanate, tetramethylene diisocyanate, and hexamethylene diisocyanate. The isocyanate crosslinking agent may be a compound (adduct) obtained by adding the above isocyanate compound to a polyol compound such as trimethylolpropane; a compound (alophanate) obtained by adding the above isocyanate compound to a polyol such as polyether polyol, polyester polyol, acrylic polyol (acryl polyol), polybutadiene polyol, and polyisoprene polyol; and derivatives of the above isocyanate compounds such as isocyanurates. Specific examples of the derivatives include trimethylolpropane / toluene diisocyanate trimer adducts (e.g., Coronate L manufactured by Tosoh Corporation), trimethylolpropane / hexamethylene diisocyanate trimer adducts (e.g., Coronate HL manufactured by Tosoh Corporation), isocyanurate forms of hexamethylene diisocyanate (e.g., Coronate HX manufactured by Tosoh Corporation), and allophanate forms obtained by addition reaction of hexamethylene diisocyanate and acrylic polyol (e.g., Coronate 2770 manufactured by Tosoh Corporation).
[0099] The isocyanate crosslinking agent may be a non-aromatic ring type. The non-aromatic ring type isocyanate crosslinking agent can particularly contribute to the |Δb of the adhesive sheet 1 formed by the adhesive composition containing the crosslinking agent. * | is reduced. It should be noted that, in this specification, "non-aromatic ring type" refers to a compound that does not contain an aromatic ring. A compound containing an aromatic ring is an aromatic ring type. Examples of non-aromatic ring type isocyanate type crosslinking agents are alicyclic isocyanate compounds, aliphatic isocyanate compounds and their derivatives. Non-aromatic ring type isocyanate type crosslinking agents can be aliphatic isocyanate compounds and their derivatives, and can also be hexamethylene diisocyanate (HDI) type compounds and their derivatives.
[0100] When the adhesive composition forming the adhesive sheet 1 contains an isocyanate crosslinking agent, its blending amount is, for example, 0.1 to 10 parts by weight, 0.2 to 5 parts by weight, 0.25 to 3 parts by weight, 0.3 to 1 part by weight, or further 0.3 to 0.6 parts by weight relative to 100 parts by weight of the polymer.
[0101] Examples of peroxide crosslinking agents include di(2-ethylhexyl) peroxydicarbonate, di(4-tert-butylcyclohexyl) peroxydicarbonate, di-sec-butyl peroxydicarbonate, tert-butyl peroxyneodecanoate, tert-hexyl peroxypivalate, tert-butyl peroxypivalate, dilauroyl peroxide, di-n-octanoyl peroxide, 1,1,3,3-tetramethylbutyl peroxy-2-ethylhexanoate, di(4-methylbenzoyl) peroxide, benzoyl peroxide, tert-butyl peroxyisobutyrate, and 1,1-di(tert-hexylperoxy)cyclohexane. Among peroxide crosslinking agents, benzoyl peroxide (BPO) is preferred because of its excellent crosslinking reaction efficiency.
[0102] When the adhesive composition forming the adhesive sheet 1 contains a peroxide-based crosslinking agent, its blending amount is, for example, 0.005 to 5 parts by weight, 0.01 to 3 parts by weight, 0.05 to 2 parts by weight, 0.07 to 1 part by weight, 0.07 to 0.5 parts by weight, 0.07 to 0.3 parts by weight, and further 0.07 to 0.25 parts by weight relative to 100 parts by weight of the polymer.
[0103] <Additives>
[0104] The adhesive composition forming the adhesive sheet 1 (for example, an adhesive composition (I) comprising a (meth) acrylic polymer (A) as a main component) may further include materials other than the above. Examples of the material are additives. Examples of additives are silane coupling agents, antioxidants, colorants such as pigments and dyes, ultraviolet absorbers, surfactants, plasticizers, tackifiers, surface lubricants, leveling agents, reoperation improvers, softeners, inhibitors, rust inhibitors, inorganic fillers, organic fillers, powders such as metal powders, particles, and foils. Relative to 100 parts by weight of polymer, the additive can be matched in a total of, for example, less than 10 parts by weight, preferably less than 5 parts by weight, and more preferably less than 3 parts by weight.
[0105] Examples of the silane coupling agent include epoxy group-containing silane coupling agents such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; amino group-containing silane coupling agents such as 3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-triethoxysilyl-N-(1,3-dimethylbutylene)propylamine, and N-phenyl-γ-aminopropyltrimethoxysilane; (meth)acryl group-containing silane coupling agents such as 3-acryloxypropyltrimethoxysilane and 3-methacryloxypropyltriethoxysilane; and isocyanate group-containing silane coupling agents such as 3-isocyanatepropyltriethoxysilane.
[0106] When the adhesive composition forming the adhesive sheet 1 contains a silane coupling agent, the amount thereof may be, for example, 5 parts by weight or less, 3 parts by weight or less, 1 part by weight or less, 0.5 parts by weight or less, 0.2 parts by weight or less, 0.1 parts by weight or less, or further may be 0.05 parts by weight or less relative to 100 parts by weight of the polymer. The adhesive composition may not contain a silane coupling agent.
[0107] The type of adhesive composition forming the adhesive sheet 1 is, for example, an emulsion type, a solvent type (solution type), an active energy ray curable type (photocurable type), and a hot melt type (hot melt type). From the viewpoint of being able to form an adhesive sheet 1 with excellent durability, the adhesive composition may be a solvent type or an active energy ray curable type, or may be a solvent type. The solvent type adhesive composition may not contain a photocuring agent such as an ultraviolet curing agent.
[0108] The adhesive sheet 1 can be formed from an adhesive composition by the following method. Regarding the solvent type, for example, an adhesive composition or a mixture of an adhesive composition and a solvent is applied to a substrate film to form a coating film, and the formed coating film is dried to form an adhesive sheet 1. The adhesive composition is thermally cured by the heat during drying. Regarding the active energy ray curing type (photocuring type), for example, a mixture of a monomer (group) that will become a given polymer by polymerization, and a partial polymer of the monomer (group) used as needed, a polymerization initiator, an additive, and a solvent is applied to a substrate film, and the formed coating film is irradiated with active energy rays to form an adhesive sheet 1. Before irradiating the active energy rays, the coating film can be dried to remove the solvent. The substrate film can be a film (release liner) to which a release treatment has been applied to the coating surface.
[0109] The pressure-sensitive adhesive sheet 1 formed on the substrate film can be transferred to any layer. In addition, the substrate film may be the polarizing film 2. In this case, an optical laminate 10 including the pressure-sensitive adhesive sheet 1 and the polarizing film 2 can be obtained.
[0110] The coating of the substrate film can be carried out by a known method, for example, by roll coating, lick roll coating, gravure coating, reverse coating, roll brushing, spray coating, dip roll coating, rod coating, blade coating, air knife coating, curtain coating, die lip coating, extrusion coating using a die coater, etc.
[0111] For solvent-based coatings, the drying temperature after coating is, for example, 40 to 200° C. The drying time is, for example, 5 seconds to 20 minutes, 5 seconds to 10 minutes, or 10 seconds to 5 minutes. For active energy ray-curable coatings, the drying temperature and drying time when drying after coating may be within the above ranges.
[0112] The composition and mixture applied to the substrate film preferably have a viscosity suitable for handling and application. Therefore, in the case of an active energy ray-curable type, the mixture applied preferably contains a partial polymer of the monomer (group).
[0113] The thickness of the pressure-sensitive adhesive sheet 1 is, for example, 2 μm to 55 μm, 2 μm to 30 μm, 5 μm to 25 μm, or even 10 μm to 20 μm.
[0114] (Polarizing Film)
[0115] The polarizing film 2 is typically a laminate including a polarizer and a protective film (transparent protective film). The protective film is disposed, for example, in contact with the principal surface (surface having the largest area) of the polarizer. The polarizer may be disposed between two protective films.
[0116] The polarizer is not particularly limited, and examples thereof include: a polarizer obtained by adsorbing a dichroic substance such as iodine and a dichroic dye on a hydrophilic polymer film such as a polyvinyl alcohol film, a partially formalized polyvinyl alcohol film, and a partially saponified film of an ethylene-vinyl acetate copolymer, and then uniaxially stretching the film; a polyene oriented film such as a dehydrated product of polyvinyl alcohol and a dehydrochlorinated product of polyvinyl chloride, etc. The polarizer is typically formed of a polyvinyl alcohol film and a dichroic substance such as iodine.
[0117] The thickness of the polarizer is not particularly limited, for example, it can be 80 μm or less, 50 μm or less, 30 μm or less, 25 μm or less, and further 20 μm or less. The lower limit of the thickness of the polarizer is not particularly limited, for example, it is 1 μm or more, 5 μm or more, 10 μm or more, and further 15 μm or more. A thin polarizer (for example, a thickness of 20 μm or less) suppresses dimensional changes and can contribute to the durability of the optical laminate, especially the durability at high temperatures.
[0118] As the material of the protective film, for example, thermoplastic resins with excellent transparency, mechanical strength, thermal stability, moisture barrier properties, isotropy, etc. can be used. Specific examples of such thermoplastic resins include cellulose resins such as cellulose triacetate, polyester resins, polyethersulfone resins, polysulfone resins, polycarbonate resins, polyamide resins, polyimide resins, polyolefin resins, (meth)acrylic resins, cyclic polyolefin resins (norbornene resins), polyarylate resins, polystyrene resins, polyvinyl alcohol resins, and mixtures thereof. The material of the protective film can be a thermosetting resin or ultraviolet curing resin such as (meth)acrylic acid, urethane, acrylic urethane, epoxy, silicone, etc. In the case where the polarizing film 2 has two protective films, the materials of the two protective films can be the same or different from each other. For example, a protective film formed of a thermoplastic resin can be bonded to one main surface of the polarizer via an adhesive, and a protective film formed of a thermosetting resin or an ultraviolet curing resin can be bonded to the other main surface of the polarizer. The protective film can contain one or more arbitrary additives. Examples of the additive include ultraviolet absorbers, antioxidants, lubricants, plasticizers, release agents, anti-coloring agents, flame retardants, nucleating agents, antistatic agents, pigments, and colorants.
[0119] The moisture permeability of the protective film is not particularly limited and can be 200 g / (m 2 ·day) or less, or 50g / (m 2 ·day) or less. In this case, it is possible to suppress the intrusion of moisture in the air into the interior of the polarizing film 2, and suppress the change in the moisture content of the polarizing film 2. As a result, it is possible to suppress the occurrence of curling and dimensional changes of the polarizing film 2 during storage. Examples of materials for forming the protective film with low moisture permeability include polyester polymers, polycarbonate polymers, aromatic ester polymers, amide polymers, olefin polymers, cyclic olefin polymers, (meth) acrylic polymers, and mixtures thereof.
[0120] The moisture permeability of the protective film can be measured by the following method based on the moisture permeability test (cup method) of JIS Z0208:1976. First, the protective film is cut into a diameter of 60 mm to prepare a measurement sample. Next, the measurement sample is set in a moisture permeable cup configured with about 15g of calcium chloride. The moisture permeable cup is placed in a constant temperature machine set at a temperature of 40°C and a humidity of 92% RH for 24 hours, thereby conducting a moisture permeability test. By measuring the increase in the weight of calcium chloride before and after the test, the moisture permeability of the protective film can be determined.
[0121] The thickness of the protective film can be appropriately determined, and is generally about 10 to 200 μm in view of strength, workability such as handling properties, and thin film properties.
[0122] The polarizer and the protective film are usually bonded together via a water-based adhesive or the like. Examples of the water-based adhesive include isocyanate adhesives, polyvinyl alcohol adhesives, gelatin adhesives, vinyl latex, water-based polyurethane, and water-based polyester. Examples of adhesives other than the above-mentioned adhesives include ultraviolet curing adhesives and electron beam curing adhesives. Electron beam curing adhesives for polarizing films show suitable adhesion to various protective films. The adhesive may also contain a metal compound filler.
[0123] In the polarizing film, a retardation film or the like may be formed on the polarizer instead of the protective film. Another protective film or a retardation film may be further provided on the protective film.
[0124] The protective film may be provided with a hard coat layer on the surface opposite to the surface to be bonded to the polarizer, or may be subjected to treatment for the purpose of anti-reflection, anti-sticking, diffusion, anti-glare, etc.
[0125] The polarizing film 2 is not limited to the above-mentioned examples.
[0126] Another example of the optical layered body of the present embodiment is shown in Figure 2 . Figure 2 The optical laminate 10 (10B) has a laminated structure in which a release liner 3, an adhesive sheet 1, and a polarizing film 2 are laminated in this order. The optical laminate 10B can be used as a polarizing film with an adhesive sheet by peeling off the release liner 3. The following examples can be combined with each other as long as they are not technically contradictory.
[0127] Examples of the material constituting the release liner 3 include plastic films such as polyethylene, polypropylene, polyethylene terephthalate, and polyester films, porous materials such as paper, cloth, and nonwoven fabrics, nets, foam sheets, metal foils, and appropriate thin sheets such as laminates thereof. Plastic films are preferably used because of their excellent surface smoothness.
[0128] The plastic film is not particularly limited as long as it can protect the adhesive sheet 1, and examples thereof include polyethylene films, polypropylene films, polybutylene films, polybutadiene films, polymethylpentene films, polyvinyl chloride films, vinyl chloride copolymer films, polyethylene terephthalate films, polybutylene terephthalate films, polyurethane films, and ethylene-vinyl acetate copolymer films.
[0129] The thickness of the release liner 3 is usually 5 to 200 μm, preferably about 5 to 100 μm. If necessary, the release liner 3 may be subjected to mold release and antifouling treatment using silicone, fluorine, long-chain alkyl or fatty acid amide release agents, silica powder, etc., or antistatic treatment such as coating, mixing, or vapor deposition. In particular, by appropriately subjecting the surface of the release liner 3 to a release treatment such as silicone treatment, long-chain alkyl treatment, or fluorine treatment, the releasability from the adhesive sheet 1 can be further improved.
[0130] As described above, the base film used when producing the pressure-sensitive adhesive sheet 1 may be used as the release liner 3 .
[0131] Another example of the optical layered body of the present embodiment is shown in Figure 3 . Figure 3 The optical laminate 10 (10C) has a laminated structure in which a release liner 3, an adhesive sheet 1, a phase difference film 5, an interlayer adhesive 4, and a polarizing film 2 are laminated in this order. The optical laminate 10C can be used by being attached to, for example, an image display unit after the release liner 3 is peeled off.
[0132] A retardation film obtained by stretching a polymer film or a retardation film obtained by orienting and fixing a liquid crystal material can be used as the retardation film 5. The retardation film 5 has birefringence in the plane and / or in the thickness direction, for example.
[0133] The phase difference film 5 includes a phase difference film for antireflection (refer to Japanese Patent Application Publication No. 2012-133303
[0221] ,
[0222] , and
[0228] ), a phase difference film for viewing angle compensation (refer to Japanese Patent Application Publication No. 2012-133303
[0225] and
[0226] ), and a tilted orientation phase difference film for viewing angle compensation (refer to Japanese Patent Application Publication No. 2012-133303
[0227] ).
[0134] The specific structure of the retardation film 5 , such as the retardation value, the arrangement angle, the three-dimensional birefringence, whether it is a single layer or a multilayer, etc., is not particularly limited, and a known retardation film can be used.
[0135] The thickness of the retardation film 5 is preferably 20 μm or less, more preferably 10 μm or less, further preferably 1 to 9 μm, and particularly preferably 3 to 8 μm.
[0136] The retardation film 5 may include, for example, a quarter-wave plate and / or a half-wave plate in which a liquid crystal material is oriented and fixed.
[0137] A known adhesive may be used as the interlayer adhesive 4 , and the adhesive sheet 1 may be used for the interlayer adhesive 4 .
[0138] Another example of the optical layered body of the present embodiment is shown in Figure 4 , Figure 4 The optical laminate 10 (10D) has a laminated structure in which a release liner 3, an adhesive sheet 1, a phase difference film 5, an interlayer adhesive 4, a polarizing film 2, and a protective film 6 are laminated in this order. The optical laminate 10D can be used by being attached to, for example, an image display unit after the release liner 3 is peeled off.
[0139] The protective film 6 has the function of protecting the polarizing film 2 as the outermost layer during the circulation and storage of the optical laminate 10D, and when the optical laminate 10D is introduced into the image display device. In addition, when introduced into the image display device, it can be a protective film 6 that functions as a window to the external space. The protective film 6 is typically a resin film. The resin constituting the protective film 6 is, for example, polyester such as PET, polyolefins such as polyethylene and polypropylene, acrylic acid, cycloolefins, polyimides and polyamides, preferably polyesters. However, it should be noted that the protective film 6 is not limited to the above examples, and the protective film 6 can also be a glass film or a laminated film including a glass film. The protective film 6 can be subjected to surface treatments such as anti-glare, anti-reflection, and antistatic.
[0140] The protective film 6 may be bonded to the polarizing film 2 via any adhesive, or may be bonded using the adhesive sheet 1 .
[0141] The optical layered body of the present embodiment may include any layer other than the above-mentioned layers.
[0142] The optical laminate of the present embodiment can be circulated and stored in the form of a winding body formed by winding a strip-shaped optical laminate, or in the form of a monolithic optical laminate. The optical laminate of the present embodiment is suitable for image display devices used in environments that are particularly prone to static electricity, especially for vehicle-mounted displays. As vehicle-mounted displays, for example, instrument panels for car navigation devices, instrument clusters (cluster panels), mirror displays, etc. The instrument cluster is a panel that displays the driving speed of the vehicle, the speed of the engine, etc.
[0143] The optical laminate of this embodiment can be used, for example, for an image display panel and an image display device (for example, a liquid crystal display panel and a liquid crystal display device) with a backlight. However, the use of the optical laminate of this embodiment is not limited to the above examples. It is not limited to the light from the backlight, and can also be used for irradiating high-intensity light.
[0144] [Image Display Panel]
[0145] An example of the image display panel of this embodiment is shown in Figure 5 . Figure 5 The image display panel 11A includes an optical laminate 10A and further includes, for example, an image display unit 30A. Specifically, the optical laminate 10A is bonded to the image display unit 30A via the adhesive sheet 1. Figures 2 to 4 The optical layered body 10A (except the release liner 3 ) is replaced with the optical layered body 10B, 10C or 10D.
[0146] The image display unit 30A includes, for example, an image forming layer 32, a first transparent substrate 31, and a second transparent substrate 33. The image forming layer 32 is, for example, disposed between the first transparent substrate 31 and the second transparent substrate 33, and is in contact with the first transparent substrate 31 and the second transparent substrate 33. The adhesive sheet 1 of the optical laminate 10A is in contact with, for example, the first transparent substrate 31 of the image display unit 30A.
[0147] The image forming layer 32 is, for example, a liquid crystal layer containing liquid crystal molecules that are uniformly oriented in the absence of an electric field. A liquid crystal layer containing such liquid crystal molecules is suitable for an IPS (In-Plane-Switching) method. However, the liquid crystal layer can also be used for a TN (Twisted Nematic) type, an STN (Super Twisted Nematic) type, a π type, a VA (Vertical Alignment) type, and the like. In this specification, an image display unit having a liquid crystal layer is sometimes referred to as a liquid crystal unit, and an image display panel having a liquid crystal unit is sometimes referred to as a liquid crystal panel. However, the image forming layer 32 is not limited to a liquid crystal layer, and can also be, for example, an EL light-emitting layer.
[0148] The thickness of the image forming layer 32 is, for example, 1.5 μm to 4 μm.
[0149] As materials of the first transparent substrate 31 and the second transparent substrate 33, glass and polymers can be cited, for example. In this specification, a transparent substrate composed of a polymer is sometimes referred to as a polymer film. As polymers constituting the transparent substrate, for example, polyethylene terephthalate, polycycloolefin, polycarbonate, etc. can be cited. The thickness of the transparent substrate composed of glass is, for example, 0.1 mm to 1 mm. The thickness of the transparent substrate composed of a polymer is, for example, 10 μm to 200 μm.
[0150] The image display unit 30A may further include other layers in addition to the image forming layer 32, the first transparent substrate 31, and the second transparent substrate 33. As other layers, for example, a color filter, an easy adhesion layer, and a hard coating layer can be cited. The color filter is, for example, arranged closer to the visible side than the image forming layer 32, preferably between the first transparent substrate 31 and the adhesive sheet 1 of the optical laminate 10A. The easy adhesion layer and the hard coating layer are, for example, arranged on the surface of the first transparent substrate 31 or the second transparent substrate 33.
[0151] The image display panel 11A may further include other components in addition to the optical stack 10A and the image display unit 30A. For example, the image display panel 11A may further include a conductive structure (not shown) electrically connected to the side of the optical stack 10A. If the conductive structure is grounded, it is easy to suppress the optical stack 10A from being charged due to static electricity. The conductive structure may cover the entire side of the optical stack 10A, or may partially cover the side of the optical stack 10A. The ratio of the area of the side of the optical stack 10A covered by the conductive structure to the area of the entire side of the optical stack 10A is, for example, 1% or more, preferably 3% or more.
[0152] Examples of the material of the conductive structure include conductive pastes made of metals such as silver and gold, conductive adhesives, and other conductive materials. The conductive structure may be wiring extending from the side surface of the optical laminate 10A.
[0153] The image display panel 11A may further include other optical films in addition to the polarizing film 2. Examples of other optical films include polarizing films, reflective plates, reflective plates, viewing angle compensation films, brightness enhancement films, and other films that can be used in image display devices. The image display panel 11A may include one or two or more of these other optical films.
[0154] When the other optical film is a polarizing film, the polarizing film can be bonded to the second transparent substrate 33 of the image display unit 30A via an adhesive sheet, for example. The polarizing film has, for example, the structure described above for the polarizing film 2. In the polarizing film as the other optical film, the transmission axis (or absorption axis) of the polarizer is, for example, orthogonal to the transmission axis (or absorption axis) of the polarizer in the polarizing film 2. As the material of the adhesive sheet for bonding the polarizing film to the second transparent substrate 33, the material described above for the adhesive sheet 1 can be used. The thickness of the adhesive sheet is not particularly limited, and is, for example, 1 to 100 μm, preferably 2 to 50 μm, more preferably 2 to 40 μm, and further preferably 5 to 35 μm.
[0155] Another example of the image display panel of this embodiment is shown in Figure 6 . Figure 6 The image display panel 11B further includes a conductive layer 40 disposed between the optical layered body 10A and the image display unit 30A.
[0156] The conductive layer 40 is, for example, a layer containing a conductive agent. As the conductive agent, those described above for the adhesive sheet 1 can be used. However, the conductive agent is not limited to the above examples. The conductive layer 40 can contain various conductive agents, for example: inorganic cationic conductive agents, carbon nanotubes, ITO, ATO, conductive polymers as a composite with a dopant (as an example, a composite of poly(3,4-ethylenedioxythiophene) and polystyrene sulfonic acid: PEDOT / PSS), etc. The thickness of the conductive layer 40 is, for example, 5 nm to 180 nm. The surface resistivity of the conductive layer 40 is, for example, 1.0×10 6 Ω / □~1.0×10 10 Ω / □, preferably 1.0×10 8 Ω / □~1.0×10 9 Ω / □.
[0157] Another example of the image display panel of this embodiment is shown in Figure 7 . Figure 7 The image display panel 11C includes an image display unit 30B further including a touch sensing electrode unit 35. In the image display unit 30B, the touch sensing electrode unit 35 is arranged between the first transparent substrate 31 and the second transparent substrate 33. The touch sensing electrode unit 35 has the functions of a touch sensor and a touch drive. The image display panel 11C is a so-called embedded image display panel, and the image display unit 30B is a so-called embedded image display unit.
[0158] The touch sensing electrode portion 35 includes, for example, a touch sensor electrode 36 and a touch drive electrode 37. The touch sensor electrode 36 refers to a (receiving) electrode for touch detection. The touch sensor electrode 36 and the touch drive electrode 37 can be independently formed by various patterns. For example, when the image display unit 30B is in the form of a flat plate, the touch sensor electrode 36 and the touch drive electrode 37 can be independently arranged in the X-axis direction and the Y-axis direction, respectively, to form a pattern in which they cross at right angles. Figure 7 In the touch sensing electrode section 35, the touch sensor electrode 36 may be arranged closer to the visible side than the touch drive electrode 37. However, the touch drive electrode 37 may also be arranged closer to the visible side than the touch sensor electrode 36. In the touch sensing electrode section 35, the touch sensor electrode 36 and the touch drive electrode 37 may also be integrated.
[0159] exist Figure 7 In the embodiment, the touch sensing electrode portion 35 is disposed between the image forming layer 32 and the first transparent substrate 31 (closer to the visible side than the image forming layer 32). However, the touch sensing electrode portion 35 may also be disposed between the image forming layer 32 and the second transparent substrate 33 (closer to the lighting system side than the image forming layer 32).
[0160] In the touch sensing electrode portion 35 , the touch sensor electrodes 36 and the touch drive electrodes 37 may not be in contact with each other. For example, the touch sensor electrodes 36 may be arranged between the image forming layer 32 and the first transparent substrate 31 , and the touch drive electrodes 37 may be arranged between the image forming layer 32 and the second transparent substrate 33 .
[0161] The driving electrodes in the touch sensing electrode unit 35 (the touch driving electrodes 37 or electrodes in which the touch sensor electrodes 36 and the touch driving electrodes 37 are integrated) may also serve as common electrodes for controlling the image forming layer 32 .
[0162] The touch sensor electrode 36 (capacitive sensor) and the touch drive electrode 37 constituting the touch sensing electrode portion 35, or the electrode formed by integrating them, functions as a transparent conductive layer. The material of the transparent conductive layer is not particularly limited, and examples thereof include metals such as gold, silver, copper, platinum, palladium, aluminum, nickel, chromium, titanium, iron, cobalt, tin, magnesium, tungsten, and alloys thereof. The material of the transparent conductive layer may also be an oxide of a metal such as indium, tin, zinc, gallium, antimony, zirconium, and cadmium. As the oxide, specifically, indium oxide, tin oxide, titanium oxide, cadmium oxide, and mixtures thereof may be mentioned. The material of the transparent conductive layer may also be a metal compound such as copper iodide. The material of the transparent conductive layer is preferably indium oxide (ITO) containing tin oxide, tin oxide (ATO) containing antimony, and the like, and ITO is particularly preferred. When the material of the transparent conductive layer is ITO, the content of indium oxide in the transparent conductive layer is preferably 80 to 99% by weight, and the content of tin oxide is preferably 1 to 20% by weight.
[0163] The electrodes constituting the touch sensing electrode portion 35 (touch sensor electrodes 36, touch drive electrodes 37, or electrodes formed by integrating them) can be formed between the first transparent substrate 31 and the second transparent substrate 33 in the form of a transparent electrode pattern by conventional methods. The transparent electrode pattern is electrically connected to, for example, a lead formed at the end of the transparent substrate. The lead is connected to, for example, a controller IC. As the shape of the transparent electrode pattern, any shape corresponding to the purpose, such as a comb shape, a stripe shape, a diamond shape, etc., can be adopted. The thickness of the transparent electrode pattern is, for example, 10nm to 100nm. The width of the transparent electrode pattern is, for example, 0.1mm to 5mm.
[0164] [Image display device]
[0165] The image display device of this embodiment includes, for example, an image display panel 11A and a lighting system. Figures 6-7The image display panel 11A is replaced by the image display panels 11B and 11C. In the image display device, the image display panel 11A is, for example, arranged closer to the visible side than the lighting system. The lighting system, for example, has a backlight or a reflector, which irradiates light to the image display panel 11A. The luminosity of the light irradiated by the backlight to the image display panel 11A may be 15,000 candela or more, or 16,000 candela or more, 17,000 candela or more, 18,000 candela or more, 19,000 candela or more, and further may be 20,000 candela or more.
[0166] The image display device is, for example, a liquid crystal display. However, the image display device is not limited to the above examples, and the image display device may be an electroluminescent (EL) display, a plasma display (PD), a field emission display (FED: Field Emission Display), etc. The image display device may be used for household appliances, in-vehicle use, public information display (PID) use, etc., and may be an in-vehicle display.
[0167] Example
[0168] Hereinafter, the present invention will be described in more detail by way of examples. However, the present invention is not limited to the examples shown below.
[0169] <Weight average molecular weight of (meth)acrylic polymer>
[0170] The weight average molecular weight (Mw) of the (meth)acrylic polymer was measured by GPC (gel permeation chromatography).
[0171] ·Analysis device: Made by Tosoh Corporation, HLC-8120GPC
[0172] ·Chromatographic column: G7000H manufactured by Tosoh Corporation XL +GMH XL +GMH XL
[0173] · Pillar size: 7.8mmφ×30cm each, total 90cm
[0174] Column temperature: 40℃
[0175] Flow rate: 0.8mL / min
[0176] Injection volume: 100μL
[0177] ·Eluent: Tetrahydrofuran
[0178] Detector: Differential Refractometer (RI)
[0179] Standard sample: polystyrene
[0180] [Preparation of (meth)acrylic polymer A1]
[0181] A monomer mixture containing 81.93 parts by weight of n-butyl acrylate (BA), 1.00 parts by weight of acrylic acid (AA), 1.00 parts by weight of N-vinyl pyrrolidone (NVP), 16.00 parts by weight of phenoxyethyl acrylate (PEA) and 0.07 parts by weight of 4-hydroxybutyl acrylate (HBA) was added to a four-necked flask equipped with a stirring blade, a thermometer, a nitrogen inlet tube and a condenser. Furthermore, 0.1 parts by weight of 2,2'-azobisisobutyronitrile (AIBN; manufactured by Kishida Chemical Co., Ltd.) as a polymerization initiator was added together with 100 parts by weight of ethyl acetate to 100 parts by weight of the monomer mixture. While slowly stirring the mixture, nitrogen was introduced into the flask to replace the nitrogen. The liquid temperature in the flask was maintained at about 55°C and a polymerization reaction was performed for 8 hours, thereby preparing a solution of a (meth)acrylic polymer A1 having a weight average molecular weight (Mw) of 2 million.
[0182] [Preparation of (meth)acrylic polymer A2]
[0183] A solution of a (meth)acrylic polymer A2 having a weight average molecular weight (Mw) of 2,000,000 was prepared in the same manner as in the preparation of the (meth)acrylic polymer A1, except that the monomer mixture added to the flask was made to contain 79.43 parts by weight of BA, 3.50 parts by weight of AA, 1.00 parts by weight of NVP, 16.00 parts by weight of PEA, and 0.07 parts by weight of HBA.
[0184] [Preparation of (meth)acrylic polymer A3]
[0185] A solution of a (meth)acrylic polymer A3 having a weight average molecular weight (Mw) of 1,000,000 was prepared in the same manner as in the preparation of the (meth)acrylic polymer A1, except that the monomer mixture added to the flask was made to contain 79.00 parts by weight of BA, 3.50 parts by weight of AA, 1.00 parts by weight of NVP, 16.00 parts by weight of PEA, and 0.50 parts by weight of HBA.
[0186] The monomers used in the synthesis of each (meth)acrylic polymer and the added amount are summarized in Table 1 below.
[0187] [Table 1]
[0188] BA AA NVP PEA HBA Al 81.93 1.00 1.00 16.00 0.07 A2 79.43 3.50 1.00 16.00 0.07 A3 79.00 3.50 1.00 16.00 0.50
[0189] [Preparation of (meth)acrylic adhesive composition]
[0190] (Example 1)
[0191] A solution of the (meth)acrylic adhesive composition of Example 1 was prepared by mixing 1 part by weight of an isocyanate crosslinking agent (Coronate L; trimethylolpropane toluene diisocyanate; aromatic type, manufactured by Tosoh Corporation), 0.2 parts by weight of a peroxide crosslinking agent (benzoyl peroxide; BPO), and 1 part by weight of 1-ethyl-3-methylimidazole bis(fluorosulfonyl)imide salt (EMI-FSI) as a conductive agent with respect to 100 parts by weight of the solid content of the solution of the (meth)acrylic polymer A1.
[0192] (Examples 2 to 6, Comparative Examples 1 to 2)
[0193] As shown in Table 2 below, an isocyanate crosslinking agent, a peroxide crosslinking agent (not mixed in Example 6), and a conductive agent (not mixed in Comparative Example 2) were mixed with each other based on 100 parts by weight of the solid content of the solution of the (meth)acrylic polymer to prepare solutions of the (meth)acrylic adhesive compositions of Examples 2 to 6 and Comparative Examples 1 to 2. In Table 2, C / L is Coronate L, C / 2770 is a non-aromatic isocyanate crosslinking agent (Coronate 2770 manufactured by Tosoh Corporation; an allophanate obtained by addition reaction of hexamethylene diisocyanate and acrylic polyol), and LiTFSI is an inorganic cationic conductive agent (lithium bis(trifluoromethanesulfonyl)imide).
[0194] [Table 2]
[0195]
[0196] ※The unit of the amount is weight part
[0197] [Preparation of adhesive sheet]
[0198] The solution of each adhesive composition was applied to one side of a polyethylene terephthalate film (release liner; manufactured by Mitsubishi Chemical Polyester Film Co., Ltd., MRF38) surface-treated with a silicone release agent so that the thickness of the adhesive sheet after drying was 20 μm. The obtained coating film was dried at 155° C. for 1 minute, thereby forming an adhesive sheet on the surface of the release liner.
[0199] <Measurement of surface resistivity>
[0200] The surface resistivity of the produced PSA sheet was measured using Hiresta MCP-HT450 manufactured by Mitsubishi Chemical Analytech Co., Ltd. at an applied voltage of 250 V for 10 seconds. The surface resistivity was measured in an environment of a temperature of 25°C ± 5°C and a relative humidity of 50 ± 5%.
[0201] [Production of optical laminate]
[0202] <Production of polarizing film>
[0203] The polyvinyl alcohol film was stretched to 3 times while being dyed in an iodine solution at a temperature of 30°C and a concentration of 0.3% by weight for 1 minute between rollers with different speed ratios. Next, it was immersed in an aqueous solution at a temperature of 60°C containing boric acid at a concentration of 4% by weight and potassium iodide at a concentration of 10% by weight for 0.5 minutes, and stretched to a total stretch ratio of 6 times. Next, it was immersed in an aqueous solution at a temperature of 30°C containing potassium iodide at a concentration of 1.5% by weight for 10 seconds and washed, and then dried at 50°C for 4 minutes, thereby obtaining a polarizer with a thickness of 18μm. A transparent protective film with a thickness of 30μm formed by a modified acrylic polymer having a lactone ring structure was bonded to one side of the polarizer using a polyvinyl alcohol adhesive. Furthermore, a transparent protective film with a thickness of 47μm formed on a cellulose triacetate film (manufactured by Konica Minolta, Ltd., KC4UY) was bonded to the other side of the polarizer using a polyvinyl alcohol adhesive. The resulting film was heated and dried in an oven set at 70° C. for 5 minutes to produce a polarizing film.
[0204] <Production of optical laminate>
[0205] Next, each adhesive sheet of Examples and Comparative Examples formed on a release liner was transferred to the polarizing film prepared above to prepare an optical laminate (polarizing film with adhesive sheet). The adhesive sheet was transferred to the surface of the polarizing film on the side of the transparent protective film formed of a modified acrylic polymer.
[0206] <Yellowing of the peripheral area>
[0207] The coloration (yellowing of the peripheral portion) of the optical laminate when exposed to high-intensity light and placed at high temperature was evaluated by the above-mentioned evaluation method. The glass plate of the transparent member on the front surface of the image display panel used was 0.5 mm thick alkali-free glass. The glass plate was bonded to the adhesive sheet of the produced optical laminate. The surface light source used was a backlight for a liquid crystal display device, which had a light-emitting area capable of irradiating the entire optical laminate placed on the light source with light equivalent to the CIE standard light source D65 at a luminous intensity of 15,000 candela. A heating furnace was used in the heating test. b *The measurement was performed using LPF-200 manufactured by Otsuka Electronics. * |, and the degree of yellowing of the peripheral portion was evaluated as follows. Note that in the reference example, the same evaluation was performed except that the luminous intensity of the light irradiated from the backlight to the optical layered body of Comparative Example 1 was reduced to 10,000 candela.
[0208] A: |Δb * |Below 0.30
[0209] B: |Δb * |More than 0.30 and less than 0.45
[0210] C: |Δb * |More than 0.45 and less than 0.60
[0211] D: |Δb * |More than 0.60
[0212] <Durability (High temperature durability)>
[0213] The durability (high temperature durability) of the optical laminate was evaluated by the following method. The produced optical laminate was fixed to the surface of a glass plate (Corning, EAGLE XG) via its adhesive sheet. The fixing was carried out in an atmosphere of 24°C and 50% RH. Next, after being treated in an autoclave at 50°C and 5 atmospheres (absolute pressure) for 15 minutes, it was allowed to stand until it was cooled to 24°C, and after the bonding of the optical laminate to the glass plate was stabilized, it was placed in a heated atmosphere of 90°C or 95°C for 500 hours. After standing, the atmosphere was restored to 24°C and 50% RH, and visual observation was used to confirm whether the polarizing film was peeled off from the glass plate and whether bubbles were generated between the glass plate and the polarizing film. The durability was evaluated as described below.
[0214] A: No changes in appearance such as foaming and peeling were observed.
[0215] B: A small amount of individual peeling or foaming was observed at the edge, but it was within a range that did not cause a problem in practical use.
[0216] C: A small amount of continuous peeling or foaming was observed at the edge, but it was within the range of no problem in practical use.
[0217] D: Significant peeling or foaming was observed at the edge, which was problematic in practical use.
[0218] <Antistatic Properties>
[0219] The antistatic property of the optical laminate was evaluated by the following method (ESD test). The produced optical laminate was fixed to a Figure 7 Next, the liquid crystal display panel with the optical laminate fixed thereto was placed on a backlight, and static electricity was emitted from the surface of the polarizing film, which was the exposed surface on the visible side, by an electrostatic discharge gun at an applied voltage of 15 kV. The time from the moment of emission to the disappearance of the whitish portion due to static electricity was measured, and the antistatic property was evaluated as follows.
[0220] A: Disappear within 1 second
[0221] B: Disappears within more than 1 second and less than 10 seconds
[0222] C: Disappears within more than 10 seconds and less than 60 seconds
[0223] D: Disappears after more than 60 seconds
[0224] The evaluation results of each optical layered body in Examples and Comparative Examples are shown in Table 3 below together with the surface resistivity of the pressure-sensitive adhesive sheet included in each optical layered body.
[0225] [Table 3]
[0226]
[0227] ※The luminance of the backlight in the yellowing evaluation of the reference example is 10,000 candela
[0228] As shown in Table 3, compared with the optical layered body of the comparative example, the optical layered body of the example can ensure antistatic properties and suppress yellowing of the peripheral portion when combined with a high-intensity backlight.
[0229] Industrial Applicability
[0230] The optical layered body of the present invention can be used in image display devices such as liquid crystal displays.
Claims
1. An optical laminate comprising a polarizing film and an adhesive sheet, The adhesive sheet contains an organic cationic conductive agent, The optical stack has a |Δb of less than 0.60 * |, in, The |Δb * | is the chromaticity difference Δb determined by the following evaluation method * The absolute value of <Evaluation Method> (1) The optical laminate is cut into a rectangle of 220 mm×110 mm with the absorption axis of the polarizing film as the long side, and a glass plate is laminated so that the adhesive sheet is sandwiched together with the polarizing film to form a test sample; (2) placing the formed test sample on a surface light source, irradiating the entire test sample with white light having a luminosity of 15,000 candela through the surface light source, and simultaneously conducting a heating test at 95° C. and for 500 hours; (3) The test sample after the heating test was irradiated with white light of 15000 candela through the surface light source, and the L values of the transmitted light of the white light at the center and the end of the test sample were measured. * a * b * Chroma b in color system * 0 and b * 1 , and according to the formula: Δb * =b * 1 -b * 0 Find the Δb * .
2. The optical layered body according to claim 1, in, The adhesive sheet has 9×10 11 Surface resistivity below Ω / □.
3. The optical layered body according to claim 1, in, The PSA sheet is a sheet formed from a PSA composition containing a (meth)acrylic polymer as a main component.
4. The optical layered body according to claim 3, in, The (meth)acrylic polymer has a structural unit derived from a hydroxyl group-containing monomer at a content of 1% by weight or less.
5. The optical layered body according to claim 3, in, The (meth)acrylic polymer has a structural unit derived from a carboxyl group-containing monomer at a content of 3% by weight or more.
6. The optical layered body according to claim 1, in, The adhesive sheet is a sheet formed of an adhesive composition including an isocyanate-based cross-linking agent.
7. The optical layered body according to claim 6, in, The isocyanate cross-linking agent is a non-aromatic ring type.
8. The optical layered body according to claim 6, in, The adhesive composition further includes a peroxide-based crosslinking agent. 9 . An image display panel comprising the optical layered body according to claim 1 . 10 . An image display device comprising the image display panel according to claim 9 .
11. The image display device according to claim 10, further comprising a lighting system including a backlight. The luminous intensity of the backlight irradiating the image display panel is 15000 candela or more.